Resin composition for semiconductor packaging and copper foil-coated resin containing the same

The resin composition for semiconductor packages, with adjusted dielectric constant and thermal expansion, addresses signal loss and reliability issues in high-frequency circuit boards by using modified epoxy resin and ceramic fillers, ensuring minimal signal loss and maintaining structural integrity.

JP7562843B2Active Publication Date: 2024-10-07LG INNOTEK CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2023513502
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-09-08
Filing Date
2021-08-17
Publication Date
2024-10-07
Estimated Expiration
2041-08-17

AI Technical Summary

Technical Problem

Existing circuit boards for high-frequency applications face challenges in minimizing signal transmission loss while maintaining reliability, as they often suffer from warping, cracking, and peeling due to the use of low dielectric materials, which also compromise adhesive strength and mechanical integrity.

Method used

A resin composition for semiconductor packages is developed, comprising a resin and a filler with specific porosity and depressed portions, which adjusts the dielectric constant to 2.5Dk or less, while maintaining rigidity and reducing thermal expansion, using modified epoxy or maleimide resin with ceramic fillers like SiO2, ZrO2, HfO2, and TiO2.

Benefits of technology

The solution provides a circuit board with reduced signal loss and improved reliability by adjusting the dielectric constant and thermal expansion, allowing for fine circuit patterns and preventing unintended via hole expansion during manufacturing processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007562843000006
    Figure 0007562843000006
  • Figure 0007562843000007
    Figure 0007562843000007
  • Figure 0007562843000008
    Figure 0007562843000008
Patent Text Reader

Abstract

The resin composition for semiconductor packaging according to the embodiment is a composite of a resin and a filler disposed within the resin, the filler having at least one depression on its surface, the filler having a content in the range of 10 vol.% to 40 vol.% of the total volume of the resin composition, and a porosity corresponding to the volume occupied by the depression out of the total volume of the filler having a range of 20% to 35%.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The examples relate to a resin composition for semiconductor packaging, in particular to a resin composition for semiconductor packaging having a low dielectric constant, and to a resin with copper foil, a copper foil laminate, and a circuit board containing the same. [Background technology]

[0002] A printed circuit board (PCB) is a board that is made by printing a circuit line pattern with a conductive material such as copper on an electrically insulating board, and is a board immediately before electronic components are mounted. In other words, it refers to a circuit board on which the mounting position of each component is determined and the circuit pattern that connects the components is printed and fixed on the surface of a flat plate in order to densely mount many different types of electronic elements on the flat plate.

[0003] Components mounted on the printed circuit board can transmit signals generated by the components through circuit patterns connected to each component.

[0004] On the other hand, with the recent trend towards more sophisticated functions in portable electronic devices and the like, signals are becoming increasingly higher in frequency in order to process large amounts of information at high speed, and there is a demand for circuit patterns on printed circuit boards that are suitable for high-frequency applications.

[0005] The circuit patterns of such printed circuit boards should minimize signal transmission loss and allow signal transmission without degrading the quality of high-frequency signals.

[0006] The transmission loss of the circuit pattern of the printed circuit board is mainly composed of conductor loss caused by a thin metal film such as copper, and dielectric loss caused by an insulator such as an insulating layer.

[0007] Conductor loss caused by a thin metal film is related to the surface roughness of a circuit pattern. That is, as the surface roughness of a circuit pattern increases, transmission loss may increase due to a skin effect.

[0008] Therefore, reducing the surface roughness of the circuit pattern has the effect of preventing a decrease in transmission loss, but it has the problem of reducing the adhesive strength between the circuit pattern and the insulating layer.

[0009] Also, due to the reduction caused by the dielectric, a material with a small dielectric constant can be used as an insulating layer for a circuit board.

[0010] However, in circuit boards for high frequency applications, the insulating layer is required to have chemical and mechanical properties suitable for use in circuit boards in addition to a low dielectric constant.

[0011] In particular, insulating layers used in circuit boards for high frequency applications should have isotropic electrical properties for ease of circuit pattern design and processing, low reactivity with metal wiring materials, low ion transfer, sufficient mechanical strength to withstand processes such as chemical mechanical polishing (CMP), low moisture absorption to prevent peeling or an increase in dielectric constant, heat resistance to withstand the processing temperatures of the processes, and a low thermal expansion coefficient to prevent cracks due to temperature changes.

[0012] In addition, insulating layers used in circuit boards for high frequency applications should meet various requirements, such as adhesion, crack resistance, low stress, and low high-temperature gas generation, which can minimize various stresses and peeling that may occur at the interface with other materials (e.g., metal thin films).

[0013] Thus, insulating layers used in circuit boards for high frequency applications should preferentially have low dielectric constant and low coefficient of thermal expansion properties, thereby allowing the overall circuit board thickness to be slimmed down.

[0014] However, when manufacturing a circuit board using insulating layers of low-dielectric material that are thinner than the limit, reliability problems such as warping, cracking, and peeling occur, and the severity of reliability problems such as warping, cracking, and peeling increases as the number of insulating layers of low-dielectric material increases.

[0015] Therefore, there is a need for a method that can realize fine circuit patterns while slimming down circuit boards using insulating layers made of low dielectric materials, and can also solve reliability problems such as warping, cracking, and peeling. Summary of the Invention [Problem to be solved by the invention]

[0016] In the embodiments, it is intended to provide a resin composition for semiconductor packaging, a copper foil-coated resin, and a circuit board including the same, which have improved reliability.

[0017] In addition, the present invention provides a resin composition for semiconductor packaging having a low dielectric constant and a low thermal expansion coefficient, a copper foil-coated resin, and a circuit board including the same.

[0018] In the proposed embodiments, the technical problems to be solved are not limited to the technical problems mentioned above, and other technical problems not mentioned will be clearly understood by a person having ordinary skill in the art to which the embodiments pertain from the description below. [Means for solving the problem]

[0019] The resin composition for semiconductor packages of the first embodiment is a composite of a resin and a filler disposed within the resin, the filler includes at least one depression on a surface, the filler has a content in the range of 10 vol.% to 40 vol.% of the total volume of the resin composition, and a porosity corresponding to the volume occupied by the depression out of the total volume of the filler is in the range of 20% to 35%.

[0020] The insulating film has a dielectric constant of 2.5 Dk or less.

[0021] Moreover, the recess has a groove shape that does not penetrate the filler.

[0022] Moreover, the depression has a shape of a through hole penetrating the filler.

[0023] The resin may be formed of a modify epoxy or maleimide series.

[0024] The resin has a dielectric constant in the range of 2.3Dk to 2.5Dk.

[0025] The filler is SiO 2 , ZrO 3 , HfO 2 , and TiO 2 The ceramic material may include any one of the following:

[0026] The filler has a dielectric constant in the range of 3.7Dk to 4.2Dk.

[0027] The filler has a content in the range of 10 vol. % to 15 vol. %, and the porosity is in the range of 20% to 35%.

[0028] The filler has a content in the range of 15 vol. % to 30 vol. %, and the porosity is in the range of 30% to 35%.

[0029] The filler has a content in the range of 30 vol. % to 40 vol. %, and the porosity is in the range of 32% to 35%.

[0030] The resin also includes a central first region, a second region above the first region adjacent to an upper surface of the resin, and a third region below the first region adjacent to a lower surface of the resin, and the filler is disposed in the second and third regions excluding the first region.

[0031] Meanwhile, in the embodiment, a copper foil laminated resin (RCC) may be provided by laminating and pressing a copper foil on one or both sides of the resin composition for semiconductor packaging.

[0032] On the other hand, the circuit board of the embodiment includes a plurality of insulating layers, a circuit pattern arranged on a surface of at least one of the plurality of insulating layers, and a via penetrating at least one of the plurality of insulating layers, and at least one of the plurality of insulating layers includes the copper foil laminate resin.

[0033] Moreover, the plurality of insulating layers are all made of the copper foil laminate resin.

[0034] Further, the multiple insulating layers include a first insulating section including at least one insulating layer, a second insulating section arranged on the first insulating section and including at least one insulating layer, and a third insulating layer arranged below the first insulating section and including at least one insulating layer, wherein the insulating layer constituting the first insulating section includes prepreg, and the insulating layers constituting the second insulating section and the entire third insulating section each include the copper foil laminate resin.

[0035] The resin composition for semiconductor packages according to the second embodiment is a resin composition which is a composite of a porous resin having first pores and a porous filler having second pores and disposed within the porous resin, the porous filler has a content in the range of 30 vol.% to 40 vol.% of the total volume of the resin composition, and at least one of the first porosity of the porous resin and the second porosity of the porous filler has a content in the range of 10% to 35%.

[0036] Furthermore, the dielectric constant Dk of the resin composition obtained by combining the porous resin and the porous filler is 2.5 or less.

[0037] The second pores have a recess shape that does not penetrate the porous filler.

[0038] Moreover, the second pores have the shape of through-holes penetrating the porous filler.

[0039] The porous resin is formed of a modify epoxy or maleimide series.

[0040] The porous resin has a dielectric constant Dk in the range of 2.3 to 2.5.

[0041] The porous filler is preferably SiO 2 , ZrO 3 , HfO 2 , and TiO 2 The ceramic material may include any one of the following:

[0042] The porous filler has a dielectric constant Dk in the range of 3.7 to 4.2.

[0043] The first porosity of the porous resin is in the range of 10% to 20%, and the second porosity of the porous filler is in the range of 30% to 35%.

[0044] The first porosity of the porous resin is in the range of 21% to 25%, and the second porosity of the porous filler is in the range of 20% to 35%.

[0045] The first porosity of the porous resin is in the range of 26% to 30%, and the second porosity of the porous filler is in the range of 15% to 35%.

[0046] The first porosity of the porous resin ranges from 31% to 35%, and the second porosity of the porous filler ranges from 10% to 35%.

[0047] The second porosity of the porous filler is in the range of 10% to 20%, and the first porosity of the porous resin is in the range of 30% to 35%.

[0048] The second porosity of the porous filler is in the range of 21% to 35%, and the first porosity of the porous resin is in the range of 10% to 35%.

[0049] The resin also includes a central first region, a second region above the first region, and a third region below the first region, and the filler is disposed in the second region and the third region excluding the first region.

[0050] The resin composition for semiconductor packages of the third embodiment is a resin composition which is a composite of a porous resin including first pores, glass fibers disposed in the porous resin, and a porous filler including second pores disposed in the porous resin, wherein the porous filler has a content in the range of 20 vol.% to 30 vol.% in the total volume of the resin composition, and at least one of the first porosity of the porous resin and the second porosity of the porous filler has a content in the range of 10% to 35%.

