Anti-fogging resin composition and laminated film

A laminated film with a polyvinyl alcohol-based antifogging resin composition addresses the challenge of high adhesion by enabling easy removal and recycling, maintaining effective antifogging properties.

JP7563105B2Active Publication Date: 2024-10-08MITSUBISHI CHEM CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020175657
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-10-19
Publication Date
2024-10-08
Estimated Expiration
2040-10-19

AI Technical Summary

Technical Problem

Existing anti-fogging resin layers on polyester films are difficult to peel off due to high adhesion, making recycling challenging, and they lose antifogging properties during recycling processes.

Method used

A laminated film with an antifogging resin composition containing polyvinyl alcohol resin, an acid catalyst, and an ammonium base-containing compound, which can be easily removed after use by dissolving in solvents or peeling off, maintaining antifogging properties during use.

Benefits of technology

The laminated film achieves good antifogging performance during use and allows for easy recycling by removing the resin layer, enhancing industrial utility and sustainability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007563105000001
    Figure 0007563105000001
  • Figure 0007563105000002
    Figure 0007563105000002
  • Figure 0007563105000003
    Figure 0007563105000003
Patent Text Reader

Abstract

To provide a laminate film that has high anti-fogging performance during its use, and allows an anti-fogging resin layer to be removed for recycling a base film after its use, and an anti-fogging resin composition forming the anti-fogging resin layer.SOLUTION: An anti-fogging resin composition contains (A) a polyvinyl alcohol resin with a degree of saponification of 50-99 mol% and with an average degree of polymerization of 200 or more and 1800 or less and also contains (B) an acid catalyst and (C) at least one selected from ammonium salt group-containing compounds. A laminate film has, on at least one side of a base film, an anti-fogging resin layer formed from the anti-fogging resin composition.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an anti-fogging resin composition and a laminate film having a resin layer formed from the resin composition. [Background technology]

[0002] Polyester films have excellent properties such as mechanical strength, dimensional stability, flatness, heat resistance, chemical resistance, and optical properties, and also have excellent cost performance, and therefore are used in a variety of applications.

[0003] Anti-fog films that have been given anti-fog properties have been proposed as applications for polyester films. Anti-fog films that use surfactants are known, but there are problems with their use, such as the fact that the surfactant system exerts anti-fog properties by bleeding out, making the surface of the anti-fog resin layer sticky, or that the anti-fog resin layer easily falls off when rubbed. In response to this, an anti-fogging biaxially oriented polyester film has been proposed that has a coating layer formed from polyvinyl alcohol and an isobutylene-maleic anhydride copolymer as a biaxially oriented polyester film having excellent anti-fogging properties (see Patent Document 1). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 5-310976 Summary of the Invention [Problem to be solved by the invention]

[0005] The anti-fog resin layer described in Patent Document 1 has good anti-fog properties, but the anti-fog resin layer has high adhesion to the base film, making it difficult to peel off the anti-fog resin layer, and thus posing a problem in terms of recyclability. That is, although a suitable level of anti-fog properties is necessary during use, when considering recycling of the polyester film, it may be desirable to quickly remove the anti-fog resin layer after use and reuse the film. Therefore, there has been a need for a laminate film having an anti-fogging resin layer that has a suitable anti-fogging property during use and yet has good recyclability. The present invention has been made in consideration of the above-mentioned circumstances, and an object of the present invention is to provide a laminate film that has good anti-fogging performance during use and from which the anti-fogging resin layer can be peeled off after use to recycle the base film, and an anti-fogging resin composition that constitutes the anti-fogging resin layer. [Means for solving the problem]

[0006] In view of the above-mentioned circumstances, the present inventors have conducted extensive research and found that the above-mentioned problems can be easily solved by using an anti-fog resin composition having a specific composition and a laminate film having an anti-fog resin layer formed from the resin composition, and have completed the present invention. That is, the present invention provides the following items [1] to

[21] .

