Polymer film, electricity storage device, and method for manufacturing electricity storage device
By adding a lithium salt to create voids in the polymer film, the conductivity and lithium ion concentration are enhanced, addressing the issue of increased film resistance and improving the input/output characteristics and energy density of electricity storage devices.
Patent Information
- Application Number
- JP2019167266
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2019-09-13
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2039-09-13
AI Technical Summary
Existing polymer films used as separators in electricity storage devices face issues with increased film resistance, leading to deteriorated input/output characteristics due to reduced pore diameter and porosity, which affects the performance and efficiency of the devices.
Incorporating a lithium salt that is solid at room temperature and dissolves in the electrolyte into a polymer membrane to create voids, enhancing the polymer film's conductivity and lithium ion concentration, thereby improving input/output characteristics.
The polymer film with voids and increased lithium ion concentration reduces reaction resistance, improving the input/output characteristics and energy density of the electricity storage device.
Smart Images

Figure 0007562941000002 
Figure 0007562941000003 
Figure 0007562941000004
Abstract
Description
[Technical field]
[0001] Disclosed herein are polymeric membranes, power storage devices, and methods for making power storage devices. [Background technology]
[0002] Conventionally, as this type of electric storage device, for example, a separator consisting of a separation function layer and a support layer has been proposed, in which the separation function layer has a smaller pore size and a lower porosity than the support layer, and is densely structured (see, for example, Patent Document 1). In this electric storage device, it is possible to suppress the movement of metal foreign matter from the positive electrode plate side to the negative electrode plate side, thereby suppressing the deposition of metal foreign matter on the negative electrode plate side, thereby ensuring battery performance and safety. In addition, as a device to be used in an electric storage device, an assembly in which an electrode and a separator are integrated, obtained by coating an electrode with a fluorine-based polymer emulsion or suspension and drying it, has been proposed (see, for example, Patent Document 2). It is said that this integrated electrode separator can provide a more uniform and thinner separator layer at a lower cost than conventional free-standing separators. Also, for use in power storage devices, a separator has been proposed that is obtained by applying a vinylidene fluoride copolymer obtained by copolymerizing vinylidene fluoride and acryloyloxyethyl succinic acid to a separator and drying the copolymer (see, for example, Patent Document 3). It is said that this separator does not impede the movement of ions such as lithium ions. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2017-84765 A [Patent Document 2] Special Publication No. 2015-533453 [Patent Document 3] International Publication No. 2014 / 002937 Brochure Summary of the Invention [Problem to be solved by the invention]
[0004] However, in Patent Document 1, the pore size and porosity of the separator on the negative electrode side are reduced in order to suppress dendrite precipitation of the metal components that have migrated from the positive electrode at the negative electrode, which may result in a decrease in input / output characteristics. In Patent Document 2, a fluoropolymer aqueous dispersion is directly applied to the electrode body and dried at about 170°C, but it is presumed that the dispersion cannot be applied to materials that are not resistant to water or drying. In Patent Document 3, the dispersibility of the solvent containing the copolymer is controlled to control the porosity and increase the adhesion between a general polyolefin-based separator and a positive electrode or a negative electrode, but the Gurley air permeability, which is correlated with the membrane resistance, is increased by forming a resin membrane, which may result in a decrease in the input / output characteristics of the electricity storage device. As described above, when a single or composite polymer membrane is used as a separator for an electricity storage device, an increase in membrane resistance is inevitable, which may result in a decrease in input / output characteristics.
[0005] The present disclosure has been made in consideration of such problems, and has as its main object to provide a polymer film, an electricity storage device, and a method for manufacturing an electricity storage device that can further improve input / output characteristics. [Means for solving the problem]
[0006] As a result of intensive research to achieve the above-mentioned object, the inventors discovered that by adding a lithium salt that is solid at room temperature and dissolves in an electrolyte to prepare a polymer membrane separating the positive electrode and the negative electrode, and then dissolving the lithium salt in the electrolyte to form voids, the liquid retention, electrical conductivity, IV resistance, etc. of the electrolyte can be improved, and the input / output characteristics of the electricity storage device can be improved, thereby completing the invention disclosed in this specification.
[0007] That is, the polymer membrane disclosed herein is A polymer film used to be interposed between a positive electrode and a negative electrode of an electricity storage device, The material is made of a resin capable of conducting lithium ions and / or a resin that holds an electrolyte capable of conducting lithium ions, has pores that can be confirmed by a secondary electron microscope image, and the average surface pore density of the pores is 0.1 pores / μm 2 That is all.