[0051] Furthermore, the dielectric constant Dk of the resin composition obtained by combining the porous resin and the porous filler is 2.5 or less.

[0052] The glass fibers occupy a range of 50 vol. % to 70 vol. % of the total volume of the resin composition.

[0053] The second pores have a recess shape that does not penetrate the porous filler or a through-hole shape that penetrates the porous filler.

[0054] The porous resin is formed of a modify epoxy or maleimide series.

[0055] The porous resin has a dielectric constant Dk in the range of 2.3 to 2.5.

[0056] The porous filler is preferably SiO 2 , ZrO 3 , HfO 2 , and TiO 2 The ceramic material may include any one of the following:

[0057] The porous filler has a dielectric constant Dk in the range of 3.7 to 4.2.

[0058] The first porosity of the porous resin is in the range of 10% to 20%, and the second porosity of the porous filler is in the range of 30% to 35%.

[0059] The first porosity of the porous resin is in the range of 21% to 25%, and the second porosity of the porous filler is in the range of 20% to 35%.

[0060] The first porosity of the porous resin is in the range of 26% to 30%, and the second porosity of the porous filler is in the range of 15% to 35%.

[0061] The first porosity of the porous resin ranges from 31% to 35%, and the second porosity of the porous filler ranges from 10% to 35%.

[0062] The second porosity of the porous filler is in the range of 10% to 20%, and the first porosity of the porous resin is in the range of 30% to 35%.

[0063] The second porosity of the porous filler is in the range of 21% to 35%, and the first porosity of the porous resin is in the range of 10% to 35%. Effect of the Invention

[0064] In the embodiment, a resin composition for semiconductor packaging is provided that constitutes an insulating layer or insulating film that is a composite of a resin and a filler. In this case, the filler in the embodiment includes at least one recess on the surface. In the embodiment, the dielectric constant of the resin, the dielectric constant of the filler, the resin content, the filler content, and the ratio of the recess in the filler (e.g., porosity) can be adjusted to set the dielectric constant of the insulating layer or insulating film to 2.5 Dk or less while maintaining the rigidity of the insulating layer or insulating film, thereby providing a circuit board suitable for high frequency signal transmission. In the embodiment, the filler includes a recess, which can reduce the degree of thermal expansion that occurs when the temperature of the filler changes, thereby improving the thermal deformation rate of the insulating layer that is a composite of the filler and a resin.

[0065] Further, the resin in the embodiment is a porous resin including pores, and thus may include first pores. In the embodiment, the dielectric constant of the resin, the dielectric constant of the filler, the resin content, the filler content, the porosity of the resin, and the porosity of the filler may be adjusted to set the dielectric constant Dk of the insulating layer or insulating film to 2.5 or less while maintaining the rigidity of the insulating layer or insulating film, thereby providing a circuit board suitable for high frequency signal transmission.

[0066] Furthermore, the insulating layer or insulating film in the embodiment may be a prepreg. That is, the prepreg in the embodiment includes a resin, glass fibers in the resin, and a filler. The resin is porous including a first pore. Also, the filler includes a second pore corresponding to a through-type or a non-through-type. In the embodiment, the dielectric constant Dk of the prepreg can be adjusted to 2.5 or less while maintaining the rigidity of the prepreg corresponding to the insulating layer or insulating film by adjusting the dielectric constant of the glass fiber, the dielectric constant of the resin, the dielectric constant of the filler, the content of the resin, the content of the filler, the content of the glass fiber, the porosity of the resin, and the porosity of the filler, thereby providing a circuit board suitable for high frequency signal transmission.

[0067] Meanwhile, the resin composition in the embodiment may include a first region in the center, a second region above the first region, and a third region below the first region. In this case, the filler in the embodiment may be selectively disposed only in the second and third regions excluding the first region. Differently from this, the filler in the embodiment is disposed in the first to third regions, and the content of the filler disposed in the first region is set to be smaller than the content of the filler disposed in the second and third regions, respectively. As a result, in the embodiment, in the process of forming a via hole in the insulating layer or insulating film and then performing desmearing, it is possible to prevent unintended size expansion of the via hole, thereby forming a fine via.

[0068] Therefore, in the embodiment, the insulating layer is formed using a copper foil laminate resin having a low dielectric constant, thereby making it possible to provide a highly reliable circuit board in which the thickness of the circuit board is slimmed down and signal loss is minimized even in the high frequency band. [Brief description of the drawings]

[0069] [Figure 1] FIG. 2 is a diagram showing a copper foil-coated resin according to the first embodiment. [Diagram 2] FIG. 2 is a cross-sectional view specifically showing the filler of FIG. [Diagram 3] FIG. 2 is a diagram showing a copper foil-coated resin according to a modified example of FIG. [Figure 4] FIG. 4 is a cross-sectional view specifically showing the filler of FIG. [Diagram 5] FIG. 2 is a diagram for explaining the arrangement structure of filler in a copper foil-coated resin according to an embodiment. [Figure 6] FIG. 11 is a diagram showing a change in size of a via hole according to a comparative example. [Figure 7] FIG. 11 is a diagram showing a change in size of a via hole according to an embodiment of the present invention. [Figure 8] FIG. 13 is a diagram showing a copper foil-coated resin according to a second embodiment. [Figure 9]FIG. 13 is a diagram showing a copper foil laminate including a composition for a semiconductor package according to a third embodiment. [Figure 10] FIG. 2 is a diagram showing a circuit board according to the first embodiment. [Figure 11] FIG. 11 is a diagram showing a circuit board according to a second embodiment. [Figure 12] FIG. 13 is a diagram showing a circuit board according to a third embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0070] Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the accompanying drawings. However, the technical concept of the present invention is not limited to some of the embodiments described, and may be embodied in various different forms, and one or more of the components of the embodiments may be selectively combined or substituted within the scope of the technical concept of the present invention.

[0071] Furthermore, the terms (including technical and scientific terms) used in the embodiments of the present invention may be interpreted as having a meaning commonly understood by a person of ordinary skill in the art to which the present invention belongs, unless otherwise clearly and specifically defined and described, and commonly used terms, such as predefined terms, may have their meaning interpreted taking into account the contextual meaning of the relevant art.

[0072] In addition, the terms used in the embodiments of the present invention are intended to describe the embodiments and are not intended to limit the present invention. In the present specification, the singular form can include the plural form unless otherwise specified in the phrase, and when described as "A and (and) at least one (or more) of B and C", it can include one or more of all combinations that can be combined with A, B, and C.

[0073] In addition, in describing the components of the present invention, terms such as first, second, A, B, (a), (b), etc. are used. Such terms are merely used to distinguish the components from other components, and are not intended to limit the essence, order, or sequence of the components.

[0074] Furthermore, when a component is described as being "coupled," "coupled," or "connected" to another component, it includes not only cases where the component is directly coupled, coupled, or connected to the other component, but also cases where the component is "coupled," "coupled," or "connected" by another component between the component and the other component.

[0075] In addition, when it is described as being formed or disposed "on or under" each component, "on or under" includes not only the case where the two components are in direct contact with each other, but also the case where one or more other components are formed or disposed between the two components.

[0076] In addition, when it is expressed as "above" or "below," it can include the meaning of not only the upward direction but also the downward direction based on one component.

[0077] In one embodiment, the resin composition for semiconductor packaging may be a composite of resin and filler. For example, the resin composition for semiconductor packaging in one embodiment may have a structure in which a resin and a certain amount of filler are dispersed in the resin. In one embodiment, a copper foil layer may be laminated and pressed onto at least one surface of the resin composition for semiconductor packaging composed of the composite of resin and filler as described above, to produce a resin coated copper (RCC). Thus, the resin coated copper in one embodiment may include an insulating film (or insulating layer) composed of a composite of resin and filler, and a copper foil layer laminated and pressed onto at least one surface of the insulating film.

[0078] In another embodiment, the resin composition for semiconductor packaging is a composite of resin and filler, and may have a structure in which a certain amount of filler and glass fiber (glass cloth) are dispersed in the resin. In another embodiment, a copper clad laminate (CCL) may be manufactured by laminating and pressing a copper foil layer on at least one surface of the resin composition for semiconductor packaging composed of the composite of resin and filler as described above. Thus, the copper clad laminate in another embodiment includes a copper foil layer laminated and pressed on at least one surface of a prepreg composed of a composite of resin, filler, and glass fiber.

[0079] Hereinafter, a resin composition for semiconductor packaging in one embodiment will be described. For example, the resin composition for semiconductor packaging described below may refer to a resin composition for semiconductor packaging applied to a resin coated with copper foil RCC (Resin Coated Copper). Specifically, the resin coated with copper foil including an insulating film (or insulating layer) having a low dielectric constant and a low thermal expansion coefficient and a copper foil layer according to one embodiment will be described below.

[0080] FIG. 1 is a diagram showing a copper foil-coated resin according to a first embodiment, and FIG. 2 is a cross-sectional view specifically showing the filler of FIG.

[0081] 1 and 2, the copper foil-coated resin according to the first embodiment includes an insulating film 110 (or an insulating layer or a resin composition for a semiconductor package) and a copper foil layer 120 disposed on one surface of the insulating film 110. The insulating film 110 can also be called an insulating layer. Hereinafter, for convenience of explanation, the insulating film will be described as the insulating layer 110.

[0082] The insulating layer 110 includes a resin 111 and a filler 112 dispersed in the resin 111. The insulating layer 110 may be a resin for semiconductor packaging. In an embodiment, the dielectric constant Dk of the insulating layer 110 can be adjusted to 2.5 or less by changing the composition in the insulating layer 110 constituting the resin for semiconductor packaging. Hereinafter, the resin for semiconductor packaging is referred to as the insulating layer 110, and a resin composition for semiconductor packaging corresponding to the insulating layer 110 will be specifically described.

[0083] Such an insulating layer 110 is a composite of a resin 111 and a filler 112. The insulating layer 110 may have a specific third dielectric constant that is a combination of a first dielectric constant possessed by the resin 111 and a second dielectric constant possessed by the filler 112.

[0084] In this case, the third dielectric constant Dk of the insulating layer 110 in the embodiment may be 2.5 or less. This allows the insulating layer 110 in the embodiment to be applied to a circuit board suitable for high frequency applications. This allows the insulating layer 110 in the embodiment to minimize signal loss, thereby improving reliability.

