(Meth)acrylic acid copolymer

A (meth)acrylic acid copolymer with high sulfonic acid (salt) group-containing monomer content effectively inhibits silica scale, addressing the limitations of existing inhibitors and providing enhanced silica scale suppression.

JP7562433B2Active Publication Date: 2024-10-07NIPPON SHOKUBAI CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2021004778
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-01-15
Publication Date
2024-10-07
Estimated Expiration
2041-01-15

AI Technical Summary

Technical Problem

Existing scale inhibitors do not effectively inhibit silica scale, necessitating a need for improved silica scale inhibitors.

Method used

A (meth)acrylic acid copolymer comprising structural units derived from (meth)acrylic acid, sulfonic acid (salt) group-containing monomers, and ether bond-containing monomers, with a sulfonic acid (salt) group-containing monomer content exceeding 30% by mass, enhancing silica scale inhibition.

Benefits of technology

The copolymer exhibits excellent ability to suppress silica components, making it suitable as a scale inhibitor for silica scale and a water treatment agent.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007562433000001
    Figure 0007562433000001
  • Figure 0007562433000002
    Figure 0007562433000002
  • Figure 0007562433000003
    Figure 0007562433000003
Patent Text Reader

Abstract

To provide a (meth)acrylic acid system copolymer capable of suitably using as a suppressor of, for example, silica scale because of being excellent in suppressive ability of the silica scale.SOLUTION: A copolymer comprising a structural unit derived from (meth)acrylic acid (salt), a structural unit derived from a sulfonic acid (salt) group-containing monomer, and a structural unit derived from an ether bond-containing monomer, in which a content ratio of the structural unit derived from the sulfonic acid (salt) group-containing monomer relative to 100 mass% of a total structural units exceeds 30 mass%.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a (meth)acrylic acid-based copolymer, and more particularly to a (meth)acrylic acid-based copolymer used for inhibiting scale such as silica scale. [Background technology]

[0002] For example, in geothermal power generation, industrial cooling water, and seawater desalination, the generation of scale such as calcium carbonate and silica can be a problem.

[0003] For example, the copolymer described in Patent Document 1 improves the dispersibility of hydrophobic particles and also exhibits excellent chelating ability for calcium ions, making it possible to exhibit extremely good scale prevention ability for the piping and inside of geothermal power generation equipment, and it is disclosed that it can be suitably used as a scale inhibitor for geothermal power generation equipment. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2016-64382 A Summary of the Invention [Problem to be solved by the invention]

[0005] As mentioned above, various scale inhibitors have been proposed, but there has been a demand for further improvement in the ability to inhibit silica scale. Therefore, an object of the present invention is to provide a (meth)acrylic acid-based copolymer that has excellent silica scale inhibition capability and can therefore be suitably used, for example, as a silica scale inhibitor. [Means for solving the problem]

[0006] The present inventors have conducted various investigations to achieve the above object and have arrived at the present invention. That is, the (meth)acrylic acid-based copolymer of the present disclosure is a copolymer containing structural units derived from (meth)acrylic acid (salt), structural units derived from a sulfonic acid (salt) group-containing monomer, and structural units derived from an ether bond-containing monomer, and is a (meth)acrylic acid-based copolymer in which the content of structural units derived from sulfonic acid (salt) group-containing monomer exceeds 30 mass% relative to 100 mass% of all structural units. Effect of the Invention

[0007] The (meth)acrylic acid-based copolymer of the present disclosure exhibits a good ability to inhibit silica components, etc. Therefore, the (meth)acrylic acid-based copolymer of the present disclosure can be preferably used as a scale inhibitor for silica scale, etc., or as a water treatment agent. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] The present invention will be described in detail below. In addition, a combination of two or more of the individual preferred embodiments of the present invention described below is also a preferred embodiment of the present invention.

[0009] [(Meth)acrylic acid-based copolymer of the present disclosure] The (meth)acrylic acid-based copolymer of the present disclosure includes a copolymer containing a structural unit derived from (meth)acrylic acid (salt), a structural unit derived from a monomer containing a sulfonic acid (salt) group, and a structural unit of a monomer containing an ether bond, and the content ratio of the structural unit derived from the monomer containing a sulfonic acid (salt) group to 100% by mass of all structural units exceeds 30% by mass. The above copolymer is also referred to as the "copolymer of the present disclosure."

