Lithium iron phosphate-lithium rich oxide composite and its preparation and use

The lithium iron phosphate-lithium rich oxide composite, produced via mechanofusion and processing, addresses the capacity and energy density limitations of LiFePO4, enhancing battery performance and reducing costs.

JP7562870B2Active Publication Date: 2024-10-07HUBEI RT ADVANCED MATERIALS CO LTD
View PDF 16 Cites 0 Cited by

Patent Information

Application Number
JP2023544616
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-10-28
Filing Date
2020-12-31
Publication Date
2024-10-07
Estimated Expiration
2040-12-31

AI Technical Summary

Technical Problem

Existing lithium iron phosphate (LiFePO4) materials in lithium-ion batteries face limitations in specific capacity and energy density, nearing the theoretical limits and requiring improvement.

Method used

A lithium iron phosphate-lithium rich oxide composite is produced through mechanofusion and subsequent sieving and demagnetization, maintaining the crystal structure of LiFePO4 while adding extra active lithium ions, enhancing specific capacity and energy density.

Benefits of technology

The method improves the specific capacity and energy density of lithium-ion batteries with a simple manufacturing process and reduced raw material usage, lowering costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007562870000003
    Figure 0007562870000003
  • Figure 0007562870000004
    Figure 0007562870000004
  • Figure 0007562870000005
    Figure 0007562870000005
Patent Text Reader

Abstract

The present invention relates to the field of lithium-ion batteries and discloses a lithium iron phosphate-lithium-rich oxide composite and its manufacturing method and use, which includes the steps of (1) mechano-fusing LiFePO4 and lithium-rich oxide in a weight ratio of 100:2-15 under a protective gas atmosphere, and (2) sequentially sieving and demagnetizing the mechanofused material to obtain the lithium iron phosphate-lithium-rich oxide composite. The method of the present invention obtains a lithium iron phosphate-lithium-rich oxide composite by mechano-fusing a specific amount of lithium-rich oxide and LiFePO4, thereby improving the electrochemical performance of LiFePO4 lithium-ion batteries.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the field of lithium ion batteries, and in particular to a lithium iron phosphate-lithium rich oxide composite and its preparation and use.

[0002] This application claims priority to Chinese Patent Application No. 202011171827.0, filed on October 28, 2020, the contents of which are incorporated herein by reference. [Background technology]

[0003] Commercially available lithium ion batteries have the characteristics of high energy density, high working voltage, long cycle life, no memory effect, little environmental pollution, etc., and are widely used in electronic products, power batteries, energy storage, etc., and their application range is constantly expanding and related to various aspects of life. The positive electrode material of lithium ion batteries is one of the core materials of lithium ion batteries, accounting for about 30% of the cost of the battery, and the positive electrode material directly affects the energy density of lithium ion batteries and determines the overall performance of lithium ion batteries.

[0004] Since Goodenough first reported in 1997 that olivine-type lithium iron phosphate (LiFePO4) material has the function of releasing lithium, LiFePO4 has attracted the attention of both academic and industrial circles. By using carbon coating and ion doping technology, the drawback of LiFePO4's low intrinsic conductivity can be overcome, and by using nano-sizing and other technologies, the drawback of LiFePO4's slow lithium ion diffusion speed can be overcome, greatly improving its performance. Combined with the advantages of wide supply source, low cost, small impact on the environment, long cycle life and high safety performance, LiFePO4 has become one of the current mainstream positive electrode materials for lithium-ion batteries.

[0005] With the ever-increasing market demand for the comprehensive performance of LiFePO4, such as specific capacity, compression density, rate characteristics, cycle life and BOM cost, the specific capacity of LiFePO4 in the prior art is approaching the limit of theoretical specific capacity, and how to improve the specific capacity and energy density of LiFePO4 lithium ion battery is an urgent problem to be solved. Summary of the Invention [Problem to be solved by the invention]

[0006] The present invention aims to overcome the defect that the specific capacity of LiFePO4 materials in the prior art is close to the theoretical specific capacity limit and cannot be further improved, by providing a lithium iron phosphate-lithium rich oxide composite and a method for preparing the same, thereby improving the specific capacity and energy density of LiFePO4 lithium ion batteries. [Means for solving the problem]

[0007] In order to achieve the above object, according to a first aspect of the present invention, there is provided a method for producing a lithium iron phosphate-lithium rich oxide composite, the method comprising the steps of: (1) mechanofusion of LiFePO4 and lithium-rich oxide in a weight ratio of 100:2-15 under a protective gas atmosphere; and (2) sieving and demagnetizing the mechanofused material to obtain the lithium iron phosphate-lithium rich oxide composite.

