Lithium secondary battery
The introduction of a lithium transition metal oxide with stabilized crystalline phase in lithium secondary batteries addresses the issues of gas generation and capacity loss, improving safety and performance by suppressing side reactions and stabilizing the crystalline structure.
Patent Information
- Application Number
- JP2023544139
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-08-04
- Filing Date
- 2022-07-01
- Publication Date
- 2024-10-07
- Estimated Expiration
- 2042-07-01
AI Technical Summary
Lithium secondary batteries using metal or metal oxide-based negative electrode active materials face challenges such as large volume changes during charging and discharging, irreversible reactions, and gas generation due to side reactions at the positive electrode, which affect capacity and safety.
Incorporation of a lithium transition metal oxide, represented by Li6Co1-x-yZnxCyO4, where x and y are within specific ranges, to stabilize the crystalline phase and minimize side reactions with the electrolyte, thereby suppressing gas generation and improving battery performance.
The lithium transition metal oxide stabilizes the crystalline phase, reducing gas generation and enhancing the safety and lifespan of lithium secondary batteries by minimizing irreversible capacity loss and maintaining electrical conductivity.
Smart Images

Figure 0007562219000001 
Figure 0007562219000002 
Figure 0007562219000003
Abstract
Description
[Technical field]
[0001] [CROSS REFERENCE TO RELATED APPLICATIONS] This application claims the benefit of priority based on Korean Patent Application No. 10-2021-0102551 dated August 4, 2021, and all contents disclosed in the documents of that Korean patent application are incorporated herein by reference.
[0002] The present invention relates to a lithium secondary battery. [Background technology]
[0003] 2. Description of the Related Art As electronic devices become more multifunctional and consume more power, many attempts have been made to increase the capacity of lithium secondary batteries and improve their charge / discharge efficiency.
[0004] As an example, a technology has been proposed in which a positive electrode active material containing 80% or more Ni is used as the positive electrode material for the positive electrode of a lithium secondary battery, and a metal or metal-based negative electrode active material such as SiO, Si or SiC is used as the negative electrode together with a carbon-based negative electrode active material such as natural graphite or artificial graphite.
[0005] Metal and metal oxide-based anode active materials enable higher capacity than carbon-based anode active materials. However, since the volume change of metal and metal oxide-based anode active materials during charging and discharging is much larger than that of graphite, it is difficult to increase the metal and metal oxide content in the anode to more than 15%. In addition, when metal and metal oxide are added to the anode, irreversible reactions occur during initial charging and discharging, resulting in greater lithium loss than when carbon-based anode active materials are used. Therefore, when metal and metal oxide-based anode active materials are used, the amount of lithium lost increases as the capacity of the battery increases, and the amount of initial capacity decrease also increases accordingly.
[0006] Therefore, various methods have been researched to increase the capacity of lithium secondary batteries or reduce the irreversible capacity, one of which is prelithiation, which is a concept of replenishing lithium within the battery that is consumed during the formation of the solid electrolyte interphase layer (SEI) in the initial state.
[0007] Various methods have been proposed for prelithiation in batteries.
[0008] One example is a method of electrochemically lithiating the negative electrode before the battery is operated. However, the lithiated negative electrode is very unstable in air, and it is difficult to scale up the process using the electrochemical lithiating method.
[0009] Another example is a battery that uses lithium metal or lithium silicide (Li x However, since the powder is highly reactive and has poor atmospheric stability, it is difficult to establish suitable solvents and process conditions for coating the negative electrode.
[0010] One method of pre-lithiating the positive electrode is to coat the positive electrode with an amount of positive electrode material equal to the amount of lithium consumed in the negative electrode. However, since the amount of positive electrode material added increases due to the low capacity of the positive electrode material itself, the energy density and capacity per weight of the final battery are reduced by the amount of the increased positive electrode material.
[0011] Therefore, a material suitable for battery spare lithiation in the positive electrode must have the irreversible property of releasing at least twice as much lithium as existing positive electrode materials during the first charge, and then not reacting with lithium during discharge. An additive that meets these conditions is called a sacrificial positive electrode material.
[0012] In the case of commercial batteries, the electrolyte is injected into the case containing the stacked cathode, separator, and anode, and then the battery first goes through a formation process to perform charge / discharge operations. During this process, a reaction occurs to form an SEI layer on the anode, and gas is generated due to the decomposition of the electrolyte. During the formation process, the sacrificial cathode material releases lithium and reacts with the electrolyte while being decomposed, and gases such as N2, O2, and CO2 generated during this process are collected through a gas pocket removal process.
[0013] As the sacrificial positive electrode material, an over-lithiated positive electrode material made of a lithium-rich metal oxide is widely used. As the over-lithiated positive electrode material, Li6CoO4, Li5FeO4, and Li6MnO4, which have an anti-fluorite structure, are well known. The theoretical capacity of these materials is 977mAh / g for Li6CoO4, 867mAh / g for Li5FeO4, and 1001mAh / g for Li6MnO4, which are sufficient for use as a sacrificial positive electrode material. Among them, Li6CoO4 has the best electrical conductivity and good electrochemical properties for use as a sacrificial positive electrode material.
[0014] During the formation process, Li6CoO4 is gradually released and decomposed, causing the crystal phase to collapse, and O2 gas is inevitably generated during this process. Ideally, Li6CoO4 should not generate additional gas during the charge / discharge cycle after the formation process. If gas is continuously generated during charging and discharging, the pressure inside the battery increases, the distance between the electrodes increases, and the battery capacity and energy density decrease. In severe cases, the battery may burst due to being unable to withstand the pressure, resulting in an explosion.
[0015] Therefore, there is a need to develop a technology that can inactivate or stabilize the final crystalline phase of Li6CoO4 so that it is electrochemically inactive so that no additional gas is generated during charge-discharge cycling. Summary of the Invention [Problem to be solved by the invention]
[0016] The present invention provides a lithium secondary battery containing a lithium transition metal oxide capable of suppressing side reactions with an electrolyte and mitigating gas generation at the positive electrode. [Means for solving the problem]
[0017] Hereinafter, a lithium secondary battery according to an embodiment of the present invention will be described in more detail.
[0018] The terms and words used in this specification and the claims should not be interpreted as being limited to their ordinary or dictionary meanings, but should be interpreted as having meanings and concepts that correspond to the technical idea of the present invention, based on the principle that the inventor can appropriately define the concept of the term in order to best describe his / her invention.
[0019] Unless otherwise defined herein, all technical and scientific terms have the same meaning as commonly understood by a person of ordinary skill in the art to which the present invention belongs. The terms used in the description of the present invention are merely for the purpose of effectively describing a specific embodiment and are not intended to limit the present invention.
[0020] As used herein, the singular forms "a," "an," and "the" include the plural forms as well, unless the context clearly indicates to the contrary.
[0021] As used herein, the meaning of "comprising" is to embody certain properties, regions, integers, steps, operations, elements, components and / or components, and does not exclude the presence or addition of other certain properties, regions, integers, steps, operations, elements, components and / or groups.
[0022] Since the present invention can be modified in various ways and can have various forms, a specific embodiment will be exemplified and described in detail below. However, it should be understood that this is not intended to limit the present invention to the specific disclosed form, but rather to include all modifications, equivalents, or alternatives falling within the spirit and technical scope of the present invention.
[0023] In this specification, when the positional relationship of two parts is described, for example, "on," "at the top," "below," "to the side," etc., one or more other parts may be located between the two parts, unless the words "immediately" or "directly" are used.
[0024] In this specification, when a temporal context is described, for example, "after," "following," "next to," or "before," it may also include cases where the context is not consecutive, unless the words "immediately" or "directly" are used.
[0025] As used herein, the term "at least one" should be understood to include all possible combinations of one or more of the associated items.
[0026] The term "cathode additive" as used herein refers to a material that has an irreversible property of releasing at least twice as much lithium as conventional cathode materials during initial charging of a battery, and not reacting with lithium during subsequent discharge. The cathode additive may also be called a sacrificial positive electrode material. The cathode additive compensates for lithium loss, thereby recovering the lost capacity of the battery and increasing the capacity of the battery, and inhibits gas generation to prevent the battery from exploding, thereby improving the life characteristics and safety of the battery.
[0027] The term "stabilization of the crystal phase" as used herein means suppressing the oxidative property of amorphous CoO2 that occurs after initial charging of a lithium secondary battery containing a lithium cobalt oxide-based positive electrode additive containing a different element. By suppressing the oxidative property of amorphous CoO2, side reactions between CoO2 and the electrolyte can be prevented, thereby suppressing gas generation.
[0028] According to one embodiment of the present invention, a positive electrode including a positive electrode material layer including a positive electrode active material, a positive electrode additive, a conductive material, and a binder; a negative electrode including a negative electrode material layer including a negative electrode active material, a conductive material, and a binder; A separation membrane; an electrolyte; The positive electrode additive includes a lithium transition metal oxide represented by the following formula 1, [Chemical formula 1] Li6Co 1-x-y Zinc x M y O4 In the above Chemical Formula 1, M is a Group 2 element, a Group 13 element, a Group 14 element, a Period 5 transition metal, or a Period 6 transition metal; x is between 0.01 and 0.7; y is between 0.01 and 0.2; 0.05≦(x+y)≦0.80.
[0029] As a result of the inventors' continued research, it has been confirmed that a lithium transition metal oxide having two or more different elements satisfying the composition of Chemical Formula 1 can minimize side reactions with an electrolyte, suppress gas generation at the positive electrode during charging and discharging of a lithium secondary battery, and ensure excellent battery performance. This is expected because the lithium transition metal oxide having two or more different elements satisfying the composition maintains a more stable crystal phase and minimizes the decrease in initial charge capacity. Therefore, the lithium transition metal oxide can improve the safety and life characteristics of a lithium secondary battery.
