Non-thermoplastic polyimide film, polyimide laminate film, method for producing non-thermoplastic polyimide film, and method for producing polyimide laminate film
A polyimide laminate film with a phase-separated structure of non-thermoplastic and solvent-soluble polyimides addresses the issue of cracks in via formation, maintaining board integrity by reducing stress through a novel film composition.
Patent Information
- Application Number
- JP2020170913
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-10-09
- Publication Date
- 2024-10-07
- Estimated Expiration
- 2040-10-09
AI Technical Summary
Existing methods for forming vias in polyimide laminated films for flexible printed circuit boards using lasers result in cracks and peeling due to residual stress during the desmear process, which current solutions like heat treatment do not adequately address.
A polyimide laminate film composed of a non-thermoplastic polyimide precursor and solvent-soluble polyimide, forming a phase-separated structure with polyimide domains of 10 μm or less, which reduces stress and prevents cracks during via formation.
The film effectively suppresses cracks on the inner walls of vias during the via formation process without altering the manufacturing process, ensuring the integrity of the flexible printed circuit boards.
Smart Images

Figure 0007562362000005 
Figure 0007562362000001 
Figure 0007562362000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a polyimide laminate film for flexible printed circuit boards that suppresses the occurrence of cracks on the inner walls of vias in a process of forming vias in the polyimide laminate film by using a laser, and a method for producing the polyimide laminate film. [Background technology]
[0002] Among the flexible printed circuit boards (hereafter referred to as FPCs) used in tablets, smartphones, etc., two-layer flexible printed circuit boards (hereafter referred to as two-layer FPCs) that use polyimide film are seeing growing demand in the market due to their excellent heat resistance. When manufacturing these FPCs, copper foil is attached to both sides of the polyimide film to create a copper-clad laminate, and there is a process in which holes (vias) are formed in this copper-clad laminate for the purpose of forming circuits, and the inner surface of the vias is copper-plated to ensure electrical continuity between the top and bottom of the laminate.
[0003] There are two types of via formation process: the through-hole method, in which a drill or laser is used to open a through hole in the copper foil on both sides, and the blanked via-hole method, in which only the copper foil on one side is etched and the insulating layer is removed with a laser, leaving the copper foil on the other side. In particular, the blanked via-hole method is used frequently for fine FPCs in order to make effective use of the area.
[0004] After the vias are formed, wet desmearing (cleaning with an alkaline potassium permanganate aqueous solution) is often performed to remove and clean the resin residues adhering to the inside of the vias and the copper foil surface. However, residual stress accumulates locally in the laser processing area used for via formation, and the desmearing process after via formation can cause defects such as cracks and peeling around the vias, which is an issue. Patent Document 1 discloses a method of suppressing the occurrence of defects such as cracks by performing heat treatment after laser processing to reduce residual stress, and Patent Document 2 discloses polyimide with improved resistance to alkaline solutions as a measure to prevent defects, but no process has been found that fundamentally prevents this problem from occurring. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2012-186377 A [Patent Document 2] JP 2017-179148 A Summary of the Invention [Problem to be solved by the invention]
[0006] The present invention provides a polyimide laminate film that suppresses the occurrence of cracks on the inner walls of vias in a process of forming vias in a polyimide laminate film for flexible printed circuit boards using a laser. [Means for solving the problem]
[0007] It has been found that a polyimide laminate film obtained from a mixture of a non-thermoplastic polyimide precursor and a solvent-soluble polyimide can provide a polyimide laminate film that suppresses the generation of cracks on the inner wall of a via after a via formation process using a laser.
[0008] [1] A method for producing a non-thermoplastic polyimide film by producing a non-thermoplastic polyimide film by imidizing a mixture of a non-thermoplastic polyimide precursor (polyamic acid) and a solvent-soluble polyimide, and then forming a phase-separated structure in the film having domains of solvent-soluble polyimide with island structures of 10 μm or less.
[0009] [2] The non-thermoplastic polyimide film according to [1], wherein the inflection point temperature of the film obtained from the solvent-soluble polyimide used in the production of the non-thermoplastic polyimide film is 290°C or lower.
[0010] [3] The non-thermoplastic polyimide film according to [1] or [2], characterized in that the weight average molecular weight of the non-thermoplastic polyimide precursor (polyamic acid) used in the production of the non-thermoplastic polyimide film is 150,000 or more.
[0011] [4]. The diamine compound used in the solvent-soluble polyimide is 2,2-bis(4-aminophenyl)hexafluoropropane, 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane, 2,2'-bis[4-(4-amino-2-trifluoromethylphenoxy)phenyl]hexafluoropropane, 4,4'-bis[4-(4-amino-2-trifluoromethyl)phenoxy]-octafluorobiphenyl, bis[4-(4-aminophenoxy)phenyl]sulfone, 1,3-bis[2-(4-aminophenyl)-2-propyl]benzene, bis[4-(3-aminophenoxy)phenyl] The method for producing a non-thermoplastic polyimide film according to any one of [1] to [3], characterized in that the polyimide film contains one or more compounds selected from the group consisting of sulfone, 1,1-bis(4-aminophenyl)cyclohexane, 9,9-bis(4-amino-3-fluorophenyl)fluorene, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 1,4-bis[2-(4-aminophenyl)-2-propyl]benzene, 1,3-bis(3-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 4,4'-bis(4-aminophenoxy)biphenyl, and 1,4-bis(4-aminophenoxy)benzene.
[0012] [5]. The non-thermoplastic polyimide film according to any one of [1] to [4], characterized in that the acid dianhydride used in the solvent-soluble polyimide contains one or more compounds selected from 2,2'-hexafluoropropylidenediphthalic dianhydride, 3,3',4,4'-perfluoroisopropylidenediphthalic dianhydride, 3,3',4,4'-diphenylsulfonetetracarboxylic dianhydride, 9,9-bis(3,4-dicarboxyphenyl)fluorene dianhydride, dicyclohexyl-3,4,3',4'-tetracarboxylic dianhydride, and ethylenediaminetetraacetic dianhydride.
[0013] [6] The method for producing a non-thermoplastic polyimide film according to any one of [1] to [5], wherein the solvent-soluble polyimide used in the production of the non-thermoplastic polyimide film contains 2,2-bis(4-aminophenoxyphenyl)propane.
[0014] [7] A method for producing a polyimide laminate film, comprising forming a thermoplastic polyimide resin layer on at least one side of a non-thermoplastic polyimide film produced by the method for producing a non-thermoplastic polyimide film according to any one of [1] to [6].
[0015] [8] A non-thermoplastic polyimide film characterized by forming a phase-separated structure having domains of solvent-soluble polyimide with island structures of 10 μm or less and domains of non-thermoplastic polyimide with a sea structure within the film.
[0016] [9] The non-thermoplastic polyimide film according to [8], wherein the inflection point temperature of the film obtained from the solvent-soluble polyimide used in the production of the non-thermoplastic polyimide film is 290°C or lower.
[0017]
[10] The non-thermoplastic polyimide film according to [8] or [9], characterized in that the weight average molecular weight of the non-thermoplastic polyimide precursor (polyamic acid) used in the production of the non-thermoplastic polyimide film is 150,000 or more.
