Method for manufacturing film for bags containing bamboo powder, and method for manufacturing bags

By mixing bamboo powder with a compatibilizer and polyethylene resin, and using inflation molding, a stable film for bags is produced, addressing the limitations of forming film-like items with bamboo fibers.

JP7562352B2Active Publication Date: 2024-10-07諸藤 俊郎
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2020160086
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-09-24
Publication Date
2024-10-07
Estimated Expiration
2040-09-24

AI Technical Summary

Technical Problem

Existing technologies are limited in forming film-like items such as bags using bamboo fibers due to their tendency to become fracture points and difficulty in controlling molding temperature, making continuous molding difficult.

Method used

A method involving mixing bamboo powder with a compatibilizer and polyethylene resin, followed by heating, drying, and inflation molding to create a film suitable for bags, using specific ratios and processing conditions to ensure stability and dispersion.

Benefits of technology

The method enables the production of a stable bamboo powder-containing film that can be formed into bags, overcoming the challenges of fracture points and molding temperature control, allowing for continuous manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007562352000002
    Figure 0007562352000002
  • Figure 0007562352000003
    Figure 0007562352000003
  • Figure 0007562352000004
    Figure 0007562352000004
Patent Text Reader

Abstract

To provide a method for producing a film that contains bamboo powder made from bamboo and is suitable for inflation molding of a bag.SOLUTION: A method for producing a film for a bag containing bamboo powder includes: a first mixing step for mixing bamboo powder with a compatibilizer and heating the mixture to prepare a dry first composition; a second mixing step for mixing the first composition with a polyethylene resin, and then kneading and pelletizing the mixture, to prepare a dry second composition; and a molding step for inflation-molding the second composition to prepare a film.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a bamboo powder-containing bag film using bamboo powder and a method for producing the same, and also to a bag using the bag film and a method for producing the same. [Background technology]

[0002] Bamboo is a plant that is widely distributed throughout Japan. It is used in scenic landscapes, such as in bamboo forests, as one of the elements that make up gardens. It is also widely used industrially, taking advantage of its workability, strength, and weather resistance. On the other hand, it has a high reproductive ability and fast growth rate, which is thought to inhibit the growth of other plants and have little effect in disaster prevention, so measures to deal with abandoned bamboo forests and bamboo thickets are also problematic. There is also consideration of using such bamboo as an industrial material.

[0003] Patent Document 1 discloses bamboo fiber characterized in that in a differential curve of thermal weight loss, there is substantially no peak in the temperature range of 180 to 320°C, there is a peak in the temperature range of 300 to 400°C, and the content of fibers with a fiber length of 1000 μm or less is 80 mass% or more, as well as a method for producing a composite material using the same.

[0004] Patent Document 2 discloses a molded body for laying, which is characterized by having a specific gravity in the range of 1 to 2, and is produced by melt-molding a composition containing bamboo powder, which contains 80 mass% or more of components with a fiber length of 250 μm or less and 10 mass% or more of short fibers in the length range of 63 to 250 μm, and plastic in a weight ratio of 1:9 to 8:2.

[0005] Patent Document 3 discloses a composite molded body that is produced by mixing a thermoplastic plastic and bamboo-derived powder with an average aspect ratio of 5 or more in a mass ratio range of 80:20 to 30:70 and extrusion molding or injection molding, in which the bamboo-derived powder has its long sides oriented in the melt flow direction and has a thermal expansion coefficient of 30 ppm / °C or less in the melt flow direction. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2012-40701 A [Patent Document 2] JP 2014-9539 A [Patent Document 3] JP 2015-921 A Summary of the Invention [Problem to be solved by the invention]

[0007] Patent documents 1 to 3 relate to techniques using bamboo fibers processed into powder. These involve drying and burning bamboo fibers (bamboo powder) as appropriate. This allows bamboo to be reused, and contributes to carbon offsetting more than using products that mainly use plastic resins. However, products manufactured using such compositions are limited to thick products such as cases, cups, trays, and cutlery that can be molded by injection molding, etc. Furthermore, film-like products such as bags have not been molded. This is thought to be because the bamboo fibers are easily the starting point of breakage when considering the thickness of the film when molded into bags, etc., making continuous molding difficult, and controlling the molding temperature difficult.

[0008] In this situation, the present invention aims to provide a film containing bamboo powder that is suitable for forming bags. [Means for solving the problem]

[0009] The present inventors have conducted extensive research to solve the above problems, and as a result have found that the following invention meets the above object, thereby completing the present invention.