[0030] The lithium transition metal oxide contains two or more different elements satisfying the above composition, and thus the crystal phase can be stabilized compared to lithium cobalt oxides such as Li6CoO4. In the present invention, the stabilization of the crystal phase means suppressing the oxidation of amorphous CoO2 formed after the initial charge of a lithium secondary battery containing the lithium cobalt oxide.
[0031] In relation to this, when a lithium secondary battery containing Li6CoO4 is fully charged and the crystalline phase of the electrode is examined by X-ray diffraction (XRD), it shows a tendency to lack amorphous patterns. 2+ The cation is Co 4+ is oxidized to a cation, then O 2- Gas is generated by the oxidation of anions. When charging is completed, CoO2 (Co 4+ ) but since this composition does not exhibit crystallinity, no pattern is observed.
[0032] Co 4+ In the case of cations, either left as is or during discharge (reduction reaction), Co 2+ Cations and Co 3+ Because of its strong oxidizing tendency to reduce to cations, it oxidizes the surrounding electrolyte and causes side reactions. The side reactions cause electrolytes such as carbonates to decompose, generating gases such as CO2, CO, and H2. When the charge-discharge cycle is then performed, the Co that was reduced during charging 2+ Cations and Co 3+ The cation is Co 4+ It is oxidized to a positive ion and re-oxidized to Co during discharge. 4+ The cation is Co 2+ Cations and Co 3+ It is reduced to a cation, and the side reaction causes continuous gas generation.
[0033] In order to suppress such side reactions, Co 4+It is necessary to suppress the oxidizing tendency of the cations to reduce. For example, by introducing a different element, Co 4+ One method is to stabilize the oxidation number of a cation.
[0034] In the lithium transition metal oxide, a different element having a fixed oxidation number during charging and discharging of the battery is introduced, whereby Co 4+ It is expected to have the effect of lowering the average oxidation number of the cation. 4+ The oxidizing property of the cations is suppressed, and the generation of gas due to the side reaction is suppressed.
[0035] However, as the amount of a different element having a fixed oxidation number increases during charging and discharging of the battery, the initial charge capacity may relatively decrease and the electrical conductivity may tend to decrease. Therefore, by introducing zinc (Zn), a fourth period transition metal, as the main element of the different element and introducing a subelement (M) that can complement the electrochemical properties of the main element, it is possible to achieve a stabilizing effect of the crystal phase and ensure excellent battery performance.
[0036] The lithium transition metal oxide has a composition in which two or more different elements are introduced into Li6CoO4 by alloying or doping.
[0037] Here, the term "alloy" refers to a lithium transition metal oxide in which 10 mol % or more of the different element is introduced based on all metal elements excluding lithium, and the term "doping" refers to a lithium transition metal oxide in which less than 10 mol % of the different element is introduced based on all metal elements excluding lithium.
[0038] The lithium transition metal compound contains zinc (Zn), which is a fourth period transition metal, as a main element among the different elements.
[0039] The lithium transition metal compound contains one or more elements selected from the group consisting of Group 2 elements, Group 13 elements, Group 14 elements, fifth period transition metals, and sixth period transition metals as secondary elements in the different elements.
[0040] Specifically, the Group 2 elements include one or more selected from the group consisting of Mg, Ca, Sr, and Ba; the Group 13 elements include one or more selected from the group consisting of Al, Ga, and In; the Group 14 elements include one or more selected from the group consisting of Si, Ge, and Sn; the fifth period transition metals include one or more selected from the group consisting of Y, Zr, Nb, Mo, Tc, Ru, Rh, Pd, Ag, and Cd; and the sixth period transition metals include one or more selected from the group consisting of Lu, Hf, Ta, W, Re, Os, Ir, Pt, and Au.
[0041] Preferably, in terms of ease of alloying or doping with lithium cobalt oxide and stabilization of the crystal phase, the main element in the different elements may be Zn, which is a fourth period transition metal, and the sub-elements may be one or more elements selected from the group consisting of Al, Mg, Ti, Zr, Nb, and W.
[0042] Zn, Al, Mg, Ti, Zr, Nb, and W are well substituted for the Co site in the anti-fluorite lattice structure, which is the crystalline phase of Li6CoO4, and have the property that their own oxidation number does not change. For example, Zn exists in the Li6ZnO4 crystalline phase and easily forms an alloy with Li6CoO4, and its oxidation number remains unchanged at 2+. 4+ The oxidizing properties of the cations can be effectively suppressed.
[0043] The foreign element is selected in consideration of whether it is present in the anti-fluorite lattice structure of the lithium cobalt oxide and whether it has a fixed oxidation number during charging and discharging of the battery.
[0044] For example, Zn in the fourth period transition metal has a Li6ZnO4 crystal phase and easily forms an alloy with Li6CoO4. The oxidation number of Zn remains constant at 2+. 4+ The oxidizing properties of the cations can be effectively suppressed.
[0045] As another example, in the case of Li5FeO4 and Li6MnO4, which do not satisfy the above composition, an anti-fluorite lattice structure can be formed. However, Mn has multiple oxidation numbers of 2+, 3+, 4+, and 7+, and Fe has multiple oxidation numbers of 2+ and 3+. Therefore, when the raw materials of the lithium cobalt oxide, such as CoO, MnO, and Fe2O3, are mixed and sintered, Mn or Fe is oxidized and Co 2+ The cations are reduced to form a single crystal phase with no anti-fluorite lattice structure. 0 Even if a single-crystal phase alloyed Li6CoO4 is produced, the oxidation number of Mn or Fe can easily change within the operating voltage, so the Co after the initial charge is 4+ The oxidizing properties of cations are difficult to suppress.
[0046] In the lithium transition metal oxide, the different element is contained in an amount of 5 mol % to 80 mol % based on the total metal elements excluding lithium.
[0047] In order to achieve the stabilization effect of the crystal phase, the content of the different elements is preferably 5 mol% or more based on the total metal elements excluding lithium. However, if an excessive amount of different elements is introduced, the electrical conductivity of the lithium transition metal oxide decreases, the resistance of the electrode increases, and the performance of the battery deteriorates. Therefore, the content of the different elements is preferably 80 mol% or less based on the total metal elements excluding lithium.
[0048] Specifically, the content of the different elements may be 5 mol% or more, alternatively 10 mol% or more, alternatively 15 mol% or more, based on the total amount of metal elements excluding lithium; and 80 mol% or less, alternatively 70 mol% or less, alternatively 60 mol% or less.
[0049] Preferably, the content of the different elements may be 10 mol % to 80 mol %, alternatively 10 mol % to 70 mol %, alternatively 15 mol % to 70 mol %, alternatively 15 mol % to 60 mol %, based on the total metal elements excluding lithium.
[0050] Furthermore, the content ratio of the main element and the sub-element is determined within the range of the content of the different element.
[0051] As an example, zinc (Zn), which is a fourth period transition metal among the different elements, is contained in the lithium transition metal oxide in an amount of 1 mol % to 70 mol % based on the total metal elements excluding lithium.
[0052] In order to achieve the stabilization effect of the crystal phase, the content of zinc (Zn) in the lithium transition metal oxide is preferably 1 mol % or more based on the total metal elements excluding lithium. However, if an excessive amount of a different element is introduced, the electrical conductivity of the lithium transition metal oxide decreases, the resistance of the electrode increases, and the performance of the battery deteriorates. Therefore, the content of zinc (Zn) in the lithium transition metal oxide is preferably 70 mol % or less based on the total metal elements excluding lithium.
[0053] Specifically, the zinc (Zn) content in the lithium transition metal oxide may be 1 mol% or more, alternatively 5 mol% or more, alternatively 10 mol% or more, alternatively 15 mol% or more, alternatively 20 mol% or more, based on the total amount of metal elements excluding lithium; and 70 mol% or less, alternatively 60 mol% or less, alternatively 50 mol% or less, alternatively 40 mol% or less, or alternatively 30 mol% or less.
[0054] Preferably, the content of zinc (Zn) in the lithium transition metal oxide can be 1 mol% to 70 mol%, alternatively 5 mol% to 70 mol%, alternatively 10 mol% to 70 mol%, alternatively 10 mol% to 60 mol%, alternatively 15 mol% to 60 mol%, alternatively 15 mol% to 50 mol%, alternatively 20 mol% to 50 mol%, alternatively 20 mol% to 40 mol%, or alternatively 20 mol% to 30 mol% based on all metal elements excluding lithium.
[0055] The stabilization effect of the crystalline phase of the lithium transition metal oxide is expected to be proportional to the content of the foreign element, but as the amount of electrochemically inactive foreign element such as Zn increases, the initial charge capacity may relatively decrease and the electrical conductivity may tend to decrease.
[0056] Therefore, the content of the sub-element in the different elements is preferably 1 mol % or more based on the total metal elements excluding lithium.
[0057] However, if an excessive amount of a different element is introduced, the electrical conductivity of the lithium transition metal oxide decreases, the resistance of the electrode increases, and the performance of the battery deteriorates. Therefore, the content of the sub-element in the lithium transition metal oxide is preferably 20 mol % or less based on the total metal elements excluding lithium.
[0058] Specifically, the content of the minor element in the lithium transition metal oxide may be 1 mol % or more, alternatively 2 mol % or more, alternatively 3 mol % or more; and 20 mol % or less, alternatively 17 mol % or less, alternatively 15 mol % or less, based on the total metal elements excluding lithium.
[0059] Preferably, the content of the subelement in the lithium transition metal oxide may be 1 mol % to 20 mol %, alternatively 2 mol % to 20 mol %, alternatively 2 mol % to 17 mol %, alternatively 3 mol % to 17 mol %, or alternatively 3 mol % to 15 mol %, based on the total metal elements excluding lithium.
[0060] The lithium transition metal oxide is represented by the following formula 1: [Chemical formula 1] Li6Co 1-x-y Zinc x M y O4 In the above Chemical Formula 1, M is a Group 2 element, a Group 13 element, a Group 14 element, a Period 5 transition metal, or a Period 6 transition metal; x is between 0.01 and 0.7; y is between 0.01 and 0.2; 0.05≦(x+y)≦0.80.
