Double-sided laminated paper and paper cups

The double-sided laminated paper with thermoplastic resin layers and a cellulose nanofiber barrier layer addresses the brittleness and cracking issues of conventional cellulose nanofiber layers, providing enhanced bending resistance and gas barrier properties for packaging materials.

JP7562959B2Active Publication Date: 2024-10-08TOPPAN HOLDINGS INC
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2020035174
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-03-02
Publication Date
2024-10-08
Estimated Expiration
2040-03-02

AI Technical Summary

Technical Problem

Conventional cellulose nanofiber-based barrier layers are brittle and prone to cracking under stress, making them unsuitable for use in packaging materials, and paper-based substrates exacerbate this issue due to surface unevenness and susceptibility to paper fibers.

Method used

A double-sided laminated paper structure is developed, featuring a thermoplastic resin layer on both sides of a base paper with a cellulose nanofiber barrier layer, which enhances bending resistance and reduces surface unevenness, using specific cellulose nanofiber and water-soluble polymer ratios to improve adhesion and flexibility.

Benefits of technology

The laminated paper exhibits excellent gas barrier properties and bending resistance, maintaining integrity during processing and use, even when filled with contents, by minimizing cracks and gaps, thus ensuring effective gas barrier performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007562959000002
    Figure 0007562959000002
  • Figure 0007562959000003
    Figure 0007562959000003
  • Figure 0007562959000004
    Figure 0007562959000004
Patent Text Reader

Abstract

To provide a double-sided laminated paper in which crack is hardly caused in a barrier layer containing cellulose nanofibers when processing is performed or a content is filled, namely a double-sided laminated paper including a barrier layer having a high bending resistance, and a paper cup composed of the double-sided laminated paper.SOLUTION: There is provided a double-sided laminated paper 100 in which a thermoplastic resin layer 20 is laminated on both sides of a barrier paper 10 having a base paper 1 and a barrier layer 2 containing cellulose nanofibers formed on the base paper 1, wherein an oxygen permeability at 30°C and 40% RH is 50 cc / m2 day or less after bending for 2 seconds on a mandrel having a diameter of 8 mm or more where a surface on which the barrier layer 2 is formed is faced outside, in accordance with JIS K5600-5-1:1999 Testing methods for paints Part 5: Mechanical property of film Section 1: Bend test (cylindrical mandrel).SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a double-sided laminated paper for packaging food and the like, and a paper cup made of the double-sided laminated paper. [Background technology]

[0002] In the field of packaging materials for food and other products, gas barrier properties that block gases such as oxygen from permeating the packaging material are required to protect the contents.

[0003] Conventionally, aluminum and polyvinylidene chloride, which are less affected by temperature and humidity, have been used as gas barrier materials. However, when these materials are incinerated, aluminum has a problem of clogging the exhaust port and inside the furnace, reducing the incineration efficiency, and polyvinylidene chloride may have a problem of generating dioxins. Therefore, there is a demand to switch gas barrier materials to materials with less environmental impact. For example, as described in Patent Document 1, it is being promoted to switch a part of polyvinylidene chloride to polyvinyl alcohol and ethylene-vinyl alcohol copolymers that do not contain aluminum or chlorine, even though they are materials made from the same fossil resources. In addition, it is expected that petroleum-derived materials will be switched to biomass materials in the future. Conventionally, petroleum-derived resin films such as polyethylene terephthalate (PET) have been widely used as the substrate of gas barrier materials. However, it is expected that the substrate of gas barrier materials will be switched to paper, which is a representative biomass material, and the use of paper for packaging materials is progressing.

[0004] As a new gas barrier material, cellulose nanofibers have been attracting attention. In addition to being biodegradable, cellulose nanofibers are also excellent in physical properties such as gas barrier properties, strength, elastic modulus, dimensional stability, heat resistance, and crystallinity. Therefore, cellulose nanofibers are expected to be applied to functional materials. As cellulose-based materials, for example, cellulose nanofibers obtained by dispersing cellulose fibers generated by oxidation reaction using a 2,2,6,6-tetramethyl-1-piperidine-N-oxy radical (hereinafter referred to as "TEMPO") catalyst as described in Patent Document 2 and Patent Document 3, cellulose nanofibers obtained by introducing carboxymethyl groups into glucose units and then dispersing them as described in Patent Document 4, and cellulose nanofibers obtained by mechanical fiberization after enzyme treatment and alkali treatment as described in Patent Document 5 are known. By coating and laminating these cellulose nanofibers on a substrate, a gas barrier material capable of suppressing oxygen permeability can be obtained. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 7-164591 [Patent Document 2] JP 2008-308802 A [Patent Document 3] JP 2008-1728 A [Patent Document 4] JP 2013-185122 A [Patent Document 5] Japanese Patent Application Publication No. 6-10288 Summary of the Invention [Problem to be solved by the invention]

[0006] However, a barrier layer containing cellulose nanofibers is hard and brittle even when applied to a substrate and formed into a film, and is therefore easily cracked. Furthermore, when paper is used as the substrate, the surface is more uneven than that of a resin substrate, and is more susceptible to the effects of paper fibers. Therefore, the barrier layer containing cellulose nanofibers according to the conventional technology cannot withstand the stress of bending and folding when processed and molded into packaging materials, etc., and cracks occur, making it difficult to maintain the barrier properties. Furthermore, even after processing and molding into a packaging container, it cannot withstand the weight when contents are placed inside, and cracks may occur in the barrier layer other than the folded parts, making it difficult to maintain the gas barrier properties.