[0010] <1> A first mixing step of mixing bamboo powder and a compatibilizer and drying the mixture by heating to obtain a first composition; a second mixing step of mixing the first composition with a polyethylene resin, kneading the mixture, pelletizing, and drying to obtain a second composition; A method for producing a bamboo powder-containing bag film, comprising a molding step of obtaining a film by inflation molding the second composition. <2> The above-mentioned compatibilizer includes at least one selected from the group consisting of low molecular weight ethylene-propylene copolymers, maleic anhydride oxides of ethylene-propylene copolymers, and maleic anhydride modified high density polyethylenes. <1> The manufacturing method described in <3> The first mixing step is a step of mixing the bamboo powder in a mass ratio of 70 to 95 parts by mass and the compatibilizer in a mass ratio of 5 to 30 parts by mass, and drying the mixture at a heating temperature of 70 to 120° C. for 30 minutes or more. <1> or <2> The manufacturing method described in <4> The water content of the first composition after drying is 0.5% by mass or less. <3> The manufacturing method described in <5> The second mixing step comprises mixing the first composition in a mass ratio of 3 to 35 parts by mass and the polyethylene resin in a mass ratio of 65 to 97 parts by mass, kneading the mixture at a melting temperature of 150 to 190° C., pelletizing the mixture, and drying the mixture at a heating temperature of 70 to 120° C. for 30 minutes or more. <1> ~ <4> 13. The method for producing a semiconductor device according to any one of the preceding claims. <6> The molding step comprises mixing 40 to 100 parts by mass of pellets of the second composition and 0 to 60 parts by mass of pellets of a polyethylene resin and molding the mixture. <1> ~ <5> 13. The method for producing a semiconductor device according to any one of the preceding claims. <7> The bamboo powder is treated with superheated steam at 180 to 320°C and has an average fiber length of 400 μm or less. <1> ~ <6> 13. The method for producing a semiconductor device according to any one of the preceding claims. <8> The above <1> ~ <7> A method for manufacturing a bag, comprising a processing step of processing a bamboo powder-containing bag film described in any one of the above to provide a welded portion at the bottom seal or side seal. <9> A bamboo powder-containing film for bags, comprising 3 to 30 parts by mass of bamboo powder, 55 to 90 parts by mass of polyethylene resin, and 3 to 15 parts by mass of a compatibilizer, and having a thickness of 20 to 180 μm. <10> The above <9> A bag having a surface portion of the bamboo powder-containing bag film described in 1 and a welded portion of the bamboo powder-containing bag film. Effect of the Invention

[0011] According to the present invention, a film containing bamboo powder and suitable for forming bags can be obtained. [Brief description of the drawings]

[0012] [Figure 1] FIG. 1 is a flow diagram of a manufacturing method of the present invention. [Diagram 2] FIG. 1 is a diagram showing an outline of an inflation molding apparatus used in the manufacturing method of the present invention. [Diagram 3] 1 is an image of a film blown out of a nozzle in an embodiment according to the present invention. [Figure 4] 1 is an image of a roll of bag film produced according to an embodiment of the present invention. [Diagram 5] 1 is an image of a bag made according to an embodiment of the present invention. [Figure 6] 1 is an enlarged image of a surface portion of a bag manufactured according to an embodiment of the present invention. [Figure 7] 11 is an image showing an example of a usage state of another bag manufactured according to an embodiment of the present invention. [Figure 8] 11 is an image of another bag made according to an embodiment of the present invention. [Figure 9] 11 is an enlarged image of a surface portion of another bag manufactured according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The following is a detailed description of the embodiments of the present invention, but the following description of the constituent elements is one example (representative example) of the embodiment of the present invention, and the present invention is not limited to the following content as long as the gist of the present invention is not changed. Note that in this specification, when the expression "~" is used, it is used as an expression including the numerical values ​​before and after it.

[0014] [Method of manufacturing the bamboo powder-containing bag film of the present invention] The manufacturing method of the bamboo powder-containing bag film of the present invention includes a first mixing step of mixing bamboo powder with a compatibilizer and heating and drying to obtain a first composition, a second mixing step of mixing the first composition with a polyethylene resin, kneading, pelletizing, and drying to obtain a second composition, and a molding step of inflation molding the second composition to obtain a film. In this application, the manufacturing method of the bamboo powder-containing bag film of the present invention may be abbreviated as "the manufacturing method of the present invention". According to the manufacturing method of the present invention, film for use in bags containing bamboo powder can be efficiently manufactured by inflation molding.

[0015] [Bamboo powder-containing bag film of the present invention] The bamboo powder-containing bag film of the present invention contains 3 to 30 parts by mass of bamboo powder, 55 to 90 parts by mass of polyethylene resin, and 3 to 15 parts by mass of a compatibilizer, and has a thickness of 20 to 180 μm. In this application, the bamboo powder-containing bag film of the present invention may be simply abbreviated as "the bag film of the present invention". The bamboo powder-containing bag film of the present invention contains bamboo powder and is suitable for forming bags. In addition, the bag film of the present invention can be manufactured by the manufacturing method of the present invention in this application, and the corresponding configurations in this application can be used mutually.

[0016] The inventors have investigated the use of bamboo fibers and bamboo powder to make films by inflation molding and to mold bags using the films, as one of the effective uses of bamboo. However, because bamboo fibers are strong, even if they are pulverized by defibration, they still have a size of several hundred μm. Therefore, when attempting to mold very thin films such as those by inflation molding, it was found that simply mixing the bamboo powder with polyethylene makes molding difficult, probably because the bamboo powder is too large compared to the thickness of the film. When considering the use of such bamboo powder, it was found that even if a coupling agent or the like was used at the stage of mixing in the inflation molding device, the bamboo powder did not disperse immediately, making it very difficult to use. However, after various investigations, it was found that stable inflation molding can be achieved by dispersing the bamboo powder and polyethylene in advance using a compatibilizer, and this led to the present invention. The present invention is based on such findings.