[0061] Preferably, the group 2 elements include one or more selected from the group consisting of Mg, Ca, Sr, and Ba; the group 13 elements include one or more selected from the group consisting of Al, Ga, and In; the group 14 elements include one or more selected from the group consisting of Si, Ge, and Sn; the fifth period transition metals include one or more selected from the group consisting of Y, Zr, Nb, Mo, Tc, Ru, Rh, Pd, Ag, and Cd; and the sixth period transition metals include one or more selected from the group consisting of Lu, Hf, Ta, W, Re, Os, Ir, Pt, and Au.
[0062] Preferably, in the above Chemical Formula 1, M may be one or more elements selected from the group consisting of Al, Mg, Ti, Zr, Nb, and W.
[0063] In the above Chemical Formula 1, x may be 0.01 or more, alternatively 0.05 or more, alternatively 0.1 or more, alternatively 0.15 or more, alternatively 0.2 or more; and 0.7 or less, alternatively 0.5 or less, alternatively 0.3 or less. Preferably, x may be 0.01 to 0.7, alternatively 0.05 to 0.7, alternatively 0.1 to 0.7, alternatively 0.15 to 0.7, alternatively 0.15 to 0.5, alternatively 0.2 to 0.5, alternatively 0.2 to 0.3.
[0064] In the above Chemical Formula 1, y may be 0.01 or more, alternatively 0.02 or more, alternatively 0.03 or more; and 0.2 or less, alternatively 0.17 or less, alternatively 0.15 or less. Preferably, y is 0.01 to 0.2, alternatively 0.02 to 0.2, alternatively 0.02 to 0.17, alternatively 0.03 to 0.17, alternatively 0.03 to 0.15.
[0065] In the above Chemical Formula 1, the value of x+y is preferably 0.05 or more, alternatively 0.10 or more, alternatively 0.15 or more, alternatively 0.20 or more; and 0.80 or less, alternatively 0.70 or less, alternatively 0.60 or less, or alternatively 0.50 or less.
[0066] That is, in order to exhibit the effect of stabilizing the crystal phase of the lithium transition metal oxide, the value of x+y in the formula 1 is preferably 0.05 or more, or 0.10 or more, or 0.15 or more, or 0.20 or more. However, if the value of x+y is too large, the electrical conductivity of the lithium transition metal oxide may decrease, resulting in a decrease in battery performance. Therefore, the value of x+y in the formula 1 is preferably 0.80 or less, or 0.70 or less, or 0.60 or less, or 0.50 or less.
[0067] Specifically, in Chemical Formula 1, the value of x+y can be 0.05 to 0.80, alternatively 0.10 to 0.80, alternatively 0.15 to 0.80, alternatively 0.15 to 0.70, alternatively 0.15 to 0.60, alternatively 0.20 to 0.60, alternatively 0.20 to 0.50.
[0068] Preferably, the lithium transition metal oxide is Li6Co 0.77 Zinc 0.2 Al 0.03 O4, Li6Co 0.76 Zinc 0.2 Al 0.04 O4, Li6Co 0.75 Zinc 0.2 Al 0.05 O4, Li6Co 0.7 Zinc 0.25 Al 0.03 O4, Li6Co0.7 Zn 0.25 Al 0.05 O4、Li6Co 0.65 Zn 0.25 Al 0.1 O4、Li6Co 0.67 Zn 0.3 Al 0.03 O4、Li6Co 0.66 Zn 0.3 Al 0.04 O4、Li6Co 0.65 Zn 0.3 Al 0.05 O4、Li6Co 0.6 Zn 0.3 Al 0.1 O4、Li6Co 0.77 Zn 0.2 Mg 0.03 O4、Li6Co 0.76 Zn 0.2 Mg 0.04 O4、Li6Co 0.75 Zn 0.2 Mg 0.05 O4、Li6Co 0.72 Zn 0.25 Mg 0.03 O4、Li6Co 0.7 Zn 0.25 Mg 0.05 O4、Li6Co 0.65 Zn 0.25 Mg 0.1 O4、Li6Co 0.67 Zn 0.3 Mg 0.03 O4、Li6Co 0.66 Zn 0.3 Mg 0.04 O4、Li6Co 0.65 Zn 0.3 Mg 0.1 O4、Li6Co 0.77 Zn 0.25 Ti 0.03 O4、Li6Co 0.67 Zn 0.2 Ti 0.04 O4、Li6Co 0.76 Zn 0.2 Ti 0.05 O4、Li6Co 0.72 Zn 0.25 Ti 0.03 O4、Li6Co 0.7 Zn 0.25 Ti0.05 O4、Li6Co 0.65 Zn 0.25 You 0.1 O4、Li6Co 0.67 Zn 0.3 You 0.03 O4、Li6Co 0.66 Zn 0.3 You 0.04 O4、Li6Co 0.65 Zn 0.3 You 0.05 O4、Li6Co 0.6 Zn 0.3 You 0.1 O4、Li6Co 0.77 Zn 0.2 Zr 0.04 O4、Li6Co 0.75 Zn 0.2 Zr 0.05 O4、Li6Co 0.72 Zn 0.25 Zr 0.03 O4、Li6Co 0.7 Zn 0.25 Zr 0.05 O4、Li6Co 0.65 Zn 0.25 Zr 0.1 O4、Li6Co 0.67 Zn 0.3 Zr 0.03 O4、Li6Co 0.66 Zn 0.3 Zr 0.04 O4、Li6Co 0.65 Zn 0.3 Zr 0.05 O4、Li6Co 0.6 Zn 0.3 Zr 0.1 O4、Li6Co 0.77 Zn 0.2 Nb 0.03 O4、Li6Co 0.76 Zn 0.2 Nb 0.04 O4、Li6Co 0.75 Zn 0.2 Nb 0.05 O4、Li6Co 0.72 Zn 0.25 Nb 0.03 O4、Li6Co 0.7 Zn 0.25 Nb 0.05 O4、Li6Co 0.65Zinc 0.25 Nb 0.1 O4, Li6Co 0.67 Zinc 0.3 Nb 0.03 O4, Li6Co 0.66 Zinc 0.3 Nb 0.04 O4, Li6Co 0.65 Zinc 0.3 Nb 0.05 O4, Li6Co 0.6 Zinc 0.3 Nb 0.1 O4, Li6Co 0.77 Zinc 0.2 W 0.03 O4, Li6Co 0.76 Zinc 0.2 W 0.04 O4, Li6Co 0.75 Zinc 0.2 W 0.05 O4, Li6Co 0.72 Zinc 0.25 W 0.03 O4, Li6Co 0.7 Zinc 0.25 W 0.05 O4, Li6Co 0.65 Zinc 0.25 W 0.1 O4, Li6Co 0.67 Zinc 0.3 W 0.03 O4, Li6Co 0.66 Zinc 0.3 W 0.04 O4, Li6Co 0.65 Zinc 0.3 W 0.05 O4, and Li6Co 0.6 Zinc 0.3 W 0.1 The compound may comprise one or more compounds selected from the group consisting of O4.
[0069] The lithium transition metal oxide can be produced by a method including a first step of solid-phase mixing lithium oxide, cobalt oxide, and an oxide of a different element, and a second step of firing the mixture obtained in the first step in an inert atmosphere at a temperature of 550°C to 750°C to obtain the lithium transition metal oxide.
[0070] In the first step, a raw material mixture containing lithium oxide, cobalt oxide and a different element oxide is prepared.
[0071] As the lithium oxide, any oxide containing lithium, such as Li2O, can be used without any particular limitation.
[0072] As the cobalt oxide, any oxide containing cobalt, such as CoO, can be used without any particular limitation.
[0073] The hetero element oxide may be an oxide of zinc (Zn), which is a fourth period transition metal oxide, and an oxide of at least one element selected from the group consisting of Group 2 elements, Group 13 elements, Group 14 elements, fifth period transition metals, and sixth period transition metals. As a non-limiting example, the hetero element oxide may be an oxide containing the hetero element, such as ZnO, Mg, Al2O3, TiO2, ZrO2, Nb2O2, and WO3, without any particular limitation.
[0074] The raw material mixture is prepared by solid-phase mixing of the lithium oxide, the cobalt oxide, and the different element oxide so as to satisfy the above-mentioned stoichiometric ratio.
[0075] In the second step, the raw material mixture obtained in the first step is fired at a temperature of 550° C. to 750° C. in an inert atmosphere to obtain the lithium transition metal oxide.
[0076] The second step is carried out under an inert atmosphere formed using inert gases such as Ar, N2, Ne, and He.
[0077] In the second step, the mixture obtained in the first step is preferably heated in an inert atmosphere at a temperature increase rate of 1.0° C. / min to 12.0° C. / min to reach the firing temperature.
[0078] If the heating rate is too slow, crystal seeds are formed slowly, and the crystal growth continues, resulting in excessive particle size. Therefore, the heating rate is preferably 1.0° C. / min or more. However, if the heating rate is too fast, crystal seeds are generated in large quantities at a very fast rate, resulting in a relatively insufficient particle growth time, resulting in relatively low crystallinity and relatively small particle size. Therefore, the heating rate is preferably 12.0° C. / min or less.
