Nonaqueous electrolyte for lithium secondary battery and lithium secondary battery containing same

The non-aqueous electrolyte with specific additives forms stable films on electrodes, addressing gas generation and structural instability in lithium secondary batteries, improving high-temperature durability and cycle performance.

JP7562220B2Active Publication Date: 2024-10-07LG ENERGY SOLUTION LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023544394
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-09-21
Filing Date
2022-09-22
Publication Date
2024-10-07
Estimated Expiration
2042-09-22

AI Technical Summary

Technical Problem

Lithium secondary batteries face issues with gas generation, electrolyte decomposition, and structural instability due to high-temperature exposure and repeated charging/discharging, particularly in high-content nickel positive electrodes, leading to decreased performance and capacity retention.

Method used

A non-aqueous electrolyte for lithium secondary batteries containing a lithium salt, organic solvent, and a compound with propargyl, carbonate, and phosphite groups that form stable films on electrode surfaces, suppressing transition metal elution and side reactions.

Benefits of technology

The electrolyte enhances high-temperature durability and cycle characteristics by forming robust SEI and CEI films, reducing gas generation and resistance, and maintaining capacity and structural integrity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007562220000001
    Figure 0007562220000001
  • Figure 0007562220000002
    Figure 0007562220000002
  • Figure 0007562220000003
    Figure 0007562220000003
Patent Text Reader

Abstract

The present invention provides a non-aqueous electrolyte for a lithium secondary battery and a lithium secondary battery having improved high-temperature durability by including the non-aqueous electrolyte. Specifically, the non-aqueous electrolyte for a lithium secondary battery may include a lithium salt, a non-aqueous organic solvent, and a compound represented by Chemical Formula 1 as an additive.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application claims the benefit of priority to Korean Patent Application No. 10-2021-0127159 filed on September 27, 2021 and Korean Patent Application No. 10-2022-0119103 filed on September 21, 2022, and all contents disclosed in the documents of said Korean patent applications are incorporated as part of this specification. The present invention relates to a non-aqueous electrolyte for a lithium secondary battery and a lithium secondary battery containing the same. [Background technology]

[0002] As modern society becomes more and more dependent on electrical energy, the amount of electrical energy produced is also increasing. In particular, renewable energy power generation, which does not cause environmental problems during the production of electrical energy, is attracting attention as a next-generation power generation system. In the case of such renewable energy, since it shows intermittent power generation characteristics, a large-capacity power storage device is indispensable for a stable supply of power. In particular, in recent years, research into high-performance power storage devices that are lighter and smaller in volume has been actively conducted in order to develop electric vehicles with high specifications.

[0003] Lithium-ion batteries are currently in the spotlight as the power storage device that exhibits the highest energy density commercially available. The lithium ion battery is composed of a positive electrode made of a transition metal oxide containing lithium, a negative electrode capable of storing lithium, an electrolyte solution containing an organic solvent containing a lithium salt, and a separator.

[0004] In the case of the positive electrode, energy is stored through the oxidation-reduction reaction of the transition metal, which means that the transition metal must be an essential component of the positive electrode material.

[0005] Meanwhile, when lithium secondary batteries are exposed to high temperature environments or undergo repeated charging and discharging, oxidation and reductive decomposition of the electrolyte occurs, which induces gas generation inside the cell and deteriorates the battery performance.

[0006] In particular, in the case of a secondary battery using a high-nickel (High-Ni) positive electrode, the carbonate solvent used as the main solvent in the electrolyte is decomposed by reactive oxygen compounds formed in the positive electrode at a certain voltage or higher, generating a large amount of gas, which results in the depletion of the carbonate content and a corresponding decrease in ion conductivity, resulting in a significant deterioration of battery performance.

[0007] Furthermore, Lewis acids such as HF formed by the decomposition of electrolyte salt corrode the passive film formed at the electrode-electrolyte interface, inducing the elution of transition metals from the positive electrode and reducing the structural stability of the positive electrode. The eluted transition metals are electro-deposited on the surface of the negative electrode, promoting the decomposition of the electrolyte solvent, accelerating the generation of gas and reducing the capacity retention rate of the battery.

[0008] Therefore, in order to solve these various problems, it is necessary to develop a nonaqueous electrolyte that can form a stable coating on the surface of the electrode and suppress the electrodeposition of the eluted transition metal onto the negative electrode and ion replacement. Summary of the Invention [Problem to be solved by the invention]

[0009] The present invention has been made to solve the above problems, and has an object to provide a non-aqueous electrolyte for a lithium secondary battery that contains an additive capable of forming a stable coating on the surface of an electrode.

[0010] Another object of the present invention is to provide a lithium secondary battery having improved high-temperature durability by containing the nonaqueous electrolyte for lithium secondary batteries. [Means for solving the problem]

[0011] In order to achieve the above object, one embodiment of the present invention comprises: The present invention provides a non-aqueous electrolyte for a lithium secondary battery, comprising a lithium salt, a non-aqueous organic solvent, and a compound represented by the following chemical formula 1 as an additive:

[0012] [ka]

[0013] In the above Chemical Formula 1, R is a substituted or unsubstituted alkylene group having 1 to 5 carbon atoms.

[0014] On the other hand, another embodiment of the present invention is a negative electrode including a negative electrode active material, a positive electrode including a positive electrode active material, a separator interposed between the negative electrode and the positive electrode, and a non-aqueous electrolyte; The nonaqueous electrolyte solution for lithium secondary batteries according to the present invention is used to provide a lithium secondary battery. Effect of the Invention

[0015] The compound represented by Chemical Formula 1 contained in the non-aqueous electrolyte of the present invention contains functional groups such as propargyl and carbonate groups (-OC(=O)O-) that are easily reduced on the surface of the negative electrode, and can form a strong SEI or passivation film on the surface of the negative electrode. In addition, the compound represented by Chemical Formula 1 contains a phosphite group (-PO3) in its structure, and can form a strong cathode-electrolyte interphase (CEI) protective layer on the surface of not only the negative electrode but also the positive electrode. Therefore, it is possible to effectively prevent the transition metal from leaching out from the positive electrode, to prevent side reactions between the positive electrode and the electrolyte at high temperatures, and to reduce the deterioration of the SEI film caused by the decomposition products of the lithium salt.