[0017] This is a flow chart showing an example of the steps involved in the manufacturing method of the present invention. The manufacturing method of the present invention includes a step S11 of mixing bamboo powder with a compatibilizer, a step S21 of mixing the first composition obtained in step S11 with a polyethylene resin, and a step S31 of inflation molding the second composition obtained in step S21. This produces a bag film. This bag film can be appropriately molded into various bags to produce bags.

[0018] [First mixing step (S11)] The first mixing step is a step of mixing bamboo powder and a compatibilizer, and obtaining a first composition by heating and drying. Polyethylene resin is used as the main material for inflation molding, but polyethylene resin is difficult to mix with bamboo powder, and simply mixing polyethylene resin and bamboo powder and putting it into the hopper will not allow stable production of film by inflation molding. If the compatibilizer is mixed here when putting it into the hopper of the inflation molding device, it will not be mixed sufficiently and molding will not be stable, and it is also possible that the bamboo powder and the compatibilizer have absorbed moisture during storage. For this reason, the bamboo powder and the compatibilizer are mixed and dispersed in advance, heated to blend them together partially on the surface, and then dried to remove moisture. This improves the mixability with polyethylene in the subsequent process, and prevents bubbles, uneven thickness, and resin breakage caused by moisture.

[0019] [Bamboo powder] Bamboo powder is used to be incorporated into the bamboo powder-containing film. The bamboo powder in the present invention is obtained by crushing bamboo and powdering it into fibers. It is also preferable to use bamboo powder that has been heated and dried to reduce components that are easily volatilized during the film-forming process, such as moisture. The bamboo powder is preferably treated with superheated steam at 180 to 320°C and has a fiber length of 200 to 400 μm.

[0020] In a broad sense, bamboo is a general term for species of the subfamily Bambusoideae of the family Poaceae of the order Poales, whose stems become woody like woody plants. It is said that there are 600 species of bamboo growing in Japan, including Madake bamboo, Moso bamboo, and Hachiku bamboo, and any of these can be used in the present invention. Moreover, any of the trunks, branches, leaves, and roots may be used as bamboo. The trunks, which are rich in cellulose fiber components and have a large amount of them, can be preferably used.

[0021] Bamboo contains cellulose, hemicellulose and lignin as its main components. Hemicellulose plays a role in binding cellulose and lignin, or cellulose itself. It is preferable to use bamboo powder of the present invention that has a reduced amount of hemicellulose.

[0022] In the differential curve of thermal weight loss, bamboo powder has substantially no peak in the temperature range of 180 to 320°C, but has a peak in the temperature range of 300 to 400°C, and can be mainly composed of fibers with a fiber length of 1000 μm or less, with the content of these fibers being 80 mass% or more.

[0023] In addition, the bamboo powder is bamboo powder whose main component is at least 50% by mass of cellulose fiber, and in addition to the cellulose fiber, it may contain bamboo-derived components such as lignin powder and a powder component that is a combination of both cellulose and lignin components.

[0024] The differential curve of the thermal weight loss can be measured by a differential thermal gravimetric analyzer or the like. The peak in the temperature range of 180 to 320°C is due to the decomposition of hemicellulose, and the bamboo fiber having substantially no peak in this temperature range means that the bamboo fiber does not substantially contain hemicellulose. The peak in the temperature range of 300 to 400°C is due to the decomposition of cellulose, and the bamboo fiber having a peak in this temperature range means that the bamboo fiber contains cellulose. It is preferable to use bamboo powder that is substantially free of hemicellulose and rich in cellulose. The content of cellulose in the bamboo powder varies depending on the type of bamboo used as the raw material and the part of the bamboo. For example, it is known that the composition of the trunk of Moso bamboo is about 50% cellulose, and about 25% hemicellulose and lignin.

[0025] The fiber length of bamboo powder can be obtained by microscopic observation. The mass percentage of fiber lengths of 1000 μm or less is obtained by measuring the cumulative frequency percentage of fiber lengths and replacing it with mass percentage, based on the fact that fiber length and mass are substantially proportional to each other.

[0026] The fiber length of the bamboo powder is preferably 1000 to 10 μm, more preferably 500 to 50 μm. If the fiber length is extremely long, it may be difficult to disperse the bamboo powder uniformly while maintaining the fiber length. The fiber diameter is preferably 150 to 1 μm, more preferably 100 to 10 μm.

[0027] The average fiber length of the bamboo powder is preferably 400 μm or less. The average fiber length can be the arithmetic average of the bamboo fiber length measured directly on the fibers in a 1 cm x 1 cm image. If the average fiber length is too large, the thin film may cause uneven thickness or may become a breakage starting point during transportation. The average fiber length is preferably 380 μm or less, and more preferably 350 μm or less. There is no need to set a lower limit for the average fiber length, but since finer crushing is required to reduce the average fiber length and operation may be difficult, a lower limit such as 10 μm or more, 50 μm or more, or 100 μm or more may be set.

[0028] In addition, it is preferable that the bamboo powder has an average aspect ratio of 5 or more. The average aspect ratio of the fibers of the bamboo powder is the average value of the fiber length divided by the fiber diameter, and the longer the fiber, the larger the aspect ratio. The average aspect ratio of the bamboo powder can be 5 or more, 10 or more, or 15 or more. On the other hand, there is no particular upper limit to the average aspect ratio of the bamboo powder, but it may be, for example, up to about 100. Here, the average aspect ratio of the bamboo powder is the arithmetic average value of the aspect ratios obtained by measuring all fibers in a 1 cm x 1 cm image obtained by observation with a microscope with adjustable magnification using an image statistical processing method.