[0010] <Structural unit derived from (meth)acrylic acid (salt)> In this disclosure, (meth)acrylic acid refers to acrylic acid, methacrylic acid, and salts thereof. The above salt is not particularly limited, but examples thereof include alkali metal salts, alkaline earth metal salts, transition metal salts, and ammonium salts. In the present disclosure, the structural unit derived from (meth)acrylic acid (salt) refers to a structural unit in which the carbon-carbon double bond of (meth)acrylic acid (salt) is replaced with a carbon-carbon single bond. For example, if acrylic acid is CH2=CH(COOH), the structural unit derived from acrylic acid can be represented as -CH2-CH(COOH)-. The structural unit derived from (meth)acrylic acid (salt) can be formed, for example, by radical polymerization of (meth)acrylic acid (salt). Note that the structural unit derived from (meth)acrylic acid (salt) is not limited to a structural unit formed by polymerization of (meth)acrylic acid (salt), as long as it has the same structure as the structure in which the carbon-carbon double bond of (meth)acrylic acid (salt) is replaced with a carbon-carbon single bond, and may be, for example, a structural unit formed by a post-reaction after polymerization. The content of the structural unit derived from (meth)acrylic acid (salt) in the copolymer of the present disclosure is 15% by mass or more and less than 70% by mass, preferably 35% by mass or more and less than 70% by mass, more preferably 50% by mass or less than 70% by mass, based on 100% by mass of the structural units derived from all monomers constituting the copolymer of the present disclosure. The content of the structural unit derived from the (meth)acrylic acid (salt) is calculated in terms of (meth)acrylic acid. The term "in terms of (meth)acrylic acid" means that even if the structural unit derived from the (meth)acrylic acid (salt) is a structural unit derived from a (meth)acrylic acid salt, the mass is calculated as (meth)acrylic acid. By being in the above range, the scale inhibitor of the present disclosure tends to have improved scale inhibition ability.

[0011] <Structural unit derived from monomer containing sulfonic acid (salt) group> In the present disclosure, a sulfonic acid (salt) group-containing monomer refers to a compound that contains at least one carbon-carbon double bond and a sulfonic acid (salt) group. The at least one carbon-carbon double bond is usually radically polymerizable. The above salt is not particularly limited, but examples thereof include alkali metal salts, alkaline earth metal salts, transition metal salts, and ammonium salts. In the present disclosure, the structural unit derived from a sulfonic acid (salt) group-containing monomer refers to a structural unit in which at least one carbon-carbon double bond of a sulfonic acid (salt) group-containing monomer is replaced with a carbon-carbon single bond. Note that the structural unit derived from a sulfonic acid (salt) group-containing monomer may have the same structure as the structure in which at least one carbon-carbon double bond of a sulfonic acid (salt) group-containing monomer is replaced with a carbon-carbon single bond, and is not limited to a structural unit formed by polymerization of a sulfonic acid (salt) group-containing monomer, and may be, for example, a structural unit formed by a post-reaction after polymerization. The content of the structural unit derived from the sulfonic acid (salt) group-containing monomer in the copolymer of the present disclosure is more than 30% by mass and 60% by mass or less, preferably more than 30% by mass and 50% by mass or less, more preferably more than 30% by mass and 45% by mass or less, based on 100% by mass of the structural units derived from all monomers constituting the copolymer of the present disclosure. The content of the structural unit derived from the sulfonic acid (salt) group-containing monomer is calculated in terms of sodium salt. The calculation in terms of sodium salt means that even if the sulfonic acid (salt) group contained in the structural unit derived from the sulfonic acid (salt) group-containing monomer is, for example, an acid-type sulfonic acid group, the mass is calculated as the sodium salt of the sulfonic acid group. By being in the above range, the scale inhibitor of the present disclosure tends to have improved scale inhibition ability.

[0012] Specific examples of sulfonic acid (salt) group-containing monomers include vinyl sulfonic acid and its salts, styrene sulfonic acid and its salts, (meth)allyl sulfonic acid and its salts, 3-(meth)allyloxy-2-hydroxypropanesulfonic acid and its salts, 3-(meth)allyloxy-1-hydroxypropanesulfonic acid and its salts, 2-(meth)allyloxyethylenesulfonic acid and its salts, 2-acrylamido-2-methylpropanesulfonic acid and its salts, etc. Since the scale inhibitor of the present disclosure tends to have improved scale inhibition ability, 3-(meth)allyloxy-2-hydroxypropanesulfonic acid and its salts are preferred, and 3-allyloxy-2-hydroxypropanesulfonic acid and its sodium salt are more preferred.