[0008] According to a second aspect of the present invention, there is provided a lithium iron phosphate-lithium rich oxide composite produced by the method described above.

[0009] According to a third aspect of the present invention, there is provided a method for producing a lithium-rich electrolyte comprising the steps of: A lithium iron phosphate-lithium rich oxide composite is provided in which the weight ratio of the lithium iron phosphate to the lithium rich oxide is 100:2-15.

[0010] According to a fourth aspect of the present invention, there is provided an application of the lithium iron phosphate-lithium rich oxide composite in a lithium ion battery.

[0011] According to a fifth aspect of the present invention, there is provided a method for producing a positive electrode sheet for a lithium ion battery, the method comprising the steps of: (a) mechanofusion of LiFePO4 and lithium-rich oxide in a weight ratio of 100:2-15 under a protective gas atmosphere; (b) sieving and demagnetizing the mechanofused material to obtain a lithium iron phosphate-lithium rich oxide composite; (c) mixing the lithium iron phosphate-lithium rich oxide composite, a conductive agent, and an adhesive in the presence of a solvent to obtain a positive electrode slurry; and (d) applying the positive electrode slurry onto a current collector foil material and then drying to obtain a positive electrode sheet for a lithium ion battery.

[0012] According to a sixth aspect of the present invention, there is provided a lithium ion battery comprising a lithium ion battery positive electrode sheet produced by the method according to the fifth aspect above. Effect of the Invention

[0013] Compared with the prior art, the present invention has at least the following advantages:

[0014] The method of the present invention uses a certain ratio of lithium-rich oxide and LiFePO4 to mechano-fusion to obtain a lithium iron phosphate-lithium-rich oxide composite, which improves the specific capacity and energy density of LiFePO4 lithium-ion batteries, while the method has a simple manufacturing process, uses fewer raw materials, and reduces the manufacturing cost. [Brief description of the drawings]

[0015] [Figure 1]2 is a charge / discharge curve of a coin-shaped half cell made of the lithium iron phosphate-lithium rich oxide composite of Example 1. [Diagram 2] 1 is a charge / discharge curve of a coin-type half cell made of LiFePO4 of Comparative Example 1. [Diagram 3] 1 shows charge and discharge curves of a coin-type full battery manufactured using the lithium iron phosphate-lithium rich oxide composite of Example 2. [Figure 4] 1 is a charge / discharge curve of a coin-type full battery manufactured using LiFePO4 of Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] Hereinafter, specific embodiments of the present invention will be described with reference to the drawings. It should be understood that the specific embodiments described herein are merely for the purpose of explaining and interpreting the present invention, and are not intended to limit the present invention.

[0017] The endpoints of the ranges and any values ​​disclosed herein are not intended to be limited to the exact ranges or values, and the ranges or values ​​should be understood to include values ​​that are close to those ranges or values. For ranges of numerical values, the endpoints of the ranges, between the endpoints of the ranges and the single point values, and the single point values ​​can be combined with each other to obtain one or more new numerical ranges, and these numerical ranges should be considered to be specifically disclosed herein.

[0018] As previously mentioned, according to a first aspect of the present invention, there is provided a method for producing a lithium iron phosphate-lithium rich oxide composite, the method comprising the steps of: (1) mechanofusion of LiFePO4 and lithium-rich oxide in a weight ratio of 100:2-15 under a protective gas atmosphere; and (2) sieving and demagnetizing the mechanofused material to obtain the lithium iron phosphate-lithium rich oxide composite.