[0007] The present invention has been made in consideration of the above-mentioned problems, and aims to provide double-sided laminated paper in which cracks are less likely to occur in the barrier layer containing cellulose nanofibers when processed or filled with contents, i.e., double-sided laminated paper containing a barrier layer with high bending resistance, and a paper cup made of this double-sided laminated paper. [Means for solving the problem]

[0008] In order to solve the above problems, a double-sided laminated paper according to one embodiment of the present invention is a double-sided laminated paper in which a thermoplastic resin layer is laminated on both sides of a barrier paper having a base paper and a barrier layer containing cellulose nanofibers formed on the base paper, and the double-sided laminated paper has an oxygen transmission rate of 50cc / m2 at 30°C and 40% RH after bending for 2 seconds with a mandrel of 8 mm or more in diameter with the surface on which the barrier layer is formed facing outward, in accordance with JIS K5600-5-1:1999 "General test methods for paints - Part 5: Mechanical properties of coating films - Section 1: Bending resistance (cylindrical mandrel method)". 2 It is a double-sided laminated paper characterized by having a shelf life of less than 10 days. Effect of the Invention

[0009] According to one aspect of the present invention, a double-sided laminated paper is prepared by laminating thermoplastic resin layers on both sides of a barrier paper having a barrier layer containing cellulose nanofibers formed on a base paper, and the double-sided laminated paper has a barrier layer that is less susceptible to the unevenness of the base paper surface, has a small gap between the substrate (base paper) and the barrier layer, and has excellent flex resistance. Therefore, it is possible to provide a double-sided laminated paper that has excellent gas barrier properties and excellent flex resistance that can withstand processing and molding, and a paper cup made of the double-sided laminated paper. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a cross-sectional view showing a schematic structure of a barrier paper according to an embodiment of the present invention. [Diagram 2] 1 is a cross-sectional view showing a schematic structure of a double-sided laminated paper according to an embodiment of the present invention. [Diagram 3] FIG. 1 is a perspective view showing a typical shape of a paper cup according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, an embodiment to which the present invention is applied will be described in detail with reference to the drawings. Note that the drawings used in the following description are for explaining the configuration of the embodiment of the present invention, and the size, thickness, dimensions, etc. of each part shown in the drawings may differ from the dimensional relationship of the actual laminate. "Barrier paper" FIG. 1 is a cross-sectional view showing a schematic structure of a barrier paper according to an embodiment of the present invention. As shown in FIG. 1, the barrier paper (laminate) 10 according to this embodiment comprises a base paper 1 and a barrier layer 2 containing cellulose nanofibers formed on the base paper 1, i.e., on one surface 1a of the base paper 1. The base paper 1 is not particularly limited and can be appropriately selected from printing paper and packaging paper depending on the application. Examples of the base paper 1 include glassine paper, parchment paper, high-grade printing paper, medium-grade printing paper, low-grade printing paper, thin printing paper, colored wood-free paper, art paper, coated paper, kraft paper, cardboard base paper, coated cardboard, ivory paper, card paper, and cup base paper.

[0012] The base paper 1 has a basis weight of 400 g / m 2 It is preferable that the basis weight is 30 g / m or less. 2 More than 400g / m 2 More preferably, the basis weight is within the range of 150 g / m 2 More than 400g / m 2 More preferably, the basis weight is within the range of 180 g / m 2 More than 400g / m 2 Most preferably, it is within the following range: The basis weight of base paper 1 is 400 g / m 2 If the basis weight of the base paper 1 is less than 400 g / m, the stress applied to the barrier layer 2 when the barrier paper 10 is bent will not be too large, and the stress will not cause cracks in the barrier layer 2 or reduce the gas barrier properties. 2 If it is less than this, the increase in cost can be suppressed.

[0013] In addition, when the barrier paper 10 is used for normal packaging purposes, the basis weight of the base paper 1 is 180 g / m 2 The basis weight of the base paper 1 is preferably 180 g / m or more. 2 When the basis weight of the base paper 1 is 30 g / m or more, sufficient strength can be maintained for normal packaging applications. 2 If the basis weight is 150 g / m or more, the strength of the base paper 1 can be maintained to a level that does not cause problems in use for normal packaging purposes. 2 If the strength is equal to or greater than this, the strength can be maintained to a degree that does not cause any problems even if the material is used multiple times in normal packaging applications. Natural cellulose fibers are used as the raw material for the cellulose nanofibers contained in the barrier layer 2. Examples of natural cellulose fibers include various wood pulps obtained from coniferous trees and broad-leaved trees, non-wood pulps obtained from kenaf, bagasse, straw, bamboo, cotton, seaweed, and the like, cellulose fibers obtained from sea squirts, and cellulose fibers produced by microorganisms.