[0013] <Structural units derived from ether bond-containing monomers> In the present disclosure, the ether bond-containing monomer refers to a compound containing at least one carbon-carbon double bond and an ether bond. However, a sulfonic acid (salt) group-containing monomer is not included in the ether bond-containing monomer even if it is a compound containing an ether bond. The at least one carbon-carbon double bond is usually radically polymerizable. In the present disclosure, the structural unit derived from an ether bond-containing monomer refers to a structural unit in which at least one carbon-carbon double bond of an ether bond-containing monomer is replaced with a carbon-carbon single bond. Note that the structural unit derived from an ether bond-containing monomer may have the same structure as the structure in which at least one carbon-carbon double bond of an ether bond-containing monomer is replaced with a carbon-carbon single bond, and is not limited to a structural unit formed by polymerization of an ether bond-containing monomer, and may be, for example, a structural unit formed by a post-reaction after polymerization. The content of the structural unit derived from the ether bond-containing monomer in the copolymer of the present disclosure is 0.5% by mass or more and 30% by mass or less, preferably 1% by mass or more and 25% by mass or less, more preferably 1.5% by mass or more and 20% by mass or less, and most preferably 2% by mass or more and 15% by mass or less, based on 100% by mass of the structural units derived from all monomers constituting the copolymer of the present disclosure. In addition, when the structural unit derived from the ether bond-containing monomer contains an acid group such as a carboxyl group (salt), the content is calculated in terms of acid. The term "acid equivalent" means that even if the structural unit derived from the monomer contains a salt of an acid group, the mass is calculated as the corresponding acid. The mass of the structural units derived from other monomers described later is calculated in the same manner. By being in the above range, the scale inhibitor of the present disclosure tends to have improved scale inhibition ability. Examples of ether bond-containing monomers include vinyl ethers such as ethyl vinyl ether, butyl vinyl ether, and benzyl vinyl ether; (meth)allyl ethers such as ethyl methallyl ether, butyl methallyl ether, and benzyl methallyl ether; and isoprenyl ethers such as ethyl isoprenyl ether, butyl isoprenyl ether, and benzyl isoprenyl ether. However, since there is a tendency for scale inhibition ability to be particularly improved, a monomer represented by the following general formula (1) is preferred.

[0014] [ka] (In the above general formula (1), R 0 R represents a hydrogen atom or a methyl group. 1 represents a CH2 group, a CH2CH2 group, or a direct bond. X represents a hydroxyl group, a group represented by the following general formula (2), or a group represented by the following general formula (3). Y represents a hydroxyl group, a group represented by the following general formula (2), or a group represented by the following general formula (3). However, one of X and Y represents a hydroxyl group, and the other represents a group represented by the following general formula (2) or a group represented by the following general formula (3).

[0015] [ka] (In the above general formulas (2) and (3), R 2 are the same or different and each represents an alkylene group having 2 to 4 carbon atoms. n represents an oxyalkylene group (-OR 2 R is the average number of moles of 0 to 5. 3 , R 4 , R 5 each independently represents an alkyl group having 1 to 20 carbon atoms. Since the scale inhibition ability of the scale inhibitor of the present disclosure tends to improve, R 3 , R 4 , R 5More preferably, the number of carbon atoms is 1 to 12, even more preferably 1 to 8, and most preferably 1 to 4. The alkyl group may be linear or branched, may contain a cyclic structure, and may have a substituent. Examples of the substituent include an alkoxy group, an aryl group, a hydroxyl group, a carboxy group, an amino group, and a heterocyclic group. When the alkyl group has a substituent, the number of the substituents may be one or more, and it is preferable that the alkyl group including the substituent has the above carbon number.