[0019] In the method of the present invention, a lithium iron phosphate-lithium rich oxide composite is obtained by mechanofusion of a specific ratio of lithium rich oxide and LiFePO4 by physical processing, and the bonding between two oxides in the lithium iron phosphate-lithium rich oxide composite is excellent, and the combination of lithium iron phosphate and lithium rich oxide does not affect the crystal structure of lithium iron phosphate. The combined lithium rich oxide provides extra active lithium ions to lithium iron phosphate, which can compensate for the active lithium lost during the initial charge and discharge process of lithium iron phosphate, thereby improving the specific capacity and energy density of lithium ion batteries.

[0020] According to the present invention, the method of mechanofusion of the LiFePO4 and the lithium-rich oxide and the device used for mechanofusion are not particularly limited, and may be any conventional physical processing method that can obtain a composite having excellent electrochemical performance of the present invention.

[0021] According to a preferred specific embodiment of the present invention, in step (1), the mechanofusion of the LiFePO4 and the lithium-rich oxide is carried out in an efficient fusion device.

[0022] According to the present invention, the supply source of the LiFePO4 is not particularly limited, and can be commercially available, or can be produced by the conventional LiFePO4 production method in this field, such as ferrous oxalate process, red iron oxide process, iron phosphate process, liquid phase process, etc., and the LiFePO4 can be of high capacity type, high compression type, high magnification, long life, etc., and is not particularly limited thereto.

[0023] According to the present invention, the lithium-rich oxide refers to an oxide having a lithium mole number greater than 1 per unit molecular weight.

[0024] Preferably, the lithium-rich oxide is Li5FeO4 and / or Li6CoO4, more preferably Li6CoO4. The inventors have selected Li5FeO4 and / or Li6CoO4, and in particular Li6CoO4 and LiFePO4, to obtain a lithium iron phosphate-lithium-rich oxide composite obtained by mechanofusion, which has better electrochemical performance, such as specific capacity.

[0025] According to the present invention, the source of the lithium-rich oxide, such as Li5FeO4 and Li6CoO4, is not particularly limited, and may be a commercially available product, or may be produced by a method for producing conventional lithium-rich oxides in this field, such as Li5FeO4 and Li6CoO4, as long as it can be mechanofused with LiFePO4 to obtain a lithium iron phosphate-lithium-rich oxide composite having a high specific capacity.

[0026] According to the present invention, in order to obtain a lithium iron phosphate-lithium rich oxide composite with excellent electrochemical performance, the weight ratio of LiFePO4 to lithium rich oxide needs to be controlled within the range of 100:2 to 15. In a specific embodiment, the weight ratio of LiFePO4 to lithium rich oxide is, for example, 100:2, 100:3, 100:4, 100:5, 100:6, 100:7, 100:8, 100:9, 100:10, 100:11, 100:12, 100:13, 100:14, 100:15, and any value within the range consisting of any two of these point values.

[0027] In order to obtain a lithium iron phosphate-lithium rich oxide composite having better electrochemical performance, the weight ratio of the LiFePO4 to the lithium rich oxide is 100:2-10.

[0028] Preferably, in step (1), the conditions of the mechanofusion are a fusion speed of 300 to 2500 rpm and a fusion time of 3 to 60 minutes. The fusion speed is 300 to 2500 rpm, for example, 500 rpm, 600 rpm, 700 rpm, 800 rpm, 900 rpm, 1000 rpm, 1100 rpm, 1200 rpm, 1300 rpm, 1400 rpm, 1500 rpm, 1600 rpm, 1700 rpm, 1800 rpm, 1900 rpm, 2000 rpm, 2100 rpm, 2200 rpm, 2300 rpm, 2400 rpm, or 2500 rpm, and the fusion time is 3 to 60 min, for example, 5 min, 10 min, 15 min, 20 min, 25 min, 30 min, 35 min, 40 min, 45 min, 50 min, 55 min, or 60 min.

[0029] Preferably, in step (1), when LiFePO4 is mechanofused with a lithium-rich oxide, the fusion speed is 1000-1500 rpm and the fusion time is 10-30 min.

