Positive electrode and lithium secondary battery including same

A double-layer positive electrode with varying nickel content in lithium nickel manganese cobalt oxide layers stabilizes structural changes, reducing resistance and enhancing performance in lithium secondary batteries, particularly for electric vehicles.

JP7562849B2Active Publication Date: 2024-10-07LG ENERGY SOLUTION LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023519128
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-01-08
Filing Date
2022-01-07
Publication Date
2024-10-07
Estimated Expiration
2042-01-07

AI Technical Summary

Technical Problem

Lithium secondary batteries with high nickel content positive electrodes experience increased resistance at low State of Charge (SOC) due to structural changes, affecting output and stability, and are costly.

Method used

A positive electrode with a double-layer structure, where the lower layer has a lower nickel content and the upper layer has a higher nickel content, is manufactured using a specific composition of lithium nickel manganese cobalt oxide materials, enhancing structural stability and reducing resistance.

Benefits of technology

The double-layer structure improves high-temperature cycle performance and prevents resistance increase, enabling better output and suitability for high-capacity, high-density electric vehicle batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007562849000002
    Figure 0007562849000002
  • Figure 0007562849000001
    Figure 0007562849000001
Patent Text Reader

Abstract

Provided is a positive electrode comprising: a positive electrode current collector; and a positive electrode active material layer located on at least one surface of the positive electrode current collector, wherein the positive electrode active material layer comprises: a lower layer region in surface contact with the positive electrode current collector and including a first positive electrode active material and a first binder polymer; and an upper layer region in surface contact with the lower layer region and extending to a surface of the positive electrode active material layer and including a second positive electrode active material and a second binder polymer, wherein the Ni content of the second positive electrode active material in the upper layer region is higher than the Ni content of the first positive electrode active material in the lower layer region. A lithium secondary battery including the positive electrode is also provided.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a positive electrode and a lithium secondary battery including the same, and more particularly to a positive electrode having high initial efficiency and excellent rapid charging performance, and a lithium secondary battery including the same.

[0002] This application claims priority to Korean Patent Application No. 10-2021-0002853, filed on January 8, 2021, the entire contents of which are incorporated herein by reference in their entirety in the specification and drawings. [Background technology]

[0003] As technological development and demand for mobile devices increases, the demand for secondary batteries as an energy source is growing rapidly. Among these secondary batteries, lithium secondary batteries, which have high energy density and voltage, long cycle life, and low discharge rate, have been commercialized and are widely used.

[0004] A lithium secondary battery has an electrode assembly in which a porous separator is interposed between a positive electrode and a negative electrode, each of which has an active material applied to a current collector, and an electrolyte containing a lithium salt is impregnated in the electrode assembly. The electrode is manufactured by applying a slurry, in which the active material, binder, and conductive material are dispersed in a solvent, to the current collector, followed by drying and pressing.

[0005] Lithium secondary batteries are secondary batteries in which lithium ions are responsible for the electrical conduction between electrodes in the charge and discharge reaction, and have features such as high energy density and small memory effect compared to other secondary batteries such as nickel-metal hydride batteries and nickel-cadmium batteries. Therefore, their applications are expanding from small power sources such as portable electronic devices and household electrical appliances to stationary power sources such as power storage devices, UPS devices, and power leveling devices, and medium- to large-sized power sources such as driving power sources for ships, railways, hybrid vehicles, and electric vehicles, and new improvements in battery performance are required. For example, in vehicle applications such as hybrid vehicles and electric vehicles, high energy density is required to achieve longer driving distances, and high output is required to improve acceleration response.

[0006] In order to realize high-power and high-energy density secondary batteries for electric vehicles, electrodes are being manufactured using positive electrodes with a high nickel (Ni) content.

[0007] However, when using a positive electrode with a high Ni composition compared to a positive electrode with a low Ni composition, there is an impact on the resistance change according to the battery's SOC (State of Charge), and the resistance of most secondary batteries is high. To solve this problem, research is still needed to control the resistance of electrodes and cells through the design of the structure and composition of the positive electrode. Summary of the Invention [Problem to be solved by the invention]

[0008] Therefore, the present invention is intended to solve the above problems, and an object of the present invention is to provide a positive electrode in which an increase in resistance at a low SOC during discharge is prevented, and a secondary battery including the positive electrode. [Means for solving the problem]

[0009] In order to achieve the above object of the present invention, according to one aspect of the present invention, a positive electrode according to the following embodiment is provided.

[0010] According to the first embodiment, A positive electrode current collector; a positive electrode active material layer located on at least one surface of the positive electrode current collector, the positive electrode active material layer includes a lower layer region in surface contact with the positive electrode current collector and including a first positive electrode active material and a first binder polymer, and an upper layer region in surface contact with the lower layer region and extending to a surface of the positive electrode active material layer, the upper layer region including a second positive electrode active material and a second binder polymer, A positive electrode is provided, in which a first positive electrode active material in the lower layer region is represented by Chemical Formula 1 below, a second positive electrode active material in the upper layer region is represented by Chemical Formula 2 below, and a Ni content of the second positive electrode active material is greater than a Ni content of the first positive electrode active material: [Chemical formula 1] Li 1+a [Ni x Mn y Co z ]M1 t O2 In the above formula, 0≦a≦0.2, 0.4≦x≦0.9, 0 <y<1、0<z<1、0≦t<0.1、x+y+z+t=1であり、 M1 is one or more elements selected from the group consisting of Co, Mn, Ni, Al, Fe, V, Cr, Ti, Ta, Mg, Mo, Zr, W, Sn, Hf, Nd, and Gd; [Chemical formula 2] Li 1+b [Ni u Mn v Co w ]M2 s O2 In the above formula, 0≦b≦0.2, 0.4≦u≦0.9, 0 <v<1、0<w<1、0≦s<0.1、u+v+w+s=1であり、 M2 is one or more elements selected from the group consisting of Co, Mn, Ni, Al, Fe, V, Cr, Ti, Ta, Mg, Mo, Zr, W, Sn, Hf, Nd and Gd.