[0029] Such bamboo powder can be produced as follows. Bamboo powder can be produced by heating bamboo with normal pressure superheated steam at a temperature of 180 to 320 ° C., and then defibrating it into a fibrous form. Defibration can be performed by any suitable method, for example, by applying a weak force in water or the like over a long period of time. In this case, after defibration, the bamboo is dried to remove and adjust the moisture. In order to avoid energy consumption caused by adding moisture to the bamboo powder that has been dried by heating with normal pressure superheated steam and then drying it again, and to efficiently obtain bamboo powder with the desired fiber length in a short period of time, it is preferable to defibrate the bamboo by either or both of crushing and pulverization. At this time, the heat treatment time is not particularly limited, but it is preferable that it is 1 to 3 hours.

[0030] Here, normal pressure superheated steam is different from pressurized saturated steam obtained by heating at a constant volume, and refers to superheated steam at 100°C or higher under standard atmospheric pressure, which is obtained by further heating steam at 100°C in an expandable state.

[0031] Since the pressure of normal pressure superheated steam is normal pressure, for example, when a reaction vessel is used, the vessel does not need to be pressure-resistant, and scale-up is easy. In addition, the components decomposed and removed by normal pressure superheated steam are discharged with the steam flow, so when a reaction vessel is used, for example, the decomposition vapor does not liquefy and remain in the reaction vessel. Furthermore, at or above the reverse transition temperature to water of 170°C, the drying speed of the treated material is faster than that of dry air, so there is no need for a drying process for the product after treatment.

[0032] Heat treatment can be carried out by placing the bamboo in an atmospheric pressure reaction vessel and introducing atmospheric pressure superheated steam. In this case, the bamboo is cut to a size that can be contained inside the atmospheric pressure reaction vessel, for example, a maximum dimension of several tens of centimeters. If a large atmospheric pressure reaction vessel is used, cutting the bamboo is practically unnecessary.

[0033] The heat treatment may also be performed by spraying normal pressure superheated steam onto a continuous conveyor, in which case cutting of the bamboo is essentially unnecessary and continuous processing increases processing efficiency.The heat treatment may also be performed by spraying normal pressure superheated steam inside a rotary kiln, in which case contact between the bamboo and steam becomes more uniform and the bamboo can be crushed and pulverized simultaneously inside the device, increasing processing efficiency.

[0034] If the temperature of the normal pressure superheated steam is less than 180°C, hemicellulose may not be sufficiently removed. It is more preferable that the temperature of the normal pressure superheated steam is 190°C or higher, 200°C or higher, or 210°C or higher. On the other hand, if the temperature of the normal pressure superheated steam exceeds 320°C, the cellulose may be decomposed and removed, resulting in a decrease in the yield of bamboo powder. The upper limit of the temperature may be 300°C or lower, or 280°C or lower.

[0035] After the heat treatment, the bamboo can be easily crushed because the easily decomposable hemicellulose has been decomposed and removed by volatilization. Crushing and crushing can be carried out using an appropriate device. In addition, a two-stage process of coarse crushing followed by fine crushing may be carried out. After crushing or crushing, it is preferable to further sieve the bamboo powder.

[0036] Such bamboo powder can be obtained by a simple method that does not substantially involve chemical processing using alkaline or acidic substances, and does not require high pressure processing or post-processing of the chemicals used.

[0037] For such bamboo powder, please refer to Japanese Patent No. 5656167, Japanese Patent No. 5669072, and Japanese Patent No. 5656174, and these bamboo fibers and bamboo powder can be used.

[0038] [Compatibilizer] The compatibilizer can be one designed for the production of composite materials of polyethylene and various fillers. For example, low molecular weight ethylene-propylene copolymers, maleic anhydride oxides of ethylene-propylene copolymers, maleic anhydride modified high density polyethylenes, etc. can be used. An example of a low molecular weight ethylene-propylene copolymer is "Hiwax (registered trademark) 110P" manufactured by Mitsui Chemicals, Inc. An example of a maleic anhydride oxide of ethylene-propylene copolymer is "Hiwax (registered trademark) 1105A" manufactured by Mitsui Chemicals, Inc. An example of a maleic anhydride modified high density polyethylene is "Admer (registered trademark) HE810" manufactured by Mitsui Chemicals, Inc.

[0039] [First composition] In the first mixing step, it is preferable to mix 70 to 95 parts by mass of bamboo powder and 5 to 30 parts by mass of the compatibilizer in a mass ratio. The bamboo powder may be 75 parts by mass or more, or 80 parts by mass or more. The bamboo powder may be 90 parts by mass or less, or 88 parts by mass or less. The compatibilizer may be 10 parts by mass or more, or 12 parts by mass or more. The compatibilizer may be 25 parts by mass or less, or 20 parts by mass or less. Since the bamboo powder and the compatibilizer are solids such as powders at room temperature, they may be weighed out to a predetermined mass ratio and mixed in powder form.