[0079] Specifically, the heating rate may be 1.0° C. / min or more, alternatively 1.3° C. / min or more, alternatively 1.40° C. / min or more, alternatively 1.45° C. / min or more, alternatively 1.50° C. / min or more; and 12.0° C. / min or less, alternatively 10.0° C. / min or less, alternatively 6.0° C. / min or less, alternatively 4.0° C. / min or less, alternatively 2.00° C. / min or less, alternatively 1.95° C. / min or less, alternatively 1.90° C. / min or less. Preferably, the heating rate may be 1.0° C. / min to 12.0° C. / min, alternatively 1.3° C. / min to 12.0° C. / min, alternatively 1.3° C. / min to 10.0° C. / min, alternatively 1.4° C. / min to 10.0° C. / min, alternatively 1.4° C. / min to 6.0° C. / min, alternatively 1.45° C. / min to 6.0° C. / min, alternatively 1.45° C. / min to 4.0° C. / min, alternatively 1.5° C. / min to 4.0° C. / min, alternatively 1.5° C. / min to 2.0° C. / min, alternatively 1.45° C. / min to 2.0° C. / min, alternatively 1.45° C. / min to 1.95° C. / min, alternatively 1.50° C. / min to 1.95° C. / min, alternatively 1.50° C. / min to 1.90° C. / min.
[0080] The firing is carried out at a temperature of 550°C to 750°C.
[0081] In order to generate crystal seeds at an appropriate rate, the firing temperature is preferably 550°C or higher. However, if the firing temperature is too high, a sintering phenomenon occurs in which the grown crystal particles solidify together. Therefore, the firing temperature is preferably 750°C or lower.
[0082] Specifically, the firing temperature may be 550° C. or more, alternatively 580° C. or more, alternatively 600° C. or more; and 750° C. or less, alternatively 720° C. or less, alternatively 700° C. or less. Preferably, the firing temperature may be 580° C. to 750° C., alternatively 580° C. to 720° C., alternatively 600° C. to 720° C., alternatively 600° C. to 700° C.
[0083] The calcination is carried out for 2 to 20 hours at the calcination temperature. The calcination time can be adjusted in consideration of the time it takes for the crystals to be stabilized after the different element is introduced into the lithium cobalt oxide in the form of an alloy or doping. Specifically, the calcination time can be 2 hours or more, or 3 hours or more, or 4 hours or more; and 20 hours or less, or 19 hours or less, or 18 hours or less. Preferably, the calcination time can be 3 hours to 20 hours, or 3 hours to 19 hours, or 4 hours to 19 hours, or 4 hours to 18 hours.
[0084] The lithium transition metal oxide obtained in the second step has a cumulative 50% particle size (D50) of 1 μm to 30 μm as measured by a laser diffraction scattering particle size distribution measurement. If necessary, a step of pulverizing and classifying the lithium transition metal oxide may be performed so that the lithium transition metal oxide falls within the above D50 value range.
[0085] In order to prevent a side reaction with the electrolyte from worsening due to a very large specific surface area, the D50 value is preferably 1 μm or more. However, if the particle size is too large, it is difficult to uniformly coat the cathode material containing the lithium transition metal oxide on the current collector, and the current collector may be damaged during the rolling process after drying. Therefore, the D50 value is preferably 30 μm or less.
[0086] Specifically, the lithium transition metal oxide has a D50 value of 1 μm or more, alternatively 3 μm or more, alternatively 5 μm or more; and 30 μm or less, alternatively 27 μm or less, alternatively 25 μm or less. Preferably, the lithium transition metal oxide has a D50 value of 3 μm to 30 μm, alternatively 3 μm to 27 μm, alternatively 5 μm to 27 μm, alternatively 5 μm to 25 μm.
[0087] If necessary, the compound represented by Formula 1 obtained in the second step may be washed and dried.
[0088] As a non-limiting example, the washing step can be performed by mixing the compound of Formula 1 and a washing solution in a weight ratio of 1:2 to 1:10 and stirring the mixture. The washing solution can be distilled water, ammonia water, etc. The drying can be performed by heat treatment at a temperature of 100°C to 200°C or 100°C to 180°C for 1 hour to 10 hours.
[0089] The lithium transition metal oxide can minimize side reactions with an electrolyte and suppress gas generation at the positive electrode during charging and discharging of the lithium secondary battery. Therefore, the positive electrode additive for lithium secondary batteries containing the lithium transition metal oxide can improve the safety and life characteristics of the lithium secondary battery.
[0090] The positive electrode additive for a lithium secondary battery containing the lithium transition metal oxide has a property of irreversibly releasing lithium during charging and discharging of the lithium secondary battery, and therefore, the positive electrode additive for a lithium secondary battery can be included in the positive electrode of a lithium secondary battery and serve as a sacrificial positive electrode material for prelithiation.
[0091] Preferably, the lithium transition metal oxide of Formula 1 is included as a positive electrode additive in a positive electrode for a lithium secondary battery.
[0092] The positive electrode for the lithium secondary battery may include a positive electrode layer including a positive electrode active material, a positive electrode additive, a conductive material, and a binder. The positive electrode additive may include the lithium transition metal oxide.
[0093] Specifically, the positive electrode for a lithium secondary battery includes a positive electrode layer including a positive electrode active material, a positive electrode additive, a conductive material, and a binder; and a current collector supporting the positive electrode layer.
[0094] To increase the capacity of a battery to a higher capacity, the ratio of negative active material in the negative electrode must be increased, and this increases the amount of lithium consumed in the SEI layer. Therefore, after calculating the amount of lithium consumed in the SEI layer of the negative electrode, the amount of sacrificial positive electrode material to be applied to the positive electrode side can be calculated backwards to determine the design capacity of the battery.
[0095] According to one embodiment, the cathode additive, which is a sacrificial cathode material, is included in an amount of more than 0 wt % and not more than 15 wt % based on the total weight of the cathode material layer.
[0096] In order to compensate for the irreversible lithium consumed in the formation of the SEI layer, the content of the positive electrode additive is preferably greater than 0 wt % based on the total weight of the positive electrode material layer.
[0097] However, if the positive electrode additive is contained in excess, the content of the positive electrode active material exhibiting reversible charge / discharge capacity is reduced, the capacity of the battery is reduced, and the remaining lithium in the battery may be plated on the negative electrode, causing a short circuit of the battery or impairing safety. Therefore, the content of the positive electrode additive is preferably 15 wt % or less based on the total weight of the positive electrode material layer.
[0098] Specifically, the content of the positive electrode additive may be greater than 0 wt %, alternatively 0.5 wt % or more, alternatively 1 wt % or more, alternatively 2 wt % or more, alternatively 3 wt % or more, based on the total weight of the positive electrode material layer; and 15 wt % or less, alternatively 12 wt % or less, alternatively 10 wt % or less.
[0099] Preferably, the content of the positive electrode additive can be 0.5 wt% to 15 wt%, or 1 wt% to 15 wt%, or 1 wt% to 12 wt%, or 2 wt% to 12 wt%, or 2 wt% to 10 wt%, or 3 wt% to 10 wt% based on the total weight of the positive electrode material layer.
[0100] As the positive electrode active material, any compound applicable to a lithium secondary battery in the technical field to which the present invention pertains can be used without particular limitation.
[0101] As non-limiting examples, the positive electrode active material can be NCM (Li[Ni, Co, Mn]O2), NCMA (Li[Ni, Co, Mn, Al]O2), LiCoO2, LiNiO2, LiMnO2, LiMn2O2, LiNi 1-d Co d O2, LiCo 1-d Mn d O2, LiNi 1-d Mn d O2 (where 0 ≦ d < 1 above), Li(Ni a Co b Mn c )O4 (0 < a < 2, 0 < b < 2, 0 < c < 2, a + b + c = 2), LiMn 2-e Ni e O4, LiMn 2-e Co e O4 (where 0 < e < 2 above), LiCoPO4, and LiFePO4, etc. As the positive electrode active material, one or a mixture of two or more of the above examples can be used.
[0102] According to one embodiment, the positive electrode active material is contained in an amount of 80 wt% to 98 wt% based on the total weight of the positive electrode material layer.
[0103] Specifically, the content of the positive electrode active material can be 80 wt% or more, or 82 wt% or more, or 85 wt% or more; and 98 wt% or less, or 95 wt% or less, or 93 wt% or less, or 90 wt% or less based on the total weight of the positive electrode material layer.
[0104] Preferably, the content of the positive electrode active material may be 82% by weight to 98% by weight, alternatively 82% by weight to 95% by weight, alternatively 82% by weight to 93% by weight, alternatively 85% by weight to 93% by weight, alternatively 85% by weight to 90% by weight, based on the total weight of the positive electrode layer.
[0105] The conductive material is used to impart electrical conductivity to the electrodes.
[0106] The conductive material can be used without any particular limitation as long as it does not cause chemical changes in the battery and has electronic conductivity. Non-limiting examples of the conductive material include carbon-based materials such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, thermal black, and carbon fiber; graphite such as natural graphite and artificial graphite; metal powder or metal fiber such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive polymers such as polyphenylene derivatives. The conductive material can be one or a mixture of two or more of the above examples.
[0107] The content of the conductive material is adjusted within a range that exhibits an appropriate level of conductivity without inducing a decrease in the capacity of the battery. Preferably, the content of the conductive material may be 0.5 wt% to 10 wt%, or 1 wt% to 10 wt%, or 1 wt% to 5 wt%, based on the total weight of the positive electrode layer.
[0108] The binder is used to improve adhesion of the positive electrode material layer to the current collector.
[0109] As non-limiting examples, the binder may be polyvinylidene fluoride (PVdF), vinylidene fluoride-hexafluoropropylene copolymer (PVdF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated-EPDM, styrene-butadiene rubber (SBR), fluororubber, etc. As the binder, one or a mixture of two or more of the above examples may be used.
[0110] The content of the binder is adjusted within a range that exhibits an appropriate level of adhesiveness while not inducing a decrease in the capacity of the battery. Preferably, the content of the binder may be 0.5 wt % to 10 wt %, or 1 wt % to 10 wt %, or 1 wt % to 5 wt %, based on the total weight of the positive electrode layer.
[0111] The current collector may be made of any material that is applicable to electrodes of lithium secondary batteries in the technical field to which the present invention pertains, without any particular limitation.
[0112] Non-limiting examples of the current collector include stainless steel; aluminum; nickel; titanium; calcined carbon; or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, or the like.