[0011] According to the second embodiment, in the first embodiment, The first positive electrode active material may have a Ni content of 40 to 75 mol % of the total transition metals in the first positive electrode active material, and the second positive electrode active material may have a Ni content of 80 to 90 mol % of the total transition metals in the second positive electrode active material.

[0012] According to the third embodiment, in the first or second embodiment, The first positive electrode active material may have a Ni content of 50 to 75 mol % of the total transition metals in the first positive electrode active material, and the second positive electrode active material may have a Ni content of 81 to 90 mol % of the total transition metals in the second positive electrode active material.

[0013] According to the fourth embodiment, in one of the first to third embodiments, The first positive electrode active material may have a Ni content of 65 to 70 mol % of the total transition metals in the first positive electrode active material, and the second positive electrode active material may have a Ni content of 86 to 90 mol % of the total transition metals in the second positive electrode active material.

[0014] According to the fifth embodiment, in one of the first to fourth embodiments, The weight ratio of the lower layer region to the upper layer region of the positive electrode active material layer may be 20:80 to 80:20.

[0015] According to the sixth embodiment, preparing a lower layer slurry including a first positive electrode active material represented by the following formula 1, a first binder polymer, and a first dispersion medium, and preparing an upper layer slurry including a second positive electrode active material represented by the following formula 2, a second binder polymer, and a second dispersion medium, wherein a Ni content of the second positive electrode active material is higher than a Ni content of the first positive electrode active material; coating at least one surface of a positive electrode current collector with the lower layer slurry, and coating the upper layer slurry on the lower layer slurry; and drying the coated lower layer slurry and the coated upper layer slurry simultaneously to form a positive electrode active material layer. [Chemical formula 1] Li 1+a [Ni x Mny Co z ]M1 t O2 In the above formula, 0≦a≦0.2, 0.4≦x≦0.9, 0 <y<1、0<z<1、0≦t<0.1、x+y+z+t=1であり、 M1 is one or more elements selected from the group consisting of Co, Mn, Ni, Al, Fe, V, Cr, Ti, Ta, Mg, Mo, Zr, W, Sn, Hf, Nd, and Gd; [Chemical formula 2] Li 1+b [Ni u Mn v Co w ]M2 s O2 In the above formula, 0≦b≦0.2, 0.4≦u≦0.9, 0 <v<1、0<w<1、0≦s<0.1、u+v+w+s=1であり、 M2 is one or more elements selected from the group consisting of Co, Mn, Ni, Al, Fe, V, Cr, Ti, Ta, Mg, Mo, Zr, W, Sn, Hf, Nd and Gd.

[0016] According to the seventh embodiment, in the sixth embodiment, The first positive electrode active material may have a Ni content of 40 to 75 mol % of the total transition metals in the first positive electrode active material, and the second positive electrode active material may have a Ni content of 80 to 90 mol % of the total transition metals in the second positive electrode active material.

[0017] According to the eighth embodiment, in the sixth or seventh embodiment, The first positive electrode active material may have a Ni content of 50 to 75 mol % of the total transition metals in the first positive electrode active material, and the second positive electrode active material may have a Ni content of 81 to 90 mol % of the total transition metals in the second positive electrode active material.

[0018] According to the ninth embodiment, in one of the sixth to eighth embodiments, The first positive electrode active material may have a Ni content of 65 to 70 mol % of the total transition metals in the first positive electrode active material, and the second positive electrode active material may have a Ni content of 86 to 90 mol % of the total transition metals in the second positive electrode active material.

[0019] According to the tenth embodiment, A lithium secondary battery including a positive electrode according to any one of the first to fifth embodiments is provided. Effect of the Invention

[0020] According to one embodiment of the present invention, a positive electrode active material layer includes a lower region in surface contact with a positive electrode current collector and including a first positive electrode active material and a first binder polymer, and an upper region located on the lower region. The Ni content of the second positive electrode active material in the upper region is controlled to be greater than the Ni content of the first positive electrode active material in the lower region. As a result, a resistance increase that causes a rapid output decrease at a low SOC during discharge is prevented, and a secondary battery including the same can be provided.

[0021] In addition, according to an embodiment of the present invention, the positive electrode is more effective in a high loading positive electrode in which a large amount of positive electrode active material is coated, and can be applied to the realization of batteries for high capacity and high density electric vehicles (EVs).

[0022] The following drawings attached to this specification are illustrative of preferred embodiments of the present invention, and serve to further understand the technical concept of the present invention together with the detailed description of the invention. Therefore, the present invention should not be interpreted as being limited to the matters described in the drawings. [Brief description of the drawings]

[0023] [Figure 1] 1 is a graph showing high-temperature capacity retention rates according to an increase in cycles of the secondary batteries produced in Example 1, Example 2, Comparative Example 1, and Comparative Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0024] The present invention will be described in detail below. The terms and words used in the present specification and claims should not be interpreted as being limited to their ordinary and dictionary meanings, but should be interpreted as having meanings and concepts that correspond to the technical ideas of the present invention, based on the principle that the inventors themselves can appropriately define the concepts of terms in order to best describe the invention.