[0016] <Structural units derived from other monomers> The copolymer of the present disclosure may, if desired, have structural units derived from monomers other than (meth)acrylic acid (salt), structural units derived from sulfonic acid (salt) group-containing monomers, and structural units derived from ether bond-containing monomers (also referred to as structural units derived from other monomers). In the present disclosure, the structural unit derived from another monomer refers to a structural unit in which at least one carbon-carbon double bond of another monomer is replaced with a carbon-carbon single bond. Note that the structural unit derived from another monomer may have the same structure as the structure in which at least one carbon-carbon double bond of the other monomer is replaced with a carbon-carbon single bond, and is not limited to a structural unit formed by polymerization of the other monomer, and may be, for example, a structural unit formed by a post-reaction after polymerization. In the copolymer of the present disclosure, the content of structural units derived from other monomers is 0% by mass or more and 15% by mass or less, preferably 0% by mass or more and 10% by mass or less, and more preferably 0% by mass or more and 5% by mass or less, relative to 100% by mass of structural units derived from all monomers constituting the copolymer of the present disclosure. Examples of the other monomers include carboxyl group-containing monomers such as maleic acid, itaconic acid, and salts thereof; unsaturated alcohols such as (meth)allyl alcohol and isoprenol, and monomers obtained by adding alkylene oxides thereto; polyalkylene glycol chain-containing monomers such as (meth)acrylic acid esters of alkoxyalkylene glycols; vinyl aromatic monomers having heterocyclic aromatic hydrocarbon groups such as vinylpyridine and vinylimidazole; dialkylaminoalkyl (meth)acrylates such as dimethylaminoethyl acrylate, dimethylaminoethyl methacrylate, and dimethylaminopropyl acrylate; dialkylaminoalkyl (meth)acrylamides such as dimethylaminoethyl acrylamide, dimethylaminoethyl methacrylamide, and dimethylaminopropyl acrylamide; allylamines such as diallyl alkylamines and diallyl dimethylamine; and quaternized products thereof. N-vinyl monomers such as N-vinyl formamide, N-vinyl acetamide, N-vinyl-N-methyl formamide, N-vinyl-N-methyl acetamide, and N-vinyl oxazolidone; amide monomers such as (meth)acrylamide, N,N-dimethyl acrylamide, N-isopropyl acrylamide, and t-butyl acrylamide; hydroxyl group-containing monomers such as (meth)allyl alcohol and isoprenol; (meth)acrylic acid alkyl ester monomers such as butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and dodecyl (meth)acrylate; (meth)acrylic acid hydroxyalkyl monomers such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, and 2-hydroxyhexyl (meth)acrylate; vinyl aryl monomers such as styrene, indene, and vinyl aniline; isobutylene, vinyl acetate, and the like. The copolymer of the present disclosure contains one or more types of structural units derived from (meth)acrylic acid (salt), structural units derived from a sulfonic acid (salt) group-containing monomer, and structural units derived from an ether bond-containing monomer, and may contain one or more types of structural units derived from other monomers as necessary.

[0017] <Physical properties of the copolymer of the present disclosure> The copolymer of the present disclosure preferably has a weight average molecular weight (Mw) of 3000 or more and 200000 or less, more preferably 5000 or more and 150000 or less, even more preferably 10000 or more and 100000 or less, and particularly preferably 10000 or more and 80000 or less. By being in the above range, the scale inhibition ability tends to be further improved. The copolymer of the present disclosure contains acid groups such as carboxylic acid (salt) groups and sulfonic acid (salt) groups, but the acid groups of the copolymer of the present disclosure may be partially or completely neutralized. The neutralization rate can be calculated, for example, by conventional acid-base titration. The copolymer of the present disclosure may contain structural units derived from a polymerization initiator or a chain transfer agent, such as a hydroxyl group, a sulfonic acid (salt) group, or a hypophosphorous acid (salt) group, at the main chain terminal or the like. In the copolymer of the present disclosure, the content of structural units derived from a sulfonic acid (salt) derived from a polymerization initiator or a chain transfer agent contained in the main chain is preferably 15% by mass or less, more preferably 10% by mass or less, and particularly preferably 6% by mass or less, relative to 100% by mass of the copolymer of the present disclosure.

[0018] [Method for producing the copolymer of the present disclosure] The method for producing the copolymer of the present disclosure is not particularly limited, but it is usually preferable to produce the copolymer by polymerizing structural units derived from (meth)acrylic acid (salt), a sulfonic acid (salt) group-containing monomer, and an ether bond-containing monomer, and, as necessary, other monomers. In the process for producing the copolymer of the present disclosure, a polymerization initiator is usually used. Examples of the polymerization initiator include persulfates such as sodium persulfate, potassium persulfate, and ammonium persulfate, hydrogen peroxide, azo compounds, and peroxides. In the process for producing the copolymer of the present disclosure, it is preferable to use a polymerization solvent and a chain transfer agent. Examples of the chain transfer agent include hydrogen peroxide, hypophosphorous acid (salts) such as sodium hypophosphite, hydrogen sulfite (salts) such as sodium hydrogen sulfite, and mercapto compounds.

[0019] [Uses of the Copolymer of the Present Disclosure] The copolymer of the present disclosure can exhibit high performance in aqueous applications and can be preferably used as a scale inhibitor for use in geothermal power generation processes, oil well and gas well processes, seawater desalination processes or waste liquid concentration processes using forward osmosis membranes or reverse osmosis membranes, boiler water circulation systems, cooling water circulation systems, and the like. The copolymer of the present disclosure can be preferably used as a scale inhibitor for, for example, silica scale or calcium carbonate, and is most preferably used as a scale inhibitor for silica scale.