[0016] In this way, by using the non-aqueous electrolyte solution of the present invention containing the compound of Chemical Formula 1, a lithium secondary battery having improved high-temperature storage characteristics and cycle characteristics can be realized. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] The present invention will now be described in more detail. The terms and words used in this specification and the claims should not be interpreted in a limited manner to their ordinary or dictionary meanings, but should be interpreted in a manner that is consistent with the technical idea of ​​the present invention, based on the principle that the inventors can appropriately define the concepts of terms in order to best describe their invention.

[0018] In general, in lithium secondary batteries, a non-aqueous electrolyte is decomposed during initial charging and discharging to form a coating having passivation ability on the surfaces of the positive and negative electrodes, thereby ensuring high-temperature storage characteristics. However, the coating can be deteriorated by Lewis acid substances such as HF and PF5, which are generated by thermal decomposition of lithium salts (such as LiPF6) widely used in lithium-ion batteries. That is, the transition metal is dissolved from the positive electrode due to the attack of the Lewis acid substance, causing the positive electrode structure to collapse, and at this time, highly reactive active oxygen compounds are generated, causing the electrolyte to decompose. Alternatively, the transition metal that has migrated to the negative electrode via the electrolyte is electrodeposited on the negative electrode, causing self-discharge of the negative electrode and destroying the solid electrolyte interphase (SEI) film that provides passivation ability to the negative electrode, promoting the decomposition reaction of the additional electrolyte and increasing the interface resistance of the negative electrode.

[0019] In the present invention, a non-aqueous electrolyte for lithium secondary batteries, which has improved SEI formation and strengthening effects by including a compound having a propargyl group (-C≡C-), a phosphite group (-PO3), and a carbonate group (-OC(=O)O-) as an additive in its molecular structure, and a lithium secondary battery including the same are provided. In particular, when a high-nickel (High-Ni)-based positive electrode active material is introduced as a positive electrode component, thermal stability may be rapidly reduced, but in the present invention, it has been confirmed that such a problem can be solved by using a non-aqueous electrolyte including a compound represented by the following chemical formula 1 as an additive.

[0020] Nonaqueous electrolyte for lithium secondary batteries Specifically, one embodiment of the present invention comprises: The present invention provides a non-aqueous electrolyte for a lithium secondary battery, comprising a lithium salt, a non-aqueous organic solvent, and a compound represented by the following chemical formula 1 as an additive:

[0021] [ka]

[0022] In the above Chemical Formula 1, R is a substituted or unsubstituted alkylene group having 1 to 5 carbon atoms.

[0023] (1) Lithium salt First, the lithium salt will be described as follows. The lithium salt may be any one that is commonly used in non-aqueous electrolytes for lithium secondary batteries without any limitations. For example, the cation may be Li + The anion is F. - , Cl - , Br - , I - , NO3 - , N(CN)2 - , BF4 - , ClO4 - , B 10 Cl 10 - , AlCl4 - , AlO4 - , PF6 - , CF3SO3 - , CH3CO2 - , CF3CO2 - , AsF6 - , SbF6 - , CH3SO3 - , (CF3CF2SO2)2N - , (CF3SO2)2N - , (FSO2)2N - , (PO2F2) - , (FSO2)(POF2)N - , BF2C2O4 - , BC4O8 - , PF4C2O4 - , PF2C4O8- , (CF3)2PF4 - , (CF3)3PF3 - , (CF3)4PF2 - , (CF3)5PF - , (CF3)6P - , C4F9SO3 - , CF3CF2SO3 - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , CF3(CF2)7SO3 - , and SCN - The composition may include at least one selected from the group consisting of:

[0024] Specifically, the lithium salt is LiCl, LiBr, LiI, LiBF4, LiClO4, LiB 10 Cl 10 , LiAlCl4, LiAlO4, LiPF6, LiCF3SO3, LiCH3CO2, LiCF3CO2, LiAsF6, LiSbF6, LiCH3SO3, LiN(SO2F)2(lithium bis(fluorosulfonyl)imide, LiFSI), LiN(SO2CF2CF3)2(lithium bis(pentafluoroethanesulfonyl)imide, LiBETI), and LiN(SO2CF3)2(lithium bis(trifluoromethanesulfonyl)imide, LiTFSI) may be included as a single substance or a mixture of two or more substances selected from the group consisting of, and in addition to the above-mentioned lithium salts, lithium salts commonly used in electrolytes for lithium secondary batteries may be used without limitation. Specifically, the lithium salt may include at least one of LiBF4, LiPF6, LiN(SO2F)2, and LiN(SO2CF3)2, and more specifically, may include LiPF6.

[0025] The lithium salt may be appropriately changed within a range that is normally usable, but in order to obtain an optimal effect of forming a coating for preventing side-corrosion on the electrode surface, it may be contained in the electrolyte at a concentration of 0.8 M to 3.0 M, specifically, at a concentration of 1.0 M to 3.0 M. When the concentration of the lithium salt satisfies the above range, the viscosity of the nonaqueous electrolyte can be controlled so as to realize optimal impregnation, and the mobility of lithium ions can be improved, thereby obtaining an effect of improving the capacity characteristics and cycle characteristics of the lithium secondary battery.

[0026] (2) Non-aqueous organic solvent The non-aqueous organic solvent is described as follows. As the non-aqueous organic solvent, various organic solvents commonly used in non-aqueous electrolytes may be used without limitation, and there is no limitation on the type of the organic solvent as long as it can minimize decomposition due to an oxidation reaction during the charge / discharge process of the secondary battery and can exhibit desired properties together with the additives.

[0027] Specifically, the non-aqueous organic solvent may include a cyclic carbonate compound, a linear carbonate compound, a linear ester compound, or a mixture thereof.