[0025] The positive electrode according to one embodiment of the present invention comprises: A positive electrode current collector; a positive electrode active material layer located on at least one surface of the positive electrode current collector, the positive electrode active material layer includes a lower layer region in surface contact with the positive electrode current collector and including a first positive electrode active material and a first binder polymer, and an upper layer region in surface contact with the lower layer region and extending to a surface of the positive electrode active material layer, the upper layer region including a second positive electrode active material and a second binder polymer, The first positive electrode active material in the lower layer region is represented by Chemical Formula 1 below, and the second positive electrode active material in the upper layer region is represented by Chemical Formula 2 below, and the Ni content of the second positive electrode active material is higher than the Ni content of the first positive electrode active material. [Chemical formula 1] Li 1+a [Ni x Mn y Co z ]M1 t O2 In the above formula, 0≦a≦0.2, 0.4≦x≦0.9, 0 <y<1、0<z<1、0≦t<0.1、x+y+z+t=1であり、 M1 is one or more elements selected from the group consisting of Co, Mn, Ni, Al, Fe, V, Cr, Ti, Ta, Mg, Mo, Zr, W, Sn, Hf, Nd, and Gd; [Chemical formula 2] Li 1+b [Ni u Mn v Co w ]M2 s O2 In the above formula, 0≦b≦0.2, 0.4≦u≦0.9, 0 <v<1、0<w<1、0≦s<0.1、u+v+w+s=1であり、 M2 is one or more elements selected from the group consisting of Co, Mn, Ni, Al, Fe, V, Cr, Ti, Ta, Mg, Mo, Zr, W, Sn, Hf, Nd and Gd.

[0026] The present invention proposes a technique for manufacturing a positive electrode by disposing two types of positive electrode active materials with different Ni contents in the upper and lower layers of the positive electrode using a double layer (DLD) coating technique for the positive electrode, and controlling the Ni content of the positive electrode active material in the upper layer to be higher than the Ni content of the positive electrode active material in the lower layer. By utilizing this, the present invention aims to control the resistance of the lower SOC region, which affects the output of the secondary battery.

[0027] In addition, the present invention is more effective in a high loading electrode where a large amount of positive electrode active material is coated, and can be applied to the realization of batteries for high capacity and high density electric vehicles (EVs). In general, a high Ni content positive electrode active material, which is a positive electrode active material with a high Ni content, means a material containing 80 mol % or more of Ni among all transition metals.

[0028] Such high-content Ni positive electrode active materials tend to show a rapid increase in resistance and a decrease in output at the lower SOC because they have a wider range of structural changes and weaker structural stability during charge / discharge behavior.

[0029] In the present invention, by disposing a positive electrode active material with a low Ni content in the lower layer region of the bilayer positive electrode active material layer, the structural stability can be improved and the increase in resistance can be improved.

[0030] According to an embodiment of the present invention, the Ni content of the first positive electrode active material may be 40 to 75 mol%, 50 to 75 mol%, 55 to 75 mol%, 60 to 75 mol%, 65 to 75 mol%, or 65 to 70 mol% of the total transition metals of the first positive electrode active material.

[0031] The Ni content of the second positive electrode active material may be 80 to 90 mol %, 81 to 90 mol %, 82 to 90 mol %, 84 to 90 mol %, or 86 to 90 mol % of the total transition metals of the second positive electrode active material.

[0032] The first and second positive active materials may be primary particles or secondary particles formed by agglomerating primary particles together through a granulation process.

[0033] In a particle size distribution diagram, the first positive electrode active material may have an average particle size (D50) of 3 μm to 15 μm, specifically 5 μm to 12 μm, and more specifically 6 μm to 10 μm.

[0034] The second positive electrode active material may have a D50 of 5 μm to 20 μm, specifically, 7 μm to 18 μm, and more specifically, 10 μm to 15 μm.

[0035] In this specification, "particle size Dn" means the particle size at the n% point of the cumulative particle number distribution according to particle size. D50 is the particle size at the 50% point of the cumulative particle number distribution according to particle size, i.e., it is called the average particle size, D90 is the particle size at the 90% point of the cumulative particle number distribution according to particle size, and D10 is the particle size at the 10% point of the cumulative particle number distribution according to particle size.

[0036] The Dn can be measured using a laser diffraction method. Specifically, the powder to be measured is dispersed in a dispersion medium, and then introduced into a commercially available laser diffraction particle size measuring device (e.g., Microtrac S3500). When the particles pass through a laser beam, the difference in the diffraction pattern according to the particle size is measured to calculate the particle size distribution. D10, D50, and D90 can be measured by calculating the particle diameters at the points of 10%, 50%, and 90% of the cumulative particle number distribution according to the particle diameter in the measuring device.