[0020] [Water treatment agent of the present disclosure] The water treatment agent of the present disclosure contains the copolymer of the present disclosure. The water treatment agent of the present disclosure preferably contains the copolymer of the present disclosure at, for example, 1% by mass or more and 70% by mass or less. More preferably, the copolymer is contained at 1 to 50% by mass, particularly preferably 1 to 40% by mass, most preferably 1 to 30% by mass, and most preferably 1 to 20% by mass. The water treatment agent of the present disclosure may contain components other than the copolymer of the present disclosure. Examples of components other than the copolymer of the present disclosure include solvents such as water, pH adjusters such as alkalis and acids, oxygen scavengers, anticorrosives, chelating agents, phosphonic acids (salts) such as aminotrimethylenephosphonic acid, 1-hydroxyethylidene-1,1-diphosphonic acid, and salts thereof, carboxyl-containing polymers other than the copolymer of the present disclosure, surfactants, defoamers, pitch control agents, slime control agents, and the like. The water treatment chemical of the present disclosure is not particularly limited, but can be preferably used, for example, as a scale inhibitor for preventing scale from occurring in various types of water.

[0021] [Scale inhibitor of the present disclosure] The scale inhibitor of the present disclosure contains the copolymer of the present disclosure. The scale inhibitor of the present disclosure preferably contains the copolymer of the present disclosure in an amount of, for example, 10% by mass or more and 100% by mass or less. More preferably, the amount is 20% by mass or more and 70% by mass or less. The scale inhibitor of the present disclosure may contain components other than the copolymer of the present disclosure. Examples of components other than the copolymer of the present disclosure include solvents such as water, pH adjusters such as alkalis and acids, oxygen scavengers, anticorrosive agents, chelating agents, phosphonic acids (salts) such as aminotrimethylenephosphonic acid, 1-hydroxyethylidene-1,1-diphosphonic acid, and salts thereof, carboxyl-containing polymers other than the copolymer of the present disclosure, surfactants, defoamers, pitch control agents, slime control agents, and the like. The scale inhibitor of the present disclosure is not particularly limited, but can be preferably used as an inhibitor of silica scale or calcium carbonate, for example. The scale inhibitor of the present disclosure is particularly excellent in terms of silica scale inhibition ability, and therefore can be preferably used as a silica scale inhibitor.

[0022] [Uses of the scale inhibitor of the present disclosure] The scale inhibitor of the present disclosure can exhibit high performance in aqueous applications, and can be preferably used as a scale inhibitor for use in geothermal power generation processes, oil well and gas well processes, seawater desalination processes or waste liquid concentration processes using forward osmosis membranes or reverse osmosis membranes, boiler water circulation systems, cooling water circulation systems, etc. The scale inhibitor of the present disclosure can be preferably used as a scale inhibitor for silica scale and calcium carbonate.

[0023] [Scale prevention method of the present disclosure] The scale prevention method of the present disclosure uses the scale inhibitor of the present disclosure or the copolymer of the present disclosure. The scale prevention method of the present disclosure preferably includes a step of adding the scale inhibitor of the present disclosure or the copolymer of the present disclosure to a system to be prevented from scaling. Also, preferably, the method includes a step of controlling the amount of the copolymer of the present disclosure in the system to be prevented from scaling so that it is within a predetermined range. The content of the copolymer of the present disclosure in the system to be prevented from scaling is preferably 0.1 ppm or more and 500 ppm or less, more preferably 1 ppm or more and 300 ppm or less. EXAMPLES

[0024] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. In addition, unless otherwise specified, "parts" means "parts by mass" and "%" means "% by mass". <Weight average molecular weight measurement conditions (GPC)> Equipment: Tosoh Corporation HLC8320 Column: SHODEX Asahipak GF-310-HQ, Showa Denko Corporation; GF-710-HQ, GF-1G-7B Column temperature: 40℃ Flow rate: 0.5ml / min Calibration curve: Polyacrylic acid standard from American Polymer Standards Corporation Eluent: 0.1N sodium acetate <Silica scale inhibition rate evaluation test> Preparation of borate buffer solution: 7.420 g of boric acid, 1.753 g of sodium chloride, 19.069 g of sodium borate decahydrate, and ion-exchanged water were added to make a total of 1000 g. Preparation of magnesium aqueous solution: 8.115 g of magnesium sulfate heptahydrate was mixed with ion-exchanged water to make a total of 1000 g. Preparation of silica aqueous solution: 2.129 g of sodium metasilicate nonahydrate was mixed with ion-exchanged water to make a total of 150 g. 1. When testing at a polymer concentration of 50 ppm 73g of pure water and 2g of borate buffer solution were added to the container and stirred. 10g of the above silica aqueous solution, 5g of polymer aqueous solution diluted to 0.1%, and 10g of magnesium aqueous solution were further added while stirring. Then, the mixture was stirred for 18 hours while immersed in a warm bath at 60°C. After 18 hours, the mixture was suction filtered using a polyethersulfone (PES) membrane (manufactured by AS ONE Corporation) with 0.1μm openings. The Si concentration of the obtained filtrate was measured by ICP (optical emission spectroscopy) and converted into SiO2. Silica scale inhibition rate (%) = SiO2 concentration in filtrate (ppm) / SiO2 concentration in feed (ppm) The silica scale inhibition rate was judged according to the following criteria. <Silica scale inhibition rate evaluation criteria> Over 90%: Yes 50% or more but less than 90%: △ Less than 50%: × 2. When testing at a polymer concentration of 60 ppm The evaluation was carried out in the same manner as in the test with a polymer concentration of 50 ppm, except that the amount of pure water added was changed from 73 g to 72 g, and the amount of the 0.1% diluted polymer aqueous solution was changed from 5 g to 6 g.