[0014] The cellulose nanofibers used in the present invention are preferably those that maintain at least a part of their fibrous shape even when dispersed in water, i.e., those that allow fibrous substances to be observed when an aqueous dispersion of cellulose nanofibers is observed under an electron microscope, and those that allow cellulose type I crystal peaks to be observed when the cellulose nanofibers are measured by X-ray diffraction.

[0015] The cellulose fibers used may be chemically treated as necessary. The chemical treatment method is not particularly limited, but examples include a method in which cellulose fibers are oxidized and carboxylated using the above-mentioned TEMPO as a catalyst and an oxidizing agent such as sodium hypochlorite or a bromide such as sodium bromide while adjusting the pH. This method produces cellulose fibers in which the hydroxyl group at the C6 position of cellulose is carboxylated, i.e., cellulose fibers having a carboxy group at the C6 position of cellulose. This carboxylated cellulose fiber swells due to increased electrostatic repulsion between the cellulose fibers, and a dispersion of cellulose nanofibers can be prepared by mechanical treatment with low energy input.

[0016] An example of a chemical treatment method is a method of carboxymethylating cellulose fibers. An example of this chemical treatment method is as follows. Sodium hydroxide is added and mixed as a mercerizing agent to a solvent containing cellulose fibers to perform a mercerization treatment of the cellulose fibers, and then a carboxymethylating agent is added in an amount of 0.05 to 10.0 times by mole per glucose residue to perform an etherification reaction, thereby obtaining cellulose fibers with carboxymethyl groups introduced therein. These cellulose fibers with carboxymethyl groups introduced therein can be easily made into cellulose nanofibers because electrostatic repulsion occurs between the cellulose fibers due to the carboxymethyl groups. Further, as another chemical treatment method, for example, the cellulose fibers can be subjected to a pretreatment such as phosphorylation, phosphorous oxidation, enzyme treatment, chemical treatment (alkali treatment, acid treatment, swelling chemical treatment), ozone treatment, etc. The material for the barrier layer 2 can be cellulose nanofibers obtained by washing pretreated cellulose fibers or by pulverizing the pretreatment solution into a suspension.

[0017] A method for producing the barrier paper 10 according to this embodiment will be described with reference to FIG. First, the cellulose fibers are refined (defibrated) (cellulose fiber refinement process). The method for pulverizing the cellulose fibers is not particularly limited, and examples thereof include mechanical treatment using a dispersing device such as a high-pressure homogenizer, an ultrasonic homogenizer, grinder grinding, freeze grinding, or a media mill. Furthermore, the cellulose fibers may be subjected to the above-mentioned chemical treatment as a pre-processing step prior to the mechanical treatment. By controlling the degree of mechanical treatment or chemical treatment as desired, it is possible to obtain cellulose nanofibers with the desired fiber shape and particle diameter (fiber diameter).

[0018] The cellulose nanofibers contained in the barrier layer 2 preferably have an average fiber length in the range of 100 nm to 30 μm, more preferably in the range of 100 nm to 10 μm. It is difficult and unrealistic to manufacture cellulose nanofibers with an average fiber length less than 100 nm (short), even by combining chemical pretreatment and dispersion treatment. When the barrier layer 2 is formed, cellulose nanofibers with an average fiber length greater than 30 μm (long) may have poor smoothness and may affect barrier properties, such as fibers protruding from the barrier layer 2 due to the presence of coarse fibers in the layer. In addition, cellulose nanofibers with an average fiber length greater than 30 μm (long) are not preferable because fine gaps are likely to be formed between the coarse paper fibers and the barrier layer 2 when the barrier layer 2 is formed on the base paper 1, reducing adhesion to the base paper 1. These fiber lengths can be measured, for example, by observing the shape using an apparatus such as an AFM (atomic force microscope) or an SEM (scanning electron microscope), measuring the fiber lengths of a large number of arbitrary samples, and taking the average, or by measuring the particle size using a particle size distribution meter for the coating liquid, etc. In this embodiment, the measured values ​​from the former observation were used.

[0019] In the barrier paper 10 according to this embodiment, the barrier layer 2 preferably contains a water-soluble polymer that is compatible with cellulose nanofibers, as a material capable of filling the gaps between the cellulose nanofibers contained in the barrier layer 2. A barrier layer 2 containing cellulose nanofibers and a water-soluble polymer, for example, inhibits the intrusion and penetration of deterioration factors such as water vapor and dirt, and as a result tends to reduce the deterioration of gas barrier properties due to bending, etc.

[0020] Examples of the water-soluble polymer that can be used include polyvinyl alcohol (PVA), ethylene-vinyl alcohol copolymer, carboxymethyl cellulose (CMC), polyacrylic acid, polyacrylamide, polyethyleneimine, polyethylene oxide, starch, pectin, and alginic acid. These water-soluble polymers have, for example, excellent film-forming properties, transparency, flexibility, and good compatibility with cellulose fibers, and therefore can easily fill the gaps between the cellulose nanofibers to form a barrier layer 2 that has both strength and adhesion. Polyvinyl alcohol (PVA) is obtained by saponifying polyvinyl acetate, and includes so-called partially saponified PVA in which 10% to 20% of acetate groups remain, and fully saponified PVA in which only 1% to 2% of acetate groups remain.