[0037] According to an embodiment of the present invention, the first positive electrode active material contained in the lower layer region of the positive electrode and the second positive electrode active material contained in the upper layer region are nickel-cobalt-manganese lithium oxide active materials with different Ni contents, so that a mixed region (intermixing) in which these different types of active materials are mixed may exist at a portion where the lower layer region and the upper layer region contact each other. This is because, when a lower layer slurry including the first positive electrode active material and an upper layer slurry including the second positive electrode active material are coated on a current collector simultaneously or successively with a very short time difference and then dried simultaneously to form an active material layer, a predetermined mixed region is generated at the interface where the lower layer slurry and the upper layer slurry come into contact before drying, and the mixed region is formed in the form of a layer of the mixed region while being dried.

[0038] In one embodiment of the present invention, the weight ratio (ratio of loading amount per unit area) of the lower layer region to the upper layer region of the positive electrode active material layer may be 20:80 to 80:20, and more particularly, 30:70 to 70:30. When this weight ratio range is satisfied, the adhesive strength between the current collector and the positive electrode active material layer is further increased, and excellent fast charging performance can be exhibited.

[0039] In one embodiment of the present invention, the ratio of the thickness of the upper layer region to the thickness of the lower layer region may be 20:80 to 80:20, and more particularly, 30:70 to 70:30. When this thickness ratio range is satisfied, the adhesive strength between the current collector and the positive electrode active material layer is further increased, and excellent fast charging performance can be exhibited.

[0040] In an embodiment of the present invention, the total thickness of the positive electrode active material layer is not particularly limited and may be, for example, 40 to 200 μm. In addition, in the positive electrode active material layer, the thickness of the lower layer region may be 20 to 150 μm or 30 to 100 μm, and the thickness of the upper layer region may be 20 to 150 μm or 30 to 100 μm.

[0041] When the thickness of the upper layer region and the thickness of the lower layer region are within this range, the adhesive strength between the current collector and the positive electrode active material layer is further increased, thereby providing excellent fast charging performance.

[0042] The weight percentage of the first binder polymer in the underlayer region may be greater than the weight percentage of the second binder polymer in the overlayer region.

[0043] Specifically, the ratio (a / b) of the weight % (a) of the first binder polymer in the solid content of the lower layer slurry to the weight % (b) of the second binder polymer in the solid content of the upper layer slurry can be 1 to 5, 1.1 to 5, 1 to 4, 1.2 to 4, 1 to 3, 1.5 to 3, or 2.1 to 3.

[0044] When the ratio of the weight percentage of the first binder in the lower layer region to the weight percentage of the second binder in the upper layer region satisfies such a range, excellent adhesion between the current collector and the positive electrode active material layer and rapid charging performance can be exhibited.

[0045] In an embodiment of the present invention, the ratio (wt%) of the first binder polymer in the lower layer region of the positive electrode active material layer may be 1 to 3 wt%, 1.5 to 2.5 wt%, or 1.5 to 2.4 wt%, and the ratio (wt%) of the second binder polymer in the upper layer region of the positive electrode active material layer may be 0.5 to 3 wt%, 1 to 2.5 wt%, or 1 to 2.4 wt%.

[0046] In an embodiment of the present invention, the total weight percentage of the first binder polymer and the second binder polymer in the positive electrode active material layer may be 1 to 3 wt%, 1 to 2 wt%, 2 to 3 wt%, 1 to 2.4 wt%, or 2.4 to 3 wt%.

[0047] A method for producing a positive electrode according to one aspect of the present invention includes the steps of: preparing a lower layer slurry including a first positive electrode active material represented by the following formula 1, a first binder polymer, and a first dispersion medium, and preparing an upper layer slurry including a second positive electrode active material represented by the following formula 2, a second binder polymer, and a second dispersion medium, wherein a Ni content of the second positive electrode active material is higher than a Ni content of the first positive electrode active material; coating at least one surface of a positive electrode current collector with the lower layer slurry, and coating the upper layer slurry on the lower layer slurry; and drying the coated lower layer slurry and the upper layer slurry simultaneously to form a positive electrode active material layer. [Chemical formula 1] Li 1+a [Ni x Mn y Co z ]M1 t O2 In the above formula, 0≦a≦0.2, 0.4≦x≦0.9, 0 <y<1、0<z<1、0≦t<0.1、x+y+z+t=1であり、 M1 is one or more elements selected from the group consisting of Co, Mn, Ni, Al, Fe, V, Cr, Ti, Ta, Mg, Mo, Zr, W, Sn, Hf, Nd, and Gd; [Chemical formula 2] Li 1+b [Ni u Mn v Co w ]M2 s O2 In the above formula, 0≦b≦0.2, 0.4≦u≦0.9, 0 <v<1、0<w<1、0≦s<0.1、u+v+w+s=1であり、 M2 is one or more elements selected from the group consisting of Co, Mn, Ni, Al, Fe, V, Cr, Ti, Ta, Mg, Mo, Zr, W, Sn, Hf, Nd and Gd.

[0048] The positive electrode current collector is not particularly limited as long as it does not induce chemical changes in the battery and has conductivity, and examples of the positive electrode current collector include stainless steel, aluminum, nickel, titanium, baked carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, silver, etc., aluminum-cadmium alloy, etc. The thickness of the positive electrode current collector is not particularly limited, but may be a commonly used thickness of 3 to 500 μm.

[0049] The first and second positive active materials may be included in an amount of 80 to 99 wt % based on the total weight of the lower layer slurry and the upper layer slurry, respectively.

[0050] The positive electrode active material layer may further include a conductive material, and therefore, the lower layer slurry and the upper layer slurry may each further include a conductive material.