[0018]
[11] . The diamine compound used in the solvent-soluble polyimide is 2,2-bis(4-aminophenyl)hexafluoropropane, 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane, 2,2'-bis[4-(4-amino-2-trifluoromethylphenoxy)phenyl]hexafluoropropane, 4,4'-bis[4-(4-amino-2-trifluoromethyl)phenoxy]-octafluorobiphenyl, bis[4-(4-aminophenoxy)phenyl]sulfone, 1,3-bis[2-(4-aminophenyl)-2-propyl]benzene, bis[4-(3-aminophenoxy)phenyl] The non-thermoplastic polyimide film according to any one of [8] to
[10] , characterized in that it contains one or more compounds selected from the group consisting of 1,1-bis(4-aminophenyl)cyclohexane, 9,9-bis(4-amino-3-fluorophenyl)fluorene, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 1,4-bis[2-(4-aminophenyl)-2-propyl]benzene, 1,3-bis(3-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 4,4'-bis(4-aminophenoxy)biphenyl, and 1,4-bis(4-aminophenoxy)benzene.
[0019]
[12] . The non-thermoplastic polyimide film according to any one of [8] to
[11] , characterized in that the acid dianhydride used in the solvent-soluble polyimide contains one or more compounds selected from 2,2'-hexafluoropropylidenediphthalic dianhydride, 3,3',4,4'-perfluoroisopropylidenediphthalic dianhydride, 3,3',4,4'-diphenylsulfonetetracarboxylic dianhydride, 9,9-bis(3,4-dicarboxyphenyl)fluorene dianhydride, dicyclohexyl-3,4,3',4'-tetracarboxylic dianhydride, and ethylenediaminetetraacetic dianhydride.
[0020]
[13] The non-thermoplastic polyimide film according to any one of [8] to
[12] , wherein the solvent-soluble polyimide used in the production of the non-thermoplastic polyimide film contains 2,2-bis(4-aminophenoxyphenyl)propane.
[0021]
[14] A polyimide laminate film, comprising the non-thermoplastic polyimide film according to any one of [8] to
[13] and a thermoplastic polyimide resin layer formed on at least one surface of the non-thermoplastic polyimide film. Effect of the Invention
[0022] The polyimide laminate obtained by the present invention can provide a flexible printed circuit board that suppresses cracks on the inner walls of vias that occur during the via formation process by laser processing, without any special changes to the film production process. [Brief description of the drawings]
[0023] [Figure 1] FIG. 1 is a diagram showing an example of an optical microscope image used for actual discrimination in a hole crack test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0024] In the present invention, it has been found that a non-thermoplastic polyimide film is produced by imidizing a mixture of a non-thermoplastic polyimide precursor (polyamic acid) and a solvent-soluble polyimide, and a phase-separated structure having an island structure of solvent-soluble polyimide domains of 10 μm or less is formed in the film, and a polyimide laminate film that suppresses the generation of cracks on the inner wall of a via after a via formation process using a laser can be obtained. Details are described below.
[0025] (Non-thermoplastic polyimide film) The non-thermoplastic polyimide film used in the polyimide laminate film of the present invention is a non-thermoplastic polyimide film characterized by forming a phase separation structure having soluble polyimide domains with island structures of 10 μm or less and non-thermoplastic polyimide domains with a sea structure in the film, and the non-thermoplastic polyimide and polyimide precursor (polyamic acid) that constitute this sea structure are not particularly limited.
[0026] (Non-thermoplastic polyimide precursors (polyamic acids)) In particular, film materials used in polyimide laminate films for flexible printed circuit boards preferably contain rigid structures such as biphenyl structures and phenyl structures in the polymer molecules from the viewpoint of dimensional stability, etc. Furthermore, biphenyl structures are less symmetrical than phenyl structures, and a decrease in the symmetry of the polymer primary structure inhibits molecular packing, so that the elastic modulus decreases when softened above a certain temperature, making them more preferable from the viewpoint of stress relaxation.
[0027] Specific examples of diamine monomers having a biphenyl structure include 4,4'-diamino-2,2'-dimethylbiphenyl, 4,4'-diaminobiphenyl, 4,4'-diamino-2,2'-dimethylbiphenyl, 4,4'-diamino-3,3'-dimethylbiphenyl, 4,4'-diamino-2,2'-dimethoxybiphenyl, 4,4'-diamino-3,3'-dimethoxybiphenyl, 3,3',5,5'-tetramethylbenzidine, and 4,4'-bis(4-aminophenoxy)biphenyl. However, 4,4'-diaminobiphenyl and 4,4'-diamino-3,3'-dimethylbiphenyl are carcinogenic to humans, so they are not preferred for practical use. For practical use, 4,4'-diamino-2,2'-dimethylbiphenyl is particularly preferred.
[0028] In addition, among 100% of the diamine monomer components constituting the non-thermoplastic polyimide precursor (polyamic acid), the more rigid monomer components there are, the lower the linear expansion coefficient due to the formation of an aggregate structure, and the more effective the film is for excellent dimensional stability, but if the content is too high, the linear expansion coefficient of the resulting film becomes too low, which is not preferable, and the optimal content for a film for flexible printed circuit boards is preferably 10 to 50 mol%, more preferably 15 to 40 mol%, and even more preferably 20 to 35 mol%. As other diamine monomers to be used, aromatic diamines with high heat resistance are preferable. For example, 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 1,3-bis(4-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, 4,4'-diaminodiphenylpropane, 4,4'-diaminodiphenylmethane, benzidine, 3,3'-dichlorobenzidine, 4,4'-diaminodiphenyl sulfide, 3,3'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl ether, 3,3'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 1,5-diaminonaphthalene, 4,4'-diaminodiphenyldiethylsilane, 4,4'-diaminodiphenylsilane, 4,4'-diaminodiphenylethylphosphine oxide, 4,4'-diaminodiphenyl N-methylamine, 4,4'-diaminodiphenyl Examples of the diamine include N-phenylamine, 1,4-diaminobenzene (p-phenylenediamine), 1,3-diaminobenzene, and 1,2-diaminobenzene. The content of the other diamine used is preferably 50 to 90 mol %, more preferably 60 to 85 mol %, and further preferably 65 to 80 mol %.
[0029] It is preferable to use a combination of 4,4'-diaminodiphenyl ether and paraphenylenediamine, since this allows adjustment of the flexibility of the polymer while maintaining high heat resistance. In this case, the content of 4,4'-diaminodiphenyl ether is preferably 40 to 70 mol%, more preferably 45 to 65 mol%, and even more preferably 50 to 65 mol%, and the content of paraphenylenediamine is preferably 10 to 50 mol%, more preferably 15 to 40 mol%, and even more preferably 15 to 30 mol%.
[0030] As the acid dianhydride monomer used in the non-thermoplastic polyimide precursor (polyamic acid) of the present invention, an aromatic acid dianhydride is preferred from the viewpoint of heat resistance.