[0030] According to the method of the invention, the protective gas may be any gas capable of providing various protective atmospheres conventionally used in the art.

[0031] Preferably, in step (1), the protective gas is nitrogen gas and / or an inert gas.

[0032] More preferably, in step (1), the protective gas is nitrogen gas and / or argon gas.

[0033] Preferably, in step (2), the sieve is a vibrating sieve, and the mesh number of the sieve is 200 to 500 mesh, for example, 200 mesh, 250 mesh, 300 mesh, 350 mesh, 400 mesh, 450 mesh, or 500 mesh.

[0034] More preferably, the mesh number of the sieve is 300 mesh, and after sieving, the undersize particles are removed.

[0035] Preferably, in step (2), the magnetic force of the demagnetizer for demagnetization is 5000 to 12000GS, for example, 5000GS, 5500GS, 6000GS, 6500GS, 7000GS, 7500GS, 8000GS, 8500GS, 9000GS, 9500GS, 10000GS, 10500GS, 11000GS, 11500GS or 12000GS.

[0036] More preferably, in step (2), the magnetic force of the demagnetizer for demagnetization is 8,000 to 10,000 GS.

[0037] As mentioned above, according to a second aspect of the present invention there is provided a lithium iron phosphate-lithium rich oxide composite produced by the method described above.

[0038] As mentioned above, according to the third aspect of the present invention, a lithium-rich oxide is provided, comprising: A lithium iron phosphate-lithium rich oxide composite is provided in which the weight ratio of the lithium iron phosphate to the lithium rich oxide is 100:2-15.

[0039] In the third aspect of the present invention, preferably, the lithium-rich oxide is Li5FeO4 and / or Li6CoO4, more preferably Li6CoO4.

[0040] In the third aspect of the present invention, the weight ratio of the content of the LiFePO4 to the content of the lithium-rich oxide is preferably 100:2-10.

[0041] The lithium iron phosphate-lithium rich oxide composite material according to the present invention includes LiFePO4 and lithium rich oxide, and has excellent bonding between the two oxides. The lithium iron phosphate-lithium rich oxide composite material has excellent electrochemical performance, such as high specific capacity and high energy density.

[0042] As mentioned above, according to a fourth aspect of the present invention, there is provided an application of the lithium iron phosphate-lithium rich oxide composite in a lithium ion battery.

[0043] In the present invention, the specific operation of the application is not particularly limited, for example, the lithium iron phosphate-lithium rich oxide composite is used as a positive electrode active material to prepare a positive electrode sheet to obtain a lithium ion battery.

[0044] As mentioned above, according to a fifth aspect of the present invention, there is provided a method for producing a positive electrode sheet for a lithium ion battery, the method comprising the steps of: (a) mechanofusion of LiFePO4 and lithium-rich oxide in a weight ratio of 100:2-15 under a protective gas atmosphere; (b) sieving and demagnetizing the mechanofused material to obtain a lithium iron phosphate-lithium rich oxide composite; (c) mixing the lithium iron phosphate-lithium rich oxide composite, a conductive agent, and an adhesive in the presence of a solvent to obtain a positive electrode slurry; and (d) applying the positive electrode slurry onto a current collector foil material and then drying to obtain a positive electrode sheet for a lithium ion battery.

[0045] In the fifth aspect of the present invention, the preferred specific embodiments of step (a) and step (b), such as the selection of the type of lithium-rich oxide, the weight ratio of LiFePO4 to said lithium-rich oxide, the conditions of mechanofusion, the conditions of sieving and demagnetization, etc., are the same as those corresponding to the preferred situations of step (1) and step (2) in the method according to the first aspect above, and will not be described in detail here in the present invention in order to avoid redundant description.

[0046] In the fifth embodiment of the present invention, the obtained lithium iron phosphate-lithium rich oxide composite has the same properties as the lithium iron phosphate-lithium rich oxide composite described above, and the description thereof is omitted here in the present invention.