[0051] The conductive material is not particularly limited as long as it does not induce chemical changes in the battery and has conductivity, and examples of the conductive material include carbon black-based carbon compounds such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fibers and metal fibers; metal powders such as carbon fluoride, aluminum, and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives. The conductive material may be added in an amount of 0.1 to 20% by weight based on the total weight of the positive electrode slurry composition.

[0052] The first binder polymer and the second binder polymer are components that assist the binding between the conductive material and the active material or the positive electrode current collector, and are usually included in an amount of 0.1 to 20 wt % based on the total weight of the positive electrode slurry composition. Examples of the first binder polymer and the second binder polymer, each independently, include polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HEP), polyvinylidene fluoride, polyacrylonitrile, polymethyl methacrylate, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, polyacrylic acid, styrene butadiene rubber (SBR), lithium polyacrylate (Li-PAA), etc.

[0053] The first and second dispersion media may each independently include water or an organic solvent such as NMP (N-methyl-2-pyrrolidone), and may be used in an amount that results in a desired viscosity when the upper layer slurry and the lower layer slurry include a first positive electrode active material / a second positive electrode active material, a first binder polymer / a second binder polymer, and a conductive material.

[0054] The method for coating the lower layer slurry and the upper layer slurry is not particularly limited as long as it is a method commonly used in the art, for example, a coating method using a slot die, a Mayer bar coating method, a gravure coating method, a dip coating method, a spray coating method, etc.

[0055] In one embodiment of the present invention, when the steps of coating one side of a positive electrode current collector with the slurry for the lower layer and coating the slurry for the upper layer on the slurry for the lower layer are performed simultaneously or within a very short time, an apparatus such as a double slot die may be used.

[0056] The step of simultaneously drying the coated lower layer slurry and the coated upper layer slurry to form an active material layer may include simultaneously drying the coated lower layer slurry and the coated upper layer slurry to remove a dispersion medium in the slurry, rolling the slurry, and then vacuum drying the slurry to form an active material layer.

[0057] At this time, the rolling may be performed by a method commonly used in the art, such as roll pressing, at a pressure of 1 to 20 MPa and a temperature of 15 to 30° C. In addition, the rolling may be performed under conditions such that the porosity of the electrode (active material layer) after rolling is 20 to 40%, 25 to 35%, 20 to 30%, or 30 to 40%.

[0058] The step of drying the coated slurry may be performed at, for example, 70 to 110° C., 75 to 100° C., or 80 to 90° C. for 10 to 30 minutes, 15 to 25 minutes, or 20 to 30 minutes, and the drying temperature and time may be appropriately adjusted depending on the type and content of the dispersion medium.

[0059] In addition, after rolling the dried slurry layer, it may be vacuum dried at a temperature of 100 to 170°C, 120 to 150°C, or 130 to 150°C for about 3 to 10 hours or 5 to 8 hours, and the drying temperature and time may be appropriately adjusted depending on the type and content of the dispersion medium.

[0060] The ratio (a / b) of the weight % (a) of the first binder polymer in the solid content of the lower layer slurry to the weight % (b) of the second binder polymer in the solid content of the upper layer slurry may be 1 to 5, 1.1 to 5, 1 to 4, 1.2 to 4, 1 to 3, 1.5 to 3, or 2.1 to 3.

[0061] When the ratio of the weight percentage of the first binder in the coated lower layer slurry and the weight percentage of the second binder in the coated upper layer slurry satisfies such a range, excellent adhesive strength and rapid charging performance can be exhibited.

[0062] The weight percentage of the first binder polymer in the solid content of the lower layer slurry may be 1 to 3 weight percent, 1.5 to 2.5 weight percent, or 1.5 to 2.4 weight percent, and the weight percentage of the second binder polymer in the solid content of the upper layer slurry may be 0.5 to 3 weight percent, 1 to 2.5 weight percent, or 1 to 2.4 weight percent.

[0063] The total proportion (weight %) of the first binder polymer and the second binder polymer in the total solid content of the lower layer slurry and the upper layer slurry may be 1 to 3 weight %, 1 to 2 weight %, 2 to 3 weight %, 1 to 2.4 weight %, or 2.4 to 3 weight %.

[0064] As described above, the positive electrode active material layer has a double layer structure and includes a lower layer region that is in surface contact with the positive electrode current collector and includes a first positive electrode active material and a first binder polymer, and an upper layer region that is in surface contact with the lower layer region and extends to the surface of the positive electrode active material layer and includes a second positive electrode active material and a second binder polymer.

[0065] Another embodiment of the present invention relates to a lithium secondary battery including the positive electrode. Specifically, the lithium secondary battery may be manufactured by injecting a lithium salt-containing electrolyte into an electrode assembly including the positive electrode, the negative electrode, and a separator interposed therebetween as described above.

[0066] The negative electrode may be prepared by bonding a negative electrode active material to a negative electrode current collector by a conventional method known in the art. Non-limiting examples of the negative electrode active material include conventional negative electrode active materials used in the negative electrode of electrochemical devices, and in particular, lithium metal or lithium alloys, carbon, petroleum coke, activated carbon, graphite or other carbons, silicon metal, silicon oxide, and other lithium adsorbent materials. Non-limiting examples of the negative electrode current collector include foils made of copper, gold, nickel, copper alloys, or combinations thereof.

[0067] A negative electrode active material, a conductive material, a binder, and a solvent are mixed to prepare a slurry, which is then directly coated onto a negative electrode current collector or cast onto a separate support, and the negative electrode active material film peeled off from the support is laminated onto a negative electrode current collector to prepare a negative electrode.