[0007] [1] An anti-fogging resin composition comprising (A) a polyvinyl alcohol-based resin having a degree of saponification of 50 to 99 mol% and an average degree of polymerization of 200 or more and 1,800 or less, and comprising at least one selected from (B) an acid catalyst and (C) an ammonium base-containing compound. [2] An anti-fogging resin composition comprising (A') a modified polyvinyl alcohol resin and at least one member selected from the group consisting of (B) an acid catalyst and (C) an ammonium base-containing compound. [3] The anti-fogging resin composition according to the above [1] or [2], further comprising (D) a crosslinking agent. [4] The anti-fogging resin composition according to the above [1] or [2], wherein the content of the (B) component in the anti-fogging resin composition is 10% by mass or less, and the content of the (C) component is 30% by mass or less. [5] The anti-fogging resin composition according to the above [3], wherein the content of the component (D) is 20 mass % or less. [6] A laminate film comprising an anti-fog resin layer formed on at least one surface of a substrate film from the anti-fog resin composition according to any one of the above [1] to [5]. [7] The laminate film according to the above [6], wherein the difference between the average water droplet contact angle 20 to 60 seconds after a water droplet is dropped on the surface of the anti-fog resin layer and the average advancing contact angle 20 to 60 seconds after the liquid is discharged by the expansion method (advancing contact angle - water droplet contact angle) is 1° or more. [8] The laminate film according to the above [6] or [7], wherein a contact angle of water dropped on the surface of the anti-fogging resin layer after 60 seconds is 35° or less. [9] The laminate film according to any one of the above [6] to [8], wherein the anti-fogging resin layer is exposed to a water bath at 40° C. for 1 minute and then evaluated for anti-fogging property as rank 2 or higher. Rank 2: A water film formed and blurred the image, but visibility through the film was good.

[10] The laminate film according to any one of the above [6] to [9], which has an anti-fogging property evaluation of rank 2 or higher after a water immersion treatment (immersion at 23° C. for 1 minute).

[11] The laminate film according to any one of the above [6] to

[10] , wherein after immersion in water at 23° C. for 1 hour, the coating remaining rate (%) of the anti-fogging resin layer is 55% or less.

[12] The laminate film according to any one of the above [6] to

[11] , wherein the base film is a polyester film.

[13] The laminate film according to any one of the above [6] to

[12] , wherein the base film is a polyester film that is unstretched or stretched at least uniaxially.

[14] The laminate film according to any one of the above [6] to

[13] , wherein the anti-fogging resin layer has a thickness (after drying) of 0.01 μm to 1 μm.

[15] The laminate film according to any one of the above [6] to

[14] , further comprising a functional layer on the opposite side to the anti-fogging resin layer.

[16] The laminate film described in

[15] above, wherein the functional layer is a visibility improving layer.

[17] The laminate film according to the above

[16] , wherein the visibility improving layer is a resin layer formed from a resin composition containing a fluorine-containing compound and a crosslinking agent.

[18] A method for using a laminate film according to any one of the above [6] to

[17] , which comprises treating the laminate film with water and / or an alcohol-based solvent and then reusing the laminate film.

[19] The anti-fogging resin composition according to any one of the above [1] to [5], which is for a face shield.

[20] The laminate film according to any one of [6] to

[17] above, which is for a face shield.

[21] The use as described in

[18] above as a face shield. Effect of the Invention

[0008] According to the present invention, it is possible to provide a laminate film which has good anti-fogging properties and good recyclability, and which is of great industrial utility. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] An example of an embodiment of the present invention will be described in detail below. However, the present invention is not limited to the embodiment described below, and can be modified as desired without departing from the gist of the present invention.