[0047] In a fifth aspect of the present invention, the conductive agent is at least one selected from the group consisting of Super-P (SP), acetylene black, KS-6, and carbon nanotubes.

[0048] In a fifth embodiment of the present invention, the pressure-sensitive adhesive is at least one selected from polytetrafluoroethylene, polyvinylidene fluoride, and styrene-butadiene rubber.

[0049] In a fifth aspect of the present invention, based on the total weight of the lithium iron phosphate-lithium rich oxide composite, the conductive agent, and the adhesive, the content of the lithium iron phosphate-lithium rich oxide composite is 80 to 90% by weight, the content of the conductive agent is 5 to 10% by weight, and the content of the adhesive is 5 to 10% by weight.

[0050] In a fifth aspect of the present invention, the solvent includes at least one of N-methylpyrrolidone, N,N-dimethylformamide, N,N-diethylformamide, dimethylsulfoxide, tetrahydrofuran, and alcohol dispersants, but is not limited thereto.

[0051] Preferably, the positive electrode slurry has a solid content of 35 to 45% by weight depending on the amount of the solvent used, and the solid content refers to the total weight of the lithium iron phosphate-lithium rich oxide composite, conductive agent, and adhesive in the positive electrode slurry.

[0052] In the fifth aspect of the present invention, preferably in step (c), the mixing conditions are that the temperature is 25±2° C. and the mixing is carried out with stirring.

[0053] In the fifth aspect of the present invention, preferably, in step (d), the positive electrode slurry is applied to a foil material of a current collector, and the areal density (loading amount) of the lithium iron phosphate-lithium rich oxide composite is 8.5-9.5 mg / cm 2 to.

[0054] Preferably, the foil material of the current collector is an aluminum foil.

[0055] In the fifth aspect of the present invention, in step (d), the specific operation of the coating is not particularly limited, and can be carried out using a conventional coating operation for producing an electrode sheet in this field.

[0056] In the fifth aspect of the present invention, in step (d), the specific conditions for the drying are not particularly limited as long as the electrode sheet can be completely dried.

[0057] As mentioned above, according to a sixth aspect of the present invention, there is provided a lithium ion battery comprising a lithium ion battery positive electrode sheet produced by the method according to the fifth aspect above.

[0058] The present invention will be described in detail below with reference to examples and comparative examples, but the scope of the present invention is not limited thereto.

[0059] In the present invention, unless otherwise specified, all raw materials used are commercially available.

[0060] LiFePO4, Li5FeO4 and Li 6 Chief of Staff 4 are all purchased from Hubei Rongtong High-Tech Advanced Materials Co., Ltd.

[0061] Example 1 (1) 300g LiFePO4 and 9g Li5FeO4 are weighed and placed into the cavity of an efficient fusion device, and under the protection of nitrogen gas, the rotation speed of the main shaft is adjusted to 1000 rpm, and mechano-fused for 15 minutes, so that the two metal oxides are mechano-fused by physical processing; (2) The material obtained by mechanofusion was then passed through a 325 mesh vibrating sieve and demagnetized in a de-ironizer with a magnetic force of 10,000 GS to obtain a lithium iron phosphate-lithium rich oxide composite L1.

[0062] Example 2 (1) 300g LiFePO4 and 15g Li5FeO4 are weighed and placed into the cavity of an efficient fusion device, and under the protection of nitrogen gas, the rotation speed of the main shaft is adjusted to 1200 rpm, and mechanofusion is carried out for 20 minutes. The two metal oxides are mechanofused by physical processing. (2) The material obtained by mechanofusion was then passed through a 300 mesh vibrating sieve and demagnetized in a de-ironizer with a magnetic force of 8000GS to obtain a lithium iron phosphate-lithium rich oxide composite L2.

[0063] Example 3A (1) 300g LiFePO4 and 9g Li6CoO4 were weighed and placed into the cavity of an efficient fusion device, and under the protection of nitrogen gas, the rotation speed of the main shaft was adjusted to 1200 rpm, and the two metal oxides were mechanofused by physical processing. (2) The material obtained by mechanofusion was then sieved through a 325 mesh vibrating sieve and demagnetized in a de-ironizer with a magnetic force of 9000GS to obtain a lithium iron phosphate-lithium rich oxide composite L3A.