[0031] For example, pyromellitic dianhydride, 2,3,6,7-naphthalenetetracarboxylic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 1,2,5,6-naphthalenetetracarboxylic dianhydride, 2,2',3,3'-biphenyltetracarboxylic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, 2,2',3,3'-benzophenonetetracarboxylic dianhydride, 4,4'-oxyphthalic dianhydride, 3,4'-oxyphthalic dianhydride, 2,2-bis(3,4-dicarboxyphenyl)propanoic dianhydride, 3,4,9,10-perylenetetracarboxylic dianhydride, bis(3, 4-dicarboxyphenyl)propanoic dianhydride, 1,1-bis(2,3-dicarboxyphenyl)ethaneic dianhydride, 1,1-bis(3,4-dicarboxyphenyl)ethaneic dianhydride, bis(2,3-dicarboxyphenyl)methaneic dianhydride, bis(3,4-dicarboxyphenyl)ethaneic dianhydride, oxydiphthalic dianhydride, bis(3,4-dicarboxyphenyl)sulfonic dianhydride, p-phenylene bis(trimellitic acid monoester acid anhydride), ethylene bis(trimellitic acid monoester acid anhydride), bisphenol A bis(trimellitic acid monoester acid anhydride), and the like.
[0032] Since the non-thermoplastic polyimide film of the present invention is required to have heat resistance, it is preferable to use 3,3',4,4'-biphenyltetracarboxylic dianhydride or pyromellitic dianhydride, and since it contains a biphenyl structure, 3,3',4,4'-biphenyltetracarboxylic dianhydride is more preferable. Of the 100% acid dianhydride monomer components constituting the non-thermoplastic polyimide film, the content of 3,3',4,4'-biphenyltetracarboxylic dianhydride is preferably 20 to 60 mol%, more preferably 25 to 55 mol%, and even more preferably 30 to 50 mol%. When pyromellitic dianhydride is contained, of the 100% acid dianhydride monomer components constituting the non-thermoplastic polyimide film, the content of pyromellitic dianhydride is preferably 40 to 80 mol%, more preferably 35 to 75 mol%, and even more preferably 50 to 70 mol%.
[0033] (Production of non-thermoplastic polyimide precursors (polyamic acids)) The non-thermoplastic polyimide precursor in the present invention refers to polyamic acid before imidization, and any known method or a combination thereof can be used for its production. The polymerization method for producing the non-thermoplastic polyimide precursor is characterized by the order of addition of the monomers, and the physical properties of the polyimide obtained can be controlled by controlling the order of addition of the monomers. Therefore, any method of adding monomers can be used for producing the non-thermoplastic polyimide precursor in the present invention. Representative polymerization methods include the following methods.
[0034] For example, it can be produced by the following steps (Aa) to (Ab). (Aa): A process for reacting an aromatic diamine with an aromatic acid dianhydride in an organic polar solvent with an excess of the aromatic diamine to obtain a prepolymer having amino groups at both ends. (Ab): A step of adding an aromatic diamine having a structure different from that used in step (Aa), and further adding an aromatic acid dianhydride having a structure different from that used in step (Aa) so that the aromatic diamine and aromatic acid dianhydride are substantially equimolar in all steps, to polymerize.
[0035] Alternatively, it is also possible to obtain a non-thermoplastic polyimide precursor through the following steps (Ba) to (Bb). (Ba): a process for reacting an aromatic diamine with an aromatic dianhydride in an organic polar solvent with an excess of the aromatic dianhydride to obtain a prepolymer having an acid anhydride group at both ends, (Bb): a process for adding an aromatic dianhydride having a structure different from that used in the process (Ba), and further adding an aromatic diamine having a structure different from that used in the process (Ba) so that the aromatic diamine and aromatic dianhydride are substantially equimolar in all the processes, and polymerizing the resultant.
[0036] In the present invention, a synthesis method in which the order of addition is set so that a specific diamine or acid dianhydride is selectively bonded to any diamine or acid dianhydride (for example, steps (Aa) to (Ab) and (Ba) to (Bb)) is called sequence polymerization. Among the polymers obtained by sequence polymerization, those with two block components are called diblock copolymers, and those with three block components are called triblock copolymers. In contrast, in the present invention, a synthesis method in which the order of addition of the diamine and acid dianhydride to be bonded is not selected is called random polymerization. A polymer obtained by random polymerization is called a random copolymer. In the present invention, sequence polymerization is more preferable than random polymerization as a polymerization method for obtaining a polyimide resin that is effective in suppressing film tearing while maintaining the properties as a flexible metal-clad laminate.
[0037] The solid content of the precursor for the non-thermoplastic polyimide film of the present invention is not particularly limited, and is usually 5% by weight to 35% by weight, preferably 10% by weight to 30% by weight. When the concentration is within this range, a polyimide precursor with an appropriate molecular weight is easily obtained.
[0038] A filler may be added to the non-thermoplastic non-thermoplastic polyimide precursor of the present invention for the purpose of improving various film properties such as sliding properties, thermal conductivity, electrical conductivity, corona resistance, loop stiffness, etc. Any filler may be used, but preferred examples include silica, titanium oxide, alumina, silicon nitride, boron nitride, calcium hydrogen phosphate, calcium phosphate, mica, etc.
[0039] (Molecular weight of non-thermoplastic polyimide precursor (polyamic acid)) In addition, in the non-thermoplastic polyimide precursor used in the present invention, a higher molecular weight is preferable from the viewpoints of facilitating the formation of a phase-separated structure with the solvent-soluble polyimide and of providing an excellent crack improvement effect due to stress relaxation. The average molecular weight of the precursor (polyamic acid) measured in terms of PEG (polyethylene glycol) by GPC is preferably 150,000 or more, and more preferably 200,000 or more.
[0040] (Solvent-soluble polyimide) The diamines and acid dianhydrides used in the production of the solvent-soluble polyimide having an island structure in the present invention include the same as those used in the non-thermoplastic polyimide described above, but a flexible film is preferred because it forms a phase-separated structure as an island structure and is particularly excellent in mitigating stress applied during processing of the laminated film, and the above monomers can be used without any particular limitation. For example, 2,2-bis(4-aminophenyl)hexafluoropropane, 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane, 2,2'-bis[4-(4-amino-2-trifluoromethylphenoxy)phenyl]hexafluoropropane, 4,4'-bis[4-(4-amino-2-trifluoromethyl)phenoxy]-octafluorobiphenyl, bis[4-(4-aminophenoxy)phenyl]sulfone, 1,3-bis[2-(4-aminophenyl)-2-propyl]benzene, bis[4-(3 ... Examples of such bis(4-aminophenyl)sulfone, 1,1-bis(4-aminophenyl)cyclohexane, 9,9-bis(4-amino-3-fluorophenyl)fluorene, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 1,4-bis[2-(4-aminophenyl)-2-propyl]benzene, 1,3-bis(3-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 4,4'-bis(4-aminophenoxy)biphenyl, and 1,4-bis(4-aminophenoxy)benzene.
[0041] In particular, from the viewpoint of excellent stress relaxation, it is preferable to use 2,2-bis(4-aminophenoxyphenyl)propane as the monomer. Examples of acid dianhydrides used in the production of the solvent-soluble polyimide include 2,2'-hexafluoropropylidenediphthalic dianhydride, 3,3',4,4'-perfluoroisopropylidenediphthalic dianhydride, 3,3',4,4'-diphenylsulfonetetracarboxylic dianhydride, 9,9-bis(3,4-dicarboxyphenyl)fluorene dianhydride, dicyclohexyl-3,4,3',4'-tetracarboxylic dianhydride, and ethylenediaminetetraacetic dianhydride.