[0008] The electricity storage device disclosed in the present specification is A positive electrode and A negative electrode; The polymer film interposed between the positive electrode and the negative electrode and conducting lithium ions; It is equipped with the following:
[0009] The method for producing an electricity storage device disclosed in the present specification includes the steps of: A method for producing an electricity storage device having a positive electrode and a negative electrode, comprising the steps of: A film formation step of mixing an additive solid that is solid at room temperature and soluble in a solvent with a resin capable of conducting lithium ions and / or a resin that retains an electrolyte capable of conducting lithium ions to form an additive solid-containing polymer film; The polymer film containing the additive solid is interposed between the positive electrode and the negative electrode, and a solvent is added to dissolve the additive solid. The space formed by dissolving the additive solid is a space that can be confirmed by a secondary electron microscope image and has an average surface pore density of 0.1 pores / μm 2 a void forming step of forming the above voids in the polymer film; It includes. Effect of the Invention
[0010] The present disclosure can further improve the input / output characteristics. The reason why such an effect is obtained is presumed to be as follows. For example, since this polymer film has sufficient voids, it has high conductivity, and thus it is possible to improve the input / output characteristics of the power storage device. In addition, when the additive solid contained in the polymer film is a lithium salt, the lithium ion concentration is high near the electrode, so it is possible to reduce the reaction resistance, which is presumed to contribute to the improvement of the input / output characteristics. In addition, in a power storage device using an electrode of a columnar body having an active material, lithium ions can enter and exit at the outer peripheral surface of the columnar body, so that the input / output characteristics are improved and a high energy density can be achieved. Here, "room temperature" is defined as 15°C to 25°C. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a schematic diagram showing an example of an electricity storage device 10. [Diagram 2] FIG. 4 is a schematic diagram showing an example of an electricity storage device 10B. [Diagram 3] SEM photographs and binarized images of Experimental Examples 1, 2, and 6. [Figure 4] X-ray diffraction measurement results for Experimental Examples 1 and 6. [Diagram 5] X-ray diffraction measurement results for Experimental Examples 2 and 6. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] (polymer film) The polymer membrane described in this embodiment is used to be interposed between the positive electrode and the negative electrode of an electricity storage device. The polymer membrane has insulating properties. This polymer membrane is made of a resin capable of conducting lithium ions and / or a resin that holds an electrolyte capable of conducting lithium ions, has pores that can be confirmed in a secondary electron microscope image, and the average surface pore density of the pores is 0.1 pores / μm 2The average surface pore density was calculated by binarizing the SEM image of the surface of the polymer membrane observed with a scanning electron microscope using image analysis, counting the number of black areas present in the image as voids, and calculating the average surface pore density per unit area (μm 2 The average surface pore density of these pores is 0.1 / μm 2 At or above this level, the electrolyte can easily permeate into the polymer membrane, and therefore higher ionic conductivity can be achieved. In this polymer membrane, the average surface pore density is 0.15 / μm 2 More preferably, it is 1.0 particles / μm or more. 2 It is more preferable that the average surface pore density is 2.5 / μm3 or more, taking into consideration insulation properties, etc. 2 It is preferable that:
[0013] The polymer film may have a domain size of 1 μm or less formed on the surface of the polymer film that is identifiable in a secondary electron microscope image, and may have the voids between the domains. Here, the term "domain" refers to a region separated by a boundary that is clearly identifiable in an SEM image. In the case where the domain has a "scale-like portion that is connected to the adjacent portion," the boundary is defined and the domain is recognized as a separate domain. It is presumed that the average surface pore density is good when the domain size is 1 μm or less. In addition, similar to the domain size, it is preferable that the resin surface has roughness of 1 μm or less on average. In addition, it is preferable that the polymer film has pores on the resin surface of 300 nm or less on average. When the polymer film has pores on the average of 300 nm or less, the electrolyte can easily penetrate into the polymer film, and therefore higher ion conductivity can be exhibited.
[0014] In this polymer film, an additive solid that is solid at room temperature and dissolves in a solvent may be filled, and the space generated by dissolving the additive solid may be a void. In this polymer film, the void can be easily formed by dissolving the additive solid in a solvent. The additive solid is more preferably, for example, a salt containing an ion that is a carrier, and is preferably a lithium salt. For example, the additive solid may be, other than the lithium salt, a carbonate such as ethylene carbonate (EC). In addition, the additive solid may be, for example, a lithium salt, such as lithium bisoxalatoborate (LiBOB) or lithium difluorooxalatoborate (LiBFO), which is a boron-containing compound. In addition, the lithium salt may be, for example, an imide salt such as lithium bis(fluorosulfonyl)imide (LiFSI) or lithium bis(trifluoromethanesulfonyl)imide (LiTFSI). Of these, the additive solid is preferably LiFSI or LiBOB, and more preferably LiBOB.
[0015] Examples of the resin contained in the polymer membrane include polyvinylidene fluoride (PVdF), a copolymer of PVdF and hexafluoropropylene (PVdF-HFP), polymethyl methacrylate (PMMA), and a copolymer of PMMA and an acrylic polymer. For example, in the case of a copolymer of PVdF and HFP, a part of the electrolyte swells and gels the membrane, forming an ion-conductive membrane. The thickness of the polymer membrane is preferably 2 μm or more, more preferably 5 μm or more, and may be 7 μm or more. A thickness of 2 μm or more is preferable in terms of ensuring insulation. In particular, if the thickness of the polymer membrane is 2 μm or more, it is easy to prepare. In addition, the thickness of the polymer membrane is preferably 15 μm or less, more preferably 10 μm or less. A thickness of 15 μm or less is preferable in terms of suppressing a decrease in ion conductivity and further reducing the volume occupied by the cell. When the thickness L is in the range of 2 to 15 μm, ion conductivity and insulation are favorable.
[0016] The polymer membrane may contain an electrolyte that conducts ions, which are carriers. Examples of the electrolyte include non-aqueous solvents. Examples of the solvent for the electrolyte include solvents for non-aqueous electrolytes. Examples of the solvent include carbonates, esters, ethers, nitriles, furans, sulfolanes, and dioxolanes, which may be used alone or in combination. Specifically, examples of the carbonates include cyclic carbonates such as ethylene carbonate (EC), propylene carbonate, vinylene carbonate, butylene carbonate, and chloroethylene carbonate; chain carbonates such as dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diethyl carbonate, ethyl-n-butyl carbonate, methyl-t-butyl carbonate, di-i-propyl carbonate, and t-butyl-i-propyl carbonate; and γ-butyl carbonate. Examples of suitable electrolytes include cyclic esters such as valerolactone and γ-valerolactone, chain esters such as methyl formate, methyl acetate, ethyl acetate, and methyl butyrate, ethers such as dimethoxyethane, ethoxymethoxyethane, and diethoxyethane, nitriles such as acetonitrile and benzonitrile, furans such as tetrahydrofuran and methyltetrahydrofuran, sulfolanes such as sulfolane and tetramethylsulfolane, and dioxolanes such as 1,3-dioxolane and methyldioxolane. The electrolyte may be one in which a supporting salt containing ions that are carriers of the electricity storage device 10 is dissolved. Examples of the supporting salt include LiPF6, LiBF4, LiAsF6, LiCF3SO3, LiN(CF3SO2)2, LiC(CF3SO2)3, LiSbF6, LiSiF6, LiAlF4, LiSCN, LiClO4, LiCl, LiF, LiBr, LiI, and LiAlCl4. Among these, it is preferable to use a combination of one or more salts selected from the group consisting of inorganic salts such as LiPF6, LiBF4, LiClO4, etc., and organic salts such as LiCF3SO3, LiN(CF3SO2)2, LiC(CF3SO2)3, etc., from the viewpoint of electrical properties. The concentration of this supporting salt in the electrolyte is preferably 0.1 mol / L or more and 5 mol / L or less, more preferably 0.5 mol / L or more and 2 mol / L or less.