[0025] <Production Example 1> (1) Synthesis of monomer In a 500 mL glass four-neck flask equipped with a reflux condenser and a stirrer (paddle blade), Charge 370.0 g of n-butyl alcohol and 4.27 g of pelletized sodium hydroxide. The mixture was heated to 60°C while stirring. Next, allyl glycidyl ether (hereinafter referred to as "AG") was added. E) was added over 30 minutes, and the reaction was then carried out for 5 hours. The solution was transferred to a 1,000 ml recovery flask, and the solvent was removed using a rotary evaporator. Add 200.0 g of 20% by weight sodium chloride solution to this, and then dilute this solution in 500 ml The mixture was transferred to a separating funnel, shaken well, and then left to stand until the layers were separated, and the lower layer was removed. The upper layer was transferred to a 300 ml recovery flask and the solvent was removed using a rotary evaporator. The salt was removed by filtration to obtain monomer (1). (2) Polymerization In a 1,000 mL glass separable flask equipped with a reflux condenser and a stirrer (paddle blade), 169.2 g of pure water and 0.0168 g of Mohr's salt were charged, and the temperature was raised to 87° C. while stirring to prepare a polymerization reaction system. Next, 253.5 g of an 80% aqueous acrylic acid solution (hereinafter also referred to as "80% AA"), 277.4 g of a 40% aqueous solution of sodium 3-allyloxy-2-hydroxypropanesulfonate (hereinafter also referred to as "40% HAPS"), 12.8 g of monomer (1), 79.1 g of a 15% aqueous solution of sodium persulfate (hereinafter also referred to as "15% NaPS"), and 5.2 g of a 35% aqueous solution of sodium hydrogensulfite (hereinafter also referred to as "35% SBS") were dropped from separate nozzles into the polymerization reaction system maintained at 87° C. under stirring. The drop time of each solution was 180 minutes for 80% AA, 120 minutes for 40% HAPS, 120 minutes for monomer (1), and 170 minutes for 35% SBS. The drop speed of each solution was constant, and each solution was added continuously. For 15% NaPS, the drop speed was 0.30 g / min from 0 to 130 minutes, and 0.58 g / min from 130 to 190 minutes. After the dropwise addition of 15% NaPS was completed, the reaction solution was maintained (aged) at 87° C. for an additional 30 minutes to complete the polymerization. In this manner, polymer (1) of the present disclosure was obtained.

[0026] <Production Example 2> 168.1 g of pure water and 0.0168 g of Mohr's salt were charged into a 1,000 mL glass separable flask equipped with a reflux condenser and a stirrer (paddle blade), and the temperature was raised to 87°C while stirring to prepare a polymerization reaction system. Next, 251.8 g of 80% AA, 275.6 g of 40% HAPS, 12.7 g of monomer (1), 78.6 g of 15% NaPS, and 10.4 g of 35% SBS were dropped from separate nozzles into the polymerization reaction system maintained at 87°C while stirring. The drop times of each solution were 180 minutes for 80% AA, 120 minutes for 40% HAPS, 120 minutes for monomer (1), and 170 minutes for 35% SBS. The drop speed of each solution was constant, and each solution was continuously dropped. The 15% NaPS was added at a drop rate of 0.29 g / min from 0 to 130 minutes, and 0.58 g / min from 130 to 190 minutes. After the dropwise addition of 15% NaPS was completed, the reaction solution was maintained (aged) at 87° C. for an additional 30 minutes to complete the polymerization. In this manner, polymer (2) of the present disclosure was obtained.