[0021] When a water-soluble polymer is used, the mass ratio ((A) / (B)) of the cellulose nanofibers (A) to the water-soluble polymer (B) in the coating liquid for forming the barrier layer 2 is preferably 20 / 80 to 80 / 20. When the mass ratio of the water-soluble polymer (B) is 20 or more, the gaps between the cellulose nanofibers can be filled by the water-soluble polymer (B), which imparts flexibility to the barrier layer 2 and improves bending resistance. On the other hand, when the mass ratio of the water-soluble polymer (B) is 80 or less, the reinforcing effect of the cellulose nanofibers makes it difficult for defects to occur in the barrier layer 2. In addition, the thickening effect of the cellulose nanofibers makes it difficult for the coating liquid to become the barrier layer 2 to penetrate into the base paper 1, which can suppress a decrease in the film-forming properties of the barrier layer 2. The mass ratio ((A) / (B)) of the cellulose nanofibers (A) to the water-soluble polymer (B) in the coating liquid described above is the mass ratio ((A) / (B)) of the cellulose nanofibers (A) to the water-soluble polymer (B) in the barrier layer 2. In other words, the content of cellulose nanofibers in the barrier layer 2 is within the range of 20% by mass to 80% by mass.

[0022] Next, the coating liquid containing the cellulose nanofibers and water-soluble polymer obtained in the above-mentioned process is applied to one side 1a of the base paper 1 to form a coating film made of the coating liquid on one side 1a of the base paper 1, and then the coating film is dried to form the barrier layer 2 (barrier layer formation process). This results in a barrier paper 10 having a base paper 1 and a barrier layer 2 containing cellulose nanofibers formed on one surface 1a of the base paper 1. There is no particular limitation on the method for applying the coating liquid to one surface 1a of the base paper 1, and any known coating method can be used. Examples of the coating method include methods using a coating device such as a roll coater, a reverse roll coater, a gravure coater, a microgravure coater, a knife coater, a bar coater, a wire bar coater, a die coater, or a dip coater.

[0023] Methods for drying the coating film formed by applying the above-mentioned coating liquid to one surface 1a of the base paper 1 include, for example, natural drying, air drying, hot air drying, UV drying, hot roll drying, and infrared irradiation. The drying temperature is preferably within the range of 100° C. to 180° C. If the drying temperature is 100° C. or higher, the moisture in the coating film is removed, increasing the number of hydrogen bonds between the cellulose nanofibers, increasing the cohesive strength of the barrier layer 2, and improving the flex resistance. On the other hand, if the drying temperature is 180° C. or lower, the barrier layer 2 can be prevented from deteriorating and discoloring due to heat.

[0024] The coating weight of the barrier layer 2 is 1.4 g / m2 in terms of dry mass. 2 More than 30.0g / m 2 It is preferable that the range is 2.0 g / m 2 More than 5.0g / m 2 It is more preferable that the content is within the following range: The coating weight of the barrier layer 2 is 1.4 g / m2 in dry weight. 2 If this is the case, even if the barrier layer 2 is affected by the unevenness of the surface of the base paper 1, a sufficient amount of the barrier layer 2 is formed on the surface of the base paper 1, making it difficult for defects to occur in the barrier layer 2 and improving the gas barrier properties of the barrier layer 2. In other words, the coating amount of the barrier layer 2 is 1.4 g / m2 in dry mass. 2 If the coating weight of the barrier layer 2 is 30.0 g / m2 or more, the coating weight is less likely to be affected by the unevenness of the surface of the base paper 1, even if the base paper 1 is generally used as a packaging container material, and defects tend not to occur in the barrier layer 2. This makes it possible to improve the gas barrier properties of the barrier layer 2. The coating weight of the barrier layer 2 is 30.0 g / m2 in terms of dry mass. 2In this embodiment, the surface irregularities of the surface 1a of the base paper 1 on which the barrier layer 2 is to be coated preferably have an arithmetic mean roughness Ra in the range of 0.5 μm to 100.0 μm.

[0025] Double-sided laminated paper After forming a barrier layer 2 on a base paper 1, layers made of a thermoplastic resin (thermoplastic resin layers) 20 can be formed on both sides of the barrier paper 10 to produce a double-sided laminated paper 100. This double-sided laminated paper 100 will be described below. FIG. 2 is a cross-sectional view showing a schematic structure of a double-sided laminate paper according to an embodiment of the present invention. The double-sided laminated paper 100 of this embodiment is formed by laminating thermoplastic resin layers 20 on both sides of barrier paper 10, which has base paper 1 and a barrier layer 2 formed on one side 1a of the base paper 1, as shown in FIG.