[0085] Hereinafter, the characteristics of the resin 111 and the filler 112 for the insulating layer 110 to have the third dielectric constant Dk of 2.5 or less will be described in detail.

[0086] Prior to this, the insulating layer in the comparative example will be described.

[0087] The insulating layer of the comparative example may include a resin and a ceramic filler disposed in the resin. The ceramic filler generally has a high dielectric constant. Specifically, among the types of ceramic fillers, the ceramic filler having the lowest dielectric constant has a dielectric constant Dk of about 3.9. As a result, in the comparative example, there is a limit to lowering the dielectric constant of the insulating layer by changing the filler material.

[0088] In addition, the dielectric constant of the insulating layer of the comparative example is affected by the dielectric constant of the resin as well as the dielectric constant of the ceramic filler. The dielectric constant Dk of the resin ranges from 2.2 to 6.5 depending on the type. At this time, the dielectric constant Dk of polytetrafluoroethylene (PTFE) can be as low as about 2.2. However, polytetrafluoroethylene (PTFE) requires a high process temperature and additional insulating sheets (e.g., bonding sheets) are required to stack multiple layers, which may make it difficult to apply it to 5G high frequency boards.

[0089] Generally, the dielectric constant Dk of the resin constituting the insulating layer of the comparative example is about 2.4. Therefore, in the comparative example, the glass fiber (Glass cloth) constituting the insulating layer is removed and the prepreg type (PPG) is changed to a copper foil resin type (RCC), thereby lowering the dielectric constant Dk of the insulating layer to a level of 3.0. Furthermore, in the comparative example, the content of the low dielectric constant resin and the filler dispersed in the low dielectric constant resin is reduced, thereby reducing the dielectric constant Dk of the insulating layer to a level of 2.8. However, if the content of the filler in the insulating layer is reduced, the overall strength of the insulating layer is reduced, which causes a problem that the manufacturing process of the circuit board cannot be performed normally. Therefore, there is a limit to the reduction in the content of the filler in the insulating layer, and therefore, in the comparative example, the dielectric constant Dk of the insulating layer could not be reduced to 2.8 or less.

[0090] In contrast, in the embodiment, the resin 111 constituting the insulating layer 110 has a low dielectric constant, the filler 112 in the resin 111 has a certain content or more, and the filler 112 includes at least one recess 112a.

[0091] Preferably, the filler 112 in the embodiment includes a plurality of depressions 112a recessed inward on the surface. In this case, the plurality of depressions 112a may be formed by being depressed inward from the surface of the filler 112 to a certain depth. Preferably, the depressions 112a may be formed on the surface of the filler 112 and may be realized in the form of a groove that does not penetrate the filler 112. Preferably, the filler 112 may be a porous filler including a plurality of depressions 112a.

[0092] That is, the insulating layer 110 in the first embodiment may be a composite of a resin 111 and a porous filler 112 formed in the resin 111 and having at least one depression 112a on the surface.

[0093] Meanwhile, although the filler 112 includes the recessed portion 112a in the above description, the filler 112 is not limited thereto. For example, the filler 112 may have a structure including a plurality of concave and convex portions (not shown) protruding outward from the surface.

[0094] Thus, the porosity described below can be defined as follows:

[0095] Preferentially, when the filler 112 includes a depression, the depression 112a may be formed by forming a plurality of pores in the filler having a volume of "A." In this case, the porosity may refer to the ratio of the volume of the depression 112a to the volume of "A" of the filler 112 having a circular shape.

[0096] Furthermore, when the filler 112 includes an uneven portion, the porosity can be defined as follows. The filler 112 may have a circular shape. A plurality of uneven portions may be formed in the filler. In this case, in the case of a filler including the uneven portion, the porosity can be the volume ratio of a circle corresponding to the entire diameter of the filler including the uneven portion, or the volume of the via space since the uneven portion is not formed.

[0097] Meanwhile, the porosity of the filler can also be expressed as oil absorption (ml / 100g, LP). That is, assuming that the filler has a perfectly spherical shape, oil can be permeated into the filler. The amount of oil permeation can correspond to the volume of the empty space in the total volume of the perfectly spherical filler. Thus, the porosity can also be expressed as the oil absorption.

[0098] Alternatively, the porosity of the filler can be measured by a gas adsorption method (BET) or a mercury adsorption method. The gas adsorption method is a method in which a sample is adsorbed with a gas (usually nitrogen) to measure the specific surface area, pore size and distribution of the sample surface, and even closed micropores can be analyzed. The pore size analysis range of the gas adsorption method is 0.35nm to 200nm, and the analysis results that can be confirmed are surface area (m2 / g), pore size, total pore volume, and pore size distribution.

[0099] The gas adsorption method allows the surface area of ​​a sample to be calculated using the change in the volume of the adsorbed gas due to a change in pressure, and the shape of the pores present in the sample can be confirmed based on the shape of the curve of the gas adsorption / desorption graph that can be confirmed by the gas adsorption method.

[0100] The resin 111 in the first embodiment may have a low dielectric constant.

[0101] At this time, the types of general resins and the dielectric constants corresponding to the types of resins are as shown in FIG.

[0102] [Table 1]

[0103] As described above, the resin may include various materials. In this regard, resins including phenolic, general epoxy, and cyanate have a dielectric constant Dk of 2.6 or more, so it is difficult to reduce the dielectric constant Dk of the insulating layer 110 to 2.5 or less.

[0104] In addition, the resin containing PTFE has a low dielectric constant of about 2.2, but requires high processing temperature conditions. For example, the processing temperature required for general resin is 250°C, while the PTFE requires a processing temperature of 300°C or more. In addition, in order to manufacture a multi-layer circuit board, the PTFE requires a bonding sheet during the lamination process, which increases the overall thickness of the circuit board, making it difficult to slim down the circuit board.

[0105] In this embodiment, the dielectric constant of the resin 111 constituting the insulating layer 110 can be reduced by using a modify epoxy or maleimide series.

[0106] That is, the resin 111 in the embodiment may include a modify epoxy or maleimide series having a dielectric constant Dk in the range of 2.3 to 2.5.

[0107] The filler 112 may have a certain level of dielectric constant Dk. For example, the filler 112 may be made of a ceramic filler. At this time, the dielectric constant Dk according to the type of ceramic filler is as shown in Table 2 below.

[0108] [Table 2]

[0109] As mentioned above, the filler 112 is Al 2 O 3In the case where the filler 112 is formed, the dielectric constant Dk of the filler 112 itself is at a level of 9.0, and therefore there is a limit to how much the dielectric constant of the resin 111 alone can reduce the overall dielectric constant Dk of the insulating layer 110, which is a composite of these, to 2.5 or less.

[0110] Therefore, in the embodiment, SiO 2 , ZrO 3 , HfO 2 , and TiO 2 The filler 112 is made of any one of the ceramic materials.

[0111] Thus, the filler 112 may have a dielectric constant in the range of 3.7Dk to 4.2Dk. In this case, the dielectric constant of the filler 112 may refer to a dielectric constant in a state where the recess 112a is not formed in the filler 112. Specifically, the filler 112 is basically made of SiO 2 , ZrO 3 , HfO 2 , and TiO 2 When made of any one of the above ceramic materials, it can have a dielectric constant in the range of 3.7Dk to 4.2Dk.

[0112] At this time, the filler 112 may have the depression 112a as described above. Specifically, the depression 112a of the filler 112 in the first embodiment may be formed by being depressed inwardly on the surface of the filler 112. More specifically, the depression 112a of the filler 112 in the first embodiment may have a depth smaller than the diameter of the filler 112 and may be depressed inwardly of the filler 112. More specifically, the depression 112a of the filler 112 may be a groove formed on the surface of the filler 112 and depressed inwardly of the filler 112.

[0113] Therefore, in the embodiment, since there is a limit to how much the insulating layer 110 can have a dielectric constant of 2.5 or less by simply adjusting the materials and contents of the resin 111 and filler 112, a recess 112a is formed in the filler 112 so that the dielectric constant Dk of the insulating layer 110 formed by the combination of the resin 111 and filler 112 can be reduced to 2.5 or less.

[0114] In this case, the dielectric constant of the insulating layer 110 may be determined by the dielectric constant of the resin 111, the dielectric constant of the filler 112, the content of the resin 111, the content of the filler 112, and the ratio of the volume of the recessed portion 112a to the total volume of the filler 112. For example, the ratio of the volume of the recessed portion 112a to the total volume of the filler 112 may be expressed as porosity (%).

[0115] As described above, the resin 111 may be formed of a modify epoxy or maleimide series, and may include a modify epoxy or maleimide series having a dielectric constant Dk in the range of 2.3 to 2.5.

[0116] The filler 112 is SiO 2 , ZrO 3 , HfO 2 , and TiO 2 and may have a dielectric constant Dk in the range of 3.7 to 4.2.

[0117] On the other hand, if the filler 112 is contained in the insulating layer 110 at less than 10 vol.%, the rigidity of the insulating layer 110 is weakened, which may cause a problem in reliability during the manufacturing process of the circuit board. For example, if the filler 112 is contained in the insulating layer 110 at less than 10 vol.%, the insulating layer 110 may warp significantly during the manufacturing process of the circuit board, which may cause a problem in that the manufacturing process cannot be performed normally.

[0118] Furthermore, if the filler 112 exceeds 40 vol.% in the insulating layer 110, it may be difficult to adjust the dielectric constant Dk of the insulating layer 110 to 2.5 or less. For example, if the filler 112 exceeds 40 vol.% in the insulating layer 110, in order to adjust the dielectric constant Dk of the insulating layer 110 to 2.5 or less, the volume occupied by the recess 112a in the total volume of the filler 112 must be large, which may weaken the rigidity of the filler 112 and cause reliability problems.

[0119] Therefore, the filler 112 is set to have a range of 10 vol.% to 40 vol.% in the insulating layer 110. Correspondingly, the resin 111 is set to have a range of 60 vol.% to 90 vol.% in the insulating layer 110.

[0120] Meanwhile, the porosity, which is the ratio of the volume of the recessed portion 112a to the total volume of the filler 112, may vary depending on the content of the filler 112. For example, as the content of the filler 112 increases, the porosity may increase in proportion thereto. Also, as the content of the filler 112 decreases, the porosity may decrease. However, if the porosity, which is the ratio of the volume of the recessed portion 112a to the total volume of the filler 112, exceeds 35%, the rigidity of the filler 112 and the strength of the insulating layer 110, which is a composite of the filler 112, may be weakened, resulting in a reliability problem. Also, if the porosity, which is the ratio of the volume of the recessed portion 112a to the total volume of the filler 112, is less than 20%, it may be difficult to adjust the dielectric constant Dk of the insulating layer 110 to 2.5 or less.