[0028] The cyclic carbonate compound is a high-viscosity compound that has a high dielectric constant and effectively dissociates lithium salt in a non-aqueous electrolyte solution. Specific examples of the cyclic carbonate compound include at least one compound selected from the group consisting of ethylene carbonate (EC), propylene carbonate (PC), 1,2-butylene carbonate, 2,3-butylene carbonate, 1,2-pentylene carbonate, 2,3-pentylene carbonate, and vinylene carbonate, and among these, ethylene carbonate may be included.

[0029] The linear carbonate compound is a compound having low viscosity and low dielectric constant, and specific examples thereof may include at least one compound selected from the group consisting of dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate, ethyl methyl carbonate (EMC), methyl propyl carbonate, and ethyl propyl carbonate, and specifically may include ethyl methyl carbonate (EMC).

[0030] In the present invention, the cyclic carbonate compound and the linear carbonate compound may be mixed and used. In this case, the mixing ratio of the cyclic carbonate compound to the linear carbonate compound may be a volume ratio of 10:90 to 80:20, specifically a volume ratio of 30:70 to 50:50.

[0031] When the mixing ratio of the cyclic carbonate compound to the linear carbonate compound is within the above range, a non-aqueous electrolyte having a higher electrical conductivity can be produced.

[0032] In addition, in the present invention, a linear ester compound may be further mixed in order to improve the shortcomings of the carbonate compound and to increase safety during high temperature and high voltage operation.

[0033] The linear ester-based compound is a compound that is relatively more stable when operated at high temperatures and high voltages than cyclic carbonate-based compounds, and can improve the disadvantage of cyclic carbonate-based compounds that cause gas generation when operated at high temperatures, while also achieving high ionic conductivity.

[0034] Specific examples of the linear ester compound include at least one selected from the group consisting of methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, and butyl propionate, and specifically, at least one of ethyl propionate and propyl propionate.

[0035] Furthermore, the non-aqueous electrolyte of the present invention may further contain a cyclic ester compound, if necessary. The cyclic ester compound may include at least one selected from the group consisting of γ-butyrolactone, γ-valerolactone, γ-caprolactone, σ-valerolactone, and ε-caprolactone.

[0036] Meanwhile, in the nonaqueous electrolyte for a lithium secondary battery of the present invention, the remaining components other than the nonaqueous organic solvent, such as the lithium salt and additives, may all be nonaqueous organic solvents, unless otherwise specified.

[0037] (3) Additives The nonaqueous electrolyte for a lithium secondary battery of the present invention may contain a compound represented by the following chemical formula 1 as an additive.

[0038] [ka]

[0039] In the above Chemical Formula 1, R is a substituted or unsubstituted alkylene group having 1 to 5 carbon atoms.

[0040] The compound represented by Chemical Formula 1 contains a propargyl group as a functional group that is easily reduced on the surface of the negative electrode, and can form an SEI film with high passivation ability on the surface of the negative electrode. This not only prevents the self-discharge reaction of the graphite-based negative electrode and / or silicon-based negative electrode caused by the additional reduction and decomposition reaction of the electrolyte, but also inhibits the electrodeposition of transition metal ions eluted from the positive electrode onto the surface of the negative electrode, thereby improving the high-temperature durability of the negative electrode itself and inhibiting internal short circuits and resistance increases.

[0041] In addition, the compound represented by Chemical Formula 1 contains a carbonate group in its molecular structure, and during reduction at the negative electrode, an electron-rich chemical substance can easily attack the carbon of the carbonate group, forming a stronger SEI on the surface of the negative electrode. In particular, the compound represented by Chemical Formula 1 of the present invention also contains a phosphite group (-PO3) in its structure, and PO3- is adsorbed to the transition metal of the positive electrode structure, forming a more stable passivation film on the surface of the positive electrode.

[0042] Specifically, in the above chemical formula 1, R may be a substituted or unsubstituted alkylene group having 1 to 3 carbon atoms. In this case, the substitution may be at least one selected from halogen, a hydroxyl group (-OH), a carboxyl group (-COOH), an alkyl group having 1 to 6 carbon atoms, an alkenyl group having 2 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, a cycloalkyl group having 3 to 8 carbon atoms, a heterocycloalkyl group having 2 to 6 carbon atoms, an aryl group having 6 to 10 carbon atoms, and a heteroaryl group having 4 to 10 carbon atoms, and specifically, may be an alkyl group having 1 to 6 carbon atoms.

[0043] In addition, in the above Chemical Formula 1, R may further include at least one of an oxygen atom, a nitrogen atom, a sulfur atom, and a phosphorus (P) atom in the structure. Specifically, the compound represented by Chemical Formula 1 may be a compound represented by Chemical Formula 1a below.

[0044] [ka]

[0045] The compound represented by Formula 1 may be included in an amount of 0.1 wt % to 5.0 wt % based on the total weight of the non-aqueous electrolyte. When the compound represented by Chemical Formula 1 is contained within the above range, it is possible to effectively remove decomposition products of the electrolyte salt while minimizing disadvantages such as side reactions due to additives, reduction in initial capacity, and increase in resistance, and to form a strong passivation film on the surface of the electrode.

[0046] That is, when the compound represented by Chemical Formula 1 is contained in an amount of 0.1 wt % or more, a stable coating is formed, while a low resistance increase rate and volume increase rate can be maintained during evaluation of the durability of the battery. Also, when the compound represented by Chemical Formula 1 is contained in an amount of 5.0 wt % or less, an increase in the viscosity of the electrolyte caused by the excess compound can be prevented, and the mobility of ions in the battery can be improved, and an increase in the battery resistance can be effectively prevented by suppressing the formation of an excessive coating, thereby preventing a decrease in capacity and cycle characteristics.

[0047] Specifically, when the compound represented by Chemical Formula 1 is contained in an amount of less than 5.0 wt %, more specifically 0.5 wt % to 4.0 wt %, and preferably 0.5 wt % to 3.0 wt %, based on the total weight of the non-aqueous electrolyte, a secondary battery with improved performance can be manufactured.