[0064] Example 3B A method similar to that of Example 1 was used, except that Li5FeO4 in Example 1 was replaced with an equal weight of Li6CoO4, and the rest was the same as in Example 1, to obtain a lithium iron phosphate-lithium rich oxide composite L3B.

[0065] Example 4 A similar method to Example 3A was used, except that 300 g of LiFePO4 and 45 g of Li6CoO4 were weighed and placed in the cavity of an efficient fusion device for mechanofusion; The rest of the process was the same as in Example 3A, and a lithium iron phosphate-lithium rich oxide composite L4 was obtained.

[0066] Example 5 A method similar to that of Example 3A is used, except that the rotation speed of the spindle is adjusted to 500 rpm; The rest of the process was the same as in Example 3A, and a lithium iron phosphate-lithium rich oxide composite L5 was obtained.

[0067] Example 6 A similar method to Example 3A was used, except that the mechanofusion time was 5 min. The rest of the process was the same as in Example 3A, and a lithium iron phosphate-lithium rich oxide composite L6 was obtained.

[0068] Example 7 A method similar to that of Example 3A is used, except that the rotation speed of the spindle is adjusted to 300 rpm; The rest of the process was the same as in Example 3A, and a lithium iron phosphate-lithium rich oxide composite L7 was obtained.

[0069] Example 8 A similar method to Example 3A was used, except that the mechanofusion time was 3 minutes. The rest of the process was the same as in Example 3A, and a lithium iron phosphate-lithium rich oxide composite L8 was obtained.

[0070] Comparative Example 1 The lithium iron phosphate LiFePO4 is not subjected to any treatment and is directly added as the positive electrode active material.

[0071] Comparative Example 2 (1) 300g LiFePO4 and 3g Li5FeO4 were weighed and placed into the cavity of an efficient fusion device. Under the protection of nitrogen gas, the rotation speed of the main shaft was adjusted to 1000 rpm, and the two metal oxides were mechanofused by physical processing. (2) The material obtained by mechanofusion was successively passed through a 200 mesh vibrating sieve and demagnetized in a de-ironizer with a magnetic force of 9000GS to obtain a lithium iron phosphate-lithium rich oxide composite.

[0072] Comparative Example 3 A similar method to Example 3A was used, except that 300 g of LiFePO4 and 1.5 g of Li6CoO4 were weighed and placed in the cavity of an efficient fusion device for mechanofusion; The rest of the process was the same as in Example 3A, and a lithium iron phosphate-lithium rich oxide composite was obtained.

[0073] Comparative Example 4 A method similar to that of Example 3A was used, except that 300 g of LiFePO4 and 54 g of Li6CoO4 were weighed and placed in the cavity of an efficient fusion device for mechanofusion; The rest of the process was the same as in Example 3A, and a lithium iron phosphate-lithium rich oxide composite was obtained.

[0074] (Test Example) (1) In the present invention, the lithium iron phosphate-lithium rich oxide composites prepared in the above examples and comparative examples were subjected to XRD testing. As can be seen from the XRD test results, the lithium iron phosphate-lithium rich oxide composites prepared in the present invention are two-phase composites of lithium iron phosphate and lithium rich oxide, and the composite of lithium iron phosphate and lithium rich oxide does not affect the crystal structure of lithium iron phosphate.

[0075] (2) Electrochemical performance testing The materials prepared in the above examples and comparative examples are fabricated into lithium ion batteries, and the electrochemical performance of the lithium ion batteries is tested using a Xinwei testing system.

[0076] (Test Example 1) The lithium iron phosphate-lithium rich oxide composite of Example 1 was fabricated into a lithium ion battery, and the electrochemical performance of the lithium ion battery was tested.