[0121] Therefore, in the embodiment, the porosity, which is the ratio of the volume of the recessed portion 112a to the total volume of the filler 112, is set to be in the range of 20% to 35%. However, the ratio of the recessed portion 112a can be precisely determined depending on the content of the filler 112 in the insulating layer 110.

[0122] Specifically, the dielectric constant of the insulating layer 110 according to the ratio of the content of the filler 112 in the insulating layer 110 to the depression 112a in the filler 112 is as shown in Table 3 below.

[0123] [Table 3]

[0124] Referring to Table 3, the ratio of the depressions 112a to the total volume of the filler 112 can be defined as the porosity.

[0125] At this time, when the insulating layer 110 contains 10 vol.% of the filler 112, the porosity of the filler 112 must be 20% or more. However, when the porosity exceeds 35%, reliability problems due to rigidity as described above may occur. Thus, in an embodiment, when the insulating layer 110 contains 10 vol.% of the filler 112, the porosity of the filler 112 may be 20% to 35%. For example, when the insulating layer 110 contains 10 vol.% to 15 vol.% of the filler 112, the porosity of the filler 112 may be 20% to 35%.

[0126] Furthermore, when the insulating layer 110 contains 20 vol.% of the filler 112, the porosity of the filler 112 must be 30% or more. However, when the porosity exceeds 35%, reliability problems due to rigidity as described above may occur. Thus, in an embodiment, when the insulating layer 110 contains 20 vol.% of the filler 112, the porosity of the filler 112 may be 30% to 35%. For example, when the insulating layer 110 contains 15 vol.% to 30 vol.% of the filler 112, the porosity of the filler 112 may be 30% to 35%.

[0127] Furthermore, when the filler 112 is contained in the insulating layer 110 at 40 vol.%, the porosity of the filler 112 must be 35% or more. However, when the porosity exceeds 35%, reliability problems due to rigidity as described above may occur. Thus, in an embodiment, when the filler 112 is contained in the insulating layer 110 at 40 vol.%, the porosity of the filler 112 may be 35%. For example, when the filler 112 is contained in the insulating layer 110 at more than 30 vol.% and not more than 40 vol.%, the porosity of the filler 112 may be 32% to 35%.

[0128] As described above, in the embodiment, the dielectric constant of resin 111, the dielectric constant of filler 112, the content of resin 111, the content of filler 112, and the proportion of the recessed portion in filler 112 are adjusted so that the dielectric constant Dk of insulating layer 110, which is a composite of resin 111 and filler 112, can be adjusted to 2.5 or less.

[0129] Meanwhile, the dielectric constant of the insulating layer 110 may be measured by the following device and method. That is, the insulating layer 110 may not be used as a single product, but may be used as a copper foil laminate resin having a copper foil layer 120 laminated on at least one surface thereof. In this case, the dielectric constant of the insulating layer 110 may be measured by removing the copper foil layer 120 from the copper foil laminate resin, drying the insulating layer 110 at 100° C. for 60 minutes with the copper foil layer 120 removed, and measuring the dielectric constant by a split post dielectric resonance (SPDR) method using a N5222A PNA Network analyzer (Agilent) device and a resonator under the conditions of 25° C. and 50% RH.

[0130] According to this, in the embodiment, the dielectric constant Dk of the insulating layer 110 can be adjusted to 2.5 or less while maintaining the rigidity of the insulating layer 110, thereby providing a circuit board suitable for high frequency signal transmission. Also, in the embodiment, the filler 112 includes a recess 112a, which can reduce the degree of thermal expansion that occurs when the temperature of the filler 112 changes, thereby improving the thermal deformation rate of the insulating layer, which is a composite of the filler and the insulating layer.

[0131] FIG. 3 is a diagram showing a copper foil-coated resin according to a modified example of FIG. 1, and FIG. 4 is a cross-sectional view specifically showing the filler of FIG.

[0132] 3 and 4, the copper foil-coated resin according to the modified example includes an insulating film 110A and a copper foil layer 120 disposed on one surface of the insulating film 110A. The insulating layer 110A includes a resin 111 and a filler 112A dispersed within the resin 111.

[0133] The filler 112A in the modified example includes a plurality of depressions 112Aa recessed inward on the surface. In this case, the plurality of depressions 112Aa may be formed by being depressed inward from the surface of the filler 112 to a certain depth. Preferably, the depressions 112Aa may be formed on the surface of the filler 112A and may be realized in the shape of a hole penetrating the filler 112A. Preferably, the filler 112A may be a hollow filler including at least one depression 112Aa. That is, the depressions 112Aa of the filler 112A in the modified example may be a through hole penetrating the surface of the filler 112A, unlike the depressions of FIG. 1.

[0134] Specifically, the filler depression in Fig. 1 has a recess shape with a non-penetrating structure, but the filler depression in Fig. 3 may have a through-hole shape with a penetrating structure. That is, the insulating layer 110A in Fig. 3 may be a composite of a resin 111 and a hollow filler 112A formed in the resin 111 and including at least one depression 112Aa on the surface.

[0135] 3, the dielectric constant of insulating layer 110A, which is a composite of filler 112A and resin 111, may change depending on the ratio of through-hole shaped depressed portion 112Aa in filler 112A. That is, the dielectric constant of insulating layer 110A may be determined by the dielectric constant of resin 111, the dielectric constant of filler 112A, the content of resin 111, the content of filler 112A, and the ratio of the volume of depressed portion 112Aa to the total volume of filler 112A. In this case, the ratio of the volume of depressed portion 112Aa to the total volume of filler 112A may also be expressed as porosity.

[0136] In other words, in a filler generally having porosity, the shape of the depression may be a groove shape or a through hole shape. Specifically, the depression may be a closed groove shape in which a plurality of depressions are separated or isolated from one another within the filler. The depression may be an open hole shape in which a plurality of depressions are connected to one another within the filler. The depression 112a in the first embodiment may be configured in a closed shape within the filler, and the depression 112Aa in the second embodiment may be configured in an open shape within the filler 112A.

[0137] Meanwhile, the porosity, which corresponds to the ratio of the volume occupied by the recess 112Aa to the total volume of the filler 112A, may vary depending on the content of the filler 112A. For example, as the content of the filler 112A increases, the porosity, which is the ratio of the volume occupied by the recess 112Aa, may increase in proportion thereto. Also, as the content of the filler 112A decreases, the ratio of the volume occupied by the recess 112Aa may decrease. However, if the ratio of the recess 112Aa to the total volume of the filler 112A exceeds 35%, the rigidity of the filler 112A and the strength of the insulating layer 110A, which is a composite of the filler 112A, may be weakened, resulting in a reliability problem. Also, if the ratio of the recess 112Aa to the total volume of the filler 112A is less than 20%, it may be difficult to adjust the dielectric constant of the insulating layer 110A to 2.5 Dk or less.

[0138] In this case, the copper foil-coated resin in FIG. 3 differs from the copper foil-coated resin in FIG. 1 only in the shape of the depression formed in the filler, and other features are substantially the same, and therefore detailed description thereof will be omitted.

[0139] FIG. 5 is a diagram for explaining the arrangement structure of the filler in the copper foil-coated resin according to the first embodiment.

[0140] Referring to FIG. 5, in an embodiment of the copper foil resin, the filler can be formed in a specific area within the insulating layer.

[0141] Referring to FIG. 5(a), the copper foil-resin insulating layer 110 can be divided into a plurality of regions in the vertical direction.

[0142] For example, the insulating layer 110 may include a first region 111a in the center. The insulating layer 110 may also include a second region 111b adjacent to an upper surface of the insulating layer 110 above the first region 111a. The insulating layer 110 may also include a third region 111c adjacent to a lower surface of the insulating layer 110 below the first region 111a.

[0143] The filler 112 in the insulating layer 110 may be disposed in a specific region among a first region 111a, a second region 111b, and a third region 111c of the insulating layer 110. The filler 112 may be a porous filler including a groove-shaped depression 112a as shown in FIG. 1. That is, in the embodiment, the dielectric constant of the insulating layer 110 is adjusted to 2.5 or less by controlling the content of the filler 112 in the insulating layer 110 and the porosity of the filler 112. At this time, if the content of the filler 112 is limited and the filler 112 is distributed throughout the insulating layer 110, a problem may occur in the reliability of a via hole, which will be described later.

[0144] Thus, in the embodiment, the filler 112 may be disposed in the second region 111b and the third region 111c excluding the first region 111a of the insulating layer 110. In other words, the filler 112 in the embodiment may not be disposed in the first region 111a. For example, the filler 112 in the embodiment may be evenly sprayed and disposed in the second region 111b and the third region 111c. This is to prevent the upper and lower widths of the via hole from widening during a desmear process in the process of forming the via hole later.

[0145] However, the embodiment is not limited thereto, and the filler 112 may also be disposed in the first region 111a of the insulating layer 110. When the filler 112 is also disposed in the first region 111a of the insulating layer 110, the content of the filler disposed in the first region 111a may be smaller than the content of the filler disposed in each of the second region 111b and the third region 111c. Thus, in the embodiment, it is possible to prevent the via hole from expanding during the desmear process of the via hole.

[0146] 5(b), the insulating layer 110A of the copper foil-coated resin is substantially the same as the copper foil-coated resin of FIG 5(a). However, the filler 112A including the through-hole-shaped depressions may be concentrated in the second region 111b and the third region 111c of the insulating layer 110A of FIG 5(b).

[0147] FIG. 6 is a diagram showing the size change of the via hole according to the comparative example, and FIG. 7 is a diagram showing the size change of the via hole according to the example.

[0148] 6(a), the insulating layer 10 in the comparative example includes a resin 11 and a filler 12. At this time, the filler 12 is disposed over the entire area of ​​the insulating layer 10 in the comparative example.

[0149] In this case, a via hole VH having a first upper width a and a first lower width b is formed in the insulating layer 10 in the comparative example. In this case, in a general circuit board manufacturing process, after the via hole VH is formed, a desmear process is performed on the inner wall of the via hole VH.

[0150] At this time, when a desmear process is performed on the insulating layer 10 in the comparative example, the size of the via hole formed in the insulating layer 10 may be expanded. Specifically, the via hole VH' after the desmear process has a second upper width a' larger than the first upper width a and a second lower width b' larger than the first lower width b.