[0048] (4) Other additives In addition, the non-aqueous electrolyte of the present invention may further contain other additives to prevent the non-aqueous electrolyte from being decomposed in a high-output environment, which may lead to the collapse of the negative electrode, and to further improve low-temperature high-rate discharge characteristics, high-temperature stability, prevention of overcharging, and suppression of battery expansion at high temperatures.

[0049] Examples of such other additives include at least one selected from the group consisting of cyclic carbonate-based compounds, halogen-substituted carbonate-based compounds, sultone-based compounds, sulfate-based compounds, phosphate-based or phosphite-based compounds, borate-based compounds, benzene-based compounds, amine-based compounds, imidazole-based compounds, silane-based compounds, and lithium salt-based compounds.

[0050] Examples of the cyclic carbonate compounds include vinylene carbonate (VC) and vinyl ethylene carbonate (VEC). The halogen-substituted carbonate compounds include fluoroethylene carbonate (FEC).

[0051] The sultone compound may be, for example, at least one compound selected from the group consisting of 1,3-propane sultone (PS), 1,4-butane sultone, ethene sultone, 1,3-propene sultone (PRS), 1,4-butene sultone, and 1-methyl-1,3-propene sultone.

[0052] The sulfate compound may be, for example, ethylene sulfate (Esa), trimethylene sulfate (TMS), or methyl trimethylene sulfate (MTMS).

[0053] The phosphate or phosphite compound may be, for example, one or more compounds selected from the group consisting of lithium difluoro(bisoxalato)phosphate, lithium difluorophosphate, lithium tetrafluorooxalatophosphate, tris(trimethylsilyl)phosphate, tris(trimethylsilyl)phosphite, tris(2,2,2-trifluoroethyl)phosphate, and tris(trifluoroethyl)phosphite.

[0054] Examples of the borate-based compound include tetraphenylborate, lithium oxalyl difluoroborate (LiODFB) capable of forming a coating on the surface of the negative electrode, and lithium bisoxalate borate (LiB(C2O4)2, LiBOB).

[0055] The benzene-based compound may be fluorobenzene, and the amine-based compound may be triethanolamine or ethylenediamine.

[0056] Examples of the imidazole compound include lithium 2-trifluoromethyl-4,5-dicyanoimidazole, 1-methyl-5-propargyl imidazole, propargyl 1H-imidazole-1-carboxylate, 1-vinyl imidazole, and allyl 1H-imidazole-1-carboxylate.

[0057] The silane-based compound may be tetravinylsilane or the like. The lithium salt compound is a compound different from the lithium salt contained in the nonaqueous electrolyte, and examples of the lithium salt include LiPO2F2, LiSO3F, and LiBF4.

[0058] Among these other additives, in order to form a stronger SEI film on the surface of the negative electrode during the initial activation step, other additives having excellent film-forming effects on the surface of the negative electrode, specifically at least one selected from the group consisting of vinylene carbonate, vinyl ethylene carbonate, 1,3-propane sultone, ethylene sulfate, fluoroethylene carbonate (FEC), LiBF4, and lithium difluorophosphate (LiPO2F2), may be included.

[0059] The other additives may be used in combination of two or more compounds, and may be included in an amount of 0.01 to 30% by weight, specifically 0.01 to 20% by weight, and preferably 0.05 to 15% by weight, based on the total weight of the non-aqueous electrolyte. When the content of the other additives is within the above range, high-temperature storage and cycle characteristics are improved, side reactions in the battery caused by excessive addition are prevented, and the remaining or precipitation of unreacted substances is prevented, which is preferable.

[0060] Lithium secondary battery Another embodiment of the present invention provides a lithium secondary battery including the nonaqueous electrolyte for a lithium secondary battery of the present invention.

[0061] Specifically, the lithium secondary battery includes a positive electrode, a negative electrode, a separator interposed between the positive electrode and the negative electrode, and a non-aqueous electrolyte, and the non-aqueous electrolyte includes the non-aqueous electrolyte for lithium secondary batteries of the present invention.

[0062] Meanwhile, the lithium secondary battery of the present invention may be manufactured by forming an electrode assembly in which a positive electrode, a negative electrode, and a separator are sequentially stacked between the positive electrode and the negative electrode, housing the electrode assembly in a battery case, and then introducing the nonaqueous electrolyte of the present invention into the battery case.

[0063] The method for manufacturing the lithium secondary battery of the present invention may be carried out by a conventional method well known in the art, and will be described in detail below.

[0064] (1) Positive electrode The positive electrode according to the present invention may include a positive electrode active material layer containing a positive electrode active material, and if necessary, the positive electrode active material layer may further include a conductive material and / or a binder.

[0065] The positive electrode active material is a compound capable of reversible intercalation and deintercalation of lithium, and specifically, may include a lithium composite metal oxide containing one or more metals such as cobalt, manganese, nickel, or aluminum and lithium.

[0066] Specifically, the positive electrode active material is a lithium-cobalt-based oxide (e.g., LiCoO2, etc.), a lithium-manganese-based oxide (e.g., LiMnO2, LiMn2O4, etc.), a lithium-nickel-based oxide (e.g., LiNiO2, etc.), a lithium-nickel-manganese-based oxide (e.g., LiNi 1-Y Mn Y O2 (where 0 < Y < 1), LiMn 2-z Ni z O4 (where 0 < Z < 2), etc.), a lithium-nickel-cobalt-based oxide (e.g., LiNi 1-Y1 Co Y1 O2 (where 0 < Y1 < 1), etc.), a lithium-manganese-cobalt-based oxide (e.g., LiCo 1-Y2 Mn Y2 O2 (where 0 < Y2 < 1), LiMn 2-z1 Co z1 O4 (where 0 < Z1 < 2), etc.), a lithium-nickel-manganese-cobalt-based oxide (e.g., Li(Ni p Co q Mn r1 )O2 (where 0 < p < 1, 0 < q < 1, 0 < r1 < 1, p + q + r1 = 1), or Li(Ni p1 Co q1 Mn r2 )O4 (where 0 < p1 < 2, 0 < q1 < 2, 0 < r2 < 2, p1 + q1 + r2 = 2), etc.), a lithium-nickel-cobalt-transition metal (M) oxide (e.g., Li(Ni p2 Co q2 Mn r3 M S2)O2 (where M is selected from the group consisting of Al, Fe, V, Cr, Ti, Ta, Mg, Ti, and Mo, and p2, q2, r3, and s2 are atomic fractions of independent elements, 0 < p2 < 1, 0 < q2 < 1, 0 < r3 < 1, 0 < s2 < 1, and p2 + q2 + r3 + s2 = 1)) may be included, and any one or two or more of these compounds may be included.