[0040] [Mixing / Drying] The mixture of bamboo powder and compatibilizer is heated to 70-120°C. This heating process causes the bamboo powder and the compatibilizer to partially integrate on the surface and other areas. The lower limit of the heating temperature can be 80°C or higher, or 90°C or higher. The upper limit of the heating temperature can be 110°C or lower, or 105°C or lower. If the temperature is too low, it may be difficult to sufficiently integrate the bamboo powder, the bamboo powder may be difficult to dry, or the drying time may be long. If the temperature is too high, it may cause deterioration, volatilization, yellowing, etc.

[0041] It is preferable to heat and dry for 30 minutes or more at such a heating temperature. The heat and dry time is more preferably 1 hour or more. If the heat and dry time is too short, there is a possibility that moisture cannot be sufficiently removed. In addition, there is no need to set an upper limit on the heat and dry time, but from the viewpoint of productivity, it may be 12 hours or less, 10 hours or less, 8 hours or less, or 4 hours or less. Heat and dry can be performed in a stationary state in a constant temperature dryer or the like with the atmosphere temperature set to the above temperature and dried in a dry state.

[0042] [Moisture content] The first composition after drying preferably has a moisture content of 0.5% by mass or less. By sufficiently reducing the moisture content, it is possible to more stably prevent the occurrence of air bubbles and uneven thickness when forming a film. The bamboo powder absorbs moisture during storage and contains a few percent of moisture, which is removed by drying. The moisture content may be 0.4% by mass or less or 0.3% by mass or less. There is no need to set a lower limit for the moisture content, and it may be set to the lower limit of detection. In addition, a lower limit such as 0.01% by mass or more, 0.02% by mass or more, or 0.05% by mass or more may be set in consideration of manufacturing efficiency such as drying time. The moisture content can be measured using a moisture meter or the like. The moisture content can be determined by the change in mass at a weighing weight of about 20 grams, a drying temperature of 105°C, and a measurement time of 10 minutes. For example, it can be measured using a moisture meter "Moc63u" from Shimadzu Corporation.

[0043] [Second mixing step (S21)] The second mixing step is a step of mixing the first composition with a polyethylene resin, melting and pelletizing the mixture, and drying the second composition. The first composition is in a powder form, and therefore may not be caught in the extrusion screw from the hopper at the supply port at the time of inflation molding in the set ratio. In addition, there is a risk that the mixture may not be sufficiently mixed with the polyethylene resin by melt kneading alone in the inflation molding device. For this reason, the mixture is premixed and melt-pelletized in the second mixing step. In addition, since the mixture may come into contact with moisture during melt pelletization, the moisture is dried.

[0044] [polyethylene] The polyethylene may be a resin such as low-density polyethylene, linear low-density polyethylene, medium-density polyethylene, high-density polyethylene, metallocene-catalyzed polyethylene, modified polyethylene, etc. In particular, it is preferable to use low-density polyethylene or linear low-density polyethylene, which is suitable for forming into a film.

[0045] In the second mixing step, it is preferable to mix the first composition at a mass ratio of 3 to 35 parts by mass and the polyethylene resin at a mass ratio of 65 to 97 parts by mass. The first composition can be 5 parts by mass or more, 8 parts by mass or more, or 10 parts by mass or more. The more the first composition, the more the bamboo powder is relatively increased. The more the bamboo powder is, the greater the influence of the bamboo powder during inflation molding becomes, so that it is effective to manufacture according to the present invention. In addition, the increase in the bamboo powder further improves the usefulness as a biomass utilization product. In addition, the first composition may be contained at a higher concentration of 15 parts by mass or more, 18 parts by mass or more, or 20 parts by mass or more. In addition, the first composition may be 32 parts by mass or less, or 30 parts by mass or less. The polyethylene resin may be 70 parts by mass or more. In addition, the polyethylene resin may be 80 parts by mass or less.

[0046] Since the first composition and the polyethylene resin are solids such as powders or pellets at room temperature, they may be weighed out to a specified mass ratio and mixed in the solid state (so-called dry blend). If the polyethylene content is too low, it may not be possible to obtain a composition suitable for inflation molding. If the polyethylene content is excessive, the bamboo powder derived from the natural environment will relatively decrease. In addition, molding processing will become difficult, and unevenness in appearance and physical properties may occur, resulting in a deterioration in quality.

[0047] The first composition and the polyethylene resin are mixed, heated and kneaded at a melting temperature of 150 to 190°C, and pelletized. The raw material is fed into a hopper, melted and kneaded under heating with a screw rotated by a motor, extruded into a strand shape, and cut into pellets at a predetermined length. The strands or pellets can be cooled or solidified in water. The melting temperature may be 160°C or higher, or 170°C or higher.

[0048] The mixture of the first composition and the polyethylene resin is dried at 70 to 120°C. This removes moisture that is adsorbed by pelletization or adheres to the periphery of the pellets. The lower limit of the heating temperature can be 80°C or higher, or 90°C or higher. The upper limit of the heating temperature can be 110°C or lower, or 105°C or lower. If the temperature is too low, drying may be difficult or the drying time may be prolonged. If the temperature is too high, deterioration, volatilization, yellowing, etc. may occur.