[0113] Preferably, the current collector has a thickness of 3 μm to 500 μm. In order to increase the adhesive strength of the positive electrode layer, the current collector may have a fine unevenness formed on its surface. The current collector may have various forms such as a film, a sheet, a foil, a net, a porous body, a foam, a nonwoven fabric, etc.
[0114] The positive electrode for the lithium secondary battery is formed by laminating a positive electrode layer containing the positive electrode active material, the positive electrode additive, the conductive material, and the binder on the current collector.
[0115] According to another embodiment of the present invention, there is provided a lithium secondary battery including the lithium secondary battery positive electrode, a negative electrode, a separator, and an electrolyte.
[0116] The lithium secondary battery includes an electrode assembly in which a positive electrode and a negative electrode are wound with a separator interposed therebetween, and a case in which the electrode assembly is built in. The positive electrode, the negative electrode, and the separator are impregnated with an electrolyte.
[0117] The lithium secondary battery may have various shapes, such as a square shape, a cylindrical shape, a pouch shape, and the like.
[0118] The negative electrode may include a negative electrode material layer including an active negative electrode material, a conductive material, and a binder; and a current collector supporting the negative electrode material.
[0119] The negative electrode active material may include a material capable of reversibly intercalating and deintercalating lithium ions, lithium metal, a lithium metal alloy, a material capable of doping and dedoping lithium, and a transition metal oxide.
[0120] The material capable of reversibly intercalating and deintercalating the lithium ions may be a carbonaceous material, such as crystalline carbon, amorphous carbon, or a mixture thereof. Specifically, the carbonaceous material may be natural graphite, artificial graphite, Kish graphite, pyrolytic carbon, mesophase pitches, mesophase pitch based carbon fiber, mesocarbon microbeads, petroleum or coal tar pitch derived cokes, soft carbon, and hard carbon.
[0121] The lithium metal alloy may be an alloy of lithium with a metal selected from the group consisting of Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al, Sn, Bi, Ga, and Cd.
[0122] The material capable of doping and dedoping lithium is Si, a Si-C composite, SiO x(0 < x < 2), Si-Q alloy (where Q is an element selected from the group consisting of alkali metals, alkaline earth metals, Group 13 elements, Group 14 elements, Group 15 elements, Group 16 elements, transition metals, rare earth elements, and combinations thereof; provided that Si is excluded), Sn, SnO2, Sn-R alloy (where R is an element selected from the group consisting of alkali metals, alkaline earth metals, Group 13 elements, Group 14 elements, Group 15 elements, Group 16 elements, transition metals, rare earth elements, and combinations thereof; provided that Sn is excluded), etc. may be used. And as the substance capable of doping and undoping lithium, at least one of the above examples and SiO2 can be mixed and used. Q and R may be Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db, Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn, In, Tl, Ge, P, As, Sb, Bi, S, Se, Te, Po, etc.
[0123] And the transition metal oxide may be vanadium oxide, lithium vanadium oxide, lithium titanate, etc.
[0124] Preferably, the negative electrode contains one or more negative electrode active materials selected from the group consisting of carbonaceous substances and silicon compounds.
[0125] Specifically, the negative electrode active material is one or more carbonaceous substances selected from the group consisting of natural graphite, artificial graphite, kish graphite, pyrolytic carbon, mesophase pitch, mesophase pitch-based carbon fiber, mesocarbon microbeads, petroleum or coal-based coke, softened carbon, and hardened carbon; Si, Si-C composite, SiO x(0 < x < 2), one or more silicon compounds selected from the group consisting of the Si-Q alloy (where Q is an element selected from the group consisting of an alkali metal, an alkaline earth metal, a Group 13 element, a Group 14 element, a Group 15 element, a Group 16 element, a transition metal, a rare earth element, and combinations thereof; provided that Si is excluded); or a mixture of the carbonaceous material and the silicon compound can be included.
[0126] According to one embodiment, the negative electrode active material is contained in an amount of 85% by weight to 98% by weight based on the total weight of the negative electrode material layer.
[0127] Specifically, the content of the negative electrode active material can be 85% by weight or more, or 87% by weight or more, or 90% by weight or more; and 98% by weight or less, or 97% by weight or less, or 95% by weight or less based on the total weight of the negative electrode material layer.
[0128] Preferably, the content of the negative electrode active material can be 85% by weight to 97% by weight, or 87% by weight to 97% by weight, or 87% by weight to 95% by weight, or 90% by weight to 95% by weight based on the total weight of the negative electrode material layer.
[0129] Regarding the conductive material, the binder, and the current collector included in the negative electrode material layer, the contents described in the configuration of the positive electrode material layer are substituted.
[0130] The separator separates the positive electrode and the negative electrode and provides a migration path for lithium ions. As the separator, any material applicable to the separator of a lithium secondary battery in the technical field to which the present invention belongs can be used without particular limitation. The separator preferably has a low resistance to the ion migration of the electrolyte and excellent wettability to the electrolyte.
[0131] Specifically, the separator may be a porous polymer film made of a polyolefin polymer such as polyethylene, polypropylene, ethylene-butene copolymer, ethylene-hexene copolymer, or ethylene-methacrylate copolymer. The separator may be a multi-layer film in which two or more layers of the porous polymer film are laminated. The separator may be a nonwoven fabric containing glass fiber, polyethylene terephthalate fiber, or the like. The separator may be coated with a ceramic component or a polymer material to ensure heat resistance or mechanical strength.
[0132] Meanwhile, the electrolyte may be any electrolyte that is applicable to lithium secondary batteries in the technical field to which the present invention pertains, without any particular limitation. For example, the electrolyte may be an organic liquid electrolyte, an inorganic liquid electrolyte, a solid polymer electrolyte, a gel polymer electrolyte, a solid inorganic electrolyte, a molten inorganic electrolyte, etc.
[0133] Specifically, the electrolyte may include a non-aqueous organic solvent and a lithium salt.
[0134] The non-aqueous organic solvent may be any solvent that can act as a medium through which ions involved in the electrochemical reaction of the battery can move.
[0135] Specifically, the non-aqueous organic solvent may be an ester-based solvent such as methyl acetate, ethyl acetate, γ-butyrolactone, or ε-caprolactone; an ether-based solvent such as dibutyl ether or tetrahydrofuran; a ketone-based solvent such as cyclohexanone; an aromatic hydrocarbon-based solvent such as benzene or fluorobenzene; dimethyl carbonate (DMC), diethyl carbonate (DEC), methyl ethyl carbonate (MEC), ethyl methyl carbonate (EMC), ethylene carbonate (EC), or propylene carbonate (propylene carbonate). The solvent may be a carbonate solvent such as dimethylformamide; a dioxolane such as 1,3-dioxolane; or a sulfolane.
[0136] Among the above examples, it is preferable to use a carbonate-based solvent as the non-aqueous organic solvent.
[0137] In particular, in consideration of the charge / discharge performance of the battery and the compatibility with the sacrificial positive electrode material, it is preferable to use a mixture of a cyclic carbonate (e.g., ethylene carbonate, propylene carbonate) having high ionic conductivity and high dielectric constant and a linear carbonate (e.g., ethyl methyl carbonate, dimethyl carbonate, diethyl carbonate) having low viscosity as the nonaqueous organic solvent. In this case, it is advantageous to use a mixture of the cyclic carbonate and the linear carbonate in a volume ratio of 1:1 to 1:9 in order to exhibit the above-mentioned performance.
[0138] As the non-aqueous organic solvent, it is preferable to use a mixture of ethylene carbonate (EC) and ethyl methyl carbonate (EMC) in a volume ratio of 1:2 to 1:10; or a mixture of ethylene carbonate (EC), ethyl methyl carbonate (EMC) and dimethyl carbonate (DMC) in a volume ratio of 1-3:1 to 9:1.
[0139] The lithium salt contained in the electrolyte dissolves in the non-aqueous organic solvent and acts as a source of lithium ions in the battery to enable basic lithium secondary battery operation and to facilitate the movement of lithium ions between the positive electrode and the negative electrode.
[0140] Specifically, the lithium salt may be LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiN(SO2F)2, LiFSI (lithium bis(fluorosulfonyl)imide), LiCl, LiI, and LiB(C2O4)2, etc. Preferably, the lithium salt may be LiPF6, LiFSI, and mixtures thereof.
[0141] The lithium salt is contained in the electrolyte at a concentration of 0.1 M to 2.0 M. The lithium salt contained in the above concentration range can provide the electrolyte with appropriate conductivity and viscosity, thereby exhibiting excellent electrolyte performance.
[0142] Optionally, the electrolyte contains additives for the purposes of improving the life characteristics of the battery, suppressing the decrease in battery capacity, and improving the discharge capacity of the battery.
[0143] For example, the additive may be a haloalkylene carbonate compound such as difluoroethylene carbonate, pyridine, triethyl phosphite, triethanolamine, cyclic ether, ethylenediamine, n-glyme, hexaphosphoric acid triamide, nitrobenzene derivative, sulfur, quinoneimine dye, N-substituted oxazolidinone, N,N-substituted imidazolidine, ethylene glycol dialkyl ether, ammonium salt, pyrrole, 2-methoxyethanol, aluminum trichloride, etc. The additive is contained in an amount of 0.1% by weight to 5% by weight based on the total weight of the electrolyte.
[0144] The lithium secondary battery is used as an energy supply source with improved performance and safety in the fields of portable electronic devices such as mobile phones, laptop computers, tablet computers, mobile batteries, and digital cameras; and in the fields of transportation means such as electric cars, electric bikes, and personal mobility devices. Effect of the Invention
[0145] The lithium secondary battery according to the present invention includes a lithium transition metal oxide having a lattice structure stabilized by the introduction of a different element, thereby suppressing gas generation during charging and discharging, and exhibiting improved safety and life characteristics. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0146] The following examples are provided to specifically explain the function and effect of the present invention. However, these examples are presented as examples to help understand the invention. The following examples are not intended to limit the scope of the invention in any way, and it is obvious to those skilled in the art that various changes and modifications are possible within the scope of the present invention and the technical concept.