[0067] Among them, in terms of improving the capacity characteristics and safety of the battery, the positive electrode active material may include at least one selected from the group consisting of lithium-cobalt-based oxides, lithium-manganese-based oxides, lithium-nickel-manganese-cobalt-based oxides, and lithium-nickel-cobalt-transition metal (M) oxides.

[0068] Specifically, the positive electrode active material may include at least one selected from lithium-nickel-manganese-cobalt-based oxides having a nickel content of 55 atm% or more and lithium-nickel-cobalt-transition metal (M) oxides having a nickel content of 55 atm% or more. Specifically, the positive electrode active material may include a lithium-nickel-manganese-cobalt-based oxide represented by the following Chemical Formula 2.

[0069] [Chemical Formula 2] Li(Ni a Co b Mn c M d )O2

[0070] In the Chemical Formula 2, M is W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, or Mo, a, b, c, and d are atomic fractions of independent elements, 0.55 ≦ a < 1, 0 < b ≦ 0.3, 0 < c ≦ 0.3, 0 ≦ d ≦ 0.1, and a + b + c + d = 1.

[0071] Specifically, the a, b, c, and d may be in the ranges 0.60≦a≦0.95, 0.01≦b≦0.20, 0.01≦c≦0.20, and 0≦d≦0.05, respectively.

[0072] More specifically, a, b, c, and d may be 0.80≦a≦0.95, 0.02≦b≦0.15, 0.02≦c≦0.15, and 0≦d≦0.03, respectively.

[0073] Specifically, the positive electrode active material is, for example, Li(Ni 0.6 Mn 0.2 Co 0.2 )O2, Li(Ni 0.65 Mn 0.2 Co 0.15 )O2, Li(Ni 0.7 Mn 0.2 Co 0.1 )O2, Li(Ni 0.8 Mn 0.1 Co 0.1 )O2, and Li(Ni 0.85 Co 0.05 Mn 0.08 Al 0.02 ) O2.

[0074] On the other hand, when high-content nickel (High-Ni) with Ni content exceeding 0.55 is used as the lithium transition metal oxide, Li +1 Ion and Ni +2 Because the size of the ions is similar, Li +1 Ion and Ni +2The cation mixing phenomenon occurs, where the position of ions changes. In other words, nickel transition metals with d orbitals should have a regular octahedral structure when coordinated in high temperature environments according to the change in the oxidation number of Ni contained in the positive electrode active material, but when external energy is supplied, the order of the energy levels changes, or a disproportionation reaction that changes the oxidation number forms a twisted octahedron, resulting in deformation and collapse of the crystal structure of the positive electrode active material. Furthermore, when stored at high temperatures, a side reaction between the positive electrode active material and the electrolyte causes the transition metals, especially nickel metal, to dissolve from the positive electrode active material, and other side reactions occur, causing the electrolyte to run out and the performance of the secondary battery to deteriorate due to the collapse of the structure of the positive electrode active material.

[0075] In the present invention, such problems can be improved by using a non-aqueous electrolyte containing a specific additive and a positive electrode containing a high-content nickel (High-Ni) transition metal oxide as a positive electrode active material. That is, the non-aqueous electrolyte of the present invention forms a strong ion-conductive coating on the surface of the positive electrode, and Li +1 Ion and Ni +2 The cation mixing phenomenon of ions is suppressed, and side reactions between the positive electrode and the electrolyte, metal elution, etc. are effectively suppressed, thereby mitigating the structural instability of the high-capacity electrode. Therefore, a sufficient amount of nickel transition metal can be secured to ensure the capacity of the lithium secondary battery, thereby increasing the energy density and improving the output characteristics.

[0076] The positive electrode active material may be included in the positive electrode active material layer in an amount of 70% by weight to 99% by weight, specifically 75% by weight to 99% by weight. In this case, if the content of the positive electrode active material is less than 70% by weight, the energy density may be reduced, resulting in a reduced capacity.

[0077] The conductive material is not particularly limited as long as it does not induce a chemical change in the battery and has conductivity, and examples of the conductive material that can be used include carbon powders such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black; graphite powders such as natural graphite, artificial graphite, and graphite with highly developed crystal structures; conductive fibers such as carbon fibers and metal fibers; conductive powders such as carbon fluoride powder, aluminum powder, and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives. The conductive material is usually added to the positive electrode active material layer in an amount of 1 to 30% by weight.

[0078] The binder is a component that plays a role in improving the adhesion between the positive electrode active material particles and the adhesive strength between the positive electrode active material and the current collector, and is usually added in an amount of 1 to 30% by weight in the positive electrode active material layer. Examples of such binders include fluororesin-based binders including polyvinylidene fluoride (PVDF) or polytetrafluoroethylene (PTFE); rubber-based binders including styrene butadiene rubber (SBR), acrylonitrile butadiene rubber, and styrene-isoprene rubber; cellulose-based binders including carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, and regenerated cellulose; polyalcohol-based binders including polyvinyl alcohol; polyolefin-based binders including polyethylene and polypropylene; polyimide-based binders; polyester-based binders; and silane-based binders.

[0079] The positive electrode of the present invention as described above may be manufactured by a method for manufacturing a positive electrode well known in the art. For example, the positive electrode may be manufactured by a method of dissolving or dispersing a positive electrode active material, a binder, and / or a conductive material in a solvent to prepare a positive electrode slurry, which is then coated on a positive electrode current collector, and then dried and rolled to form a positive electrode active material layer, or by a method of casting the positive electrode active material layer on another support, peeling off the support, and laminating the resulting film on the positive electrode current collector.