[0017] In this polymer film, the resin may be a copolymer of polyvinylidene fluoride and hexafluoropropylene, and may be one that does not show a diffraction peak in the range of 2θ=25° to 28° in X-ray diffraction measurement using a Cu tube. In a polymer film filled with an additive solid that is solid at room temperature and dissolves in a solvent, it is more preferable that the diffraction peak disappears and the polymer film becomes amorphous.
[0018] (Electricity storage device) The power storage device includes a positive electrode, a negative electrode, and a polymer film that is interposed between the positive electrode and the negative electrode and conducts lithium ions. The power storage device may also have an electrolyte solution containing a solvent in at least one of the positive electrode, the negative electrode, and the polymer film. The electrolyte solution may also contain an additive solid that is filled in the polymer film and is solid at room temperature and dissolves in the solvent. In particular, the power storage device is preferably one in which the negative electrode is a columnar body containing a negative electrode active material, and the polymer film is formed on the outer peripheral surface of the negative electrode. The power storage device having a columnar electrode is preferable because of its structure, since it can further improve the energy density and input / output characteristics compared to a planar electrode.
[0019] Here, the power storage device may be, for example, an electric double layer capacitor, a hybrid capacitor, a pseudo electric double layer capacitor, a lithium secondary battery, a lithium ion battery, or the like. The term "room temperature" refers to 15°C to 25°C. The term "columnar" refers to a thickness that does not bend, as well as a thickness that is bendable and fibrous. The negative electrode may be columnar, and its cross section may be circular or polygonal. The positive electrode may be present around the negative electrode, or may be filled in the space between the negative electrodes. The power storage device may have a structure in which a plurality of negative electrodes are bound together in a state adjacent to the positive electrode via a polymer film. The secondary battery may contain an electrolyte in one or more of the negative electrode, the positive electrode, and the polymer film. The positive electrode and the negative electrode may have a current collecting member such as a current collecting wire embedded therein, or may not have the current collecting member. For ease of explanation, the following description will be given mainly as an example of a lithium secondary battery having a structure in which the negative electrode is a columnar body surrounded by a positive electrode, and in which lithium ions are used as the carrier.
[0020] Next, the electricity storage device disclosed in this embodiment will be described with reference to the drawings. FIG. 1 is a schematic diagram showing an example of an electricity storage device 10. FIG. 2 is a schematic diagram showing an example of an electricity storage device 10B having planar electrodes. As shown in FIG. 1, the electricity storage device 10 includes a negative electrode 11, a negative electrode current collector 12, a polymer film 20, a positive electrode 16, and a positive electrode current collector 17. This electricity storage device 10 includes a negative electrode 11 made of a columnar negative electrode active material, and a positive electrode 16 made of a positive electrode active material layer formed around the negative electrode 11 with a polymer film 20 interposed therebetween. This electricity storage device 10 has a structure in which a plurality of negative electrodes 11 are bound together with the polymer film 20 and the positive electrode 16 interposed therebetween. This electricity storage device 10 may also have a structure in which 50 or more negative electrodes 11 are bound together. The polymer film 20 has voids that can be confirmed in a secondary electron microscope image, and the average surface pore density of the voids is 0.1 pores / μm 2 Although the above is the case, the domain 21 may be formed on the surface.
[0021] The negative electrode 11 is a columnar material containing an active material. In this electricity storage device 10, a plurality of columnar negative electrodes are arranged in a predetermined direction. The outer circumference of the negative electrode 11, except for the end faces, faces the positive electrode 16 via the polymer film 20. For example, the negative electrode 11 may have a capacity of 1 / n of the negative electrode capacity of the entire cell, and n pieces of the negative electrode 11 may be connected in parallel to the negative electrode current collector 12. The diameter D of the cross section perpendicular to the longitudinal direction of the negative electrode 11 is preferably 10 μm or more, more preferably 15 μm or more, and may be 30 μm or more. The diameter D of the negative electrode 11 is preferably 800 μm or less, more preferably 500 μm or less, and may be 400 μm or less. When the diameter D is 10 μm or more, the strength of the electrode structure can be ensured, and stable charging and discharging can be performed. When the diameter D is 800 μm or less, the moving distance of the carrier ions is not too long, and high output performance can be obtained. In addition, when the diameter D is in the range of 10 to 500 μm, the energy density per unit volume can be increased. Alternatively, in this range, the moving distance of the carrier ions can be shortened, and charging and discharging can be performed with a larger current. The length of the columnar body in the longitudinal direction can be appropriately determined depending on the application of the secondary battery, and may be, for example, in the range of 20 mm to 200 mm. When the length of the columnar body is 20 mm or more, the battery capacity can be increased, and when it is 200 mm or less, the electric resistance of the negative electrode can be reduced, which is preferable. The negative electrode may contain a carbon material as a negative electrode active material. Examples of the carbon material include one or more of graphites, cokes, glassy carbons, non-graphitizable carbons, and pyrolytic carbons. Among these, graphites such as artificial graphite and natural graphite are preferable. In addition, the carbon fiber may have a graphite structure. For example, such carbon fibers are preferably those in which the crystals are oriented in the longitudinal direction, which is the fiber direction. In addition, it is preferable that the crystals are oriented radially from the center to the outer periphery when viewed in cross section in a direction perpendicular to the longitudinal direction (fiber direction). Alternatively, the columnar negative electrode may be one in which a composite oxide capable of absorbing and releasing carrier ions is formed into a columnar body.Examples of the composite oxide include lithium titanium composite oxide and lithium vanadium composite oxide. The negative electrode may have a conductive component formed on at least a part of its surface. The conductive component can further increase the conductivity. The conductive component is not particularly limited as long as it is a material with high conductivity, and may be, for example, a metal.