[0026] Methods for forming the thermoplastic resin layer 20 on both sides of the barrier paper 10 include, for example, wet lamination, dry lamination, solventless lamination, thermal lamination, and melt extrusion lamination. The thermoplastic resin layer 20 may be formed on the entire surface or part of the substrate (barrier paper 10) as necessary. The material of the thermoplastic resin layer 20 is not particularly limited, and is preferably a polyolefin resin. The polyolefin resin contained in the thermoplastic resin layer 20 can be selected from, for example, polyethylene-based resins such as low-density polyethylene resin (LDPE), medium-density polyethylene resin (MDPE), high-density polyethylene resin (HDPE), and linear low-density polyethylene resin (LLDPE), polypropylene-based resins such as polypropylene resin, propylene-ethylene random copolymer, and propylene-ethylene block copolymer, with linear low-density polyethylene resin (LLDPE) being preferred in terms of workability, processability, and economy. In particular, in the laminate (double-sided laminated paper 100) of this embodiment, the thermoplastic resin layer 20 has a melt mass flow rate (MFR) in the range of 3.0 g / 10 min to 8.0 g / 10 min, and the density of the thermoplastic resin layer 20 is 910 kg / m 3 More than 930kg / m 3 It is preferable to use LLDPE having a melt mass flow rate and density within the following ranges for the thermoplastic resin layer 20. By using LLDPE having a melt mass flow rate and density within these numerical ranges, the barrier layer 2 is resistant to stress during molding and is less likely to crack, so that sufficient barrier properties can be maintained even after molding. The thickness of the thermoplastic resin layer 20 is preferably within a range of 10 μm to 100 μm. When the thickness of the thermoplastic resin layer 20 is within this range, the layer can reliably withstand the stress during molding and the barrier layer 2 is less likely to crack, so that sufficient barrier properties can be maintained even after molding.

[0027] When forming the thermoplastic resin layer 20 on the barrier paper 10, in order to improve non-adhesion, the barrier layer 2, which is a fiber layer, may be subjected to a known surface treatment such as corona treatment, ozone treatment, plasma treatment, glow discharge treatment, or oxidation treatment using chemicals. In particular, when a thermoplastic resin layer 20 such as a polyethylene resin is formed on the barrier layer 2, which is a layer containing cellulose nanofibers, the anchor effect of the barrier layer 2 containing cellulose nanofibers is reduced, and the adhesive strength between the layers may decrease. In such cases, for example, a primer coat layer, an anchor coat layer, an adhesive layer, or the like may be arbitrarily formed between the barrier layer 2 and the thermoplastic resin layer 20.

[0028] Generally, in double-sided laminated paper such as that shown in Figure 2, when the barrier layer is thick, it has low bending resistance and tends to crack easily. However, the barrier layer 2 containing cellulose nanofibers of this embodiment has improved film strength due to the reinforcing effect of the cellulose nanofibers. In particular, when the coating film thickness is thicker than the fiber length of the cellulose nanofibers, the reinforcing effect of the cellulose nanofibers is efficiently exerted. This is because the cellulose nanofibers in the coating film can be uniformly dispersed within the coating film, and a smooth barrier layer 2 can be formed without protruding from the coating surface.

[0029] The double-sided laminated paper 100 according to the present embodiment has an oxygen permeability of 50 cc / m2 at 30°C and 40% RH after bending the paper around a mandrel with a diameter of 8 mm or more with the surface on which the barrier layer 2 is formed facing outward, in accordance with JIS K5600-5-1:1999 "General test methods for paints - Part 5: Mechanical properties of coatings - Section 1: Bending resistance (cylindrical mandrel method)". 2 ·day or less is preferable, and 10cc / m 2 It is preferable that the time is 10-24 hours or less. The coating weight of the barrier layer 2 is 1.4 g / m2 in dry weight. 2 If this is the case, the oxygen permeability at 30°C and 40% RH after bending with a mandrel with a diameter of 8 mm or more is 50 cc / m 2 ·day or less, 2.0g / m 2 If it is more than 10cc / m 2 There is an increasing tendency for the number of days or less to be If the oxygen permeability after bending is within the above range, the double-sided laminated paper 100 can exhibit good gas barrier properties even after being processed and molded into, for example, a paper cup or the like. The above-mentioned mandrel has a diameter of 8 mm, and when bent, it can apply a stress similar to that in the processing step, making it possible to perform a substitute evaluation of the deterioration of the barrier layer 2 in the actual processing step. Also, if a mandrel of less than 8 mm is used, the stress applied to the barrier layer 2 is too strong, causing extreme cracks in the barrier layer 2, and is therefore not appropriate for evaluation.

[0030] By forming a heat-sealable thermoplastic resin layer 20, a double-sided laminated paper 100 can be molded and used as a paper packaging material. It can also be imparted with stain resistance and liquid resistance against highly permeable liquids. It is particularly suitable as a packaging material for acidic contents, such as dairy products, lactic acid bacteria drinks, fermented milk, and dressings. A printed layer (not shown) may be formed as necessary before the formation of the thermoplastic resin layer 20. The printed layer may be formed on the barrier layer 2 containing cellulose nanofibers, or on the other surface 1b (the surface not in contact with the barrier layer 2) of the base paper 1, which is the substrate, depending on the application, purpose, and process. In terms of exerting functionality, it is preferable for the paper packaging material for forming a paper packaging container to have the barrier layer 2, which imparts functionality, as the inside IS of the paper packaging container such as a paper cup, and the other surface 1b of the barrier paper 10, which is the substrate, as the printed surface, i.e., the outside OS of the paper packaging container such as a paper cup, as the paper packaging material for forming a paper packaging container.