[0042] In order to obtain a solvent-soluble polyimide, it is preferable to react a diamine having a fluorine group with an acid dianhydride (particularly an aromatic acid dianhydride) in combination, since this improves the solubility in the solvent.
[0043] Examples of diamines having a fluorine group include 2,2-bis(4-aminophenyl)hexafluoropropane, 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane, 2,2'-bis[4-(4-amino-2-trifluoromethylphenoxy)phenyl]hexafluoropropane, and 4,4'-bis[4-(4-amino-2-trifluoromethyl)phenoxy]-octafluorobiphenyl. Similarly, the acid dianhydride compound preferably contains a fluorine group. Specifically, examples of the acid dianhydride include 2,2'-hexafluoropropylidenediphthalic dianhydride and 3,3',4,4'-perfluoroisopropylidenediphthalic dianhydride. In the polymer, the total content of these diamines or acid dianhydride monomers having a fluorine group is preferably 40 to 90 mol%, more preferably 60 to 85 mol%, and even more preferably 65 to 80 mol%.
[0044] (Inflection point temperature of storage modulus of solvent-soluble polyimide) In the solvent-soluble polyimide having the island structure of the present invention, the temperature at which the storage modulus in the glass region is inflection-point measured by dynamic viscoelasticity measurement (referred to as the E' inflection-point temperature) is preferably 290° C. or lower, more preferably 250° C. or lower, from the viewpoint of easily relaxing the stress in the film that occurs when cooling the high heat generated when laser processing the film laminate. A temperature of 180° C. or lower is also not preferred, since it may not be able to withstand the temperature applied during solder mounting on a flexible substrate, causing problems such as foaming.
[0045] (Molecular weight of solvent-soluble polyimide) In the solvent-soluble polyimide used in the present invention, a higher molecular weight is preferred from the viewpoint of excellent crack resistance due to improved toughness and strength of the resin. On the other hand, if the molecular weight is too large, the polyimide may not dissolve in the solvent, so there is an optimum range. The weight-average molecular weight of the solvent-soluble polyimide measured in terms of PEG (polyethylene glycol) by GPC is preferably 50,000 to 200,000, and more preferably 100,000 to 150,000.
[0046] (Non-thermoplastic polyimide film having a phase-separated structure) The non-thermoplastic polyimide film of the present invention is characterized by having a phase-separated structure having solvent-soluble polyimide domains with island structures of 10 μm or less and non-thermoplastic polyimide domains with sea structures in the film, and can suppress the occurrence of cracks after a desmearing process by mitigating the stress remaining in the film due to the heat generated during hole formation by laser processing in a flexible metal-clad laminate produced using the polyimide laminate film. Moreover, the domain size of the island-structured solvent-soluble polyimide is preferably 10 μm or less, more preferably 7 μm or less, and even more preferably 5 μm or less, because if the size is too large, the interface between the sea structure and the island structure becomes small and the generated stress cannot be sufficiently dispersed. The lower limit of the size is preferably 0.3 μm or more from the viewpoint of stress relaxation. Moreover, the domain size can be observed and measured by general TEM observation.
[0047] (Method of manufacturing a non-thermoplastic polyimide film having a phase-separated structure) The non-thermoplastic polyimide film of the present invention is characterized in that it has a phase-separated structure having solvent-soluble polyimide domains with island structures of 10 μm or less and non-thermoplastic polyimide domains with sea structures in the film, and the method for producing it is not particularly limited. In particular, a method for easily forming a uniform phase-separated structure in the film includes a method in which a non-thermoplastic polyimide precursor (polyamic acid) and a solvent-soluble polyimide solution are mixed in advance and the mixture is imidized.
[0048] In this case, the mixing temperature is about −20° C. to 50° C., preferably 10° C. to 45° C., and more preferably 20° C. to 40° C. If the temperature is lower than this range, the torque may become too high and uniform mixing may not be possible, and if the temperature is higher, partial compatibility may occur, or the precursor may decompose, making it impossible to form a uniform phase-separated structure. The mixing time is preferably 3 hours or more, and more preferably 5 hours or more. If the mixing time is too short, the polyimide precursor may not be uniformly dispersed and a phase-separated structure may not be formed, which is not preferable.
[0049] (Method of manufacturing polyimide film) The method for obtaining the non-thermoplastic polyimide film of the present invention is not particularly limited, and various known methods can be applied. For example, it is preferable that the method includes the following steps i) to iv): i) reacting an aromatic diamine with an aromatic tetracarboxylic dianhydride in an organic solvent to obtain a mixture of a non-thermoplastic polyimide precursor and a solvent-soluble polyimide solution; ii) a step of casting the film-forming dope containing the polyimide precursor from a die onto a support to form a resin layer (which may also be referred to as a liquid film); iii) heating the resin layer on the support to form a self-supporting gel film, and then peeling the gel film off the support; iv) A step of further heating to convert the remaining amic acid into an imidized form and drying to obtain a non-thermoplastic polyimide film.
[0050] ii) The steps after this can be broadly divided into thermal imidization and chemical imidization. Thermal imidization is a method in which a polyimide precursor solution is cast onto a support as a film-forming dope without using a dehydrating ring-closing agent, and imidization is promoted only by heating. On the other hand, chemical imidization is a method in which at least one of a dehydrating ring-closing agent and a catalyst is added to a polyimide precursor solution as an imidization promoter, and the resulting solution is used as a film-forming dope to promote imidization. Either method may be used, but the chemical imidization method is more productive.
[0051] As the dehydration ring-closing agent, an acid anhydride such as acetic anhydride can be suitably used. As the catalyst, a tertiary amine such as an aliphatic tertiary amine, an aromatic tertiary amine, or a heterocyclic tertiary amine can be suitably used. As the support for casting the film-forming dope, a glass plate, an aluminum foil, an endless stainless steel belt, a stainless steel drum, or the like can be suitably used. The heating conditions are set according to the thickness and production speed of the film to be finally obtained, and at least one of partial imidization and drying is performed, and then the film is peeled off from the support to obtain a polyimide precursor film (hereinafter referred to as a gel film). The ends of the gel film are fixed to avoid shrinkage during curing, and the film is heated to remove water, residual solvent, imidization promoter, dehydration ring-closing agent, etc. from the gel film, and the remaining amic acid is completely imidized to obtain a film containing polyimide. The heating conditions may be appropriately set according to the thickness and production speed of the film to be finally obtained.