[0151] Alternatively, referring to (a) of Fig. 7, an insulating layer in an embodiment may include a resin and a filler. The insulating layer may be the insulating layer of the first embodiment of Fig. 1 or the insulating layer of the second embodiment of Fig. 3. Thus, a resin 111 and the fillers 112, 112A may be disposed in the insulating layer.

[0152] In this embodiment, the insulating layer 110 is vertically divided into three regions, of which the first region 111a in the center is excluded, and the second region 111b and the third region 211c are selectively disposed above and below the first region 111a.

[0153] As a result, in the comparative example, a via hole VH having a third upper width A and a third lower width B can be formed in the insulating layer.

[0154] When a desmear process is performed on the formed via hole VH, desmearing is concentrated in the first region 111a where no filler is disposed or where the filler content is lower than in other regions. As a result, the via hole VH' after the desmear process has a fourth upper width A' corresponding to the third upper width A and a fourth lower width B' corresponding to the third lower width B.

[0155] The following describes a resin composition for a semiconductor according to Example 2. The resin composition for a semiconductor in Example 2 can be applied to a copper foil-coated resin in the same manner as in Example 1.

[0156] FIG. 8 is a diagram showing a copper foil-coated resin according to the second embodiment.

[0157] The copper foil-laminated resin 1000 according to the second embodiment includes an insulating film 1100 (or an insulating layer or a resin composition for semiconductor packages) and a copper foil layer 1200 disposed on one surface of the insulating film 1100 .

[0158] The insulating layer 1100 includes a resin 1110 and a filler 1120 dispersed within the resin 1110 .

[0159] In the second embodiment, the resin 1110 constituting the insulating layer 1100 contains a certain amount of filler 1120, and pores are formed in the resin 1110 and the filler 1120, respectively.

[0160] Specifically, the insulating layer 1100 includes 60 vol.% to 70 vol.% of the resin 1110 and 30 vol.% to 40 vol.% of the filler 1120. Here, the insulating layer 1100 of the embodiment is RCC that does not include glass fiber. Thus, in the embodiment, the filler 1120 has a content in the range of 30 vol.% to 40 vol.% so that the insulating layer 1100 can have a strength of a certain level or more in the manufacturing process of the circuit board. Also, in the embodiment, when a via (not shown) is formed in the insulating layer 1100, the filler 1120 is included in the insulating layer 1100 with a content in the range of 30 vol.% to 40 vol.% as described above so that the quality of the via can be ensured when the via (not shown) is formed in the insulating layer 1100. That is, in the manufacturing process of the circuit board, a desmear process is unavoidable after processing a via hole (not shown) in the insulating layer 1100 using a laser. At this time, if the content of the filler 1120 is less than 30 vol.%, the surface roughness of the via hole increases, which may cause signal loss. For example, if the content of the filler 1120 is less than 30 vol.%, problems may occur in the quality of the via. Also, if the content of the filler 1120 is 40 vol.% or more, it may be difficult to adjust the dielectric constant Dk of the insulating layer 1100 to a low dielectric constant, for example, 2.5 or less. Therefore, in the embodiment, the content of the filler 1120 in the insulating layer 1100 is set to 30 vol.% to 40 vol.%.

[0161] Meanwhile, in the first embodiment, there is a limit to how much the dielectric constant of the insulating layer can be reduced by simply adjusting the resin and filler contents, and therefore pores (eg, depressions) are formed in the filler.

[0162] In the second embodiment, in addition to the structure of the first embodiment, pores are formed not only in the filler but also in the resin.

[0163] To this end, the resin 1110 in the second embodiment includes the first pores 1110A. A plurality of the first pores 1110A may be formed in the resin 1110. That is, the resin 1110 in the embodiment may be a porous resin.

[0164] The resin 1110 may have a first porosity. The first porosity may correspond to a ratio of a volume of the first pores 1110A to a total volume of the resin 1110. The first porosity of the resin 1110 may be determined by a second porosity of the filler 1120, which will be described later. The first porosity of the resin 1110 will be described in detail below.

[0165] Further, the filler 1120 in the embodiment includes second pores (not shown). In this case, the second pores can be referred to as "depressions" formed on the surface of the filler 1120. Hereinafter, the "depressions" will be described as second pores. The second pores may correspond to any one of the depressions shown in FIG. 1 and FIG. 3. The second pores have already been described with reference to FIG. 1 and FIG. 3, so the description thereof will be omitted. That is, the second pores may have a recess shape with a non-through structure as shown in FIG. 1, or may have a hole shape with a through structure as shown in FIG. 3.

[0166] Meanwhile, the first porosity of the resin 1110 may be inversely proportional to the second porosity of the filler 1120. For example, the larger the first porosity of the resin 1110, the smaller the second porosity of the filler 1120. Conversely, the smaller the first porosity of the resin 1110, the larger the second porosity of the filler 1120.

[0167] Meanwhile, the dielectric constant of the insulating layer 1100 may be determined by the dielectric constant of the resin 1110, the dielectric constant of the filler 1120, the content of the resin 1110, the content of the filler 1120, a first porosity of the resin 1110, and a second porosity of the filler 1120. Meanwhile, the first porosity and the second porosity may also be referred to as a first porosity and a second porosity, and may be expressed as "porosity, %".

[0168] At this time, in the second embodiment, the resin 1110 of the insulating layer 1100 is made of a modify epoxy or maleimide series, as in the first embodiment, and the filler 1120 is made of SiO 2 , ZrO 3 , HfO 2 , and TiO 2 The ceramic material may include any one of the following:

[0169] Meanwhile, when the insulating layer 1100 contains less than 30 vol.% of the filler 1120, the rigidity of the insulating layer 1100 is weakened, which may cause reliability problems in the manufacturing process of the circuit board. For example, when the insulating layer 1100 contains less than 30 vol.% of the filler 1120, the insulating layer 1100 may warp significantly in the manufacturing process of the circuit board, which may cause a problem that the manufacturing process cannot be performed normally. Also, when the insulating layer 1100 contains less than 30 vol.%, the signal loss of the via formed in the insulating layer 1100 may increase, which may cause reliability problems. Therefore, in the embodiment, the insulating layer 1100 contains more than 30 vol.% of the filler 1120.

[0170] In addition, if the filler 1120 exceeds 40 vol.% in the insulating layer 1100, it may be difficult to adjust the dielectric constant Dk of the insulating layer 1100 to 2.5 or less. For example, if the filler 1120 exceeds 40 vol.% in the insulating layer 1100, in order to adjust the dielectric constant Dk of the insulating layer 1100 to 2.5 or less, the first porosity of the resin 1110 or the second porosity of the filler 1120 must be large in the total volume of the filler 1120, which may weaken the rigidity of the resin 1110 or the filler 1120, resulting in reliability problems.

[0171] Therefore, the filler 1120 is set to have a range of 30 vol.% to 40 vol.% in the insulating layer 1100. Correspondingly, the resin 1110 is set to have a range of 60 vol.% to 70 vol.% in the insulating layer 1100.

[0172] Meanwhile, the first porosity of the resin 1110 and the second porosity of the filler 1120 are as follows.

[0173] In an embodiment, the first porosity of the resin 1110 may range from 10% to 35%.

[0174] If the first porosity of the resin 1110 is less than 10%, it may be difficult to adjust the dielectric constant of the insulating layer 1100 to 2.5 or less. Also, if the first porosity of the resin 1110 is more than 35%, an increase in the first pores 1110A may cause reliability problems in the rigidity of the resin 1110 and the insulating layer 1100 including the resin 1110.

[0175] At this time, the first porosity of the resin 1110 may be adjusted within the range of 10% to 35% based on the second porosity of the filler 1120 .

[0176] The second porosity of the filler 1120 may be in the range of 10% to 35%.

[0177] If the second porosity of the filler 1120 is less than 10%, it may be difficult to adjust the dielectric constant of the insulating layer 1100 to 2.5 or less. If the second porosity of the filler 1120 is more than 35%, a problem may occur in the rigidity of the filler 1120 due to an increase in the second pores. For example, if the second porosity of the filler 1120 is more than 35%, a reliability problem such as cracking of the filler 1120 in the insulating layer 1100 may occur. Therefore, in an embodiment, the second porosity of the filler 1120 is adjusted to be within a range of 10% to 35%. Meanwhile, the second porosity of the filler 1120 may be adjusted based on the porosity of the resin 1110.

[0178] The dielectric constant of the insulating layer 1100 according to the first porosity of the resin 1110 and the second porosity of the filler 1120 is shown in Table 4 below.

[0179] [Table 4]

[0180] In the embodiment, the dielectric constant Dk of the insulating layer 1100 can be adjusted to 2.5 or less. Thus, the dielectric constant due to the first porosity of the resin 1110 including the first pores 1110A and the second pores of the filler 1120 having the recess-shaped second pores is as shown in Table 3. As described above, the first porosity of the resin 1110 is adjusted to be within the range of 10% to 35%. Also, the second porosity of the filler 1120 is adjusted to be within the range of 10% to 35%.

[0181] In the following, the second porosity that the filler 1120 should have will be described based on the first porosity of the resin 1110.

[0182] That is, in the embodiment, the first porosity of the resin 1110 is determined within a range of 10% to 35%, and the second porosity of the filler 1120 is adjusted based on the first porosity. Conversely, in the embodiment, the second porosity of the filler 1120 is determined within a range of 10% to 35%, and the first porosity of the resin 1110 is adjusted based on the second porosity. (1) Secondary porosity of filler 1120 due to primary porosity of resin

[0183] As described above, the first porosity of the resin 1110 may be determined within the range of 10% to 35%.

[0184] For example, the first porosity of the resin 1110 may be determined to be 10% to 20%. In this case, the second porosity of the filler 1120 is adjusted to be within the range of 30% to 35%.

[0185] Also, the first porosity of the resin 1110 may be determined to be 21% to 25%. In this case, the second porosity of the filler 1120 is adjusted to be within the range of 20% to 35%.

[0186] Also, the first porosity of the resin 1110 may be determined to be 26% to 30%. In this case, the second porosity of the filler 1120 is adjusted to be within the range of 15% to 35%.