[0068] The separator may be a conventional porous polymer film used as a separator, for example, a porous polymer film made of a polyolefin polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, or an ethylene / methacrylate copolymer, either alone or in combination. Also, an insulating thin film having high ion permeability and mechanical strength may be used. The separator may include a safety reinforced separator (SRS) in which a ceramic material is thinly coated on the surface of the separator. In addition, a conventional porous nonwoven fabric, for example, a nonwoven fabric made of a high melting point glass fiber, polyethylene terephthalate fiber, or the like, may be used, but is not limited thereto.

[0069] The electrolytic solution contains a lithium salt as an electrolyte and an organic solvent for dissolving the lithium salt.

[0070] The lithium salt can be any salt that is commonly used in electrolytes for secondary batteries without any restrictions. For example, the anion of the lithium salt can be F - , Cl - , I - , NO3 - , N(CN)2 - , BF4 - , ClO4 - , PF6 - , (CF3)2PF4 - , (CF3)3PF3 - , (CF3)4PF2 - , (CF3)5PF - , (CF3)6P - , CF3SO3 - , CF3CF2SO3 -, (CF3SO2)2N - , (FSO2)2N - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , (SF5)3C - , (CF3SO2)3C - , CF3(CF2)7SO3 - , CF3CO2 - , CH3CO2 - , SCN - , (CF3CF2SO2)2N - , or two or more of these may be used.

[0071] The organic solvent contained in the electrolytic solution may be any commonly used organic solvent without any limitation. Representative examples include one or more selected from the group consisting of propylene carbonate, ethylene carbonate, diethyl carbonate, dimethyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, dipropyl carbonate, dimethyl sulfoxide, acetonitrile, dimethoxyethane, diethoxyethane, vinylene carbonate, sulfolane, γ-butyrolactone, propylene sulfite, and tetrahydrofuran.

[0072] In particular, among the carbonate-based organic solvents, cyclic carbonates such as ethylene carbonate and propylene carbonate are highly viscous organic solvents having a high dielectric constant and capable of dissociating lithium salts in the electrolyte, and therefore can be preferably used. When such cyclic carbonates are mixed with linear carbonates having low viscosity and low dielectric constant, such as dimethyl carbonate and diethyl carbonate, in an appropriate ratio, an electrolyte solution having high electrical conductivity can be produced, and therefore such an electrolyte can be more preferably used.

[0073] Optionally, the electrolyte stored according to the present invention may further contain additives such as overcharge inhibitors that are normally included in electrolytes.

[0074] The lithium secondary battery according to an embodiment of the present invention may be manufactured by forming an electrode assembly by disposing a separator between a positive electrode and a negative electrode, housing the electrode assembly in, for example, a pouch, a cylindrical battery case, or a prismatic battery case, and then injecting an electrolyte. Alternatively, the electrode assemblies may be stacked, impregnated with an electrolyte, and then housed and sealed in a battery case.

[0075] According to an embodiment of the present invention, the lithium secondary battery may be a stack type, a winding type, a stack-and-folding type, or a cable type.

[0076] The lithium secondary battery according to the present invention can be used not only as a battery cell used as a power source for a small device, but also as a unit battery for a medium- to large-sized battery module including a large number of battery cells. Suitable examples of the medium- to large-sized devices include electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, and power storage systems, and is particularly useful in hybrid electric vehicles and renewable energy storage batteries, which are areas where high output is required.

[0077] In the following, the present invention will be described in detail with reference to examples in order to facilitate understanding of the present invention. However, the embodiments according to the present invention can be modified into many other forms, and the scope of the present invention should not be construed as being limited to the following examples. The embodiments of the present invention are provided to more completely explain the present invention to those having average knowledge in the art.

[0078] Example 1 (1) Manufacturing of positive electrodes Denka black, a conductive material, was placed in N-methylpyrrolidone (NMP) and dispersed in a high-speed dispersing device (spike mill, manufactured by Inoue Seisakusho) to prepare a conductive material dispersion. Then, the conductive material dispersion was mixed with a positive electrode active material and a binder polymer to prepare a slurry for the lower layer with a viscosity of 10,000 cps.

[0079] In this case, the lower layer slurry is a sintered body having a chemical formula of Li[Ni 0.65 Mn 0.15 Co 0.20 The positive electrode active material was 96.3% by weight of ]O2, 1.3% by weight of denka black as a conductive material, and 2.4% by weight of polyvinylidene fluoride (PVdF) as a binder polymer.

[0080] In addition, a slurry for the upper layer having a viscosity of 10,000 cps was prepared in the same manner. The upper layer slurry was made of a sintered material having a Ni content of 86% of the total transition metals, and represented by the chemical formula Li[Ni 0.86 Mn 0.05 Co 0.07 ]Al 0.02 It contains 96.3 wt% of O2 positive electrode active material, 1.3 wt% of Denka Black as a conductive material, and 2.4 wt% of polyvinylidene fluoride (PVdF) as a binder polymer.

[0081] The lower layer slurry was charged into a lower layer slurry tank of a double-layer coating machine, and the upper layer slurry was charged into an upper layer slurry tank of the coating machine, and the lower layer slurry and the upper layer slurry were simultaneously and sequentially applied onto an aluminum positive electrode current collector having a thickness of 12 μm.