[0147] [Example 1] (1) Synthesis of lithium transition metal oxides A raw material mixture was prepared by solid-phase mixing of Li2O, CoO, ZnO, and MgO in a molar ratio of Li:Co:Zn:Mg=6:0.77:0.2:0.33.
[0148] The raw material mixture was heated in an Ar atmosphere at a heating rate of 1.6°C / min for 6 hours, and then sintered at 600°C for 12 hours to obtain Li6Co 0.77 Zinc 0.2 Mg 0.03 We obtained lithium transition metal oxide, O4.
[0149] The lithium transition metal oxide was crushed using a jaw crusher, and then classified using a sieve shaker.
[0150] (2) Manufacture of lithium secondary batteries The lithium transition metal oxide (Li6Co 0.77 Zinc 0.2 Mg 0.03 O4), carbon black as a conductive material, and polyvinylidene fluoride (PVdF) as a binder were mixed in an organic solvent (N-methylpyrrolidone) in a weight ratio of 95:3:2 to prepare a cathode material slurry. The cathode material slurry was applied to one side of a current collector, which was an aluminum foil with a thickness of 15 μm, and the current collector was rolled and dried to prepare a cathode. Meanwhile, in this experiment, no cathode active material was added to the cathode material. The case where a cathode active material was added is presented in Example 6 below.
[0151] Anode material slurry was prepared by mixing natural graphite as anode active material, carbon black as conductive material, and carboxymethyl cellulose (CMC) as binder in an organic solvent (N-methylpyrrolidone) in a weight ratio of 95:3:2. The anode material slurry was applied to one side of a current collector made of copper foil with a thickness of 15 μm, and then rolled and dried to prepare an anode.
[0152] A non-aqueous organic solvent was prepared by mixing ethylene carbonate (EC), ethyl methyl carbonate (EMC) and dimethyl carbonate (DMC) in a volume ratio of 3:4:3. Lithium salts, LiPF6 at a concentration of 0.7M and LiFSI at a concentration of 0.5M, were dissolved in the non-aqueous organic solvent to prepare an electrolyte.
[0153] An electrode assembly was prepared by interposing a porous polyethylene separator between the positive and negative electrodes, and the electrode assembly was placed in a case. The electrolyte was injected into the case to prepare a pouch cell type lithium secondary battery.
[0154] [Example 2] (1) Li6Co was prepared in the same manner as in Example 1, except that Al2O3 was used instead of MgO. 0.77 Zinc 0.2 Al 0.03 (1) We fabricated a lithium transition metal oxide, O4, and (2) a lithium secondary battery containing this as a positive electrode additive.
[0155] [Example 3] (1) Li6Co was prepared in the same manner as in Example 1, except that TiO2 was used instead of MgO. 0.77 Zinc 0.2 Ti 0.03 (1) We fabricated a lithium transition metal oxide, O4, and (2) a lithium secondary battery containing this as a positive electrode additive.
[0156] [Example 4] (1) Li6Co was prepared in the same manner as in Example 1, except that ZrO2 was used instead of MgO. 0.77 Zinc 0.2 Zr 0.03(1) We fabricated a lithium transition metal oxide, O4, and (2) a lithium secondary battery containing this as a positive electrode additive.
[0157] [Example 5] (1) Li6Co was prepared in the same manner as in Example 1, except that Nb2O5 was used instead of MgO. 0.77 Zinc 0.2 Nb 0.03 (1) We fabricated a lithium transition metal oxide, O4, and (2) a lithium secondary battery containing this as a positive electrode additive.
[0158] [Example 6] (1) Li6Co was prepared in the same manner as in Example 1, except that a raw material mixture in which Li2O, CoO, ZnO and Al2O3 were mixed in a solid phase in a molar ratio of Li:Co:Zn:Al=6:0.7:0.25:0.05 was used. 0.7 Zinc 0.25 Al 0.05 (1) We fabricated a lithium transition metal oxide, O4, and (2) a lithium secondary battery containing this as a positive electrode additive.
[0159] [Example 7] (1) Li6Co was prepared in the same manner as in Example 6, except that MgO was used instead of Al2O3. 0.7 Zinc 0.25 Mg 0.05 (1) We fabricated a lithium transition metal oxide, O4, and (2) a lithium secondary battery containing this as a positive electrode additive.
[0160] [Example 8] (1) Li6Co was produced in the same manner as in Example 1, except that a raw material mixture in which Li2O, CoO, ZnO and TiO2 were mixed in a solid phase in a molar ratio of Li:Co:Zn:Ti=6:0.72:0.25:0.03 was used. 0.72 Zinc 0.25 Ti 0.03 (1) We fabricated a lithium transition metal oxide, O4, and (2) a lithium secondary battery containing this as a positive electrode additive.
[0161] [Example 9] (1) Li6Co was synthesized in the same manner as in Example 8, except that ZrO2 was used instead of TiO2. 0.72 Zinc 0.25 Zr 0.03 (1) We fabricated a lithium transition metal oxide, O4, and (2) a lithium secondary battery containing this as a positive electrode additive.
[0162] [Example 10] (1) Li6Co was prepared in the same manner as in Example 1, except that a raw material mixture in which Li2O, CoO, ZnO and Al2O3 were mixed in a solid phase in a molar ratio of Li:Co:Zn:Al=6:0.65:0.3:0.05 was used. 0.65 Zinc 0.3 Al 0.05 (1) We fabricated a lithium transition metal oxide, O4, and (2) a lithium secondary battery containing this as a positive electrode additive.
[0163] [Example 11] (1) Li6Co was produced in the same manner as in Example 1, except that a raw material mixture in which Li2O, CoO, ZnO and Al2O3 were mixed in a solid phase in a molar ratio of Li:Co:Zn:Al=6:0.65:0.25:0.1 was used. 0.65 Zinc 0.25 Al 0.1 (1) We fabricated a lithium transition metal oxide, O4, and (2) a lithium secondary battery containing this as a positive electrode additive.
[0164] [Example 12] (1) Li6Co was produced in the same manner as in Example 1, except that a raw material mixture in which Li2O, CoO, ZnO and Al2O3 were mixed in a solid phase in a molar ratio of Li:Co:Zn:Al=6:0.6:0.3:0.1 was used. 0.6 Zinc 0.3 Al 0.1 (1) We fabricated a lithium transition metal oxide, O4, and (2) a lithium secondary battery containing this as a positive electrode additive.
[0165] [Example 13] A lithium secondary battery was manufactured in the same manner as in Example 6, except that a positive electrode active material was further added during the preparation of the positive electrode, and the composition of the negative electrode active material was changed during the preparation of the negative electrode.
[0166] Specifically, the positive electrode active material is a NCMA (Li[Ni, Co, Mn, Al]O2)-based compound, NTA-X12M, L&F), and the positive electrode additive is the lithium transition metal oxide (Li6Co 0.7 Zinc 0.25 Al 0.05 O4), carbon black as a conductive material, and polyvinylidene fluoride (PVdF) as a binder were mixed in an organic solvent (N-methylpyrrolidone) in a weight ratio of 93.8:1.2:3:2 to prepare a cathode material slurry. The cathode material slurry was applied to one side of a current collector, which was an aluminum foil with a thickness of 15 μm, and then rolled and dried to prepare a cathode.
[0167] A mixture of natural graphite and SiO (weight ratio = 9:1) as the negative active material, carbon black as the conductive material, and carboxymethyl cellulose (CMC) as the binder were mixed in an organic solvent (N-methylpyrrolidone) in a weight ratio of 95:3:2 to prepare a negative electrode material slurry. The negative electrode material slurry was applied to one side of a current collector made of copper foil with a thickness of 15 μm, and then rolled and dried to prepare a negative electrode.
[0168] An electrode assembly was prepared by interposing a porous polyethylene separator between the positive and negative electrodes, and the electrode assembly was placed in a case. The electrolyte was injected into the case to prepare a pouch cell type lithium secondary battery.
[0169] [Comparative Example 1] Except for the fact that ZnO and MgO were not added and that Li2O and CoO were mixed in a molar ratio of Li:Co=6:1, (1) a lithium transition metal oxide, Li6CoO4, and (2) a lithium secondary battery containing this as a positive electrode additive were produced in the same manner as in Example 1.
[0170] [Comparative Example 2] (1) Li6Co was prepared in the same manner as in Example 1, except that no MgO was added and Li2O, CoO and ZnO were mixed in a molar ratio of Li:Co:Zn=6:0.7:0.3. 0.7 Zinc 0.3(1) We fabricated a lithium transition metal oxide, O4, and (2) a lithium secondary battery containing this as a positive electrode additive.
[0171] [Comparative Example 3] (1) Li6Co was prepared in the same manner as in Example 1, except that a raw material mixture in which Li2O, CoO, ZnO and Al2O3 were mixed in a solid phase in a molar ratio of Li:Co:Zn:Al=6:0.98:0.01:0.01 was used. 0.98 Zinc 0.01 Al 0.01 (1) We fabricated a lithium transition metal oxide, O4, and (2) a lithium secondary battery containing this as a positive electrode additive.
[0172] [Comparative Example 4] (1) Li6Co was produced in the same manner as in Example 1, except that a raw material mixture in which Li2O, CoO, ZnO and Al2O3 were mixed in a solid phase in a molar ratio of Li:Co:Zn:Al=6:0.1:0.8:0.1 was used. 0.1 Zinc 0.8 Al 0.1 (1) We fabricated a lithium transition metal oxide, O4, and (2) a lithium secondary battery containing this as a positive electrode additive.