[0010] [Anti-fog resin composition] The anti-fogging resin composition of the present invention is characterized by containing (A) a polyvinyl alcohol-based resin having a degree of saponification of 50 to 99 mol% and an average degree of polymerization of 200 or more and 1800 or less, and containing at least one member selected from (B) an acid catalyst and (C) an ammonium base-containing compound. By providing an anti-fogging resin layer formed from such a resin composition on at least one surface of a substrate film, it is possible to provide a laminate film that has excellent anti-fogging properties and allows easy recycling of the substrate film. The anti-fogging resin composition of the present invention contains (A) a polyvinyl alcohol resin as an essential component, and (B) an acid catalyst and / or (C) an ammonium base-containing compound. Therefore, the composition may be a combination of (A) component and (B) component, or a combination of (A) component and (C) component. The composition may also contain all of (A), (B) and (C) components.

[0011] (A) Polyvinyl alcohol resin Polyvinyl alcohol resins (hereinafter sometimes abbreviated as PVA resins) are resins mainly composed of vinyl alcohol structural units, obtained by saponifying polyvinyl ester resins obtained by polymerizing vinyl ester monomers, and are composed of vinyl alcohol structural units and vinyl ester structural units corresponding to the degree of saponification.

[0012] The saponification degree of the PVA resin in the present invention is 50 to 99 mol%. If the saponification degree of the PVA resin is less than 50 mol%, it is difficult to obtain the desired anti-fogging performance. On the other hand, if the saponification degree exceeds 99 mol%, the stability of the anti-fogging resin composition tends to decrease, and the recyclability may be poor due to low water solubility. From the above viewpoints, the saponification degree of the PVA resin is preferably 50 to 95 mol%, more preferably 50 to 88 mol%. The saponification degree of the PVA resin is measured in accordance with JIS K 6726.

[0013] The average degree of polymerization of the PVA-based resin is 200 to 1800, more preferably 300 to 1500, and even more preferably 500 to 1200. When the average degree of polymerization of the PVA-based resin is below the lower limit, it is difficult to form a continuous coating of the anti-fogging resin layer. On the other hand, when the average degree of polymerization is above the upper limit, the viscosity of the anti-fogging resin composition is high, and coating streaks, coating unevenness, etc. tend to easily occur. The average degree of polymerization of the PVA resin is measured in accordance with JIS K 6726.

[0014] The PVA resin can be obtained, for example, by saponifying a polyvinyl ester polymer obtained by polymerizing a vinyl ester monomer. Examples of vinyl ester monomers include vinyl formate, vinyl acetate, vinyl propionate, vinyl valerate, vinyl butyrate, vinyl isobutyrate, vinyl pivalate, vinyl caprate, vinyl laurate, vinyl stearate, vinyl benzoate, and vinyl versatate, with vinyl acetate being preferred. The PVA-based resin may be an unmodified polyvinyl alcohol resin or a modified polyvinyl alcohol resin, with the modified polyvinyl alcohol resin being preferred.

[0015] The anti-fogging resin composition of the present invention may be an anti-fogging resin composition containing (A') a modified polyvinyl alcohol resin and at least one selected from (B) an acid catalyst and (C) an ammonium base-containing compound. The average polymerization degree of the modified polyvinyl alcohol resin is not particularly limited, but is preferably from 200 to 1800, more preferably from 300 to 1500, and even more preferably from 500 to 1200. The saponification degree is also not particularly limited, but is preferably from 50 to 99 mol%, more preferably from 50 to 95 mol%, and even more preferably from 50 to 88 mol%.