[0187] Also, the first porosity of the resin 1110 may be determined to be 31% to 35%. In this case, the second porosity of the filler 1120 is adjusted to be within the range of 10% to 35%. (2) The primary porosity of the resin 1110 due to the secondary porosity of the filler 1120

[0188] On the contrary, in an embodiment, the second porosity of the filler 1120 is determined within a specific range, and based on this, the first porosity of the resin 1110 can be adjusted so that the dielectric constant Dk of the insulating layer 1100 is 2.5 or less.

[0189] For example, the second porosity of the filler 1120 may be determined to be 10% to 20%. In this case, the first porosity of the resin 1110 may be adjusted within a range of 30% to 35%.

[0190] For example, the second porosity of the filler 1120 may be determined to be 21% to 35%. In this case, the first porosity of the resin 1110 may be adjusted within a range of 10% to 35%.

[0191] As described above, in the embodiment, the dielectric constant of the resin 1110, the dielectric constant of the filler 1120, the content of the resin 1110, the content of the filler 1120, the first porosity of the resin 1110, and the second porosity of the filler 1120 are adjusted so that the dielectric constant Dk of the insulating layer 1100, which is a composite of the resin 1110 and the filler 1120, can be set to 2.5 or less.

[0192] Meanwhile, the dielectric constant of the insulating layer 1100 may be measured by the following device and method. That is, the insulating layer 1100 may not be used as a single product, but may be used as a copper foil laminate resin having a copper foil layer 120 laminated on at least one surface thereof. In this case, the dielectric constant of the insulating layer 1100 may be measured by removing the copper foil layer 120 from the copper foil laminate resin, drying the insulating layer 1100 at 100°C for 60 minutes with the copper foil layer 120 removed, and measuring the dielectric constant by a split post dielectric resonance (SPDR) method at 25°C and 50% RH using an N5222A PNA Network analyzer (Agilent) device and a resonator.

[0193] According to this embodiment, the dielectric constant of the insulating layer 1100 can be adjusted to 2.5 or less while maintaining the rigidity of the insulating layer 1100, thereby providing a circuit board suitable for high frequency signal transmission. Also, in the embodiment, the filler 1120 includes second pores, which can reduce the degree of thermal expansion that occurs when the temperature of the filler 1120 changes, thereby improving the thermal deformation rate of the insulating layer, which is a composite of the filler and the insulating layer.

[0194] Meanwhile, the filler included in the insulating layer in the second embodiment may also be concentrated in a second region adjacent to the upper surface and a third region adjacent to the lower surface of the insulating layer, as shown in FIG.

[0195] The following describes a resin composition for a semiconductor according to Example 3. The resin composition for a semiconductor in Example 3 is applicable to a copper foil laminate, unlike Examples 1 and 2.

[0196] FIG. 9 is a diagram showing a copper foil laminate including a resin composition for a semiconductor package according to a third embodiment.

[0197] The copper foil laminate according to the third embodiment includes an insulating film 2100 (or an insulating layer or a resin composition for a semiconductor package) and a copper foil layer 2200 disposed on one side of the insulating film 2100. The insulating film 2100 may be an insulating layer. The insulating film 2100 may be a prepreg (PPG). Hereinafter, for convenience of explanation, the insulating film corresponding to the prepreg will be described as the insulating layer 2100.

[0198] The insulating layer 2100 includes a resin 2110, glass fibers 2120, and a filler 2130. That is, the insulating layer 2100 may include the glass fibers 2120 and the filler 2130 dispersed in the resin 2110. That is, the insulating layer 2100 in the embodiment may be a prepreg in which a certain amount of the glass fibers 2120 and the filler 2130 are dispersed in the resin 2110. For example, the insulating layer 2100 in the embodiment may be a prepreg which is a composite of the resin 2110, the glass fibers 2120, and the filler 2130.

[0199] The insulating layer 2100 may be a resin for semiconductor packaging. In an embodiment, the dielectric constant Dk of the insulating layer 2100 can be adjusted to 2.5 or less by changing the composition in the insulating layer 2100 constituting the resin for semiconductor packaging. Hereinafter, the resin for semiconductor packaging is referred to as the insulating layer 2100, and a resin composition for semiconductor packaging corresponding to the insulating layer 2100 will be specifically described.

[0200] Such an insulating layer 2100 is a composite of resin 2110, glass fiber 2120, and filler 2130.

[0201] In this case, in the third embodiment, unlike the first and second embodiments, the insulating layer 2100 has a structure containing glass fiber 2120, which allows the insulating layer 2100 to have a certain level of strength or more, and pores are formed in the resin 2110 and filler 2130 that constitute the insulating layer 2100, respectively, so that the insulating layer 2100 can have a dielectric constant Dk of 2.5 or less.

[0202] That is, in the embodiment, the resin 2110 constituting the insulating layer 2100 contains a certain amount of glass fiber 2120 and filler 2130, and pores are formed in the resin 2110 and filler 2130, respectively.

[0203] Specifically, the filler 2130 may occupy a range of 20 vol.% to 30 vol.% with respect to the total volume of the insulating layer 2100. Here, if the content of the filler 2130 exceeds 30 vol.%, it may be difficult to adjust the dielectric constant of the insulating layer 2100 to a low dielectric constant, for example, 2.5 or less. Also, if the content of the filler 2130 is less than 20 vol.%, the insulating layer 2100 cannot have strength above a certain level. Thus, in the embodiment, the filler 2130 may have a content of 20 vol.% to 30 vol.% in the insulating layer 2100.

[0204] Furthermore, the glass fibers 2120 occupy 50 vol.% to 70 vol.% of the total volume of the insulating layer 2100. If the glass fibers 2120 exceed 70 vol.%, it may be difficult to adjust the dielectric constant Dk of the insulating layer 2100 to a low dielectric constant, for example, 2.5 or less. If the content of the glass fibers 2120 is less than 50 vol.%, the insulating layer 2100 cannot have strength above a certain level. Thus, in the embodiment, the glass fibers 2120 are set to have 50 vol.% to 70 vol.% in the insulating layer 2100.

[0205] At this time, the resin 2110 in the third embodiment includes the first pores 2110A. A plurality of the first pores 2110A may be formed in the resin 2110. That is, the resin 2110 in the embodiment may be a porous resin.

[0206] The resin 2110 may have a first porosity. The first porosity may correspond to a ratio of a volume of the first pores 2110A to a total volume of the resin 2110. The first porosity of the resin 2110 may be determined by a second porosity of the filler 2130, which will be described later. The first porosity of the resin 2110 will be described in detail below.

[0207] Furthermore, the filler 2130 in the embodiment includes second pores (not shown). In this case, the second pores can also be called "depressions" formed on the surface of the filler 2130. Hereinafter, the "depressions" will be described as second pores.

[0208] The structures of the first pores 2110A and the second pores are substantially the same as those of the first pores and the second pores of the second embodiment shown in FIG. 8, and detailed description thereof will be omitted.

[0209] Meanwhile, if the filler 2130 is contained in the insulating layer 2100 at less than 20 vol.%, the rigidity of the insulating layer 2100 is weakened, which may cause a problem in reliability during the manufacturing process of the circuit board. For example, if the filler 2130 is contained in the insulating layer 2100 at less than 20 vol.%, the insulating layer 2100 may warp significantly during the manufacturing process of the circuit board, which may cause a problem in that the manufacturing process cannot be performed normally. Also, if the filler 2130 is contained in the insulating layer 2100 at more than 30 vol.%, it may be difficult to adjust the dielectric constant Dk of the insulating layer 2100 to 2.5 or less. For example, when the filler 2130 exceeds 30 vol. % in the insulating layer 2100, in order to set the dielectric constant Dk of the insulating layer 2100 to 2.5 or less, the first porosity of the resin 2110 or the second porosity of the filler 2130 must be large in the total volume of the filler 2130, which may weaken the rigidity of the resin 2110 or the filler 2130, resulting in reliability problems.

[0210] Therefore, the filler 2130 is set to be in the range of 20 vol.% to 30 vol.% in the insulating layer 2100. Also, the glass fiber 2120 is set to be in the range of 50 vol.% to 70 vol.% in the insulating layer 2100.

[0211] Meanwhile, the resin 2110 may have no first pores 2110A and second pores may be formed only in the filler 2130 to make the insulating layer 2100 have a certain level of dielectric constant. However, in this case, it may be difficult to make the insulating layer 2100 have a dielectric constant Dk of 2.5 or less by only the second porosity of the filler 2130.

[0212] That is, in a state where the first pores 2110A are not formed in the resin 2110, the dielectric constant of the insulating layer 2100 is determined only by the second porosity of the filler 2130 as shown in Table 5 below.

[0213] [Table 5]

[0214] As shown in Table 5, when the second porosity of the second pores contained in the filler 2130 is adjusted in a state where the resin 2110 is impregnated with the glass fiber 2120, the dielectric constant Dk of the insulating layer 2100 cannot be adjusted to 2.5. Specifically, in order to adjust the dielectric constant Dk of the insulating layer 2100 to 2.5 or less in a state where the resin 2110 contains the glass fiber 2120, the second porosity of the filler 2130 must be 40% to 50% or more. However, when the second porosity of the filler 2130 exceeds 35%, the strength of the filler 2130 is weakened, and reliability problems such as cracking of the filler 2130 may occur in various environments. Accordingly, in this embodiment, the filler 2130 has second pores, and the resin 2110 is further formed with first pores 2110A, so that the dielectric constant Dk of the insulating layer 2100 is 2.5 or less by a combination of the first porosity of the resin 2110 and the second porosity of the filler 2130. Meanwhile, the first porosity of the resin 2110 and the second porosity of the filler 2130 are as follows.

[0215] In an embodiment, the first porosity of the resin 2110 may range from 10% to 35%.

[0216] If the first porosity of the resin 2110 is less than 10%, it may be difficult to set the dielectric constant Dk of the insulating layer 2100 to 2.5 or less. Also, if the first porosity of the resin 2110 is more than 35%, an increase in the first pores 2110A may cause reliability problems in the rigidity of the resin 2110 and the insulating layer 2100 including the resin 2110.

[0217] At this time, the first porosity of the resin 2110 may be adjusted within a range of 10% to 35% based on the second porosity of the filler 2130 .

[0218] The second porosity of the filler 2130 may be in the range of 10% to 35%.

[0219] If the second porosity of the filler 2130 is less than 10%, it may be difficult to adjust the dielectric constant Dk of the insulating layer 2100 to 2.5 or less. If the second porosity of the filler 2130 is more than 35%, a problem may occur in the rigidity of the filler 2130 due to an increase in the second pores. For example, if the second porosity of the filler 2130 is more than 35%, a reliability problem such as cracking of the filler 2130 in the insulating layer 2100 may occur. Therefore, in an embodiment, the second porosity of the filler 2130 is adjusted to be within a range of 10% to 35%. Meanwhile, the second porosity of the filler 2130 may be adjusted based on the porosity of the resin 2110.