[0173] [Comparative Example 5] When manufacturing the positive electrode, Li6Co is used as the positive electrode active material. 0.7 Zinc 0.25 Al 0.05 A lithium secondary battery was manufactured in the same manner as in Example 13, except that Li6CoO4 obtained in Comparative Example 1 was used instead of O4.
[0174] [Comparative Example 6] When manufacturing the positive electrode, Li6Co is used as the positive electrode active material. 0.7 Zinc 0.25 Al 0.05 Instead of O4, Li6Co obtained in the above Comparative Example 2 0.7 Zinc 0.3 A lithium secondary battery was manufactured in the same manner as in Example 13, except that O4 was used.
[0175] [Comparative Example 7] When manufacturing the positive electrode, Li6Co is used as the positive electrode active material. 0.7 Zinc 0.25 Al 0.05 Li6Co obtained in the above Comparative Example 3 was used instead of O4. 0.98 Zinc 0.01 Al 0.01 A lithium secondary battery was manufactured in the same manner as in Example 13, except that O4 was used.
[0176] [Comparative Example 8] When manufacturing the positive electrode, Li6Co was used as the positive electrode active material. 0.7 Zinc 0.25 Al 0.05 Instead of O4, Li6Co obtained in the above Comparative Example 4 0.1 Zinc 0.8 Al 0.1 A lithium secondary battery was manufactured in the same manner as in Example 13, except that O4 was used.
[0177] [Comparative Example 9] When manufacturing the positive electrode, the positive electrode active material is NCMA (Li[Ni, Co, Mn, Al]O2)-based compound, NTA-X12M, L&F), and the positive electrode additive is the lithium transition metal oxide (Li6Co 0.7 Zinc 0.25 Al 0.05 A lithium secondary battery was manufactured in the same manner as in Example 13, except that DN20 (LiNiO, Posco Chemical) was used instead of LiNiO4, carbon black was used as a conductive material, and polyvinylidene fluoride (PVdF) was used as a binder in a weight ratio of 91.2:3.8:3:2.
[0178] [Comparative Example 10] A lithium secondary battery was manufactured in the same manner as in Example 13, except that the positive electrode additive was not added during the preparation of the positive electrode.
[0179] [Test Example 1] The amount of gas generated by the lithium secondary batteries of Examples 1 to 12 and Comparative Examples 1 and 4 was measured by the following method. The amount of gas generated by the measured cumulative charge capacity is shown in Table 1. The amount of gas generated by the high-temperature storage time is shown in Table 2.
[0180] (1) Formation (initial charge) capacity and charge / discharge capacity measurement The pouch cell type lithium secondary battery was charged at a constant current and constant voltage of 0.1 C to 4.25 V and discharged at a constant current of 2.5 V at 45° C., with a 20 minute rest between charge and discharge, and then the formation capacity and charge / discharge capacity were measured.
[0181] (2) Measurement of cumulative gas generation during charging and discharging After operating the lithium secondary battery under the charge / discharge conditions in (1) above, the pouch cell was temporarily collected in a discharged state at the time when the amount of gas generated was to be measured. Using a specific gravity meter (MATSUHAKU, TWD-150DM), the difference between the original weight of the pouch cell and its weight in water was measured, the change in the volume of the pouch cell was calculated, and the amount of gas generated per weight was calculated by dividing the amount of change in volume by the weight of the electrode active material.
[0182] (3) Measurement of cumulative gas generation rate due to high-temperature storage The pouch cell-type lithium secondary battery was charged at a constant current and constant voltage of 0.1C to 4.25V at a temperature condition of 45°C, and then collected to measure the formation capacity, and then stored in a chamber at 60°C. The lithium secondary battery was removed from the chamber at intervals of one week, and a specific gravity meter (MATSUHAKU, TWD-150DM) was used to measure the difference between the original weight of the pouch cell and its weight in water, and the change in volume within the pouch cell was calculated, and the amount of gas generated per weight was calculated by dividing the amount of change in volume by the weight of the electrode active material.
[0183] Table 1 below shows the cumulative gas generation amounts after formation (0th charge / discharge) and after the 1st, 2nd, 10th, 30th and 50th cumulative cycles.
[0184] [Table 1]
[0185] As shown in Table 1 above, Examples 1 to 5 had smaller initial charge capacities than Comparative Example 1 and Comparative Example 2. However, the cumulative gas generation amount after the 50th cycle was all within 1 mL / g in Examples 1 to 5, showing a significantly excellent gas reduction effect. In particular, Example 1 had the largest initial charge capacity among Examples 1 to 5, and the cumulative gas generation amount was also relatively small. In Example 2, although the initial charge capacity was somewhat low, it was confirmed that the cumulative gas generation amount was the lowest and that it had an excellent gas reduction effect.
[0186] In the case of Ti and Zr, the effect of additional gas reduction by adding different elements was relatively small. With reference to Examples 6, 10, 11, and 12, it was confirmed that the higher the molar content of Al, the better the effect of gas reduction.
[0187] Table 2 below shows the cumulative gas generation amounts after storage at 60° C. for 1 week, 2 weeks, 3 weeks, and 4 weeks after formation (0th charge / discharge).
[0188] [Table 2]
[0189] As shown in Table 2 above, in Examples 1 to 5, the cumulative gas generation amount during high-temperature storage at 60° C. was within 1 mL / g, and it was confirmed that the gas reduction effect was significantly superior to that of Comparative Examples 1 and 2.
[0190] With reference to Examples 6 to 12, it was confirmed that the lithium transition metal oxides incorporating Al exhibited an excellent effect in reducing gas during high-temperature storage.
[0191] [Test Example 2] For the lithium secondary batteries of Example 13 and Comparative Examples 5 to 10 in which the positive electrode active material and the positive electrode additive were mixed, the capacity retention rate and the cumulative amount of gas generated due to the cumulative charge-discharge cycles were measured by the following method, and the measured capacity retention rate and the cumulative amount of gas generated are shown in Table 3 below.
[0192] (1) Formation (initial charge) capacity and charge / discharge capacity measurement The pouch cell type lithium secondary battery was cycled at 45°C with constant current-constant voltage charging at 0.1C up to 4.25V and constant current discharging up to 2.5V, with a 20 minute rest between charging and discharging, and then the formation capacity and the charge / discharge capacity up to the 100th cycle were measured.
[0193] (2) Measurement of cumulative gas generation during charging and discharging After operating the lithium secondary battery under the charge / discharge conditions in (1) above, the pouch cell was temporarily collected in a discharged state at the time when the amount of gas generated was to be measured. Using a specific gravity meter (MATSUHAKU, TWD-150DM), the difference between the original weight of the pouch cell and its weight in water was measured, the change in the volume of the pouch cell was calculated, and the amount of gas generated per weight was calculated by dividing the amount of change in volume by the weight of the electrode active material.
[0194] (3) Measurement of cumulative gas generation rate due to high-temperature storage The pouch cell-type lithium secondary battery was charged at a constant current and constant voltage of 0.1C to 4.25V at a temperature condition of 45°C, and then collected to measure the formation capacity, and then stored in a chamber at 60°C. The lithium secondary battery was removed from the chamber at intervals of one week, and a specific gravity meter (MATSUHAKU, TWD-150DM) was used to measure the difference between the original weight of the pouch cell and its weight in water, to calculate the change in volume within the pouch cell, and the amount of gas generated per weight was calculated by dividing the amount of change in volume by the weight of the electrode active material.
[0195] Table 3 below shows the formation (0th charge / discharge) capacity, the cumulative gas generation amount after the 50th and 100th cumulative cycles, and the discharge capacity retention rate after the 100th cycle.
[0196] [Table 3]
[0197] As shown in Table 3 above, the discharge capacities of Example 13 and Comparative Examples 5 to 9 were larger than that of Comparative Example 10, which did not use a positive electrode additive (sacrificial positive electrode material). This is believed to be because the sacrificial positive electrode material compensates for the irreversible lithium consumed in the formation of the SEI layer in the negative electrode.
[0198] On the other hand, in the case of Comparative Example 10, since there was no sacrificial cathode material to compensate for irreversible lithium, the lithium of the cathode material was consumed, resulting in a decrease in discharge capacity, and the discharge capacity was 201.3 mAh / g.
[0199] The cumulative gas generation amount in the 100th cycle of Example 13 was 0.07 mL / g, which was smaller than 0.24 mL / g of Comparative Example 5 and smaller than 0.20 mL / g of Comparative Example 10 in which a sacrificial positive electrode material was not applied.
[0200] In Comparative Example 9, the cumulative gas generation amount in the 50th cycle was the smallest at 0.02 mL / g, but the increase in gas generation from the 50th cycle to the 100th cycle was 0.09 mL / g, and there is a possibility that gas generation will continue to increase thereafter. This is also true for Comparative Example 6. On the other hand, in the case of Example 13, the increase in gas generation from the 50th cycle to the 100th cycle was 0.02 mL / g, and it is considered that gas generation is suppressed as the charge / discharge cycle continues.
[0201] In Example 13, Comparative Example 5, and Comparative Example 6, in which a Co-based sacrificial cathode material was used, the capacity retention rate at the 100th cycle was 88.2% or more. In Comparative Example 9, in which a Ni-based sacrificial cathode material was used, and Comparative Example 10, in which a sacrificial cathode material was not used, the capacity retention rates were 86.3% and 86.2%, respectively, which were significantly lower than Example 13.
[0202] From this, it has been confirmed that when a Co-based sacrificial cathode material, particularly a sacrificial cathode material having the composition of Chemical Formula 1, is applied to a lithium secondary battery containing an actual cathode material, not only is the initial discharge capacity maintained and the amount of gas generation in the battery suppressed, but the capacity retention rate after the 100th cycle is also excellent.
[0203] Table 4 below shows the cumulative gas generation amounts after storage at 72° C. for 1 week, 2 weeks, 3 weeks, and 4 weeks after formation (0th charge).