[0027] <Production Example 3> 167.4 g of pure water and 0.0168 g of Mohr's salt were charged into a 1,000 mL glass separable flask equipped with a reflux condenser and a stirrer (paddle blade), and the temperature was raised to 87°C while stirring to prepare a polymerization reaction system. Next, 250.9 g of 80% AA, 274.6 g of 40% HAPS, 13.4 g of monomer (1), 78.3 g of 15% NaPS, and 12.6 g of 35% SBS were dropped from separate nozzles into the polymerization reaction system maintained at 87°C under stirring. The drop times of each solution were 180 minutes for 80% AA, 120 minutes for 40% HAPS, 120 minutes for monomer (1), and 170 minutes for 35% SBS. The drop speed of each solution was constant, and each solution was continuously dropped. The 15% NaPS was added at a drop rate of 0.29 g / min from 0 to 130 minutes, and 0.58 g / min from 130 to 190 minutes. After the dropwise addition of 15% NaPS was completed, the reaction solution was maintained (aged) at 87° C. for an additional 30 minutes to complete the polymerization. In this manner, polymer (3) of the present disclosure was obtained.

[0028] <Production Example 4> In a 1,000 mL glass separable flask equipped with a reflux condenser and a stirrer (paddle blade), 117.1 g of pure water, 0.0165 g of Mohr's salt, and 13.5 g of paratoluenesulfonic acid (hereinafter also referred to as "PTS") were charged, and the temperature was raised to 87°C while stirring to prepare a polymerization reaction system. Next, 218.8 g of 80% AA, 339.8 g of 40% HAPS, 11.7 g of monomer (1), and 94.1 g of 15% NaPS were dropped from separate nozzles into the polymerization reaction system maintained at 87°C under stirring. The drop time of each solution was 180 minutes for 80% AA, 120 minutes for 40% HAPS, and 120 minutes for monomer (1). The drop speed of each solution was constant, and each solution was continuously dropped. The 15% NaPS was added at a drop rate of 0.35 g / min from 0 to 130 minutes, and 0.69 g / min from 130 to 200 minutes. After the dropwise addition of 15% NaPS was completed, the reaction solution was maintained (aged) at 87° C. for an additional 30 minutes to complete the polymerization. In this manner, polymer (4) of the present disclosure was obtained.

[0029] <Production Example 5> In a 1,000 mL glass separable flask equipped with a reflux condenser and a stirrer (paddle blade), 100.4 g of pure water, 0.0165 g of Mohr's salt, and 12.7 g of PTS were charged, and the temperature was raised to 87°C while stirring to prepare a polymerization reaction system. Next, 206.7 g of 80% AA, 321.0 g of 40% HAPS, 11.1 g of monomer (1), 88.9 g of 15% NaPS, and 54.3 g of 35% SBS were dropped from separate nozzles into the polymerization reaction system maintained at 87°C under stirring. The drop times for each solution were 180 minutes for 80% AA, 120 minutes for 40% HAPS, 120 minutes for monomer (1), and 170 minutes for 35% SBS. The drop speed of each solution was constant, and each solution was continuously dropped. The 15% NaPS was added at a drop rate of 0.33 g / min from 0 to 130 minutes, and 0.65 g / min from 130 to 200 minutes. After the dropwise addition of 15% NaPS was completed, the reaction solution was maintained (aged) at 87° C. for an additional 30 minutes to complete the polymerization. In this manner, polymer (5) of the present disclosure was obtained.

[0030] <Comparative Manufacturing Example 1> In a 1,000 mL glass separable flask equipped with a reflux condenser and a stirrer (paddle blade), 166.7 g of pure water, 0.0165 g of Mohr's salt, and 13.4 g of PTS were charged, and the temperature was raised to 87°C while stirring to prepare a polymerization reaction system. Next, 240.5 g of 80% AA, 175.5 g of 40% HAPS, 42.4 g of monomer (1), 97.1 g of 15% NaPS, and 59.4 g of 35% SBS were dropped from separate nozzles into the polymerization reaction system maintained at 87°C under stirring. The drop times for each solution were 180 minutes for 80% AA, 120 minutes for 40% HAPS, 120 minutes for monomer (1), and 170 minutes for 35% SBS. The drop speed of each solution was constant, and each solution was continuously dropped. The 15% NaPS was added at a drop rate of 0.36 g / min from 0 to 130 minutes, and 0.71 g / min from 130 to 200 minutes. After the dropwise addition of 15% NaPS was completed, the reaction solution was maintained (aged) at 87° C. for an additional 30 minutes to complete the polymerization. In this manner, a comparative polymer (1) was obtained.