[0052] (Production of polyimide laminated film) The polyimide laminate film of the present invention is a polyimide laminate film laminate obtained by laminating a thermoplastic polyimide resin layer on at least one side of the non-thermoplastic polyimide film, and the method for producing the polyimide laminate film is not particularly limited, and various known methods can be applied. For example, a co-extrusion die may be used to simultaneously form multiple resin layers containing a polyimide precursor, which is a precursor of the non-thermoplastic polyimide film of the present invention, and a thermoplastic polyimide precursor that can be an adhesive layer. In addition, a precursor of the non-thermoplastic polyimide film of the present invention may be synthesized, and the polyimide film obtained by forming the precursor into a film using the precursor may be collected, and then a resin layer containing another thermoplastic polyimide precursor may be formed on the polyimide film by coating or the like. Since a very high temperature is required for imidization, when a resin layer other than polyimide is provided, it is preferable to adopt the latter method in order to suppress thermal decomposition. When a thermoplastic polyimide resin layer is provided by coating, a thermoplastic polyimide precursor may be applied and then imidized, or a thermoplastic polyimide solution capable of forming a thermoplastic polyimide resin layer may be applied and dried. It is also possible to perform various surface treatments such as corona treatment and plasma treatment on the outermost surface of the polyimide laminate film. The overall thickness of the polyimide laminate film of the present invention is preferably 6 to 60 μm. Within this range, a thinner thickness is preferable from the viewpoint of reducing the weight of the FPC and improving the foldability, and for example, 7 to 30 μm is more preferable, and 10 to 25 μm is even more preferable.
[0053] In addition, in order to suppress warping of the polyimide laminate film, it is preferable that both sides of the non-thermoplastic polyimide layer are thermoplastic polyimide layers. When a thermoplastic polyimide layer is formed on only one side of the non-thermoplastic polyimide layer, the film may warp when the imidization reaction of the thermoplastic polyimide layer is allowed to proceed because of an asymmetric structure. The thickness of the thermoplastic polyimide layer on both sides of the non-thermoplastic polyimide layer is preferably 1 to 15 μm, and the difference in thickness between both sides is based on the thickness of the thick thermoplastic polyimide layer, and as long as the thickness of the other side is 40% or more and 100% or less, there is no problem with the film shape.
[0054] The thickness ratio of the non-thermoplastic polyimide layer and the thermoplastic polyimide layer in the multilayer polyimide film is preferably 55 / 45 to 95 / 5 in terms of controlling the linear expansion coefficient of the multilayer polyimide film. This ratio is the ratio of the total thickness of each of the non-thermoplastic polyimide layer and the thermoplastic polyimide layer even if the non-thermoplastic polyimide layer and the thermoplastic polyimide layer are multiple layers, and it is preferable that the thickness does not exceed the thickness of the non-thermoplastic polyimide layer even if the number of thermoplastic polyimide layers is increased.
[0055] (Flexible metal clad laminate) A flexible metal-clad laminate can be produced by laminating a metal foil on at least one side of a polyimide laminate film. The method for producing a flexible metal-clad laminate is not particularly limited, and various known methods can be applied. For example, a continuous process using a hot roll laminator having one or more pairs of metal rolls or a double belt press (DBP) can be used. The specific configuration of the means for carrying out the hot lamination is not particularly limited, but it is also preferable to place a protective material between the pressing surface and the metal foil in order to improve the appearance of the resulting laminate.
[0056] A means of casting a multi-layer organic solvent solution containing at least one of a thermoplastic polyimide precursor or a non-thermoplastic polyimide precursor on a metal foil can also be used. The means of casting an organic solvent solution containing a polyimide precursor on a metal foil is not particularly limited, and conventionally known means such as a die coater, a comma coater (registered trademark), a reverse coater, and a knife coater can be used. In the case of providing a polyimide resin layer in multiple layers, such as a case in which the thermoplastic polyimide resin layer and a non-thermoplastic polyimide film in the present invention are included, or in the case of providing a resin layer other than polyimide, a means of repeating the above casting and heating steps multiple times, or forming a multi-layer cast layer by co-extrusion or continuous casting and heating it at once is preferably used. In this means, a flexible metal-clad laminate is obtained at the same time as the imidization is completed. When providing metal foil on both sides of the resin layer, the metal foil may be laminated on the opposite resin layer surface by heating and pressing. The metal foil is not particularly limited, and any metal foil can be used. For example, copper, stainless steel, nickel, aluminum, and alloys of these metals can be preferably used. Furthermore, in general metal-clad laminates, copper such as rolled copper and electrolytic copper is often used, and it can also be used in the present invention.
[0057] In addition, the metal foil can be selected from those having various properties such as surface treatment and surface roughness depending on the purpose. Furthermore, the surface of the metal foil may be coated with an anti-rust layer, a heat-resistant layer, or an adhesive layer. The thickness of the metal foil is not particularly limited, and may be any thickness that can exhibit sufficient function depending on the application.
[0058] (Via formation process using laser processing) In flexible circuit board manufacturing, when forming vias in copper-clad laminates by laser processing, the laser can be irradiated to the processing area to penetrate the board and form through-holes (TH) or blind via holes (BVH) by removing only the copper foil and polyimide resin on the top surface. Known types of lasers can be used. Short-wavelength lasers such as UV-YAG lasers and excimer lasers are preferred because they have a very high absorption rate for both resin and copper and can be used for processing. For THs, a method of directly drilling through holes is also widely used.
[0059] On the other hand, a desmear treatment is performed to remove resin debris generated during processing. A wet desmear treatment is generally used, which includes a swelling step using an aqueous alkali solution or a solution containing an organic solvent, a roughening step using an aqueous alkali solution such as sodium permanganate or potassium permanganate, and a neutralization step. Cracks on the inner wall of a hole that occur during processing of a copper-clad laminate using the polyimide laminate film of the present invention often occur on the inner wall of the hole after the desmear treatment, and cracks are more likely to occur if the swelling time and roughening time in the desmear treatment are extended. In addition, a via is formed by metal plating the inside of the hole after the desmear treatment. There is no particular restriction as long as it is a general metal plating, but a plating layer of a desired thickness may be formed only by electroless copper plating, or a plating layer of a desired thickness may be formed by electrolytic copper plating after thinning an electroless copper plating layer.
[0060] (Hole crack test: Crack evaluation method) Cracks that occur on the inner wall of a via during FPC manufacturing are usually detected after FPC manufacturing by visual inspection, etc. The inventors discovered that the occurrence of cracks on the inner wall of a via during the FPC manufacturing process can be easily evaluated by cutting a test piece from the long flexible metal-clad laminate material and conducting a hole crack test to evaluate cracks that occur on the inner wall of a hole at the stage of the via formation process from laser processing to desmear processing.
[0061] In this evaluation method, the copper foil of the test piece after the desmear treatment is removed by etching, and the presence or absence of cracks on the inner wall of the via can be confirmed by observing with a polarizing microscope under crossed Nicols. It was confirmed by combining with the polarizing microscope observation that if a crack occurs on the inner wall of the via, it is detected as light leakage. EXAMPLES
[0062] The present invention will be specifically described below with reference to examples, but is not limited to these examples.
[0063] (Inflection point temperature evaluation) Using a DM6100 manufactured by SII Nano Technology, dynamic viscoelasticity was measured in an air atmosphere, and the storage modulus and inflection point temperature at each temperature were measured. Sample measurement range: width 9 mm, gripping distance: 20 mm Measurement temperature range: 0℃~440℃ Heating rate: 3℃ / min Strain amplitude: 10 μm Measurement frequency; 1Hz, 5Hz, 10Hz Minimum tension / compression force: 100mN Tension / Compression Gain: 1.5 Initial force amplitude: 100mN
[0064] (molecular weight measurement) The weight average molecular weight (Mw) was evaluated under the following conditions. [Table 1]
[0065] (TEM observation) The films used for observation were embedded in resin and ultrathin sections were prepared using an ultramicrotome (Leica UCT). Using a transmission electron microscope (TEM, Hitachi High-Technologies, H-7650), the presence or absence of sea-island structures and the domain size were measured from TEM images at 40,000x magnification at an accelerating voltage of 100 kV.