[0022] The negative electrode current collector 12 is a member having electrical conductivity, and the end face of the negative electrode 11 is electrically connected to the negative electrode current collector 12. 50 or more negative electrodes 11 may be connected in parallel to the negative electrode current collector 12. For example, the negative electrode current collector 12 may be made of carbon paper, aluminum, copper, titanium, stainless steel, nickel, iron, platinum, baked carbon, conductive polymer, conductive glass, or the like, and may also be made of aluminum or copper whose surface is treated with carbon, nickel, titanium, silver, platinum, gold, or the like for the purpose of improving adhesion, electrical conductivity, and oxidation (reduction) resistance. The shape of the negative electrode current collector 12 is not particularly limited as long as it can connect a plurality of negative electrodes 11, and examples thereof include plate-like, foil-like, film-like, sheet-like, net-like, punched or expanded, lath body, porous body, foam, and fiber group formation.
[0023] The polymer film 20 has ion conductivity for carrier ions (e.g., lithium ions) and insulates the negative electrode 11 from the positive electrode 16. As described above, the polymer film 20 is made of a resin capable of conducting lithium ions and / or a resin that retains an electrolyte capable of conducting lithium ions, has pores that can be confirmed in a secondary electron microscope image, and the average surface pore density of the pores is 0.1 pores / μm 2 The above is the case. The polymer film 20 may be coated on the surface of the negative electrode 11, or may be formed as a handleable free-standing film and then attached to the surface of the negative electrode 11. The polymer film 20 may contain the above-mentioned electrolyte that conducts ions, which are carriers.
[0024] The positive electrode 16 has a positive electrode active material and is formed on the outer periphery of the negative electrode 11 via a polymer film 20. The positive electrode 16 may be formed to have a hexagonal cross-sectional shape that includes the columnar negative electrode 11 when the power storage device 10 is produced (see FIG. 1). This shape is preferable because the positive electrode 16 is easily filled between the negative electrodes 11 when the negative electrodes 11 having the positive electrode active material formed on the outer periphery are bundled. The positive electrode 16 is not limited to having a hexagonal outer shape as long as it is present between a plurality of negative electrodes 11. The positive electrode 16 may be conductive in itself, and a current collecting member or the like may be omitted. The positive electrode 16 may be directly connected to the positive electrode current collector 17 at its end face, or may be connected to the positive electrode current collector over its entire side face. The positive electrode 16 may be formed, for example, by forming a polymer film 20 on the outer periphery of the negative electrode 11, and then applying a positive electrode composite material, which is the raw material of the positive electrode 16, to the outer periphery.
[0025] The positive electrode 16 includes a positive electrode active material. In the case where the positive electrode active material does not have electrical conductivity, for example, a conductive material having electrical conductivity may be mixed and molded. The positive electrode 16 may be, for example, a positive electrode active material, and if necessary, a conductive material and a binder mixed and molded. For example, the positive electrode active material may be a material capable of absorbing and releasing lithium, which is a carrier. For example, the positive electrode active material may be a compound having lithium and a transition metal, such as an oxide containing lithium and a transition metal element, or a phosphate compound containing lithium and a transition metal element. Specifically, a compound having a basic composition formula of Li (1-x) MnO2 (0≦x≦1, etc., same below) and Li (1-x) Lithium manganese composite oxide such as Mn2O4, with the basic composition formula Li (1-x) Lithium cobalt composite oxide with CoO2, etc., with the basic composition formula Li (1-x) Lithium nickel composite oxide such as NiO2, with the basic composition formula Li (1-x) Co a Ni b Mn c O2(a>0, b>0, c>0, a+b+c=1), Li (1-x) Co a Ni b Mn cLithium cobalt nickel manganese composite oxides such as O4 (0 < a < 1, 0 < b < 1, 1 ≤ c < 2, a + b + c = 2), lithium vanadium composite oxides with a basic composition formula such as LiV2O3, transition metal oxides with a basic composition formula such as V2O5, etc. can be used. Also, lithium iron phosphate compounds with a basic composition formula such as LiFePO4 can be used as the positive electrode active material. Among these, lithium cobalt nickel manganese composite oxides, for example, LiCo 1 / 3 Ni 1 / 3 Mn 1 / 3 O2 and LiNi 0.4 Co 0.3 Mn 0.3 O2, etc. are preferable. Note that the "basic composition formula" means that it may contain components of other elements, for example, Al, Mg, etc.
[0026] The conductive material contained in the positive electrode is not particularly limited as long as it is an electron conductive material that does not adversely affect the battery performance. For example, graphite such as natural graphite (scaly graphite, flaky graphite) or artificial graphite, acetylene black, carbon black, ketjen black, carbon whiskers, needle coke, carbon fibers, metals (copper, nickel, aluminum, silver, gold, etc.), etc. can be used as a mixture of one or more of these. The binder serves to connect and hold the active material particles and conductive material particles to maintain a predetermined shape. For example, polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVdF), fluorine-containing resins such as fluororubber, or thermoplastic resins such as polypropylene and polyethylene, ethylene propylene diene monomer (EPDM) rubber, sulfonated EPDM rubber, natural butyl rubber (NBR), etc. can be used alone or as a mixture of two or more. Also, aqueous binders such as cellulose-based or styrene butadiene rubber (SBR) aqueous dispersions can be used.
[0027] In the positive electrode 16, the content of the positive electrode active material is preferably higher, and is preferably 70% by mass or more, and more preferably 80% by mass or more, with respect to the total mass of the positive electrode 16. The content of the conductive material is preferably in the range of 0% by mass or more and 20% by mass or less, and more preferably in the range of 0% by mass or more and 10% by mass or less, with respect to the total mass of the positive electrode 16. In such a range, the decrease in the battery capacity can be suppressed and sufficient conductivity can be imparted. In addition, the content of the binder is preferably in the range of 0.1% by mass or more and 5% by mass or less, and more preferably in the range of 0.2% by mass or more and 3% by mass or less, with respect to the total mass of the positive electrode 16.