[0077] The manufacturing process for the battery is as follows: A positive electrode sheet was prepared by dispersing the lithium iron phosphate-lithium rich oxide composite L1, conductive agent Super-P, and PVDF (purchased from Solvay, USA, model number 5130) in NMP solvent at a mass ratio of 90:5:5 (solid content 42 wt%), ball milling (rotation speed 1500 rpm, time 20 min) to disperse the composite evenly, and then applying it onto an aluminum foil (the amount of the lithium iron phosphate-lithium rich oxide composite L1 supported was 9.2 mg / cm). 2 ) and dried in vacuum to produce a positive electrode sheet.

[0078] Assembling a coin-shaped half cell. Using the above positive electrode sheet, a 2025 coin-shaped half cell was assembled in a glove box filled with argon gas, a metallic lithium sheet was used as the counter electrode, a Celgard polypropylene film was used as the separator, and 1 mol / L LiPF6 / EC+DMC+EMC was used as the electrolyte, with EC:DMC:EM = 1:1:1 (volume ratio), and assembled into a 2025 coin-shaped half cell.

[0079] Assemble the entire coin cell battery. The above prepared positive electrode sheet and graphite negative electrode were assembled into a 2025 coin type full cell, the N / P ratio of the full cell was 1.5, and the separator and electrolyte were the same as those of the half cell.

[0080] Electrochemical performance testing In the charge / discharge performance test, the test temperature is 25±2°C, the test voltage range is 2.5V to 3.9V, and the charge / discharge rate is 0.2C. The charge and discharge performance of the half cell and the whole cell were tested, and the specific results are shown in Tables 1 and 2, respectively.

[0081] (Test Examples 2 to 8) A method similar to that of Test Example 1 was used, except that L1 of Test Example 1 was replaced with the composites of Examples 2 to 8 each having the same weight as L1 of Test Example 1.

[0082] All other aspects were the same as in Test Example 1, and the specific test results are shown in Tables 1 and 2, respectively.

[0083] (Comparative Test Examples 1 to 4) A method similar to that of Test Example 1 was used, except that L1 of Test Example 1 was replaced with the substances of Comparative Examples 1 to 4 each having the same weight as L1 of Test Example 1.

[0084] All other aspects were the same as in Test Example 1, and the specific test results are shown in Tables 1 and 2, respectively.

[0085] (Comparative Test Example 5) The positive electrode sheet was prepared as follows: Lithium iron phosphate, Li5FeO4, conductive agent Super-P, and PVDF were dispersed in NMP solvent in a mass ratio of 87:3:5:5 (solid content 42 wt%), and uniformly dispersed by ball milling (rotation speed 1500 rpm, time 20 min), and then coated on aluminum foil (total amount of lithium iron phosphate and Li5FeO4 supported was 9.2 mg / cm). 2 ) and dried in vacuum to produce a positive electrode sheet.

[0086] Then, a coin-type half cell and a coin-type full cell were manufactured in the same manner as in Test Example 1, and the electrochemical performance of the cells was tested. The specific results are shown in Tables 1 and 2, respectively.

[0087] [Table 1]

[0088] [Table 2]

[0089] In the present invention, the charge and discharge curve of the coin-type half cell of the lithium iron phosphate-lithium rich oxide composite L1 in Example 1 is provided as an example. As shown in FIG. 1, it can be seen that the initial charge specific capacity of the battery can be effectively improved by combining the lithium rich oxide and lithium iron phosphate.

[0090] In the present invention, the charge and discharge curve of a coin-type half cell manufactured using the lithium iron phosphate LiFePO4 of Comparative Example 1 is provided as an example, as shown in FIG. 2. As can be seen from FIG. 2, the lithium iron phosphate has an initial charge specific capacity of about 163 mAh / g and an initial discharge specific capacity of about 155 mAh / g.

[0091] In the present invention, the charge and discharge curve of the coin type full battery prepared using the lithium iron phosphate-lithium rich oxide composite of Example 2 is provided as an example. As shown in FIG. 3, it can be seen that the initial charge specific capacity and the initial discharge specific capacity of the lithium iron phosphate full battery can be effectively improved by combining the lithium rich oxide with lithium iron phosphate.

[0092] In the present invention, the charge and discharge curve of the coin type full battery manufactured using the lithium iron phosphate LiFePO4 of Comparative Example 1 is provided as an example, as shown in FIG.