[0031] <Comparative Manufacturing Example 2> 253.3g of pure water, 0.0165g of Mohr's salt, and 13.3g of PTS were charged into a 1,000mL glass separable flask equipped with a reflux condenser and a stirrer (paddle blade), and the temperature was raised to 87°C while stirring to prepare a polymerization reaction system. Next, 331.7g of 80% AA, 52.2g of monomer (1), 119.6g of 15% NaPS, and 24.4g of 35% SBS were dropped from separate nozzles into the polymerization reaction system maintained at 87°C under stirring. The drop time of each solution was 180 minutes for 80% AA, 120 minutes for monomer (1), and 170 minutes for 35% SBS. The drop speed of each solution was constant, and each solution was continuously dropped. The 15% NaPS was added at a drop rate of 0.45 g / min from 0 to 130 minutes, and 0.88 g / min from 130 to 200 minutes. After the dropwise addition of 15% NaPS was completed, the reaction solution was maintained (aged) at 87° C. for an additional 30 minutes to complete the polymerization. In this manner, a comparative polymer (2) was obtained.

[0032] <Comparative Manufacturing Example 3> In a glass separable flask with an internal volume of 1500 ml equipped with a paddle impeller (SUS316 paddle-type rotor) stirrer, a reflux condenser, and four dropping devices, 186.4 g of pure water was charged and heated to the boiling reflux temperature. Next, under stirring, 459.1 g of a mixture of 445.1 g of 37% sodium acrylate aqueous solution and 14.0 g of acrylic acid, 299.5 g of 25% HAPS, 33.7 g of 20% NaPS, and 18.3 g of 12.5% ​​aqueous hydrogen peroxide solution were dropped at a constant speed, respectively, over 120 minutes for the mixture of the aqueous sodium acrylate aqueous solution and the aqueous acrylic acid aqueous solution, 120 minutes for the 25% HAPS, 140 minutes for the 20% NaPS, and 120 minutes for the 12.5% ​​aqueous hydrogen peroxide solution. After the dropwise addition, the boiling reflux temperature was maintained for 30 minutes to complete the polymerization. In this way, a comparative polymer (3) was obtained. The results are shown in Table 1.

[0033] [Table 1] In Table 1, "composition" indicates the mass % of "structural units derived from acrylic acid (salt) / structural units derived from sulfonic acid group-containing monomers / structural units derived from ether group-containing monomers," and the silica scale inhibition rate of 50 ppm indicates the test result at a polymer concentration of 50 ppm, and 60 ppm indicates the test result at a polymer concentration of 60 ppm. The results in Table 1 make it clear that the (meth)acrylic acid-based copolymer of the present disclosure has good silica suppression ability.

Claims

1. A copolymer comprising a structural unit derived from (meth)acrylic acid (salt), a structural unit derived from a monomer containing a sulfonic acid (salt) group, and a structural unit derived from a monomer containing an ether bond, The structural unit derived from an ether bond-containing monomer is a structural unit derived from a monomer represented by the following general formula (1): A (meth)acrylic acid-based copolymer having a content of structural units derived from a sulfonic acid (salt) group-containing monomer exceeding 30 mass% relative to 100 mass% of all structural units. 【Chemistry 1】 (In the general formula (1), R 0 represents a hydrogen atom or a methyl group; R 1 represents a CH 2 group, a CH 2 CH 2 group, or a direct bond; X represents a hydroxyl group, a group represented by the following general formula (2), or a group represented by the following general formula (3); Y represents a hydroxyl group, a group represented by the following general formula (2), or a group represented by the following general formula (3); provided that either X or Y represents a hydroxyl group, and the other represents a group represented by the following general formula (2) or a group represented by the following general formula (3).) 【Chemistry 2】 (In the general formulas (2) and (3), R 2 , which may be the same or different, represents an alkylene group having 2 to 4 carbon atoms. n is the average number of moles of oxyalkylene groups (-O-R 2 -) added and represents a number from 0 to 5. R 3 , R 4 , and R 5 each independently represent an alkyl group having 1 to 20 carbon atoms.)

2. The (meth)acrylic acid-based copolymer according to claim 1, wherein the structural unit derived from the sulfonic acid (salt) group-containing monomer is a structural unit derived from 3-allyloxy-2-hydroxypropanesulfonic acid or a salt thereof.

3. A water treatment agent comprising the (meth)acrylic acid copolymer according to claim 1 or 2.

4. A scale inhibitor comprising the (meth)acrylic acid copolymer according to claim 1 or 2.

5. A silica scale inhibitor comprising the (meth)acrylic acid copolymer according to claim 1 or 2.

Citation Information

Patent Citations

  • Water treating agent

    JP1997108696A

  • Scale inhibitor for geothermal power generation

    JP2016064382A

  • Sulfonic acid group-containing polymer and method for producing the same