[0066] (Hole crack test) A 12 μm electrolytic copper foil (3EC-M3S-HTE, Mitsui Metal) was placed on both sides of the polyimide film laminate obtained in the examples and comparative examples, and a protective film (Apical 125NPI; Kaneka, thickness 125 μm) was used on both sides of the copper foil, and thermal lamination was performed under the conditions of lamination temperature 360 ° C, lamination pressure 265 N / cm (27 kgf / cm), and lamination speed 1.0 m / min to obtain a flexible metal-clad laminate. Next, the flexible metal-clad laminate was cut into a size of 5.0 cm × 20.0 cm square, and a blind via hole with a diameter of 100 μm was laser processed using a UV-YAG laser by the process of Table 2. A pattern of 10 rows of 10 pieces each was formed at 1 mm intervals for each condition (100 pieces each). After laser processing, desmear processing was performed by the process of Table 3.
[0067] After removing the copper foil by etching, the specimens were observed under a polarizing microscope at a magnification of 200x under crossed Nicols. Holes where light leaked were deemed to be cracks. In cases where the degree of light leakage was too weak to be determined, the cross section of the hole was cut and observed under a higher magnification such as an electron microscope to determine whether or not it was a crack and to classify it. Figure 1 shows an example of an optical microscope image used for the actual discrimination. After observing 100 specimens, the proportion of specimens that had cracks was calculated as a percentage. [Table 2] [Table 3]
[0068] (Synthesis of non-thermoplastic polyamic acid (polyimide precursor)) (Synthesis Example 1) In a 2000 ml glass flask, 334.13 g of N,N-dimethylformamide (hereinafter, DMF) and 17.70 g of 4,4'-diaminodiphenyl ether (hereinafter, ODA) were added, and 18.01 g of 3,3',4,4'-biphenyltetracarboxylic dianhydride (hereinafter, BPDA) was gradually added while stirring under a nitrogen atmosphere. After visually confirming that BPDA had dissolved, 7.79 g of pyromellitic dianhydride (hereinafter, PMDA) was gradually added. After visually confirming that PMDA had dissolved, the mixture was stirred for 30 minutes. Then, 5.78 g of 4'-diamino-2,2'-dimethylbiphenyl (hereinafter, m-TB) was added, 7.11 g of p-phenylenediamine (hereinafter, PDA) was added, followed by 11.85 g of PMDA, and the mixture was stirred for 30 minutes. Finally, 0.46 g of PMDA was dissolved in DMF to give a solids concentration of 7.2%, which was gradually added to the reaction solution. When the viscosity at 23°C reached 2500 poise, the addition was stopped to obtain a non-thermoplastic polyimide precursor A. The weight-average molecular weight at this time was 156,000.
[0069] (Synthesis Example 2) A glass flask with a capacity of 2000 ml was charged with 334.13 g of DMF and 17.70 g of ODA, and 18.01 g of BPDA was gradually added while stirring under a nitrogen atmosphere. After visually confirming that BPDA had dissolved, 7.79 g of PMDA was gradually added. After visually confirming that PMDA had dissolved, stirring was performed for 30 minutes. Then, 5.78 g of m-TB was added, 7.11 g of PDA was added, and then 11.85 g of PMDA was added and stirred for 30 minutes. Finally, 0.46 g of PMDA was added to the DMF solution so that the solid content concentration was 7.2%, and the addition was gradually added to the above reaction solution, and the addition was stopped when the viscosity at 23 ° C. reached 8000 poise, and a non-thermoplastic polyimide precursor B was obtained. The average weight molecular weight at this time was 251,000.
[0070] (Synthesis Example 3) In a 2000 ml glass flask, 334.13 g of DMF, 5.27 g of ODA, and 16.20 g of 2,2'-bis[4-(4-aminophenoxy)phenyl]propane (hereinafter, BAPP) were added, and 7.17 g of PMDA was gradually added while stirring under a nitrogen atmosphere. After visually confirming the dissolution of PMDA, 8.48 g of benzophenonetetracarboxylic dianhydride (hereinafter, BTDA) was added and stirred for 30 minutes. Then, 3.76 g of PDA was added, followed by 15.32 g of PMDA, and stirred for 30 minutes. Finally, a solution was prepared by dissolving 0.46 g of PMDA in DMF to a solid content concentration of 7.2%, and this solution was gradually added to the above reaction solution, and the addition was stopped when the viscosity at 23 ° C. reached 2500 poise, and a non-thermoplastic polyimide precursor C was obtained. The average weight molecular weight at this time was 159,000.
[0071] (Synthesis of Solvent-Soluble Polyimides) (Synthesis Example 4) 673.24g of DMF and 71.83g of BAPP were added to a 2000ml glass flask, and 77.01g of 2,2'-hexafluoropropylidenediphthalic dianhydride (hereinafter referred to as 6FDA) was gradually added while stirring under a nitrogen atmosphere. After visually confirming that 6FDA had dissolved, stirring was continued for 30 minutes. Finally, a DMF solution was prepared so that 2.22g of 6FDA had a solids concentration of 7.2%, and this solution was gradually added to the above reaction solution. When the viscosity at 23°C reached 2000 poise, the addition was stopped, and 158.4g of N,N-dimethylformamide, 40.66g of pyridine, and 53.5g of acetic anhydride were sequentially added to the flask, and the mixture was stirred for 3 hours while being heated to 90°C. After the temperature returned to room temperature, 2000mL of isopropyl alcohol was added to the flask, and the precipitate was collected. The precipitate was then washed three times with 1000 mL of isopropyl alcohol and dried under reduced pressure at 80° C. for 20 hours to obtain a solvent-soluble polyimide D. The weight-average molecular weight of the polyimide D was 131,000.
[0072] (Synthesis Example 5) In a 2000 ml glass flask, 673.24 g of DMF and 74.94 g of 4,4'-bis[4-(4-amino-2-trifluoromethyl)phenoxy]-octafluorobiphenyl (hereinafter referred to as 6FAPB) were added, and 51.00 g of BPDA was gradually added while stirring under a nitrogen atmosphere. After visually confirming that BPDA had dissolved, stirring was continued for 30 minutes. Finally, a DMF solution was prepared so that 1.47 g of BPDA had a solids concentration of 7.2%, and this solution was gradually added to the above reaction solution. When the viscosity at 23 ° C. reached 2000 poise, the addition was stopped, and 158.4 g of N,N-dimethylformamide, 40.66 g of pyridine, and 53.5 g of acetic anhydride were sequentially added to the flask, and the mixture was stirred for 3 hours while being heated to 90 ° C. After returning to room temperature, 2000 mL of isopropyl alcohol was added to the flask, and the precipitate was collected. The precipitate was then washed three times with 1000 mL of isopropyl alcohol, and the precipitate was dried under reduced pressure at 80° C. for 20 hours to obtain a solvent-soluble polyimide E. The weight-average molecular weight of the polyimide E was 120,500.