[0204] [Table 4]
[0205] As shown in Table 4 above, in Example 13, the cumulative gas generation amount after 4 weeks was the smallest at 0.15 mL / g. This is believed to be because, as in the results of the charge-discharge cycle, the foreign elements introduced into Li6CoO4 effectively stabilized the CoO2 formed after the initial charge, preventing side reactions with the electrolyte and suppressing the generation of additional gas due to this.
[0206] In addition, in the case of Example 13, less gas was generated than in Comparative Example 10 in which a sacrificial cathode material was not applied. However, this is expected to be due to experimental error or the cathode additive contained in the lithium secondary battery may not only suppress gas generation but also absorb the generated gas.
[0207] Although the present invention has been described above using limited examples, the present invention is not limited thereto, and it goes without saying that various modifications and variations are possible within the technical spirit of the present invention and the equivalent scope of the claims described below by a person having ordinary skill in the art to which the present invention pertains.
Claims
1. a positive electrode including a positive electrode material layer including a positive electrode active material, a positive electrode additive, a conductive material, and a binder; a negative electrode including a negative electrode material layer including a negative electrode active material, a conductive material, and a binder; A separation membrane; an electrolyte; The positive electrode additive includes a lithium transition metal oxide represented by the following formula 1: [Chemical formula 1] Li 6 Co 1-x-y Zhn x M y O 4 In the above Chemical Formula 1, M is a Group 2 element, a Group 13 element, a Group 14 element, a Period 5 transition metal, or a Period 6 transition metal; x is 0.01 to 0.7; y is 0.01 to 0.
2. A lithium secondary battery, wherein 0.05≦(x+y)≦0.
80.
2. The Group 2 element includes one or more selected from the group consisting of Mg, Ca, Sr, and Ba, The Group 13 element includes at least one selected from the group consisting of Al, Ga, and In, The Group 14 element includes at least one selected from the group consisting of Si, Ge, and Sn, The fifth period transition metal includes at least one selected from the group consisting of Y, Zr, Nb, Mo, Tc, Ru, Rh, Pd, Ag, and Cd; 2. The lithium secondary battery according to claim 1, wherein the sixth period transition metal comprises at least one selected from the group consisting of Lu, Hf, Ta, W, Re, Os, Ir, Pt, and Au.
3. 2. The lithium secondary battery according to claim 1, wherein M is at least one selected from the group consisting of Al, Mg, Ti, Zr, Nb, and W.
4. The positive electrode additive is Li 6 Co 0.77 Zn 0.2 Al 0.03 O 4 、Li 6 Co 0.76 Zn 0.2 Al 0.04 O 4 、Li 6 Co 0.75 Zn 0.2 Al 0.05 O 4 、Li 6 Co 0.7 Zn 0.25 Al 0.03 O 4 、Li 6 Co 0.7 Zn 0.25 Al 0.05 O 4 、Li 6 Co 0.65 Zn 0.25 Al 0.1 O 4 、Li 6 Co 0.67 Zn 0.3 Al 0.03 O 4 、Li 6 Co 0.66 Zn 0.3 Al 0.04 O 4 、Li 6 Co 0.65 Zn 0.3 Al 0.05 O 4 、Li 6 Co 0.6 Zn 0.3 Al 0.1 O 4 、Li 6 Co 0.77 Zn 0.2 Mg 0.03 O 4 、Li 6 Co 0.76 Zn 0.2 Mg 0.04 O 4 、Li 6 Co 0.75 Zn 0.2 Mg 0.05 O 4 、Li 6 Co 0.72 Zn 0.25 MM 0.03 O 4 、 6 Co 0.7 Zn 0.25 MM 0.05 O 4 、 6 Co 0.65 Zn 0.25 MM 0.1 O 4 、 6 Co 0.67 Zn 0.3 MM 0.03 O 4 、 6 Co 0.66 Zn 0.3 MM 0.04 O 4 、 6 Co 0.65 Zn 0.3 MM 0.1 O 4 、 6 Co 0.77 Zn 0.25 Ti 0.03 O 4 、 6 Co 0.67 Zn 0.2 Ti 0.04 O 4 、 6 Co 0.76 Zn 0.2 Ti 0.05 O 4 、 6 Co 0.72 Zn 0.25 Ti 0.03 O 4 、 6 Co 0.7 Zn 0.25 Ti 0.05 O 4 、 6 Co 0.65 Zn 0.25 Ti 0.1 O 4 、 6 Co 0.67 Zn 0.3 Ti 0.03 O 4 、 6 Co 0.66 Zn 0.3 Ti 0.04 O 4 ,LS 6 Co 0.65 Zhn 0.3 Ti 0.05 O 4 ,LS 6 Co 0.6 Zhn 0.3 Ti 0.1 O 4 ,LS 6 Co 0.77 Zhn 0.2 Zr 0.04 O 4 ,LS 6 Co 0.75 Zhn 0.2 Zr 0.05 O 4 ,LS 6 Co 0.72 Zhn 0.25 Zr 0.03 O 4 ,LS 6 Co 0.7 Zhn 0.25 Zr 0.05 O 4 ,LS 6 Co 0.65 Zhn 0.25 Zr 0.1 O 4 ,LS 6 Co 0.67 Zhn 0.3 Zr 0.03 O 4 ,LS 6 Co 0.66 Zhn 0.3 Zr 0.04 O 4 ,LS 6 Co 0.65 Zhn 0.3 Zr 0.05 O 4 ,LS 6 Co 0.6 Zhn 0.3 Zr 0.1 O 4 ,LS 6 Co 0.77 Zhn 0.2 Nb 0.03 O 4 ,LS 6 Co 0.76 Zhn 0.2 Nb 0.04 O 4 、 6 Co 0.75 Zn 0.2 Nb 0.05 O 4 、 6 Co 0.72 Zn 0.25 Nb 0.03 O 4 、 6 Co 0.7 Zn 0.25 Nb 0.05 O 4 、 6 Co 0.65 Zn 0.25 Nb 0.1 O 4 、 6 Co 0.67 Zn 0.3 Nb 0.03 O 4 、 6 Co 0.66 Zn 0.3 Nb 0.04 O 4 、 6 Co 0.65 Zn 0.3 Nb 0.05 O 4 、 6 Co 0.6 Zn 0.3 Nb 0.1 O 4 、 6 Co 0.77 Zn 0.2 W 0.03 O 4 、 6 Co 0.76 Zn 0.2 W 0.04 O 4 、 6 Co 0.75 Zn 0.2 W 0.05 O 4 、 6 Co 0.72 Zn 0.25 W 0.03 O 4 、 6 Co 0.7 Zn 0.25 W 0.05 O 4 、 6 Co 0.65 Zinc 0.25 W 0.1 O 4 , Li 6 Co 0.67 Zinc 0.3 W 0.03 O 4 , Li 6 Co 0.66 Zinc 0.3 W 0.04 O 4 , Li 6 Co 0.65 Zinc 0.3 W 0.05 O 4 , and Li 6 Co 0.6 Zinc 0.3 W 0.1 O 4 2. The lithium secondary battery according to claim 1, comprising one or more compounds selected from the group consisting of:
5. The positive electrode layer comprises 80% by weight to 98% by weight of the positive electrode active material, more than 0% by weight and not more than 15% by weight of the positive electrode additive, 0.5% by weight to 10% by weight of the conductive material, and 0.5% by weight to 10% by weight of the binder. The lithium secondary battery according to any one of claims 1 to 4.
6. 2. The lithium secondary battery according to claim 1, wherein the conductive material comprises one or more compounds selected from the group consisting of carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, thermal black, carbon fiber, natural graphite, artificial graphite, copper powder, nickel powder, aluminum powder, silver powder, zinc oxide, potassium titanate, titanium oxide, and polyphenylene.
7. 2. The lithium secondary battery according to claim 1, wherein the binder comprises one or more compounds selected from the group consisting of polyvinylidene fluoride, vinylidene fluoride-hexafluoropropylene copolymer, polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose, starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer, sulfonated-EPDM, styrene-butadiene rubber, and fluororubber.
8. The negative electrode active material is one or more carbonaceous materials selected from the group consisting of natural graphite, artificial graphite, kish graphite, pyrolytic carbon, mesophase pitch, mesophase pitch-based carbon fibers, mesocarbon microspheres, petroleum or coal-based coke, softened carbon, and hardened carbon; Si, Si-C complex, SiO x (0<x<2), one or more silicon compounds selected from the group consisting of Si-Q alloys (wherein Q is an element selected from the group consisting of alkali metals, alkaline earth metals, Group 13 elements, Group 14 elements, Group 15 elements, Group 16 elements, transition metals, rare earth elements, and combinations thereof, excluding Si); or 2. The lithium secondary battery according to claim 1, which is a mixture of the carbonaceous material and the silicon compound.
9. 10. The lithium secondary battery of claim 1, wherein the separator is a porous polymer film comprising polyethylene, polypropylene, an ethylene-butene copolymer, an ethylene-hexene copolymer, or an ethylene-methacrylate copolymer.
10. The electrolyte is LiPF 6 , LiClO 4 , LiAsF 6 , LiBF 4 , LiSbF 6 , LiAlO 4 , LiAlCl 4 , LiCF 3 SO 3 , LiC 4 F 9 SO 3 , LiN (C 2 F 5 SO 3 ) 2 , LiN (C 2 F 5 SO 2 ) 2 , LiN(CF 3 SO 2 ) 2 , LiN(SO 2 F) 2 , LiFSI (lithium bis(fluorosulfonyl)imide), LiCl, LiI, and LiB (C 2 O 4 ) 2 2. The lithium secondary battery according to claim 1, comprising one or more lithium salts selected from the group consisting of:
Citation Information
Patent Citations
Nonaqueous electrolyte cell
JP2001351690A
Lithium ion secondary battery
JP2019061750A
Nonaqueous-electrolyte secondary battery and method for manufacturing nonaqueous-electrolyte secondary battery
WO2015115052A1