[0049] Drying is preferably performed for 30 minutes or more. The drying time is more preferably 1 hour or more, 2 hours or more, or 3 hours or more. If the drying time is too short, there is a possibility that moisture cannot be sufficiently removed. In addition, there is no need to set an upper limit on the heat drying time, but from the viewpoint of productivity, it may be 24 hours or less, 12 hours or less, or 8 hours or less. Heat drying can be performed by drying the material in a stationary state in a constant temperature dryer or the like at the above-mentioned atmospheric temperature, or by drying using a hot air oven or the like.

[0050] The second composition after drying preferably has a water content of 0.5% by mass or less. By sufficiently reducing the water content, it is possible to more stably prevent air bubbles and thickness unevenness from occurring when forming a film. After pelletization, moisture of about several percent may adhere due to cooling in water or moisture absorption during storage, and this is removed by drying. The water content may be 0.4% by mass or less or 0.3% by mass or less. There is no need to set a lower limit for the water content, and it may be about the lower limit of detection. In addition, a lower limit such as 0.01% by mass or more, 0.02% by mass or more, or 0.05% by mass or more may be set in consideration of manufacturing efficiency such as drying time. The water content can be measured using a moisture meter or the like. The water content can be determined by the change in mass at a weighing weight of about 20 grams, a drying temperature of 105°C, and a measurement time of 10 minutes. For example, it can be measured using a moisture meter "Moc63u" from Shimadzu Corporation.

[0051] [Other ingredients] The bag film of the present invention may contain components other than bamboo powder, compatibilizer, and polyethylene (hereinafter, "other components"). In the bag film, the proportion of bamboo powder, compatibilizer, and polyethylene ("bamboo powder + compatibilizer + polyethylene" / bag film composition) is preferably 90% by mass or more, more preferably 95% by mass or more, and more preferably 98% by mass or more. The upper limit of this proportion may be 100% by mass, or may be 99.5% by mass or less, or 99% by mass or less. As the other components, plasticizers, weathering agents, colorants, slip agents, deodorants, etc., which are used in inflation molding of polyolefin resins, can be used.

[0052] [Molding process (process S31)] The molding step is a step of obtaining a film by inflation molding the second composition. In the molding step, each main component may be mixed in addition to the second composition, for example, it may be mixed with pellets of polyethylene resin and molded. The mixing ratio may be 40 to 100 parts by mass of pellets of the second composition and 0 to 60 parts by mass of pellets of polyethylene resin, and then molded.

[0053] [Blown film molding] The molding process is carried out by inflation molding, a film molding technique in which resin is extruded from an extruder into a tube shape, softened, and then gas is blown into the resin to inflate it while it is being pulled up.

[0054] FIG. 2 shows an outline of the structure of an inflation molding apparatus. An inflation molding apparatus 10 is an apparatus for forming a film 1 by inflation molding. A resin composition is charged from a hopper 21, and a motor 22 is rotated to rotate a screw 23, thereby extruding the resin composition from a die 24. During this extrusion, a gas such as air is blown from the lower part of the die 24 toward the upper part, as shown by the arrow in FIG. 1, to inflate the film 1 while forming it. The inflated film 1 is taken up onto a roll 4 via a guide 3, rollers 31, 32, and roller 33.

[0055] [Extrusion temperature] The extrusion temperature of the die 24 for inflation molding can be 160 to 200° C. Since the bag film of the present invention is mainly made of polyethylene resin, it can be molded under conditions similar to the molding temperature of polyethylene.

[0056] In this molding, the manufacturing method of the present invention preferably performs molding at an extrusion temperature of the die 24 of 160 to 200°C. The molding temperature can be appropriately set in consideration of the extrusion pressure, the molecular weight of the resin, the mixing ratio, the film thickness, etc. It is preferably 170°C or higher, and more preferably 175°C or higher. It is also preferably 195°C or lower. If the extrusion temperature is too low, the extrusion pressure may become too high, and extrusion or dispersion may not be possible. If the extrusion temperature is too high, deterioration due to heating may occur, causing coloration, etc. The extrusion temperature of the die 24 is set to a predetermined temperature, and the temperature of the flow path corresponding to the screw 23 from the hopper 21 to the die is increased in stages.

[0057] The thickness of the film to be molded is preferably 20 to 180 μm. The thickness of the film can be adjusted by adjusting the extrusion amount, the size of the opening of the die, the take-up speed, etc. If the film thickness is too thin, the bamboo powder will be larger than the film thickness and will become a place where stress is concentrated, making molding difficult, making winding difficult due to uneven thickness, and there is a risk of it becoming a breakage starting point when molded into a bag shape. If the film thickness is too thick, the rigidity will be too high and it may not be suitable for inflation molding. The upper limit of the film thickness may be 150 μm or less, 120 μm or less, or 100 μm or less. The lower limit of the film thickness may be 30 μm or more, or 40 μm or more.

[0058] [Bag forming] The bag film produced by the manufacturing method of the present invention can be processed into bags by using inflation-molded film bag-molding techniques such as bottom sealing, side sealing, attachment of peripheral parts, and printing. Although it contains bamboo powder, it is homogeneously dispersed in polyethylene, so it is also suitable for continuous manufacturing using thermoplastic resin molding methods such as heat sealing. By utilizing the properties of this film, a bag can be made that has a surface portion of the bag film and a welded portion of the bag film.