[0028] The positive electrode current collector 17 is a conductive member and is electrically connected to the positive electrode 16. End faces of 50 or more positive electrodes 16 are connected in parallel to the positive electrode current collector 17. The positive electrode current collector 17 may be made of the same material as the negative electrode current collector 12.
[0029] In this electricity storage device 10, the electrical conductivity (ionic conductivity) of the polymer film is preferably higher, but is preferably 0.1 mS / cm or more, more preferably 0.18 mS / cm or more, and even more preferably 0.2 mS / cm or more. If the ionic conductivity is higher, the discharge capacity can be increased. In addition, in this electricity storage device 10, the volumetric energy density is more preferably higher, for example, preferably 650 Wh / L or more, more preferably 830 Wh / L or more, and even more preferably 900 Wh / L or more. In this electricity storage device 10, the positive / negative electrode capacity ratio (negative electrode capacity / positive electrode capacity), which is the ratio of the capacity of the negative electrode active material to the capacity of the positive electrode active material, is preferably in the range of 1.0 to 1.5, more preferably 1.2 or less. The thickness of the positive electrode formed is appropriately set according to the diameter of the negative electrode and the positive / negative electrode capacity ratio, but may be, for example, in the range of 5 μm to 50 μm. The thickness of the positive electrode means, for example, the maximum thickness of the portion formed on the negative electrode.
[0030] (Method of manufacturing an electricity storage device) Next, a method for manufacturing an electric storage device will be described. Since this manufacturing method is a method for manufacturing the above-mentioned polymer film and electric storage device, the members and compounding ratios described in the above-mentioned polymer film and electric storage device are appropriately used. This manufacturing method may include a film forming step and a void forming step.
[0031] (film formation process) In this step, a process is performed to form a polymer film containing an additive solid by mixing an additive solid that is solid at room temperature and dissolves in a solvent with a resin capable of conducting lithium ions and / or a resin that holds an electrolyte capable of conducting lithium ions. The resin to be used may be one or more of polyvinylidene fluoride, a copolymer of polyvinylidene fluoride and hexafluoropropylene, polymethyl methacrylate, and a copolymer of polymethyl methacrylate and an acrylic polymer, among which a copolymer of polyvinylidene fluoride and hexafluoropropylene is preferred. The additive solid to be used may be lithium salts such as LiBOB, LiBFO, LiFSI, LiTFSI, and EC, among which LiBOB and LiFSI are preferred, and LiBOB is more preferred. The amount of the additive solid is, for example, preferably 10 parts by mass or more of the additive solid relative to 100 parts by mass of the resin, more preferably 30 parts by mass or more, and even more preferably 40 parts by mass or more. From the viewpoint of ensuring the insulation of the polymer film, the amount of the additive solid is preferably 100 parts by mass or less. The additive solid-containing polymer film may be formed directly on the negative electrode, or may be formed as a self-supporting additive solid-containing polymer film, and then the additive solid-containing polymer film may be attached to the negative electrode. The additive solid-containing polymer film may be formed, for example, by dissolving a resin in a solvent, adding an additive solid thereto, and adding a conductive material as necessary, and using the mixed solution to coat the negative electrode. The solvent for dissolving the resin may be appropriately selected depending on the resin, and examples thereof include N-methylpyrrolidone (NMP).
[0032] In this step, a positive electrode composite layer may be further formed on the surface of the additive solid-containing polymer film formed on the negative electrode. The positive electrode composite layer may be formed, for example, by adding a positive electrode active material, and if necessary, a conductive material and a binder, and further adding a solvent to form a positive electrode composite paste, and using this positive electrode composite paste. In addition, in this step, a plurality of negative electrodes on which a positive electrode composite layer has been formed may be bound to form an electrode structure.
[0033] (Void formation process) In this process, the polymer film containing the additive solid is placed between the positive and negative electrodes, and a solvent is added to dissolve the additive solid. This process creates spaces where the additive solid dissolves, and these spaces can be confirmed by secondary electron microscope images. The average surface pore density is 0.1 / μm 2 The above voids can be formed in the polymer film. The solvent for dissolving the additive solid is preferably the solvent for the electrolyte. In this way, the desired voids can be formed in the polymer film without containing any solvent other than the electrolyte.
[0034] The power storage device and polymer film described above in detail can further improve the input / output characteristics. The reason why such an effect is obtained is presumed to be as follows. For example, since this polymer film has sufficient voids, it has high conductivity, and thus it is possible to improve the input / output characteristics of the power storage device. In addition, when the additive solid contained in the polymer film is a lithium salt, the lithium ion concentration is high near the electrode, so it is possible to reduce the reaction resistance, which is presumed to contribute to improving the input / output characteristics. In addition, in a power storage device using an electrode of a columnar body having an active material, lithium ions can enter and exit the outer peripheral surface of the columnar body, so that the input / output characteristics can be improved and a high energy density can be achieved.
[0035] It goes without saying that the present disclosure is in no way limited to the above-described embodiment, and can be embodied in various forms as long as it falls within the technical scope of the present disclosure.
[0036] For example, in the above-described embodiment, the negative electrode and the positive electrode in the electricity storage device 10 do not include a current collecting member, but this is not particularly limited, and each electrode may have a current collecting member such as a current collecting wire embedded therein.
[0037] In the above-described embodiment, the electricity storage device 10 having an electrode structure in which the negative electrode 11 is laminated in a plurality of layers has been described, but the electricity storage device may have an electrode structure in which the negative electrode 11 is a single layer.
[0038] In the above-described embodiment, the carrier of the power storage device is lithium ion, but is not limited thereto, and may be alkali metal ion such as sodium ion or potassium ion, or group 2 element ion such as calcium ion or magnesium ion. The positive electrode active material may contain ions of the carrier. The electrolyte is a non-aqueous electrolyte, but may be an aqueous electrolyte.
[0039] In the above embodiment, the columnar negative electrode 11 is described as having a cylindrical shape, but is not limited thereto, and may have a polygonal prism shape such as a square prism or a hexagonal prism.