[0082] Then, the resultant was dried and rolled under a condition of 110°C to prepare a positive electrode having a double-layered coating layer. The total thickness of the positive electrode active material layer of the positive electrode was 175 μm, the thickness of the lower region of the positive electrode active material layer was 87 μm, and the thickness of the upper region of the positive electrode active material layer was 87 μm. The porosity of the positive electrode was 29%. The weight ratio of the lower region to the upper region of the positive electrode active material layer was 50:50.

[0083] (2) Manufacturing of negative electrodes A negative electrode active material slurry was prepared by dispersing 95.6 wt% of a negative electrode active material (artificial graphite), 1.0 wt% of a conductive material (Super-C), and 3.4 wt% of a binder polymer (styrene butadiene rubber) in water. The slurry was applied onto a copper negative electrode current collector with a thickness of 8 μm, which was then dried and rolled at 150°C to prepare a negative electrode. The total thickness of the negative electrode active material layer of the negative electrode was 212 μm, and the porosity was 29.0%.

[0084] (3) Battery manufacturing A polyethylene porous film was interposed between the negative and positive electrodes as a separator, and the resultant was housed in a battery case, and an electrolyte was then injected to prepare a secondary battery. The electrolyte used was a mixed solution of ethylene carbonate and ethyl methyl carbonate (volume ratio 3 / 7) in which 1.1M LiPF6 was dissolved.

[0085] Example 2 Positive electrodes, negative electrodes, and secondary batteries were manufactured in the same manner as in Example 1, except that the Ni content in the positive electrode active material was changed as shown in Table 1 below.

[0086] Comparative Example 1 Ni content is 86% of all transition metals, and the chemical formula is Li[Ni 0.86 Mn 0.05 Co 0.07 ]Al 0.02 The positive electrode active material of 96.3% by weight of O2, 1.3% by weight of Denka Black as a conductive material, and 2.4% by weight of polyvinylidene fluoride (PVdF) as a binder polymer were mixed to prepare a slurry for the lower layer with a viscosity of 10,000cps. 1+b [Ni 0.65 Mn 0.15 Co 0.20 A negative electrode active material and a negative electrode were manufactured in the same manner as in Example 1, except that a slurry for the upper layer having a viscosity of 10,000 cps was manufactured by mixing 96.3 wt% of the positive electrode active material of 1000 μm2 ...

[0087] Comparative Example 2 Denka black, a conductive material, was placed in N-methylpyrrolidone (NMP) and dispersed in a high-speed dispersing device (Spike Mill, manufactured by Inoue Seisakusho) to prepare a conductive material dispersion. Then, the conductive material dispersion was mixed with a positive electrode active material and a binder polymer to prepare a slurry with a viscosity of 10,000 cps.

[0088] In this case, the slurry is a mixture of transition metals having a chemical formula of Li[Ni 0.86 Mn 0.05 Co 0.07 ]Al 0.02 It contains 96.3 wt% of O2 positive electrode active material, 1.3 wt% of Denka Black as a conductive material, and 2.4 wt% of polyvinylidene fluoride (PVdF) as a binder polymer.

[0089] The slurry was applied onto an aluminum positive electrode current collector having a thickness of 12 μm using a single layer coater.

[0090] Then, the resultant was dried and rolled under a condition of 110° C. to prepare a positive electrode having a single coating layer laminated thereon. At this time, the total thickness of the positive electrode active material layer of the positive electrode was 175 μm.

[0091] A lithium secondary battery was manufactured in the same manner as in Example 1, except that the positive electrode thus manufactured was used.

[0092] The characteristics of the positive electrodes and lithium secondary batteries prepared in Examples 1 and 2 and Comparative Examples 1 and 2 were evaluated as follows.

[0093] Experimental example 1: Evaluation of the resistance increase rate in the lower SOC (5-20%) range compared to the resistance at SOC 50% The lithium secondary batteries prepared in Examples 1 and 2 and Comparative Examples 1 and 2 were used to evaluate the resistance increase rate in the lower SOC range (5 to 20%) relative to the resistance at SOC 50% under the following conditions and method, and the results are shown in Table 1.

[0094] The fabricated lithium secondary batteries were discharged at room temperature within the operating voltage range of 2.5 to 4.25 V, and the state of charge (SOC) was decreased by 5% from 100% to 0% at each SOC at 2.5 C. The resistance was measured and compared.

[0095] In addition, the resistance increase rate in the lower SOC range (5-20%) relative to the resistance at SOC 50% was calculated using the following formula. Resistance increase rate (%) = [(resistance at lower SOC (5-20%)) / (resistance at SOC 50%))] x 100 (In the formula, the resistance at the lower SOC (5-20%) is the average of the resistances measured at SOC 5%, 10%, 15%, and 20%.)

[0096] Experimental Example 2: Evaluation of high-temperature capacity retention rate The lithium secondary batteries of Examples 1 and 2 and Comparative Examples 1 and 2 were subjected to 170 cycles of charge and discharge at 45° C. under the following conditions to evaluate the high-temperature capacity retention rate. Charging conditions: CC (constant current) / CV (constant voltage), (4.25V, 0.005C current cutoff) Discharge condition: CC (constant current) condition 2.5V

[0097] The high temperature capacity retention rate was calculated by calculating the ratio of the discharge capacity after 170 cycles to the discharge capacity after 1 cycle, and the results are shown in Table 1 and FIG.