[0031] "Paper cup" FIG. 3 is a perspective view showing a typical shape of a paper cup according to an embodiment of the present invention. The paper cup 200 according to this embodiment is made of the barrier paper 10 according to this embodiment, with the barrier layer 2 being disposed on the inside (inner surface side) IS of the paper cup. The paper cup 200 according to this embodiment (see FIG. 3) is made of the barrier paper 10 according to this embodiment, and has excellent gas barrier properties and flex resistance because the barrier layer 2 is located on the inside IS of the paper cup. As the barrier layer 2 is located on the inside IS of the paper cup, even if an object collides with the outside of the paper cup during molding or transportation, the impact received by the barrier layer 2 can be reduced by the thermoplastic resin layer 20 and the base paper. This reduces the degree to which defects occur in the barrier layer 2, and maintains the gas barrier properties. The paper cup 200 according to this embodiment can be formed from a double-sided laminated paper 100 (see FIG. 2) in which a layer made of thermoplastic resin (thermoplastic resin layer) 20 is laminated onto the barrier paper 10 of this embodiment. As shown in FIG. 2, the thermoplastic resin layer 20 is formed on the barrier layer 2 of the barrier paper 10 and on the base paper 1.

[0032] To make the paper cup 200, first, a body material and a bottom member are made by punching out the double-sided laminated paper 100 with a die. Next, the body material and the bottom member are molded into a cup shape using a cup forming machine. Next, a separately prepared lid is peelably sealed and the paper cup 200 is obtained. In this embodiment, the configuration of the paper cup 200 formed from the double-sided laminated paper 100 has been described, but the present invention is not limited to this. As long as the packaging container is formed from the double-sided laminated paper 100, its shape is not important. The present invention is not limited to the above-described embodiment, and various modifications are possible without departing from the spirit of the present invention. Furthermore, the specific configurations and materials of each part are not limited to those exemplified in the above-described embodiment, and can be modified as appropriate.

[0033] [Example] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. [Preparation method 1 of cellulose nanofiber dispersion] 5.00 g (bone dry) of bleached, unbeaten conifer-derived kraft pulp (brightness 85%) was added to 500 ml of an aqueous solution containing 39 mg (0.05 mmol per 1 g of bone dry cellulose) of TEMPO (Sigma Aldrich) and 514 mg (1.0 mmol per 1 g of bone dry cellulose), and the mixture was stirred until the pulp was uniformly dispersed. Aqueous sodium hypochlorite solution was added to the reaction system so that the sodium hypochlorite concentration was 5.5 mmol / g, and the oxidation reaction was started at room temperature. The pH of the system decreased during the reaction, but 3M aqueous sodium hydroxide solution was gradually added to adjust the pH to 10. The reaction was terminated when the sodium hypochlorite was consumed and the pH of the system did not change. The reaction mixture was filtered through a glass filter, and then washed with a sufficient amount of water and filtered twice to obtain water-impregnated oxidized cellulose fibers with a solid content of 10% by mass. The pulp yield was 90%, the oxidation reaction took 90 minutes, and the carboxyl group content was 1.68 mmol / g. The oxidized pulp obtained in the above process was adjusted to a solid content of 1% with water and treated 10 times with a high-pressure homogenizer (20°C, 150 MPa) to obtain a dispersion of cellulose nanofibers.

[0034] [Preparation method 2 of cellulose nanofiber dispersion] Into a mixer capable of mixing pulp, 200 g (dry mass) of bleached, unbeaten kraft pulp derived from softwood (brightness 85%) and 111 g (dry mass) of sodium hydroxide were added, and water was added so that the pulp solids content became 20% (w / v). After stirring for 30 minutes at 30° C., 216 g (effective ingredient equivalent) of sodium monochloroacetate was added. After stirring for 30 minutes, the temperature was raised to 70° C. and stirring was continued for 1 hour. The reaction product was then removed, neutralized and washed to obtain a carboxymethylated pulp with a degree of carboxymethyl substitution per glucose unit of 0.25. The carboxymethylated pulp was then adjusted to 1% solids with water and stirred for approximately 60 minutes using a high-speed rotating mixer to obtain a dispersion of cellulose nanofibers.

[0035] [Comparative preparation method 1 for dispersion containing cellulose fibers (Comparative preparation method 1)] A cloudy dispersion containing cellulose fibers was obtained in the same manner as in Preparation Method 1, except that the ion-exchanged water containing pulp was treated once using a high-pressure homogenizer. [Comparative preparation method 2 for dispersion containing cellulose fiber (Comparative preparation method 2)] The dispersion liquid containing cellulose fibers obtained by Preparation Method 2 was subjected to a dispersion treatment for about 5 minutes using a high-speed rotating mixer to obtain a cloudy dispersion liquid containing cellulose fibers.