[0040] In the above-described embodiment, the positive electrode active material is a transition metal composite oxide, but is not particularly limited thereto, and may be, for example, a carbon material used in a capacitor. The carbon material is not particularly limited, but examples thereof include activated carbons, cokes, glassy carbons, graphites, non-graphitizable carbons, pyrolytic carbons, carbon fibers, carbon nanotubes, and polyacenes. Among these, activated carbons exhibiting a high specific surface area are preferred. Activated carbons as carbon materials have a specific surface area of 1000 m 2 / g or more, and 1500m 2 / g or more. 2 The specific surface area of this activated carbon is 3000 m2 for ease of preparation. 2 / g or less, and 2 / g or less is more preferable. It is considered that the positive electrode stores electricity by adsorbing and desorbing at least one of anions and cations contained in the ionically conductive medium, but it may also store electricity by inserting and desorbing at least one of anions and cations contained in the ionically conductive medium.
[0041] In the above-described embodiment, the electricity storage device 10 is a columnar electrode structure, but is not particularly limited thereto. Fig. 2 is a schematic diagram showing an example of an electricity storage device 10B having a laminated structure. This electricity storage device 10B has a negative electrode 11B having a negative electrode active material layer 13 formed on a negative electrode current collector 12B, a positive electrode 16B having a positive electrode active material layer 18 formed on a positive electrode current collector 17B, and a polymer film 20B disposed between the negative electrode 11B and the positive electrode 16B, and has a laminated structure. This polymer film 20B has voids that can be confirmed in a secondary electron microscope image, and the average surface pore density of the voids is 0.1 pores / μm 2 The above is the case. When the surface of the polymer film 20B is observed, domains 21 are formed. Even in such an electricity storage device 10B having a stacked structure, it is possible to obtain better information on the input / output characteristics. EXAMPLES
[0042] Specific examples of fabricating the above-mentioned electricity storage device will be described below as experimental examples. Experimental Examples 1 to 5 correspond to examples of the present disclosure, and Experimental Examples 6 and 7 correspond to comparative examples.
[0043] (Experimental Example 1) (Preparation of polymer films) To a solution in which vinylidene fluoride-hexafluoropropylene copolymer (PVdF-HFP) as a resin was dissolved in N-methylpyrrolidone (NMP), lithium bis(oxalato)borate (LiBOB) was added as an additive solid lithium salt that is a solid at room temperature and dissolves in a solvent in an amount of 50 parts by mass per 100 parts by mass of PVdF-HFP, and mixed until uniformly dissolved. The resulting solution was dropped into a polytetrafluoroethylene petri dish, and used as the polymer film of Experimental Example 1. The film thickness of the polymer films in Experimental Examples 1 to 7 was 10 μm.
[0044] (Experimental Examples 2 to 5) A polymer film of Experimental Example 2 was prepared in the same manner as Experimental Example 1, except that lithium bis(fluorosulfonyl)imide (LiFSI) was added to the resin as a lithium salt that is a solid at room temperature and dissolves in a solvent. A polymer film of Experimental Example 3 was prepared in the same manner as Experimental Example 1, except that ethylene carbonate (EC) was added to the resin as an additive solid that is a solid at room temperature and dissolves in a solvent. A polymer film of Experimental Example 4 was prepared in the same manner as Experimental Example 1, except that the amount of LiBOB added was 30 parts by mass relative to 100 parts by mass of the resin. A polymer film of Experimental Example 5 was prepared in the same manner as Experimental Example 1, except that the amount of LiBOB added was 10 parts by mass relative to 100 parts by mass of the resin.
[0045] (Experimental Examples 6 and 7) A polymer membrane of Experimental Example 6 was prepared in the same manner as in Experimental Example 1, except that no additive solid that was a solid at room temperature and dissolved in the solvent was added. A polymer membrane of Experimental Example 7 was prepared in the same manner as in Experimental Example 1, except that alumina (Al2O3: model number AA-03, median particle size 0.44 μm, manufactured by Sumitomo Chemical) was added as an additive solid that was not dissolved in the solvent.
[0046] (Evaluation of polymer films) (1) SEM Observation The obtained polymer film was subjected to SEM observation and X-ray diffraction measurement, and the electrolyte retention rate and electrical conductivity (ionic conductivity) were measured. In the SEM observation, the prepared polymer film was washed with a solvent (dimethyl carbonate) and dried, and then the surface of the polymer film was observed using a scanning electron microscope (S-3600N manufactured by Hitachi High-Technologies Corporation). The SEM observation was performed at a magnification of 1000 to 5000 times. In addition, the SEM image was binarized by image analysis using Nanosystem's NS2K-Lt software, and the number of black areas present in the image was counted as voids. The binarization threshold was adjusted according to the brightness of the entire image, and was set to 88 in Figure 3D, 126 in Figure 3E, and 126 in Figure 3F. Based on this count, the unit area (μm 2 Average surface pore density (pores / μm 2 ) was sought.
[0047] (2) X-ray diffraction measurement The polymer film prepared above was washed with a solvent (dimethyl carbonate) and dried, after which X-ray diffraction measurements were performed on the polymer film. The measurements were performed using an X-ray diffractometer (Rigaku, Ultima IV) using CuKα radiation (wavelength 1.54051 Å) as radiation. A graphite single crystal monochromator was used to monochromatize the X-rays, and the measurements were performed with an applied voltage of 40 kV and a current of 30 mA. The measurements were recorded at a scanning speed of 5° / min and an angle range of 2θ = 10° to 50°.
[0048] (3) Electrolyte retention rate The polymer membrane prepared above was washed with a solvent (dimethyl carbonate) and dried, after which it was immersed in a mixed solvent of ethylene carbonate (EC), dimethyl carbonate (DMC), and ethyl methyl carbonate (EMC) in a volume ratio of 30 / 40 / 30, and the liquid retention rate (mass%) was calculated from the mass change before and after immersion per unit volume. The value of Experimental Example 6 was set to 100, and the values of the other Experimental Examples were normalized.