[0080] The positive electrode current collector is not particularly limited as long as it does not induce a chemical change in the battery and has conductivity. For example, stainless steel, aluminum, nickel, titanium, baked carbon, or aluminum or stainless steel whose surface has been treated with carbon, nickel, titanium, silver, or the like may be used.

[0081] The solvent may include an organic solvent such as NMP (N-methyl-2-pyrrolidone), and may be used in an amount that provides a preferred viscosity when the positive electrode active material, and optionally a binder and a conductive material, are contained. For example, the solvent may be contained so that the solids concentration in the active material slurry containing the positive electrode active material, and optionally a binder and a conductive material, is 10% by weight to 90% by weight, and preferably 30% by weight to 80% by weight.

[0082] (2) Negative electrode Next, the negative electrode will be described. The negative electrode according to the present invention includes a negative electrode active material layer containing a negative electrode active material, and the negative electrode active material layer may further include a conductive material and / or a binder, as necessary.

[0083] The negative electrode active material may include at least one selected from the group consisting of lithium metal, a carbon material capable of reversibly intercalating / deintercalating lithium ions, a metal or an alloy of such a metal and lithium, a metal composite oxide, a material capable of doping and dedoping lithium, and a transition metal oxide.

[0084] As the carbonaceous material capable of reversibly intercalating / deintercalating lithium ions, any carbonaceous negative electrode active material generally used in lithium ion secondary batteries may be used without particular limitation. Representative examples thereof include crystalline carbon, amorphous carbon, or a combination of these. Examples of the crystalline carbon include graphite such as amorphous, plate-like, flaky, spherical, or fibrous natural graphite or artificial graphite. Examples of the amorphous carbon include soft carbon (low-temperature calcined carbon), hard carbon, mesophase pitch carbide, calcined coke, and the like.

[0085] As the metal or an alloy of these metals and lithium, a metal selected from the group consisting of Cu, Ni, Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al, and Sn, or an alloy of these metals and lithium may be used.

[0086] Examples of the metal composite oxide include PbO, PbO2, Pb2O3, Pb3O4, Sb2O3, Sb2O4, Sb2O5, GeO, GeO2, Bi2O3, Bi2O4, Bi2O5, Li x Fe2O3(0≦x≦1), Li x WO2(0≦x≦1), and Sn x Me 1-x Me’ y O z (Me: Mn, Fe, Pb, Ge; Me’: Al, B, P, Si, Group 1, Group 2, Group 3 elements of the periodic table, halogen; 0 < x ≦ 1; 1 ≦ y ≦ 3; 1 ≦ z ≦ 8) may be used.

[0087] As the material capable of doping and undoping lithium, Si, SiO x(0 < x ≤ 2), Si-Y alloy (wherein Y is an element selected from the group consisting of an alkali metal, an alkaline earth metal, a Group 13 element, a Group 14 element, a transition metal, a rare earth element, and combinations thereof, and is not Si), Sn, SnO2, Sn-Y (wherein Y is an element selected from the group consisting of an alkali metal, an alkaline earth metal, a Group 13 element, a Group 14 element, a transition metal, a rare earth element, and combinations thereof, and is not Sn), etc. may be mentioned, and at least one of these may be mixed with SiO2 and used. The element Y may be selected from the group consisting of Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db, Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn, In, Ge, P, As, Sb, Bi, S, Se, Te, Po, and combinations thereof. Examples of the transition metal oxide include lithium-containing titanium composite oxide (LTO), vanadium oxide, lithium vanadium oxide, etc.

[0088] According to one embodiment, the negative electrode active material of the present invention may be a carbon-based negative electrode active material, or may be used including a silicon-based negative electrode active material together with the carbon-based negative electrode active material. The negative electrode active material may be contained in the negative electrode active material layer at 80% to 99% by weight.

[0089] The conductive material is a component for further improving the conductivity of the negative electrode active material, and may be added in an amount of 1 to 20% by weight in the negative electrode active material layer. Such a conductive material is not particularly limited as long as it does not induce a chemical change in the battery and has conductivity, and examples thereof include graphite such as natural graphite and artificial graphite; carbon black such as acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fibers and metal fibers; conductive powders such as carbon fluoride powder, aluminum powder, and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives.

[0090] The binder is a component that aids in bonding between the conductive material, the active material, and the current collector, and is usually added in an amount of 1 to 30% by weight to the negative electrode active material layer. Examples of such binders include fluororesin-based binders including polyvinylidene fluoride (PVDF) or polytetrafluoroethylene (PTFE); rubber-based binders including styrene-butadiene rubber (SBR), acrylonitrile-butadiene rubber, and styrene-isoprene rubber; cellulose-based binders including carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, and regenerated cellulose; polyalcohol-based binders including polyvinyl alcohol; polyolefin-based binders including polyethylene and polypropylene; polyimide-based binders; polyester-based binders; and silane-based binders.

[0091] The negative electrode may be manufactured by a method for manufacturing a negative electrode well known in the art. For example, the negative electrode may be manufactured by applying a negative electrode active material slurry, which is prepared by dissolving or dispersing a negative electrode active material, and optionally a binder and a conductive material in a solvent, onto a negative electrode current collector, rolling and drying the slurry to form a negative electrode active material layer, or by casting the negative electrode active material layer onto another support, peeling off the support, and laminating the resulting film onto the negative electrode current collector.

[0092] The negative electrode current collector generally has a thickness of 3 to 500 μm. Such a negative electrode current collector is not particularly limited as long as it does not induce chemical changes in the battery and has high conductivity, and for example, copper, stainless steel, aluminum, nickel, titanium, baked carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, silver, etc., aluminum-cadmium alloy, etc. may be used. In addition, like the positive electrode current collector, fine irregularities may be formed on the surface to strengthen the binding force of the negative electrode active material, and it may be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.