[0220] The dielectric constant of the insulating layer 2100 according to the first porosity of the resin 2110 and the second porosity of the filler 2130 has already been described in Table 4, and therefore a detailed description thereof will be omitted.

[0221] As described above, in the embodiment, the dielectric constant of the resin 2110, the dielectric constant of the glass fiber 2120, the dielectric constant of the filler 2130, the content of the resin 2110, the content of the glass fiber 2120, the content of the filler 2130, the first porosity of the resin 2110, and the second porosity of the filler 2130 are adjusted so that the dielectric constant Dk of the insulating layer 2100, which is a composite of the resin 2110, the glass fiber 2120, and the filler 2130, can be adjusted to 2.5 or less.

[0222] Meanwhile, the dielectric constant of the insulating layer 2100 may be measured by the following device and method. That is, the insulating layer 2100 may not be used as a single product, but may be used as a copper foil laminate resin having a copper foil layer 120 laminated on at least one surface thereof. In this case, the dielectric constant of the insulating layer 2100 may be measured by removing the copper foil layer 120 from the copper foil laminate resin, drying the insulating layer 2100 at 100° C. for 60 minutes with the copper foil layer 120 removed, and measuring the dielectric constant by a split post dielectric resonance (SPDR) method at 25° C. and 50% RH using a N5222A PNA Network analyzer (Agilent) device and a resonator.

[0223] According to this embodiment, the dielectric constant of the insulating layer 2100 can be adjusted to 2.5 or less while maintaining the rigidity of the insulating layer 2100, thereby providing a circuit board suitable for high frequency signal transmission. Also, in the embodiment, the filler 2130 includes second pores, which can reduce the degree of thermal expansion that occurs when the temperature of the filler 2130 changes, thereby improving the thermal deformation rate of the insulating layer, which is a composite of the filler and the insulating layer.

[0224] Hereinafter, a circuit board formed using the copper foil laminated resin shown in any one of FIG. 1, FIG. 3, and FIG. 8 will be described.

[0225] FIG. 10 is a cross-sectional view of the printed circuit board according to the first embodiment.

[0226] Referring to FIG. 10, the circuit board may include an insulating substrate including first to third insulating portions 210, 220, and 230, a circuit pattern 240, and a via 250.

[0227] The insulating substrate including the first to third insulating parts 210, 220, and 230 may have a flat plate structure. The insulating substrate may be a printed circuit board (PCB). Here, the insulating substrate may be embodied as a single substrate, or alternatively, may be embodied as a multi-layer substrate in which a plurality of insulating layers are continuously stacked.

[0228] Thus, the insulating substrate may include a plurality of insulating parts 210, 220, and 230. The plurality of insulating parts include a first insulating part 210, a second insulating part 220 disposed on the upper part of the first insulating part 210, and a third insulating part 230 disposed on the lower part of the first insulating part 210.

[0229] Here, the first insulating part 210, the second insulating part 220, and the third insulating part 230 may be made of different insulating materials. Preferably, the first insulating part 210 may include glass fiber. And, unlike the first insulating part 210, the second insulating part 220 and the third insulating part 230 may not include the glass fiber. Preferably, the second insulating part 220 and the third insulating part 230 may include the copper foil laminate resin shown in any one of FIG. 1 and FIG. 3.

[0230] Thus, the thickness of each insulating layer constituting the first insulating portion 210 may be different from the thickness of each insulating layer constituting the second insulating portion 220 and the third insulating portion 230. In other words, the thickness of each insulating layer constituting the first insulating portion 210 may be greater than the thickness of each insulating layer constituting the second insulating portion 220 and the third insulating portion 230.

[0231] That is, the first insulating part 210 contains glass fiber. The glass fiber generally has a thickness of about 12 μm. Thus, the thickness of each insulating layer constituting the first insulating part 210 may be in the range of 19 μm to 23 μm, including the thickness of the glass fiber. In this case, the first insulating part 210 may contain a composition for semiconductor packages shown in FIG. 9. For example, the first insulating part 210 may be formed of a copper foil laminate of FIG. 9.

[0232] Unlike the above, the second insulating part 220 does not include the glass fiber. Preferably, each insulating layer constituting the second insulating part 220 may be made of a copper foil laminated resin RCC (Resin Coated Copper). Specifically, the second insulating part 220 may be made of a copper foil laminated resin shown in any one of Figs. 1, 3, and 8.

[0233] Thus, the thickness of each insulating layer constituting the second insulating portion 220 may be in the range of 10 μm to 15 μm. Preferably, the thickness of each layer of the second insulating portion 220 made of the copper foil laminated resin may be formed within a range not exceeding 15 μm.

[0234] Also, the third insulating part 230 does not include the glass fiber. Preferably, each insulating layer constituting the third insulating part 230 may be made of copper foil laminated resin RCC (Resin Coated Copper). Specifically, the third insulating part 230 may be made of the copper foil laminated resin shown in any one of Figs. 1, 3, and 8. Thus, each insulating layer constituting the third insulating part 230 may have a thickness in the range of 10 μm to 15 μm.

[0235] That is, the insulating part constituting the circuit board in the comparative example includes a plurality of insulating layers, and the plurality of insulating layers are all composed of prepreg (PPG) containing glass fiber. In this case, it is difficult to reduce the thickness of the glass fiber in the circuit board in the comparative example based on the PPG. This is because, when the thickness of the PPG is reduced, the glass fiber contained in the PPG may be electrically connected to the circuit pattern arranged on the surface of the PPG, which induces cracks. As a result, when the thickness of the PPG is reduced in the circuit board in the comparative example, dielectric breakdown and damage to the circuit pattern may occur. As a result, the circuit board in the comparative example has a limit in reducing the overall thickness due to the thickness of the glass fiber constituting the PPG.

[0236] In addition, the circuit board in the comparative example has a high dielectric constant because the insulating layer is made of only PPG containing glass fiber. However, there is a problem that it is difficult to use a dielectric material with a high dielectric constant as a high frequency substitute. That is, the circuit board in the comparative example has a phenomenon in which the dielectric constant is destroyed in the high frequency band because the dielectric constant of the glass fiber is high.

[0237] In this embodiment, the insulating layer is formed using a copper foil laminate resin having a low dielectric constant, thereby making it possible to provide a highly reliable circuit board in which the signal loss is minimized even in a high frequency band while making the circuit board thin. This can be achieved by the dielectric constant of each insulating layer forming the second insulating part 220 and the third insulating part 230.

[0238] The first insulating part 210 may include, from the bottom, a first insulating layer 211, a second insulating layer 212, a third insulating layer 213, and a fourth insulating layer 214. In addition, the first insulating layer 211, the second insulating layer 212, the third insulating layer 213, and the fourth insulating layer 214 may each be made of PPG containing glass fiber.

[0239] Meanwhile, in the embodiment of the present application, the insulating substrate may be configured with eight insulating layers, but the embodiment is not limited thereto, and the total number of the insulating layers may be increased or decreased.

[0240] Also, in the first embodiment, the first insulating portion 210 may be made of four layers. For example, in the first embodiment, the first insulating portion 210 may be made of four layers of prepreg.

[0241] Also, the second insulating part 220 may include a fifth insulating layer 221 and a sixth insulating layer 222 from the bottom. The fifth insulating layer 221 and the sixth insulating layer 222 constituting the second insulating part 220 may be made of a copper foil laminated resin having a low dielectric constant and a low thermal expansion coefficient. That is, in the first embodiment, the second insulating part 220 may be made of two layers. For example, in the first embodiment, the second insulating part 220 may be made of two layers of copper foil laminated resin.

[0242] Also, the third insulating part 230 may include a seventh insulating layer 231 and an eighth insulating layer 232 from the top. The seventh insulating layer 231 and the eighth insulating layer 232 constituting the third insulating part 230 may be made of a copper foil laminated resin having a low dielectric constant and a low thermal expansion coefficient. That is, in the first embodiment, the third insulating part 230 may be made of two layers. For example, in the first embodiment, the third insulating part 230 may be made of two layers of copper foil laminated resin.

[0243] Meanwhile, in the first embodiment, the total number of insulating layers is eight, of which the first insulating part 210 formed of prepreg is formed of four layers, and the second insulating part 220 and the third insulating part 230 formed of copper foil laminate resin are each formed of two layers, but this is not limited to this, and the number of insulating layers constituting the first insulating part 210 may be increased or decreased.

[0244] Meanwhile, a circuit pattern 240 may be disposed on a surface of an insulating layer constituting each of the first insulating portion 210, the second insulating portion 220, and the third insulating portion 230.

[0245] Preferably, a circuit pattern 240 may be arranged on at least one surface of each of the first insulating layer 211, the second insulating layer 212, the third insulating layer 213, the fourth insulating layer 214, the fifth insulating layer 221, the sixth insulating layer 222, the seventh insulating layer 231, and the eighth insulating layer 232.

[0246] The circuit pattern 240 is a wiring for transmitting an electrical signal and may be made of a metal material having high electrical conductivity, such as at least one metal material selected from the group consisting of gold (Au), silver (Ag), platinum (Pt), titanium (Ti), tin (Sn), copper (Cu), and zinc (Zn).

[0247] Also, the circuit pattern 240 may be formed of a paste or solder paste containing at least one metal material selected from gold (Au), silver (Ag), platinum (Pt), titanium (Ti), tin (Sn), copper (Cu), and zinc (Zn) that has excellent bonding strength. Preferably, the circuit pattern 240 may be formed of copper (Cu), which has high electrical conductivity and is relatively inexpensive.

[0248] In addition, the circuit pattern 240 may have a thickness of 12 μm±2 μm. That is, the circuit pattern 240 may have a thickness in the range of 10 μm to 14 μm.

[0249] The circuit pattern 240 can be formed by a typical circuit board manufacturing process such as an additive process, a subtractive process, a modified semi-additive process (MSAP), or a semi-additive process (SAP), and a detailed description thereof will be omitted here.

[0250] At least one via 250 is formed in at least one of the insulating layers constituting the first insulating part 210, the second insulating part 220, and the third insulating part 230. The via 250 is disposed to penetrate at least one of the insulating layers. The via 250 may penetrate only one of the insulating layers, or may be formed to commonly penetrate at least two of the insulating layers. Thus, the via 250 electrically connects circuit patterns disposed on the surfaces of different insulating layers to each other.