[0073] (Synthesis of Thermoplastic Polyimide) (Synthesis Example 6) In a 2000 ml glass flask, 673.24 g of DMF and 71.83 g of BAPP were added, and 7.72 g of BPDA was gradually added while stirring under a nitrogen atmosphere. After visually confirming that BPDA had dissolved, 31.30 g of PMDA was added and stirred for 30 minutes. Finally, a solution was prepared by dissolving 1.15 g of PMDA in DMF to a solid content concentration of 7.2%, and this solution was gradually added to the above reaction solution, and the addition was stopped when the viscosity at 23 ° C. reached 300 poise, and a thermoplastic polyimide precursor F was obtained.
[0074] (Inflection point temperature of solvent-soluble polyimide) DMF (30 g) was added to the solvent-soluble polyimides D and E (60 g) obtained in Synthesis Examples 4 and 5 above, and the mixture was stirred and degassed, and cast onto aluminum foil using a comma coater. This resin film was heated at 120°C for 3 minutes, and then the self-supporting gel film was peeled off from the aluminum foil and fixed to a metal frame, and dried at 250°C for 1 minute and 300°C for 200 seconds to obtain a polyimide film with a thickness of 20 μm.
[0075] In addition, the inflection point temperatures of the storage modulus were measured by the DMA measurement described above, and it was found that the inflection point temperature of the polyimide film obtained from solvent-soluble polyimide D was 218°C, and the inflection point temperature of the polyimide film obtained from solvent-soluble polyimide precursor E was 207°C.
[0076] Example 1 In a 500 mL separable flask, the non-thermoplastic polyimide precursor A (55 g) obtained in Synthesis Example 1 and the solvent-soluble polyimide solution D (11 g) obtained in Synthesis Example 4 were placed, and stirred and mixed for 5 hours at room temperature under a nitrogen atmosphere using a stirring blade to obtain a precursor mixture. 32.5 g of a curing agent consisting of acetic anhydride / isoquinoline / DMF (weight ratio 11.48 / 3.40 / 18.18) was added to this precursor mixture, and the mixture was stirred and degassed at a temperature below 0°C, and then coated on aluminum foil using a comma coater. After heating this resin film at 115°C x 100 seconds, the self-supporting gel film was peeled off from the aluminum foil and fixed to a metal fixing frame, and imidized at 250°C x 15 seconds and 350°C x 79 seconds to obtain a polyimide film with a thickness of 12.5 μm.
[0077] The cross-section of the obtained film was observed by TEM, and it was confirmed that the film was a polyimide film with a phase-separated structure having domains of thermoplastic polyimide up to 3.8 μm in size. Furthermore, when the film was fixed to a metal frame and heated at 450°C for 2 minutes, it retained its shape, confirming that it was non-thermoplastic.
[0078] Next, a solution of the thermoplastic polyimide precursor F obtained in Synthesis Example 6 diluted with DMF to a solid content concentration of 8% by weight was applied to both sides of the non-thermoplastic polyimide film obtained above, so that the final thickness on one side was 3 μm. Then, the film was heated at 120° C. for 2 minutes. Then, the film was heated and imidized at 350° C. for 15 seconds to obtain a polyimide laminate film.
[0079] Example 2 In a 500 mL separable flask, the non-thermoplastic polyimide precursor B (55 g) obtained in Synthesis Example 2 and the solvent-soluble polyimide solution D (11 g) obtained in Synthesis Example 4 were placed, and stirred and mixed for 5 hours at room temperature under a nitrogen atmosphere using a stirring blade to obtain a precursor mixture. 32.5 g of a curing agent consisting of acetic anhydride / isoquinoline / DMF (weight ratio 11.48 / 3.40 / 18.18) was added to this precursor mixture, and the mixture was stirred and degassed at a temperature below 0°C, and then coated on aluminum foil using a comma coater. After heating this resin film at 115°C for 100 seconds, the self-supporting gel film was peeled off from the aluminum foil and fixed to a metal fixing frame, and imidized at 250°C for 15 seconds and 350°C for 79 seconds to obtain a polyimide film with a thickness of 12.5 μm.
[0080] The cross-section of the obtained film was observed by TEM, and it was confirmed that the film was a polyimide film with a phase-separated structure having domains of thermoplastic polyimide up to 4.6 μm in size. Furthermore, when the film was fixed to a metal frame and heated at 450°C for 2 minutes, it retained its shape, confirming that it was non-thermoplastic.
[0081] Next, a solution of the thermoplastic polyimide precursor F obtained in Synthesis Example 6 diluted with DMF to a solid content concentration of 8% by weight was applied to both sides of the non-thermoplastic polyimide film obtained above, so that the final thickness on one side was 3 μm. Then, the film was heated at 120° C. for 2 minutes. Then, the film was heated and imidized at 350° C. for 15 seconds to obtain a polyimide laminate film.
[0082] Example 3 In a 500 mL separable flask, the non-thermoplastic polyimide precursor B (55 g) obtained in Synthesis Example 1 and the solvent-soluble polyimide solution E (11 g) obtained in Synthesis Example 5 were placed, and stirred and mixed for 5 hours at room temperature under a nitrogen atmosphere using a stirring blade to obtain a precursor mixture. 32.5 g of a curing agent consisting of acetic anhydride / isoquinoline / DMF (weight ratio 11.48 / 3.40 / 18.18) was added to this precursor mixture, and the mixture was stirred and degassed at a temperature below 0°C, and then coated on aluminum foil using a comma coater. After heating this resin film at 115°C x 100 seconds, the self-supporting gel film was peeled off from the aluminum foil and fixed to a metal fixing frame, and imidized at 250°C x 15 seconds and 350°C x 79 seconds to obtain a polyimide film with a thickness of 12.5 μm.
[0083] The cross-section of the obtained film was observed by TEM, and it was confirmed that the film was a polyimide film with a phase-separated structure having domains of thermoplastic polyimide up to 1.3 μm in size. Furthermore, when the film was fixed to a metal frame and heated at 450°C for 2 minutes, it retained its shape, confirming that it was non-thermoplastic.
[0084] Next, a solution of the thermoplastic polyimide precursor F obtained in Synthesis Example 6 diluted with DMF to a solid content concentration of 8% by weight was applied to both sides of the non-thermoplastic polyimide film obtained above, so that the final thickness on one side was 3 μm. Then, the film was heated at 120° C. for 2 minutes. Then, the film was heated and imidized at 350° C. for 15 seconds to obtain a polyimide laminate film.
[0085] Comparative Example 1 To the non-thermoplastic polyimide precursor C (65 g) obtained in Synthesis Example 3, 32.5 g of a curing agent consisting of acetic anhydride / isoquinoline / DMF (weight ratio 11.48 / 3.40 / 18.18) was added, and the mixture was stirred and degassed at a temperature below 0°C, and then coated on aluminum foil using a comma coater. After heating this resin film at 115°C for 100 seconds, the self-supporting gel film was peeled off from the aluminum foil and fixed to a metal frame, and imidized at 250°C for 15 seconds and 350°C for 79 seconds to obtain a polyimide film with a thickness of 12.5 μm. In addition, this film was fixed to a metal frame and heated at 450°C for 2 minutes, and the shape was maintained, confirming that it was non-thermoplastic.