[0093] The solvent may include water or an organic solvent such as NMP or alcohol, and may be used in an amount that provides a preferred viscosity when the negative electrode active material, and optionally a binder and a conductive material, etc. are contained. For example, the solvent may be contained so that the solid content concentration in the active material slurry containing the negative electrode active material, and optionally a binder and a conductive material, is 50% by weight to 75% by weight, preferably 40% by weight to 70% by weight.

[0094] (3) Separator The separator included in the lithium secondary battery of the present invention may be a commonly used conventional porous polymer film, for example, a porous polymer film made of a polyolefin polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, or an ethylene / methacrylate copolymer, either alone or in a laminated state, or a conventional porous nonwoven fabric, for example, a nonwoven fabric made of a high melting point glass fiber, a polyethylene terephthalate fiber, or the like, but is not limited thereto.

[0095] The external shape of the lithium secondary battery according to the present invention is not particularly limited, and may be a cylindrical type using a can, a square type, a pouch type, a coin type, or the like.

[0096] The present invention will be described in detail below with reference to examples. However, the examples of the present invention may be modified into various other forms, and the scope of the present invention should not be construed as being limited to the examples described below. The examples of the present invention are provided to more completely explain the present invention to those having average knowledge in the art. EXAMPLES

[0097] Example 1. (Manufacture of non-aqueous electrolyte for lithium secondary batteries) LiPF6 was dissolved in an organic solvent in which ethylene carbonate (EC) and ethyl methyl carbonate (EMC) were mixed in a volume ratio of 30:70 to give a concentration of 1.0 M, and then 0.1 wt % of the compound represented by Chemical Formula 1a, 0.5 wt % of vinylene carbonate (VC), 0.5 wt % of 1,3-propane sultone (PS), and 1.0 wt % of ethylene sulfate were added as other additives to produce a non-aqueous electrolyte for a lithium secondary battery (see Table 1 below).

[0098] (Secondary battery manufacturing) Positive electrode active material particles (Li(Ni 0.85 Co 0.05 Mn 0.08 Al 0.02 )O2), carbon black as a conductive material, and polyvinylidene fluoride as a binder were added to N-methyl-2-pyrrolidone (NMP) as a solvent in a weight ratio of 97.5:1:1.5 to prepare a positive electrode slurry (solid content 75.0 wt%). The positive electrode slurry was applied to a positive electrode current collector (aluminum thin film) with a thickness of 15 μm, dried, and roll pressed to prepare a positive electrode.

[0099] Anode active material (graphite), binder (SBR-CMC), and conductive material (carbon black) were added to water as a solvent in a weight ratio of 95:3.5:1.5 to prepare anode slurry (solid content: 60 wt%). The anode slurry was applied to a copper (Cu) thin film as anode current collector with a thickness of 6 μm, dried, and then roll pressed to prepare anode.

[0100] A porous separator polypropylene was interposed between the positive electrode and the negative electrode to prepare an electrode assembly, which was then housed in a battery case. The non-aqueous electrolyte for the lithium secondary battery was then injected into the battery case to prepare a lithium secondary battery.

[0101] Example 2. A lithium secondary battery was manufactured in the same manner as in Example 1, except that LiPF6 was dissolved in a non-aqueous organic solvent to a concentration of 1.0 M, and 0.5 wt % of the compound represented by Formula 1a, 0.5 wt % of vinylene carbonate (VC), 0.5 wt % of 1,3-propane sultone (PS), and 1 wt % of ethylene sulfate were added to the non-aqueous organic solvent to prepare a non-aqueous electrolyte (see Table 1 below).

[0102] Example 3. A lithium secondary battery was manufactured in the same manner as in Example 1, except that LiPF6 was dissolved in a non-aqueous organic solvent to a concentration of 1.0 M, and then 1.0 wt % of the compound represented by Formula 1a, 0.5 wt % of vinylene carbonate (VC), 0.5 wt % of 1,3-propane sultone (PS), and 1 wt % of ethylene sulfate were added thereto to prepare a non-aqueous electrolyte (see Table 1 below).

[0103] Example 4. A lithium secondary battery was manufactured in the same manner as in Example 1, except that LiPF6 was dissolved in a non-aqueous organic solvent to a concentration of 1.0 M, and 3.0 wt % of the compound represented by Formula 1a, 0.5 wt % of vinylene carbonate (VC), 0.5 wt % of 1,3-propane sultone (PS), and 1 wt % of ethylene sulfate were added to the non-aqueous organic solvent to prepare a non-aqueous electrolyte (see Table 1 below).

[0104] Example 5. A lithium secondary battery was manufactured in the same manner as in Example 1, except that LiPF6 was dissolved in a non-aqueous organic solvent to a concentration of 1.0 M, and 5.0 wt % of the compound represented by Formula 1a, 0.5 wt % of vinylene carbonate (VC), 0.5 wt % of 1,3-propane sultone (PS), and 1 wt % of ethylene sulfate were added to the non-aqueous organic solvent to prepare a non-aqueous electrolyte (see Table 1 below).

[0105] Comparative Example 1 A lithium secondary battery was manufactured in the same manner as in Example 1, except that LiPF6 was dissolved in a non-aqueous organic solvent to a concentration of 1.0 M, and then additives such as vinylene carbonate (VC) 0.5 wt %, 1,3-propane sultone (PS) 0.5 wt %, and ethylene sulfate 1 wt % were added to prepare a non-aqueous electrolyte (see Table 1 below).

[0106] Comparative Example 2 A lithium secondary battery was manufactured in the same manner as in Example 1, except that LiPF6 was dissolved in a non-aqueous organic solvent to a concentration of 1.0 M, and then 0.5 wt % of Prop-2yn-1-yl acetate (CAS No. 627-09-8) represented by the following Formula 3 was added as an additive instead of the compound represented by Formula 1a to prepare a non-aqueous electrolyte (see Table 1 below).