[0016] (A') Modified polyvinyl alcohol resin In the present invention, the modified polyvinyl alcohol resin may be one obtained by copolymerizing the vinyl ester monomer with a monomer having copolymerizability. Examples of the copolymerizable monomer include olefins such as ethylene, propylene, isobutylene, α-octene, α-dodecene, and α-octadecene; hydroxyl-containing α-olefins such as 3-buten-1-ol, 4-penten-1-ol, 5-hexen-1-ol, and 3,4-dihydroxy-1-butene, and derivatives thereof such as acylated products; acetoacetyl-containing monomers such as vinyl acetoacetate and acetoacetoxyalkyl (meth)acrylate; acrylic acid, methacrylic acid, crotonic acid, maleic acid, Unsaturated acids such as maleic anhydride, itaconic acid, undecylenic acid, and other carboxylic acids, their salts (sodium salts, potassium salts, and the like), monoesters, or dialkyl esters; polyoxyethylene (meth)allyl ether, polyoxyethylene (meth)acrylamide, polyoxypropylene (meth)acrylamide, polyoxyethylene (meth)acrylate, polyoxypropylene (meth)acrylate, polyoxyethylene (1-(meth)acrylamide-1,1-dimethylpropyl) ester, Polyoxyalkylene group-containing monomers such as polyoxyethylene vinyl ether, polyoxypropylene vinyl ether, polyoxyethylene allylamine, polyoxypropylene allylamine, polyoxyethylene vinylamine, and polyoxypropylene vinylamine; cationic group-containing monomers such as N-acrylamidomethyl trimethyl ammonium chloride, N-acrylamidoethyl trimethyl ammonium chloride, N-acrylamidopropyl trimethyl ammonium chloride, 2-acryloxyethyl trimethyl ammonium chloride, 2-methacryloxyethyl trimethyl ammonium chloride, 2-hydroxy-3-methacryloyloxypropyl trimethyl ammonium chloride, allyl trimethyl ammonium chloride, methallyl trimethyl ammonium chloride, 3-butene trimethyl ammonium chloride, dimethyl diallyl ammonium chloride, and diethyl diallyl ammonium chloride; nitriles such as acrylonitrile and methacrylonitrile;amides such as diacetone acrylamide, acrylamide, and methacrylamide; olefin sulfonic acids or salts thereof such as ethylene sulfonic acid, allyl sulfonic acid, and methallyl sulfonic acid; alkyl vinyl ethers; vinyl compounds such as dimethylallyl vinyl ketone, N-vinyl pyrrolidone, vinyl chloride, vinyl ethylene carbonate, 2,2-dialkyl-4-vinyl-1,3-dioxolane, and glycerin monoallyl ether; substituted vinyl acetates such as isopropenyl acetate and 1-methoxyvinyl acetate; and hydroxymethylvinylidene diacetates such as vinylidene chloride, 1,4-diacetoxy-2-butene, 1,4-dihydroxy-2-butene, vinylene carbonate, 1,3-diacetoxy-2-methylenepropane, 1,3-dipropionyloxy-2-methylenepropane, and 1,3-dibutyronyloxy-2-methylenepropane. The content of such copolymerizable monomers is usually 10 mol % or less, preferably 5 mol % or less, and particularly preferably 1 mol % or less, based on the total amount of the polymer. Among these copolymerizable monomers, from the viewpoint of obtaining good anti-fogging properties, monomers having copolymerizability with vinyl ester-based monomers are particularly preferably acetoacetyl group-containing monomers, unsaturated acids such as carboxylic acids, polyoxyalkylene group-containing monomers, and cationic group-containing monomers.

[0017] From the viewpoint of improving the anti-fogging properties before and after the water immersion treatment described in detail below, modified polyvinyl alcohol composed of a combination of a vinyl alcohol structural unit and an ethylene oxide group-containing structural unit, or a vinyl alcohol structural unit and an acetoacetyl group-containing structural unit, is preferred.

[0018] The method for polymerizing the vinyl ester monomer and the copolymerizable monomer is not particularly limited, and any conventionally known method can be used, specifically, bulk polymerization, solution polymerization, suspension polymerization, dispersion polymerization, emulsion polymerization, etc.