[0059] The bamboo powder-containing bag film of the present invention contains 3 to 30 parts by mass of bamboo powder, 55 to 90 parts by mass of polyethylene resin, and 3 to 15 parts by mass of a compatibilizer. In the bamboo powder-containing bag film, the bamboo powder may be 5 parts by mass or more, or 8 parts by mass or more. The bamboo powder may be 25 parts by mass or less, or 20 parts by mass or less. The polyethylene resin may be 60 parts by mass or more, or 70 parts by mass or more. The polyethylene resin may be 85 parts by mass or less. The compatibilizer may be 5 parts by mass or more. The compatibilizer may be 12 parts by mass or less, or 10 parts by mass or less. EXAMPLES

[0060] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the following examples unless the gist of the present invention is changed.

[0061] [Materials etc.] Bamboo powder (a): Moso bamboo was cut and treated with superheated steam for 2 hours at a temperature of 210°C ± 5°C. After that, it was crushed and defibrated to produce bamboo powder with an average fiber length of about 300 μm. Compatibilizer (a): "HIWAX (registered trademark) 1105A" manufactured by Mitsui Chemicals, Inc. (maleic anhydride oxide of ethylene propylene copolymer) Compatibilizer (b): "HIWAX (registered trademark) 110P" (low molecular weight ethylene-propylene copolymer) manufactured by Mitsui Chemicals, Inc. Compatibilizer (c): "Admer (registered trademark) HE810" manufactured by Mitsui Chemicals, Inc. (maleic anhydride modified high density polyethylene) LLDPE(a): Metallocene LLDPE EVOLUE (registered trademark) “SP2520” (Prime Polymer Co., Ltd.) Density: Approximately 925 kg / m 3 (JIS K7112)

[0062] [Test Example 1] First mixing step The bamboo powder and the compatibilizer were weighed, mixed in a blender, and placed in a stainless steel deep tray. The mixing ratios of the first composition relating to the mixed test compositions (1-1) to (1-5) are shown in Table 1. Table 1 also shows the amount of polyethylene resin used in the second mixing step. The tray containing the mixed composition was placed in a constant temperature dryer for drying. The drying temperature was set at 95° C. (actual temperature: 90 to 100° C.), and the mixture was dried for 2.5 hours to obtain a first composition.

[0063] The moisture content was measured using a moisture meter "Moc63u" manufactured by Shimadzu Corporation. Approximately 20 g was weighed, and the mass change at a drying temperature of 105°C and a measurement time of 10 minutes was taken as the moisture content. The moisture content of the bamboo powder (a) before mixing was 3.7% by mass. After drying for 2.5 hours, the moisture content of the first composition of the test compositions (1-1) to (1-5) was below the lower limit of detection, confirming that the composition was sufficiently dried.

[0064] [Table 1]

[0065] Second mixing process The first composition obtained in the first mixing step and the polyethylene resin were weighed and pelletized using a pelleter of a twin-screw extruder. The mixing ratios of the mixed test compositions (1-1) to (1-5) are shown in Table 1. The extrusion temperature for pelletization was 170°C, and the mixture was extruded in the form of strands, cut, and cooled in water to solidify. The pellets were taken out of the water and placed in a stainless steel deep tray. They were then placed in a constant temperature dryer and dried in the constant temperature dryer. The drying temperature was set at 95°C (actual temperature 90 to 100°C), and the pellets were dried for 5 hours.

[0066] The moisture content was measured using a moisture meter "Moc63u" manufactured by Shimadzu Corporation, in the same manner as for the first composition. After drying for 5 hours, the moisture content of the pellets of the second composition according to the test compositions (1-1) to (1-5) was below the lower limit of detection, and it was confirmed that the pellets were sufficiently dried.

[0067] [Test Example 2] Using pellets of the second composition containing the bamboo powder, polyethylene resin, and compatibilizer obtained in Test Example 1 (test compositions (1-1) to (1-5)), inflation molding was carried out.

[0068] [Manufacturing equipment (blowing equipment)] The main specifications of the inflation molding device used in the production test are as follows: Dies: for 50mm / 70mm tubes Raw roll width: 100mm~300mm Thickness guideline: 20μm~130μm Extrusion rate: 10kg / h~20kg / h Take-off speed: 6m / min~60m / min Gusset fold width: Maximum 50mm Winding device: Maximum winding diameter φ600mm Maximum weight 40kg

[0069] 1) 50 parts by mass of the test composition (1-1) produced in Test Example 1 and 50 parts by mass of LLDPE (a) were mixed in pellet form to prepare a test composition for molding. Each test composition was blown into a film using the blown film molding apparatus (production apparatus) described above. The conditions during production were a die temperature of 185°C, a cooling blower of 38Hz, and a tension of 1.2kgf. The target thickness of the film was 60μm, and the film width was 25cm. 2) Similarly, the test composition (1-1) was replaced with each of the test compositions (1-2) to (1-5) in turn, and inflation molding was carried out.

[0070] Using any of the test compositions (1-1) to (1-5), a film having a thickness of about 60 μm, which corresponds to the target thickness, could be stably formed over a winding length of 1000 m. FIG. 3 is an image of the vicinity of the die (see die 24 in FIG. 2) when produced using the test composition (1-1). FIG. 4 is an image of the film wound into a roll. This film is brownish in color due to the color of the bamboo powder. It also has a bamboo scent. Thus, the production method according to the present invention allowed for the stable production of a bag film.