[0036] [Rating 1] [Evaluation of cellulose nanofibers and cellulose fibers] The average fiber length of the cellulose nanofibers and cellulose fibers obtained by Preparation Methods 1 and 2 and Comparative Preparation Methods 1 and 2 was measured. Each dispersion was diluted to a concentration of 0.001%, applied to mica, and the fiber morphology was observed with an AFM. The average of the widths of 30 randomly selected individual fibers was calculated and used as the average fiber length. The results are shown below. Preparation method 1...1.5μm Preparation method 2...3.0μm Comparative preparation method 1...40μm Comparative preparation method 2...50μm

[0037] [Preparation of polyvinyl alcohol aqueous solution] 5 g of commercially available polyvinyl alcohol (product name: PVA-124, manufactured by Kuraray Co., Ltd.) was weighed out into a beaker and pure water was added to make up to 500 g. This was stirred while being heated to 100° C. to dissolve the polyvinyl alcohol in the pure water, thereby preparing an aqueous solution of polyvinyl alcohol with a solid content of 1%. [Preparation of carboxymethylcellulose aqueous solution] 5 g of commercially available carboxymethylcellulose (product name: F10LC, manufactured by Nippon Paper Industries Co., Ltd.) was weighed out into a beaker and pure water was added to make up to 500 g. This was stirred while being heated to 100° C. to dissolve the carboxymethylcellulose in the pure water, thereby preparing an aqueous solution of carboxymethylcellulose with a solid content of 1%.

[0038] [Preparation method of coating solutions 1 to 4] 100 g of each of the dispersions obtained by Preparation Methods 1 and 2 was collected, and 100 g of the above aqueous polyvinyl alcohol solution was added to each dispersion. The mixture was stirred with a stirrer for 30 minutes to prepare Coating Liquids 1 and 2. 100 g of each of the dispersions obtained in Preparation Methods 1 and 2 was collected, and 100 g of the above carboxymethylcellulose aqueous solution was added to each dispersion. The mixture was stirred with a stirrer for 30 minutes to prepare Coating Liquids 3 and 4. [Preparation of Coating Fluids 5 and 6] 160 g of each of the dispersions obtained by Preparation Methods 1 and 2 was collected, and 40 g of the above aqueous polyvinyl alcohol solution was added to each dispersion. The mixture was stirred with a stirrer for 30 minutes to prepare Coating Liquids 5 and 6.

[0039] [Preparation method of coating solutions 7 and 8] 40 g of each of the dispersions obtained by Preparation Methods 1 and 2 was collected, and 160 g of the above aqueous polyvinyl alcohol solution was added to each dispersion. The mixture was stirred with a stirrer for 30 minutes to prepare Coating Solutions 7 and 8. [Preparation of Coating Fluids 9 and 10] 180 g of each of the dispersions obtained in Preparation Methods 1 and 2 was collected, and 20 g of the above aqueous polyvinyl alcohol solution was added to each dispersion. The mixture was stirred with a stirrer for 30 minutes to prepare Coating Liquids 9 and 10.

[0040] [Preparation method of coating liquids 11 and 12] 20 g of each of the dispersions obtained by Preparation Methods 1 and 2 was collected, and 180 g of the above aqueous polyvinyl alcohol solution was added to each dispersion. The mixture was stirred with a stirrer for 30 minutes to prepare Coating Liquids 11 and 12. [Preparation method of coating liquids 13 and 14] 100 g of each of the dispersions obtained in Comparative Preparation Methods 1 and 2 was collected, and 100 g of the above aqueous polyvinyl alcohol solution was added to each dispersion. The mixture was stirred with a stirrer for 30 minutes to prepare Coating Solutions 13 and 14.

[0041] [Preparation of barrier paper in Examples 1 to 12] Cup base paper (grammage 280g / m 2 Coating Solutions 1 to 8 were applied onto a base material (manufactured by Nippon Paper Industries Co., Ltd.) by bar coating to form a coating film, which was then dried at 150°C for 10 minutes to obtain a barrier paper in which a barrier layer was formed on the cup base paper base material. The coating weight of the barrier layer is shown in Table 1. [Preparation of barrier paper for Comparative Examples 1 to 10] Cup base paper (grammage 280g / m 2Coating Liquids 1 to 4 and Coating Liquids 9 to 14 were applied onto a base material (manufactured by Nippon Paper Industries Co., Ltd.) by bar coating to form a coating film, which was then dried at 150°C for 10 minutes to obtain a barrier paper in which a barrier layer was formed on the cup base paper base material. The coating weight of the barrier layer is shown in Table 1.

[0042] [Double-sided laminated paper production] Next, a heat seal layer (thermoplastic resin layer) was laminated to both sides of the barrier paper by extrusion lamination to a thickness of 30 μm. Polyethylene LC600A (Japan Polyethylene Co., Ltd.) was used as the heat seal layer (thermoplastic resin layer). [Rating 2] The flex resistance of the barrier papers obtained in Examples 1 to 12 and Comparative Examples 1 to 10 was evaluated according to the following method.

[0043] [Flexibility test] The double-sided laminated papers obtained in Examples 1 to 12 and Comparative Examples 1 to 10 were conditioned for at least 6 hours in an environment of 23°C and 50% RH, and then wrapped around a mandrel with a diameter of 8 mm with the side on which the barrier layer was formed facing outward and bent in accordance with JIS K5600-5-1:1999 "General test methods for paints - Part 5: Mechanical properties of coatings - Section 1: Bending resistance (cylindrical mandrel method)". [Oxygen permeability measurement (isobaric method)] The oxygen permeability (cc / m) of the barrier papers obtained in Examples 1 to 12 and Comparative Examples 1 to 10 before and after the above-mentioned bending resistance test was 2 ·day) was measured according to the following method. The oxygen permeability of the barrier paper was measured in an atmosphere of 30°C and 40% RH using an oxygen permeability measuring device MOCON (product name: OX-TRAN2 / 21, manufactured by Modern Controls). The measurement results are shown in Table 1.