[0049] (4) Electrical conductivity (ionic conductivity) The polymer membrane thus prepared was washed with a solvent (dimethyl carbonate), dried, and sandwiched between two Ni electrodes to prepare a measurement cell, and the conductivity of the polymer membrane was evaluated by an AC impedance method. The measurement cell thus prepared was measured using an AC impedance analyzer (Agilent 4294A) at an open circuit voltage with an amplitude of ±500 mV, a frequency range of 1 Hz to 100 kHz, and a measurement temperature of 25°C, and the ionic conductivity (mS / cm) was calculated from the resistance between the current collectors. The value of Experimental Example 6 was set to 100, and the values of the other Experimental Examples were normalized.
[0050] (Fabrication of electricity storage devices) The resin / additive solid solution prepared above was coated on a cylindrical carbon rod having a diameter of 160 μm and a length of 6.0 cm as a negative electrode by a dipping method, and then dried to form a polymer film with a thickness of 7 μm. Next, the positive electrode active material (LiNi 0.5 Co 0.2 Mn 0.3 A positive electrode composite paste was prepared by mixing acetylene black (HS-100 manufactured by Denka Co., Ltd.) as a conductive material, acetylene black (HS-100 manufactured by Denka Co., Ltd.) as a conductive material, and polyvinylidene fluoride (PVdF) as a binder in a mass ratio of 90:6:4, to which N-methylpyrrolidone was added. The positive electrode composite paste was dip-coated onto the polymer film-coated carbon rod to form a positive electrode composite layer so that the amount of the positive electrode composite per unit length of the carbon rod was 0.35 mg / cm. Thereafter, the positive electrode composite layer was pressed to a predetermined density (2.5 g / cm) using a hydrostatic press. 3 ) was pressed. Then, both ends of the positive electrode / polymer film-coated carbon rod were connected to Ni tabs via Ag paste, and the positive electrode composite layer was connected to an Al tab via an Al foil, and the resultant was inserted into an Al laminate cell. A nonaqueous electrolyte was injected into this laminate cell and sealed to produce an evaluation cell. The nonaqueous electrolyte used was a mixed solvent of ethylene carbonate (EC), dimethyl carbonate (DMC), and ethyl methyl carbonate (EMC) in a volume ratio of 30 / 40 / 30, in which LiPF6 was dissolved at a concentration of 1M. By injecting this nonaqueous electrolyte, the added solid in the polymer film was dissolved in the solvent of the nonaqueous electrolyte, and voids were generated in the polymer film.
[0051] (IV resistance measurement) After the conditioning charge and discharge of the evaluation cell prepared above, IV measurement was performed to obtain the resistance value from the current-voltage slope. The conditioning charge and discharge was performed with an end voltage of 2.0 to 4.1 V, a current value of 0.05 C, and a test temperature of 25°C.
[0052] (Results and Discussion) FIG. 3 shows SEM photographs of Experimental Examples 1, 2, and 6, FIG. 6A shows an image of Experimental Example 1 at 5,000 times magnification, FIG. 6B shows an image of Experimental Example 4 at 5,000 times magnification, FIG. 6C shows an image of Experimental Example 1 at 100 times magnification, and FIG. 6D shows an image of Experimental Example 4 at 100 times magnification. FIG. 3 shows SEM photographs (FIGS. 3A to 3C) and binarized images (FIGS. 3D to 3F) of Experimental Examples 1, 2, and 6. FIG. 4 shows the results of X-ray diffraction measurement of Experimental Examples 1 and 6. FIG. 5 shows the results of X-ray diffraction measurement of Experimental Examples 2 and 6. Table 1 shows the type of added solid, the amount added (parts by mass) relative to 100 parts by mass of resin, and the surface pore density (pores / μm 2 ), the presence or absence of an X-ray diffraction peak near 2θ=26°, the relative liquid retention rate (-), the relative electrical conductivity (-) and the relative IV resistance (-) are also shown. Here, the liquid retention rate, electrical conductivity and IV resistance are normalized by setting the value of Experimental Example 6, which did not contain any added solid, to 100 and the values of the other Experimental Examples.
[0053] As shown in Figure 3, the surface of the polymer film of Experimental Example 6, which did not contain any added solid, was relatively flat, whereas the surfaces of the polymer films of Experimental Examples 1 and 2, which were prepared by adding LiBOB or LiFSI as the added solid, had countless fine voids distributed thereon. Also, as shown in Table 1, in Experimental Example 6, the average surface pore density of the voids was 0.1 pores / μm 2 In contrast, in Experimental Examples 1 to 5, the average surface pore density of the voids was 0.1 / μm 2 It was confirmed that the structure had a greater number of voids on the surface. The average surface pore density is preferably as high as 0.15 / μm 2 More preferably, 1.0 particles / μm or more 2It was found that the above is even more preferable. In addition, when a region separated by a boundary that can be clearly identified in an SEM image is considered to be a domain, the domain size was 80 nm in Experimental Example 1 and 320 nm in Experimental Example 2. In addition, when a domain has, for example, a "scale-like domain that is connected to the neighboring domain", the boundary is defined and recognized as a separate domain. It was presumed that if the domain size is 1 μm or less, the average surface pore density will be good. It was also presumed that, like the domain size, the resin surface preferably has roughness of 1 μm or less on average. Furthermore, it was also characterized in that the resin surface has pores of 300 nm or less on average.
[0054] As shown in Figures 4 and 5, in the polymer film of Experimental Example 6, which did not contain any added solid, the peaks derived from the PVdF-HFP crystal structure were clearly observed, whereas in the polymer films of Experimental Examples 1 and 2, which were prepared with the addition of LiBOB or LiFSI, the peak intensity was significantly reduced, suggesting a decrease in crystallinity. In particular, in Experimental Example 6, a 021 peak derived from the PVdF-HFP crystal structure was detected at 2θ = 25° to 28° (near 26°), but this disappeared in the polymer film containing the added solid.