[0071] Although the test compositions (1-1) to (1-5) were all able to produce bag films, the test composition (1-5) was the most stable, followed by the test compositions (1-1), (1-3), (1-2), and (1-4) in order of ability to produce stable molding.

[0072] [Test Example 3] Bags were formed by bottom sealing using films of each test composition according to the above-mentioned Example 1. The bags thus formed are shown in Fig. 5. The upper end of each bag has a fused portion which forms an opening, and the lower end has a fused portion and a fused portion above it, which forms the bottom of the bag when used.

[0073] Figure 6 is an enlarged image of the surface of the bag. As in the figure, black granular components derived from bamboo powder are widely dispersed. The base material is also translucent and brown, and the thicker the material, the darker the color. Figure 7 shows the bag with cargo placed inside. The bag is strong enough to be used as a bag in the same way as a conventional polyethylene bag, and because it is translucent, the contents can be seen slightly through it.

[0074] [Test Example 4] In accordance with Test Example 2, a film width of 62 cm and a thickness of 30 μm was formed using the test composition (1) in a large device. This film was used to form a bag by bottom sealing. The bag produced is shown in FIG. 8. This bag is a bag that has been gusseted by folding in the width direction on both sides to provide a 7 cm fold-in section to make it easier to widen the opening. After gusseting, the width w is 48 cm and the height h is 80 cm. Both the upper and lower ends have fusion sections with the film that are adjacent to each other in the flow direction during transport to become separate bags.

[0075] In addition, both the top and bottom ends have welded sections 5 to 10 mm from the fusion cut. The top end has welded sections extending for about 7 cm from both ends in the width direction that form the handles, and an M-shaped cut is made on the inside to provide an opening.

[0076] Figure 9 is an enlarged image of the surface of the bag. Black granular components derived from bamboo powder are widely dispersed. The base material is translucent and brownish in color.

[0077] [Comparative Example 1] The test composition (1-1) was dry-blended without premixing or drying in the mass ratio, and then the mixture was poured into the feed port of the inflation molding device used in Test Example 2 and molded. The bamboo powder and polyethylene were not mixed stably and did not disperse sufficiently, resulting in uneven distribution of the bamboo powder and the formation of air bubbles believed to be due to moisture, which prevented stable molding into a strip, and breakage occurred, making it impossible to form a stable film. [Industrial Applicability]

[0078] INDUSTRIAL APPLICABILITY The present invention can be used in bag films containing bamboo powder and is industrially useful. [Explanation of symbols]

[0079] 1. Film 10 Molding equipment 21 Hopper 22 Motor 23 Screw 24 Base 3 Guide 31, 32, 33 Roller 4 Rolls

Claims

1. A first mixing step of mixing bamboo powder and a compatibilizer and drying the mixture by heating to obtain a first composition; a second mixing step of mixing the first composition with a polyethylene resin, kneading the mixture, pelletizing, and drying to obtain a second composition; A method for producing a bamboo powder-containing bag film, comprising a molding step of obtaining a film by inflation molding the second composition.

2. 2. The method according to claim 1, wherein the compatibilizer comprises at least one selected from the group consisting of low molecular weight ethylene-propylene copolymers, maleic anhydride oxides of ethylene-propylene copolymers, and maleic anhydride modified high density polyethylenes.

3. The first mixing step mixes the bamboo powder in a mass ratio of 70 to 95 parts by mass and the compatibilizer in a mass ratio of 5 to 30 parts by mass, The method according to claim 1 or 2, wherein the drying is carried out at a heating temperature of 70 to 120° C. for 30 minutes or more.

4. The method according to claim 3 , wherein the water content of the first composition after drying is 0.5% by mass or less.

5. The second mixing step mixes the first composition in a mass ratio including 3 to 35 parts by mass and 65 to 97 parts by mass of the polyethylene resin, The method according to any one of claims 1 to 4, which comprises kneading the mixture at a melting temperature of 150 to 190°C, pelletizing the mixture, and drying the mixture at a heating temperature of 70 to 120°C for 30 minutes or more.

6. The manufacturing method according to any one of claims 1 to 5, wherein the molding step comprises mixing 40 to 100 parts by mass of pellets of the second composition and 0 to 60 parts by mass of pellets of a polyethylene resin and molding the mixture.

7. The manufacturing method described in any one of claims 1 to 6, wherein the bamboo powder is treated with superheated steam at 180 to 320°C and has an average fiber length of 400 μm or less.

8. A method for manufacturing a bag, comprising a processing step of processing a bamboo powder-containing bag film according to any one of claims 1 to 7 to provide a welded portion at the bottom seal or side seal.

Citation Information

Patent Citations

  • Easy-to-tear anti-mold and anti-bacterial bamboo fiber thin film and preparation process thereof

    CN106916365A

  • Bamboo fiber, method of manufacturing the same, and method of manufacturing composite material using the bamboo fiber

    JP2012040701A

  • Compact for laying

    JP2014009539A

  • Composite molding

    JP2015000921A

  • Bamboo powder mixed resin sheet and bamboo powder mixed resin film and applied product thereof

    JP2016023282A