[0086] Next, a solution of the thermoplastic polyimide precursor F obtained in Synthesis Example 6 diluted with DMF to a solid content concentration of 8% by weight was applied to both sides of the non-thermoplastic polyimide film obtained above so that the final thickness on one side was 3 μm. Then, the film was heated at 120° C. for 2 minutes. Then, the film was heated and imidized at 350° C. for 15 seconds to obtain a polyimide laminate film.
[0087] Comparative Example 2 A polyimide laminate was obtained in the same manner as in Comparative Example 1 above, except that the non-thermoplastic polyimide precursor A obtained in Synthesis Example 1 was used instead of the non-thermoplastic polyimide precursor C obtained in Synthesis Example 3.
[0088] (Evaluation Results) The polyimide laminate films obtained in Examples 1 to 3 and Comparative Examples 1 and 2 were used to measure the presence or absence of a sea-island structure in the non-thermoplastic film and the domain size of the island structure by TEM observation, and the hole crack test was performed by the above-mentioned method. The results are shown in Table 4. [Table 4] [Industrial Applicability]
[0089] The polyimide laminate film obtained by the present invention can provide a flexible printed circuit board which suppresses cracks on the inner wall of a via that occur during the via formation step by laser processing.
Claims
1. A method for producing a non-thermoplastic polyimide film, comprising the steps of: imidizing a mixture of a non-thermoplastic polyimide precursor (polyamic acid) and a solvent-soluble polyimide to produce a non-thermoplastic polyimide film; and forming a phase-separated structure in the film having domains of solvent-soluble polyimide with island structures of 10 μm or less, the method comprising the steps of: The solvent-soluble polyimide is soluble in N,N-dimethylformamide; The solvent-soluble polyimide has an inflection point temperature of storage elastic modulus of 290° C. or lower.
2. 2. The method for producing a non-thermoplastic polyimide film according to claim 1, wherein the non-thermoplastic polyimide precursor (polyamic acid) has a weight average molecular weight of 150,000 or more.
3. The diamine compound used in the solvent-soluble polyimide is 2,2-bis(4-aminophenyl)hexafluoropropane, 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane, 2,2'-bis[4-(4-amino-2-trifluoromethylphenoxy)phenyl]hexafluoropropane, 4,4'-bis[4-(4-amino-2-trifluoromethyl)phenoxy]-octafluorobiphenyl, bis[4-(4-aminophenoxy)phenyl]sulfone, 1,3-bis[2-(4-aminophenyl)-2-propyl]benzene, bis[4-(3-aminophenoxy)phenyl] The method for producing a non-thermoplastic polyimide film according to claim 1 or 2, characterized in that the polyimide film contains one or more compounds selected from the group consisting of sulfone, 1,1-bis(4-aminophenyl)cyclohexane, 9,9-bis(4-amino-3-fluorophenyl)fluorene, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 1,4-bis[2-(4-aminophenyl)-2-propyl]benzene, 1,3-bis(3-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 4,4'-bis(4-aminophenoxy)biphenyl, and 1,4-bis(4-aminophenoxy)benzene.
4. The method for producing a non-thermoplastic polyimide film according to any one of claims 1 to 3, characterized in that the acid dianhydride used in the solvent-soluble polyimide contains one or more compounds selected from 2,2'-hexafluoropropylidenediphthalic dianhydride, 3,3',4,4'-perfluoroisopropylidenediphthalic dianhydride, 3,3',4,4'-diphenylsulfonetetracarboxylic dianhydride, 9,9-bis(3,4-dicarboxyphenyl)fluorene dianhydride, dicyclohexyl-3,4,3',4'-tetracarboxylic dianhydride, and ethylenediaminetetraacetic dianhydride.
5. 5. The method for producing a non-thermoplastic polyimide film according to claim 1, wherein the solvent-soluble polyimide contains 2,2-bis(4-aminophenoxyphenyl)propane.
6. A method for producing a polyimide laminate film, comprising forming a thermoplastic polyimide resin layer on at least one surface of the non-thermoplastic polyimide film produced by the method for producing a non-thermoplastic polyimide film according to any one of claims 1 to 5.
7. A non-thermoplastic polyimide film having a phase separation structure formed therein, the phase separation structure having domains of a solvent-soluble polyimide having an island structure of 10 μm or less and domains of a non-thermoplastic polyimide having a sea structure, The solvent-soluble polyimide is soluble in N,N-dimethylformamide; The non-thermoplastic polyimide film, wherein the solvent-soluble polyimide has an inflection point temperature of storage elastic modulus of 290° C. or lower.
8. 8. The non-thermoplastic polyimide film according to claim 7, wherein the weight average molecular weight of the non-thermoplastic polyimide precursor (polyamic acid) is 150,000 or more.
9. The diamine compound used in the solvent-soluble polyimide is 2,2-bis(4-aminophenyl)hexafluoropropane, 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane, 2,2'-bis[4-(4-amino-2-trifluoromethylphenoxy)phenyl]hexafluoropropane, 4,4'-bis[4-(4-amino-2-trifluoromethyl)phenoxy]-octafluorobiphenyl, bis[4-(4-aminophenoxy)phenyl]sulfone, 1,3-bis[2-(4-aminophenyl)-2-propyl]benzene, bis[4-(3-aminophenoxy)phenyl]sulfone, 9. The non-thermoplastic polyimide film according to claim 7 or 8, which contains one or more compounds selected from the group consisting of 1,1-bis(4-aminophenyl)cyclohexane, 9,9-bis(4-amino-3-fluorophenyl)fluorene, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 1,4-bis[2-(4-aminophenyl)-2-propyl]benzene, 1,3-bis(3-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 4,4'-bis(4-aminophenoxy)biphenyl, and 1,4-bis(4-aminophenoxy)benzene.
10. The non-thermoplastic polyimide film according to any one of claims 7 to 9, characterized in that the acid dianhydride used in the solvent-soluble polyimide contains one or more compounds selected from 2,2'-hexafluoropropylidenediphthalic dianhydride, 3,3',4,4'-perfluoroisopropylidenediphthalic dianhydride, 3,3',4,4'-diphenylsulfonetetracarboxylic dianhydride, 9,9-bis(3,4-dicarboxyphenyl)fluorene dianhydride, dicyclohexyl-3,4,3',4'-tetracarboxylic dianhydride, and ethylenediaminetetraacetic dianhydride.
11. 11. The non-thermoplastic polyimide film according to claim 7, wherein the solvent-soluble polyimide contains 2,2-bis(4-aminophenoxyphenyl)propane.
12. A polyimide laminate film comprising the non-thermoplastic polyimide film according to any one of claims 7 to 11 and a thermoplastic polyimide resin layer formed on at least one surface of the non-thermoplastic polyimide film.
Citation Information
Patent Citations
Polyimide metal laminate and its production process
JP2004322636A
Heat-resistant adhesive and semiconductor device
JP2005163025A
Inkjet ink
JP2009120811A
Method for manufacturing polyimide metal laminate