[0093] As can be seen from the above results, the lithium iron phosphate-lithium rich oxide composite prepared by the method of the present invention has excellent electrochemical performance, for example, high specific capacity.

[0094] In particular, as can be seen from the results of Test Example 1, Test Example 3B, and Comparative Test Example 1, the lithium iron phosphate-lithium rich oxide composite obtained by mechanofusion of a lithium-rich oxide and LiFePO4, particularly by mechanofusion of Li5FeO4 and Li6CoO4 lithium-rich oxides, particularly by mechanofusion of Li6CoO4 and LiFePO4, has higher electrochemical performance, for example, higher charge / discharge specific capacity.

[0095] In particular, as can be seen from the results of Test Example 3A, Test Example 4, and Comparative Test Examples 2 to 4, the lithium iron phosphate-lithium rich oxide composite obtained when the composite ratio of LiFePO4 and lithium-rich oxide, for example Li5FeO4, Li6CoO4, is controlled to be 100:2 to 15, particularly 100:2 to 10, has higher electrochemical performance, for example, charge / discharge specific capacity.

[0096] In particular, as can be seen from the results of Test Example 1, Comparative Test Example 1, and Comparative Test Example 5, the electrochemical performance, e.g., the specific capacity, of the battery obtained by mechanofusion of lithium-rich oxide and LiFePO4 using the method of the present invention to obtain a composite is higher. Also, as can be seen from the results of Comparative Test Example 5, the electrochemical performance, e.g., the specific capacity, of the battery obtained by producing an electrode sheet using the composite of the present invention is better than that obtained by producing an electrode sheet by adding LiFePO4 and lithium-rich oxide separately during the material mixing process.

Claims

1. 1. A method for producing a lithium iron phosphate-lithium oxide composite, comprising the steps of: LiFePO having a weight ratio of 100:2-15 under a protective gas atmosphere 4 (1) Mechanofusion of a lithium-rich oxide with (2) sieving and demagnetizing the mechanofused material to obtain the lithium iron phosphate-lithium oxide composite; The lithium-rich oxide is Li 5 FeO 4 and / or Li 6 CoO 4 ; A method comprising:

2. In step (1), the LiFePO 4 and the lithium-rich oxide, the weight ratio of which is 100:2-10; 2. The method of claim 1 .

3. In step (1), the conditions of the mechanofusion are a fusion speed of 300 to 2500 rpm and a fusion time of 3 to 60 min.

3. The method according to claim 1 or 2.

4. In step (1), the protective gas is nitrogen gas and / or an inert gas. The method according to any one of claims 1 to 3.

5. In step (2), the sieve is a vibrating sieve, and the mesh number of the sieve is 200 to 500 mesh; In step (2), the magnetic force of the demagnetizer for demagnetization is 5,000 to 12,000 GS.

5. The method according to claim 1, wherein the first and second electrodes are arranged in a first direction.

6. LiFePO having a weight ratio of 100:2-15 under a protective gas atmosphere 4 (a) Mechanofusion of a lithium-rich oxide with (b) sieving and demagnetizing the mechanofused material to obtain a lithium iron phosphate-lithium oxide composite; (c) mixing the lithium iron phosphate-lithium oxide composite, a conductive agent, and an adhesive in the presence of a solvent to obtain a positive electrode slurry; and (d) applying the positive electrode slurry onto a current collector foil material and then drying to obtain a positive electrode sheet for a lithium ion battery; The lithium-rich oxide is Li 5 FeO 4 and / or Li 6 CoO 4 ; 2. A method for producing a positive electrode sheet for a lithium ion battery.

Citation Information

Patent Citations

  • Lithium ion capacitor and preparation method thereof

    CN107910197A

  • Lithium ion battery manufacturing process

    CN108682894A

  • Lithium ion battery and its manufacture

    JP1999283623A

  • Manufacturing method for graphitized powder of mesocarbon microspheres

    JP2007076929A

  • Methods of preparing electroactive insertion compounds and resulting electrode materials