[0098] [Table 1]

[0099] Referring to Table 1, it can be seen that the secondary batteries of Examples 1 and 2, which employ positive electrodes having a bilayer active material layer in which the Ni content of the second positive electrode active material in the upper layer region is controlled to be higher than the Ni content of the first positive electrode active material in the lower layer region, have a lower resistance increase rate in the lower SOC range (5 to 20%) relative to the resistance at SOC 50%, and exhibit excellent high-temperature capacity retention, compared to the secondary batteries of Comparative Example 1, which employs a positive electrode having a bilayer active material layer in which the Ni contents are reversed, and Comparative Example 2, which employs a positive electrode having a single-layer active material layer.

Claims

1. A positive electrode current collector; a positive electrode active material layer located on at least one surface of the positive electrode current collector, the positive electrode active material layer includes a lower layer region in surface contact with the positive electrode current collector, the lower layer region including a first positive electrode active material and a first binder polymer, and an upper layer region in surface contact with the lower layer region, extending to a surface of the positive electrode active material layer, the upper layer region including a second positive electrode active material and a second binder polymer, the first positive electrode active material in the lower layer region is represented by the following Chemical Formula 1, the second positive electrode active material in the upper layer region is represented by the following Chemical Formula 2, and a Ni content of the second positive electrode active material is higher than a Ni content of the first positive electrode active material, [Chemical formula 1] Li 1+a [Ni x Mn y Co z ]M1 t O 2 In the above Chemical Formula 1, 0≦a≦0.2, 0.4≦x≦0.9, 0<y<1, 0<z<1, 0≦t<0.1, and x+y+z+t=1; M1 is one or more elements selected from the group consisting of Co, Mn, Ni, Al, Fe, V, Cr, Ti, Ta, Mg, Mo, Zr, W, Sn, Hf, Nd, and Gd; [Chemical formula 2] Li 1+b [Ni u Mn v Co w ]M2 s O 2 In the above Chemical Formula 2, 0≦b≦0.2, 0.4≦u≦0.9, 0<v<1, 0<w<1, 0≦s<0.1, and u+v+w+s=1; M2 is one or more elements selected from the group consisting of Co, Mn, Ni, Al, Fe, V, Cr, Ti, Ta, Mg, Mo, Zr, W, Sn, Hf, Nd, and Gd; a Ni content of the first positive electrode active material is 50 to 75 mol % of the total transition metals of the first positive electrode active material, and a Ni content of the second positive electrode active material is 81 to 90 mol % of the total transition metals of the second positive electrode active material.

2. 2. The positive electrode according to claim 1, wherein the Ni content of the first positive electrode active material is 65 to 70 mol % of the total transition metals of the first positive electrode active material, and the Ni content of the second positive electrode active material is 86 to 90 mol % of the total transition metals of the second positive electrode active material.

3. 2. The positive electrode according to claim 1, wherein a weight ratio of the lower layer region to the upper layer region of the positive electrode active material layer is from 20:80 to 80:

20.

4. preparing a lower layer slurry including a first positive electrode active material represented by the following Chemical Formula 1, a first binder polymer, and a first dispersion medium, and preparing an upper layer slurry including a second positive electrode active material represented by the following Chemical Formula 2, a second binder polymer, and a second dispersion medium, such that a Ni content of the second positive electrode active material is higher than a Ni content of the first positive electrode active material; coating at least one surface of a positive electrode current collector with the lower layer slurry, and coating the upper layer slurry on the lower layer slurry; and drying the coated lower layer slurry and the coated upper layer slurry simultaneously to form a positive electrode active material layer. [Chemical formula 1] Li 1+a [Ni x Mn y Co z ]M1 t O 2 In the above Chemical Formula 1, 0≦a≦0.2, 0.4≦x≦0.9, 0<y<1, 0<z<1, 0≦t<0.1, and x+y+z+t=1; M1 is one or more elements selected from the group consisting of Co, Mn, Ni, Al, Fe, V, Cr, Ti, Ta, Mg, Mo, Zr, W, Sn, Hf, Nd, and Gd; [Chemical formula 2] Li 1+b[Ni u Mn v Co w ]M2 s O 2 In the above Chemical Formula 2, 0≦b≦0.2, 0.4≦u≦0.9, 0<v<1, 0<w<1, 0≦s<0.1, and u+v+w+s=1; M2 is one or more elements selected from the group consisting of Co, Mn, Ni, Al, Fe, V, Cr, Ti, Ta, Mg, Mo, Zr, W, Sn, Hf, Nd, and Gd; a Ni content of the first positive electrode active material is 50 to 75 mol % of the total transition metals of the first positive electrode active material, and a Ni content of the second positive electrode active material is 81 to 90 mol % of the total transition metals of the second positive electrode active material.

5. 5. The method for producing a positive electrode according to claim 4, wherein the Ni content of the first positive electrode active material is 65 to 70 mol % of the total transition metals of the first positive electrode active material, and the Ni content of the second positive electrode active material is 86 to 90 mol % of the total transition metals of the second positive electrode active material.

6. A lithium secondary battery comprising the positive electrode according to claim 1 .

Citation Information

Patent Citations

  • Positive electrode for nonaqueous electrolyte secondary battery, and nonaqueous electrolyte secondary battery

    JP2019029205A

  • Nonaqueous electrolyte secondary battery

    JP2019140039A

  • Electrode for secondary battery and lithium secondary battery including the same

    JP2019501492A