[0055] In addition, as shown in Table 1, it was revealed that in Experimental Examples 1 to 5, in which an additive solid that is a solid at room temperature and dissolves in a solvent was added, the properties of the electrolyte retention rate, electrical conductivity, and IV resistance were improved compared to Experimental Example 6, in which no additive solid was added. It was presumed that, for example, when components such as LiBOB, LiFSI, and EC were dissolved in the polymer solution, the crystallinity of the polymer film obtained by casting was reduced, and voids were introduced, thereby improving the electrolyte retention rate. In addition, since this effect was not expressed when particles that do not dissolve in the electrolyte, such as Al2O3 in Experimental Example 7, were added, it was presumed that the added additive solid dissolved in the electrolyte promoted the impregnation of the electrolyte into the polymer film, and further contributed to an increase in the amount of electrolyte retention in the polymer film, resulting in an improvement in electrical conductivity. In particular, it was presumed that the lithium ion conductivity could be further improved in the case where a lithium salt was added, since the lithium ion concentration was increased by dissolving the lithium salt in the electrolyte. It was found that lithium salt is more preferable as the additive solid, and LiBOB is even more preferable. It was also found that the amount of the additive is preferably 10 parts by mass or more, more preferably 30 parts by mass or more, and may be 50 parts by mass or more, relative to 100 parts by mass of the resin.
[0056] [Table 1]
[0057] It goes without saying that the present disclosure is in no way limited to the above-described embodiments, and can be embodied in various forms as long as they fall within the technical scope of the present disclosure. [Explanation of symbols]
[0058] 10,10B: electricity storage device; 11,11B: negative electrode; 12,12B: negative electrode current collector; 13: negative electrode active material layer; 16,16B: positive electrode; 17,17B: positive electrode current collector; 18: positive electrode active material layer; 20,20B: polymer film; 21: domain.
Claims
1. A polymer film used to be interposed between a positive electrode and a negative electrode of an electricity storage device, the polymer film being interposed between the positive electrode and the negative electrode and having voids formed therein by adding a solvent thereto, The battery is made of a resin that holds an electrolyte capable of conducting lithium ions, and is filled with an additive solid that is solid at room temperature and dissolves in a solvent; The added solid is at least one of lithium salt lithium bis(oxalato)borate, lithium salt lithium bis(fluorosulfonyl)imide, and ethylene carbonate, and the average surface pore density of voids that can be confirmed in a secondary electron microscope image formed by adding the solvent is 0.1 pores / μm 2 2.5 pieces / μm or more 2 is as follows: The resin is at least one of polyvinylidene fluoride, a copolymer of vinylidene fluoride and hexafluoropropylene, polymethyl methacrylate, and a copolymer of methyl methacrylate and an acrylic monomer.
2. The average surface pore density is 0.15 pores / μm 2 The polymer film according to claim 1 .
3. The average surface pore density is 1.0 pores / μm 2 The polymer film according to claim 1 .
4. The polymer film according to any one of claims 1 to 3, wherein the resin is a copolymer of vinylidene fluoride and hexafluoropropylene, and does not show a diffraction peak in the range of 2θ = 25° or more and 28° or less in X-ray diffraction measurement using a Cu tube.
5. A positive electrode and A negative electrode; The polymer film according to any one of claims 1 to 4, which is interposed between the positive electrode and the negative electrode and conducts lithium ions; A power storage device comprising:
6. The electricity storage device according to claim 5 , further comprising an electrolyte solution containing a solvent for at least one of the positive electrode, the negative electrode, and the polymer film.
7. The electricity storage device according to claim 5 , wherein an additive solid that is solid at room temperature and soluble in a solvent and that has been filled in the polymer film is dissolved in the electrolyte solution.
8. the negative electrode is a columnar body containing a negative electrode active material, The electricity storage device according to any one of claims 5 to 7, wherein the polymer film is formed on an outer peripheral surface of the negative electrode.
9. A method for producing an electricity storage device having a positive electrode and a negative electrode, comprising the steps of: A film formation step of mixing an additive solid that is solid at room temperature and soluble in a solvent into a resin that retains an electrolyte solution capable of conducting lithium ions to form an additive solid-containing polymer film; The polymer film containing the additive solid is interposed between the positive electrode and the negative electrode, and a solvent is added to dissolve the additive solid. The space formed by dissolving the additive solid is a space that can be confirmed by a secondary electron microscope image and has an average surface pore density of 0.1 pores / μm 2 and a void forming step of forming voids in the polymer film, the voids being equal to or larger than 2.5 voids / μm2 or smaller, The additive solid is at least one of lithium salts, such as lithium bis(oxalato)borate, lithium salts, such as lithium bis(fluorosulfonyl)imide, and ethylene carbonate; The method for producing an electricity storage device, wherein the resin is at least one of polyvinylidene fluoride, a copolymer of vinylidene fluoride and hexafluoropropylene, polymethyl methacrylate, and a copolymer of methyl methacrylate and an acrylic monomer.
10. In the void forming step, the average surface pore density is 0.15 / μm 2 The method for producing an electricity storage device according to claim 9 , wherein the voids described above are formed in a polymer film.
11. In the void forming step, the average surface pore density is 1.0 pores / μm 2 The method for producing an electricity storage device according to claim 9 , wherein the voids described above are formed in a polymer film.
12. The method for producing an electricity storage device according to any one of claims 9 to 11, wherein a size of a domain formed on a surface of the polymer film that is identifiable in a secondary electron microscope image is 1 μm or less, and the polymer film has the void between the domains.
13. The method for producing an electricity storage device according to any one of claims 9 to 12, wherein an additive solid that is solid at room temperature and soluble in a solvent and that has been filled in the polymer film is dissolved in the electrolyte solution.
14. the negative electrode is a columnar body containing a negative electrode active material, The method for producing an electricity storage device according to any one of claims 9 to 13, wherein the polymer film is formed on an outer peripheral surface of the negative electrode.
Citation Information
Patent Citations
Producing method for porous film, and porous film
JP2004175104A
Separator with heat-resistant insulating layer, and nonaqueous electrolyte secondary battery
JP2009087889A
Integrated electrode separator assembly for lithium-ion batteries
JP2015533453A
Lithium ion battery
JP2017084765A
Method for producing resin film for non-aqueous electrolyte secondary battery and resin film for non-aqueous electrolyte secondary battery
WO2014002937A1