[0251] The via 250 may be formed by filling a through hole (not shown) penetrating at least one of the insulating layers with a conductive material.

[0252] The through-holes may be formed by any one of mechanical, laser, and chemical processing. When the through-holes are formed by mechanical processing, milling, drilling, routing, etc. may be used, and when the through-holes are formed by laser processing, UV or CO 2 A laser method can be used, and when formed by chemical processing, the insulating layer can be opened using chemicals including aminosilane, ketones, and the like.

[0253] On the other hand, laser processing is a cutting method that focuses optical energy on a surface to melt and evaporate part of a material to create a desired shape, and can easily process complex shapes created by computer programs, as well as composite materials that are difficult to cut with other methods.

[0254] In addition, the laser processing has the advantage that the cutting diameter can be as small as 0.005 mm and the range of processable thicknesses is wide.

[0255] The laser drill is a YAG (Yttrium Aluminum Garnet) laser or a CO 2 It is preferable to use a laser or an ultraviolet (UV) laser. A YAG laser is a laser that can process both the copper foil layer and the insulating layer, and a CO 2 The laser is capable of processing only insulating layers.

[0256] After the through hole is formed, the inside of the through hole is filled with a conductive material to form the via 250. The metal material forming the via 250 may be any one selected from copper (Cu), silver (Ag), tin (Sn), gold (Au), nickel (Ni), and palladium (Pd), and the conductive material may be filled by any one of electroless plating, electrolytic plating, screen printing, sputtering, evaporation, inkjetting, and desfencing, or a combination thereof.

[0257] FIG. 11 is a diagram showing a circuit board according to a second embodiment, and FIG. 12 is a diagram showing a circuit board according to a third embodiment.

[0258] 11 and 12, in the circuit board, the number of layers in the first insulating section made of PPG and the number of layers in the second insulating section and the third insulating section made of copper foil laminate resin differ in the overall laminate structure of the insulating substrate.

[0259] Referring to FIG. 11, the circuit board in the second embodiment includes a first insulating portion 210a, a second insulating portion 220a, and a third insulating portion 230a.

[0260] The first insulating part 210a may include two layers of PPG 211a and 212a. The PPG 211a and 212a may be a conventional PPG, or may be a copper foil laminate prepreg of FIG. 9 including the resin composition for a semiconductor package according to the third embodiment of the present disclosure.

[0261] Also, the second insulating part 220a may include three layers of RCC 221a, 222a, and 223a as shown in any one of FIG. 1, FIG. 3, and FIG.

[0262] Also, the third insulating portion 230a may include three layers of RCC 231a, 232a, and 233a as shown in any one of FIG. 1, FIG. 3, and FIG.

[0263] Referring to FIG. 12, the circuit board of the third embodiment may include only one insulating portion 210b.

[0264] The insulating part 210b may have an eight-layer structure.

[0265] In addition, the insulating part 210b may include the RCCs 211b, 212b, 213b, 214b, 215b, 216b, 217b, and 218b shown in any one of FIGS.

[0266] In the embodiment, an insulating layer or insulating film is provided which is a composite of a resin and a filler. In this case, the filler in the embodiment includes at least one depression on a surface. In the embodiment, the dielectric constant of the resin, the dielectric constant of the filler, the resin content, the filler content, and the ratio of the depression in the filler (e.g., porosity) can be adjusted to set the dielectric constant of the insulating layer or insulating film to 2.5 Dk or less while maintaining the rigidity of the insulating layer or insulating film, thereby providing a circuit board suitable for high frequency signal transmission.

[0267] In addition, in the embodiment, the filler includes a depression, which can reduce the degree of thermal expansion that occurs when the temperature of the filler changes, thereby improving the thermal deformation rate of the insulating layer, which is a composite of the filler and the insulating layer.

[0268] Meanwhile, the resin composition in the embodiment may include a first region in the center, a second region above the first region, and a third region below the first region. In this case, the filler in the embodiment may be selectively disposed only in the second and third regions excluding the first region. Differently from this, the filler in the embodiment is disposed in the first to third regions, and the content of the filler disposed in the first region is set to be smaller than the content of the filler disposed in the second and third regions, respectively. As a result, in the embodiment, in the process of forming a via hole in the insulating layer or insulating film and then performing desmearing, it is possible to prevent unintended size expansion of the via hole, thereby forming a fine via.

[0269] Therefore, in the embodiment, the insulating layer is formed using a copper foil laminate resin having a low dielectric constant, thereby making it possible to provide a highly reliable circuit board in which the thickness of the circuit board is slimmed down and signal loss is minimized even in the high frequency band.

[0270] The features, structures, effects, etc. described in the above embodiments are included in at least one embodiment and are not necessarily limited to one embodiment. In addition, the features, structures, effects, etc. exemplified in each embodiment can be combined or modified in other embodiments by a person having ordinary skill in the art to which the embodiment belongs. Therefore, the contents related to such combinations and modifications should be interpreted as being included in the scope of the embodiment.

[0271] In addition, although the above description focuses on the embodiments, these are merely illustrative and do not limit the embodiments, and a person having ordinary skill in the art to which the embodiments pertain will understand that various modifications and applications not exemplified above are possible within the scope of the essential characteristics of the embodiments. For example, each component specifically illustrated in the embodiments can be modified and implemented. Differences related to such modifications and applications should be interpreted as being included in the scope of the embodiments defined in the appended claims.

Claims

1. A resin composition that is a composite of a resin and a filler disposed within the resin, The resin is divided into a plurality of regions along a thickness direction between an upper surface of the resin and a lower surface of the resin, The plurality of regions includes a first region adjacent to an upper surface of the resin, a second region adjacent to a lower surface of the resin, and a third region between the first region and the second region, The resins in the first to third regions each include the same insulating material and are provided integrally with each other; A resin composition for semiconductor packaging, wherein a content of the filler in the first region and the second region is different from a content of the filler in the third region.

2. A resin composition for semiconductor packaging as described in claim 1, wherein the filler content in the first region or the second region is greater than the filler content in the third region.

3. The surface of the filler is provided with at least one recessed portion recessed toward the inside of the filler, The filler has a content in the range of 10 vol. % to 40 vol. % of the total volume of the resin composition; 3. The resin composition for semiconductor packaging according to claim 1, wherein a porosity corresponding to a volume occupied by the recesses in the total volume of the filler is in the range of 20% to 35%.

4. The resin composition for semiconductor packaging according to claim 1 , wherein the resin composition containing the resin and the filler has a dielectric constant Dk of 2.5 or less.

5. The resin composition for semiconductor packaging according to claim 3 , wherein the depression comprises a recess that does not penetrate the filler or a through hole that penetrates the filler.

6. The resin is formed of a modified epoxy or maleimide series, 6. The resin composition for semiconductor packaging according to claim 1, wherein the resin has a dielectric constant in the range of 2.3 Dk to 2.5 Dk.

7. The filler is SiO 2 , ZrO 3 , HfO 2 , and TiO 2 The ceramic material includes any one of the following: The resin composition for semiconductor packaging according to any one of claims 1 to 6, which has a dielectric constant in the range of 3.7 Dk to 4.2 Dk.

8. The filler has a content in the range of 10 vol. % to 15 vol. %, The resin composition for semiconductor packaging according to claim 3, wherein the porosity is in the range of 20% to 35%.

9. The filler has a content in the range of 15 vol. % to 30 vol. %, The resin composition for semiconductor packages according to claim 3, wherein the porosity is in the range of 30% to 35%.

10. The filler has a content in the range of 30 vol. % to 40 vol. %, The resin composition for semiconductor packages according to claim 3, wherein the porosity is in the range of 32% to 35%.

11. A resin composition for semiconductor packaging as described in claim 2, wherein the third region does not contain a filler.

12. An insulating layer; A copper foil layer provided on at least one surface of the insulating layer, The insulating layer is A resin and a filler disposed in the resin, The insulating layer is a first region adjacent to a top surface of the insulating layer; a second region adjacent to a lower surface of the insulating layer; a third region between the first region and the second region, The resins in the first to third regions each include the same insulating material and are provided integrally with each other; A copper foil laminate resin, wherein the content of the filler in the third region is different from the content of the filler in each of the first and second regions.

13. The surface of the filler is provided with at least one recessed portion recessed toward the inside of the filler, The filler has a content ranging from 10 vol. % to 40 vol. % in the total volume of the copper foil laminate resin; The porosity corresponding to the volume occupied by the depression out of the total volume of the filler is in the range of 20% to 35%; The copper foil laminate resin according to claim 12 , wherein the dielectric constant Dk of the insulating layer containing the resin and the filler is 2.5 or less.

14. The content of the filler in each of the first and second regions is The copper foil laminate resin according to claim 12 or 13, wherein the content of the filler in the second region is greater than that in the third region.

15. The copper foil laminate resin of claim 12 , wherein the filler is absent from the third region of the resin.

16. An insulating layer comprising a resin and a filler provided within the resin; a circuit pattern disposed on the insulating layer; a via extending through the insulating layer; The insulating layer is a first region adjacent to a top surface of the insulating layer; a second region adjacent to a lower surface of the insulating layer; a third region between the first region and the second region, The resins in the first to third regions each include the same insulating material and are provided integrally with each other; A circuit board, wherein the filler content in the third region is different from the filler content in each of the first and second regions.

17. The content of the filler in each of the first and second regions is The circuit board of claim 16 , wherein the filler content is greater than that in the third region.

18. The circuit board of claim 16 , wherein the filler is absent from the third region of resin.

19. The surface of the filler is provided with at least one recessed portion recessed toward the inside of the filler, The filler has a content in the range of 10 vol. % to 40 vol. % in the total volume of the circuit board; The porosity corresponding to the volume occupied by the depression out of the total volume of the filler is in the range of 20% to 35%; The circuit board according to claim 16 , wherein the insulating layer containing the resin and the filler has a dielectric constant Dk of 2.5 or less.

Citation Information

Patent Citations

  • Board for printed circuit

    JP1992133386A

  • Laminate for both sided wiring board and both-sided wiring board

    JP2002185093A

  • Epoxy resin composition for sealing semiconductor and semiconductor device

    JP2005041937A

  • Insulating resin composition, manufacturing method therefor and electronic part

    JP2006077172A

  • Low permittivity filler, and low permittivity composition and low permittivity film using this

    JP2007161518A