[0044] [Table 1]

[0045] From the results in Table 1, the double-sided laminated papers of Examples 1 to 12 have a thickness of 1.4 g / m 2 Because the film has a barrier layer with a coating amount of this magnitude, it was found that the deterioration of oxygen permeability (the rate of change in oxygen permeability before and after bending) was small, and that the gas barrier properties were maintained even after bending. It was also found that by using a mixing ratio of cellulose nanofibers to water-soluble polymer of 20 / 80 to 80 / 20, the gaps between the cellulose nanofibers can be filled, imparting flexibility to the barrier layer and improving its bending resistance, while allowing the barrier layer to be laminated with good film-forming properties. In contrast, in Comparative Examples 1, 4, 7, and 8, the barrier layer was thin and therefore unable to conform to the irregularities on the paper surface. Although the gas barrier property was good before bending, cracks occurred in the barrier layer when the paper was bent, and the gas barrier property was significantly reduced.

[0046] In addition, in Comparative Examples 2 and 5, the amount of water-soluble polymer was small, so the gaps between the cellulose nanofibers in the barrier layer could not be filled, and cracks occurred in the barrier layer when the layer was bent, which is thought to have deteriorated the oxygen permeability. In Comparative Examples 3 and 6, the amount of water-soluble polymer was large, and the viscosity of the coating liquid was low, so the barrier layer soaked into the base paper before drying, which is likely to cause defects, and this is thought to have resulted in poor initial oxygen permeability. In Comparative Examples 9 and 10, the cellulose fibers were too large, so when the barrier layer was formed on the substrate (base paper), fine gaps were formed between the cellulose fibers and the coarse paper fibers, which is thought to have resulted in poor initial oxygen permeability.

[0047] From the above results, it can be seen that the barrier layer is 1.4 g / m 2 If the fiber length of the cellulose nanofibers contained is 100 nm or more and 30 μm or less, and the content of the cellulose nanofibers in the barrier layer is 20% by mass or more and 80% by mass or less, the gas barrier property of the double-sided laminated paper having the barrier layer is good and the deterioration of the gas barrier property after bending is small. Therefore, even if the barrier paper is used to form a packaging container, the packaging container has sufficient strength and can withstand practical use. [Industrial Applicability]

[0048] The barrier paper of the present invention has excellent gas barrier properties and flex resistance, and can therefore be used in a variety of fields, such as containers and packaging materials for food, toiletries, pharmaceuticals, medical products, and electronic components. [Explanation of symbols]

[0049] 1. Paper substrate (base paper) 2. Barrier layer 10. Barrier paper 20...Resin layer (thermoplastic resin layer) 100···Sheet material (double-sided laminated paper) 200··Paper cups IS...Inside of a paper cup OS...Outside of the paper cup

Claims

1. A double-sided laminated paper in which a thermoplastic resin layer is laminated on both sides of a laminate having a base paper and a barrier layer containing cellulose nanofibers formed on the base paper, The coating weight of the barrier layer is 1.4 g / m2 in dry weight. 2 30.0g / m or more 2 Within the following range: The content of the cellulose nanofibers in the barrier layer is within the range of 20% by mass or more and 80% by mass or less, The barrier layer further comprises a water-soluble polymer, the water-soluble polymer is an ethylene-vinyl alcohol copolymer, polyacrylic acid, polyacrylamide, polyethyleneimine, polyethylene oxide, starch, pectin, or alginic acid; The fiber length of the cellulose nanofiber in the barrier layer is within a range of 1.5 μm or more and 3.0 μm or less, The base paper has a basis weight of 400 g / m 2 or less; The thickness of the thermoplastic resin layer is in the range of 10 μm or more and 100 μm or less, the thermoplastic resin layer comprises a polyolefin resin, the coating amount of the barrier layer is within a range of 2.0 g / m 2 or more and 5.0 g / m 2 or less in terms of dry mass, the surface unevenness of the surface of the base paper on which the barrier layer is to be coated is in a range of 0.5 μm or more and 100.0 μm or less in arithmetic mean roughness Ra; The thickness of the barrier layer is greater than the fiber length of the cellulose nanofibers, According to JIS K5600-5-1:1999 "General test methods for coatings - Part 5: Mechanical properties of coatings - Section 1: Bending resistance (cylindrical mandrel method)", the oxygen transmission rate at 30°C and 40% RH after bending for 2 seconds with a mandrel of 8 mm diameter with the surface on which the barrier layer is formed facing outward is 50 cc / m 2 - Double-sided laminated paper characterized by having a shelf life of less than 1 day.

2. A paper cup, characterized in that the barrier layer of the double-sided laminated paper according to claim 1 is disposed on the inner side of the base paper.

Citation Information

Patent Citations

  • Production of fine fibrous cellulose

    JP1994010288A

  • Laminated film of gas barrier properties

    JP1995164591A

  • Fine cellulose fiber

    JP2008001728A

  • Method for producing cellulose nanofibers

    JP2008308802A

  • Gas barrier packaging material

    JP2012011651A