[0107] [ka]

[0108] [Table 1]

[0109] Meanwhile, in Table 1, the abbreviations of the compounds have the following meanings. EC: Ethylene carbonate EMC: Ethyl methyl carbonate

[0110] Experimental Example Experimental example 1. Evaluation of high-temperature storage characteristics (1) Evaluation of capacity retention and resistance increase rate after high-temperature storage The lithium secondary batteries prepared in Examples 1 to 5 and the lithium secondary batteries prepared in Comparative Examples 1 and 2 were each charged to 4.2 V under constant current / constant voltage conditions at a rate of 0.33 C at room temperature (25° C.), discharged to a depth of discharge (DOD) of 50% to match SOC of 50%, and then discharged for 10 seconds at a rate of 2.5 C. Then, the batteries were charged to 4.2 V under constant current / constant voltage conditions at a rate of 0.33 C at room temperature (25° C.), and discharged to 2.5 V under constant current conditions at a rate of 0.33 C (1 cycle), and the initial capacity and initial resistance were measured.

[0111] Then, after storing at 60°C for 6 weeks, each lithium secondary battery was cooled to room temperature (25°C), charged to 4.2V under constant current / constant voltage conditions at a rate of 0.33C, and discharged to 2.5V under constant current conditions at a rate of 0.33C, and the capacity and resistance values ​​after high-temperature storage were measured.

[0112] The capacity retention rate (%) was calculated using the following formula 1, and the calculated results are shown in the following Table 2. In addition, the resistance increase rate (%) was calculated using the following formula 2, and the calculated results are shown in the following Table 2.

[0113] [Formula 1] Capacity retention rate (%) = (discharge capacity after high-temperature storage / discharge capacity before high-temperature storage) x 100 [Formula 2] Resistance increase rate (%) = {(resistance after high temperature storage - resistance before high temperature storage) / resistance before high temperature storage} x 100

[0114] (2) Evaluation of volume increase rate (%) after high-temperature storage The lithium secondary batteries prepared in Examples 1 to 5 and the lithium secondary batteries prepared in Comparative Examples 1 and 2 were each charged to 4.2 V at room temperature (25° C.) under constant current / constant voltage conditions at a rate of 0.33 C, and then the initial thickness was measured. Then, after storing at 60° C. for 6 weeks, the thickness of each lithium secondary battery after high temperature storage was measured, and the results are shown in Table 2 below.

[0115] [Table 2]

[0116] Referring to Table 2, it can be seen that the lithium secondary batteries of Examples 1 to 5 including the non-aqueous electrolyte of the present invention had improved capacity retention (%) and reduced resistance increase (%) and thickness increase (%) compared to the secondary batteries of Comparative Examples 1 and 2. In particular, it can be seen that the improvements in capacity retention (%), resistance increase (%), and thickness increase (%) were significantly improved in Examples 1 to 4, in which the content of the compound represented by Chemical Formula 1 in the non-aqueous electrolyte was less than 5 wt %.

Claims

1. A non-aqueous electrolyte for a lithium secondary battery, comprising a lithium salt, a non-aqueous organic solvent, and a compound represented by the following chemical formula 1 as an additive: 【Chemistry 1】 In the above Chemical Formula 1, R is a substituted or unsubstituted alkylene group having 1 to 5 carbon atoms.

2. 2. The nonaqueous electrolyte for a lithium secondary battery according to claim 1, wherein in Chemical Formula 1, R is a substituted or unsubstituted alkylene group having 1 to 3 carbon atoms.

3. The nonaqueous electrolyte solution for a lithium secondary battery according to claim 1, wherein the substitution is at least one substituent selected from the group consisting of halogen, a hydroxyl group (-OH), a carboxyl group (-COOH), an alkyl group having 1 to 6 carbon atoms, an alkenyl group having 2 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, a cycloalkyl group having 3 to 8 carbon atoms, a heterocycloalkyl group having 2 to 6 carbon atoms, an aryl group having 6 to 10 carbon atoms, and a heteroaryl group having 4 to 10 carbon atoms.

4. The nonaqueous electrolyte for a lithium secondary battery according to claim 1, wherein the compound represented by Chemical Formula 1 includes a compound represented by Chemical Formula 1a: 【Chemistry 2】

5. The non-aqueous electrolyte for a lithium secondary battery according to claim 1, wherein the compound represented by Formula 1 is contained in an amount of 0.1 wt % to 5.0 wt % based on the total weight of the non-aqueous electrolyte for a lithium secondary battery.

6. The non-aqueous electrolyte for a lithium secondary battery according to claim 5, wherein the compound represented by Formula 1 is contained in an amount of 0.5 wt % to 4.0 wt % based on the total weight of the non-aqueous electrolyte for a lithium secondary battery.

7. 2. The nonaqueous electrolyte solution for a lithium secondary battery according to claim 1, further comprising at least one other additive selected from the group consisting of a cyclic carbonate-based compound, a halogen-substituted carbonate-based compound, a sultone-based compound, a sulfate-based compound, a phosphate-based or phosphite-based compound, a borate-based compound, a benzene-based compound, an amine-based compound, an imidazole-based compound, a silane-based compound, and a lithium salt-based compound.

8. a negative electrode including a negative electrode active material; a positive electrode including a positive electrode active material; a separator interposed between the negative electrode and the positive electrode; A non-aqueous electrolyte; Including, The nonaqueous electrolyte solution for lithium secondary batteries according to claim 1 .

9. 9. The lithium secondary battery according to claim 8, wherein the positive electrode active material comprises at least one selected from the group consisting of lithium-cobalt-based oxides, lithium-manganese-based oxides, lithium-nickel-manganese-cobalt-based oxides, and lithium-nickel-cobalt-transition metal (M) oxides.

10. 9. The lithium secondary battery according to claim 8, wherein the positive electrode active material includes at least one selected from a lithium-nickel-manganese-cobalt oxide having a nickel content of 55 atm % or more and a lithium-nickel-cobalt-transition metal (M) oxide having a nickel content of 55 atm % or more.

Citation Information

Patent Citations

  • Lithium titanate battery and lithium titanate battery electrolyte

    CN103326068A

  • Nonaqueous electrolyte and lithium secondary battery using the same

    JP2002280061A

  • Nonaqueous electrolyte for lithium secondary battery and lithium secondary battery comprising the same

    KR1020190033448A