[0019] (B) Acid catalyst In the present invention, it has been found that the anti-fogging performance of PVA-based resins can be improved by using an acid catalyst in combination. It is presumed that the anti-fogging performance is improved by the use of an acid catalyst, which advances the saponification of the PVA-based resin or causes crosslinking. Depending on the degree of saponification or polymerization, PVA-based resins have problems such as low solubility in solvents such as water, making it difficult to prepare a coating liquid, and high viscosity, which causes streaks during coating and deteriorates the appearance of the coating film. However, the use of an acid catalyst in combination makes it possible to process the PVA-based resin while achieving both processability and coating film performance.

[0020] Examples of the acid catalyst include inorganic acids such as hydrochloric acid, sulfuric acid, nitric acid, and phosphoric acid; oxalic acid, acetic acid, formic acid, benzoic acid, maleic acid, adipic acid, azelaic acid, sebacic acid, itaconic acid, citric acid, succinic acid, trimellitic acid, pyromellitic acid, phthalic acid, isophthalic acid, terephthalic acid, methanesulfonic acid, trifluoromethanesulfonic acid, isoprene sulfonic acid, camphorsulfonic acid, hexanesulfonic acid, octanesulfonic acid, nonanesulfonic acid, decanesulfonic acid, hexadecanesulfonic acid, benzenesulfonic acid, p-toluenesulfonic acid, cumenesulfonic acid, Dodecylbenzenesulfonic acid, naphthalenesulfonic acid, nonylnaphthalenesulfonic acid, 2-sulfobenzoic acid, 2-sulfobenzoic anhydride, methyl acid phosphate, ethyl acid phosphate, propyl acid phosphate, isopropyl acid phosphate, butyl acid phosphate, butoxyethyl acid phosphate, octyl acid phosphate, 2-ethylhexyl acid phosphate, decyl acid phosphate, lauryl acid phosphate, stearyl acid phosphate, oleyl acid phosphate , behenyl acid phosphate, phenyl acid phosphate, nonylphenyl acid phosphate, cyclohexyl acid phosphate, phenoxyethyl acid phosphate, alkoxypolyethylene glycol acid phosphate, bisphenol A acid phosphate, dimethyl acid phosphate, diethyl acid phosphate, dipropyl acid phosphate, diisopropyl acid phosphate, dibutyl acid phosphate, dioctyl acid phosphate, di-2-ethylhexyl acid phosphate organic acids such as bis(nonylphenyl)acid phosphate, dilauryl acid phosphate, distearyl acid phosphate, diphenyl acid phosphate, and bis(nonylphenyl)acid phosphate, and nitrogen compounds containing the above acids, for example, 1-amino-2-propanol, monoethanolamine, diethanolamine, 2-(methylamino)ethanol, 2-dimethylethanolamine, 2-amino-2-methyl-1-propanol, diisopropanolamine, 3-aminopropanol, 2-methylamino-2-methylpropanol, morpholine, oxazolidine, 4,Examples include those blocked with 4-dimethyloxazolidine, 3,4,4-trimethyloxazolidine, etc. (reaction products of acids and amines).

[0021] (C) Ammonium base-containing compounds In the present invention, it has been found that the anti-fogging performance can be improved by using an ammonium salt group-containing compound in combination. It has also been found that the anti-fogging resin layer can be further provided with antibacterial properties by using an ammonium salt group-containing compound in combination. This makes it possible to provide a film that has excellent anti-fogging properties and antibacterial properties, which is excellent from the viewpoint of hygiene.

[0022] The ammonium salt group-containing compound is preferably a polymeric compound having an ammonium salt group, for example, a polymer containing an ammonium salt group and a monomer having an unsaturated double bond as a component. A specific example of such a polymer is a polymer having a repeating unit that is a component represented by the following formula (1): This homopolymer or a copolymer obtained by copolymerizing a plurality of other components may also be used.

[0023] [ka]

[0024] In the above formula (1), R 2 is -O- or -NH-, R 3 is an alkylene group having 1 to 6 carbon atoms or other structure capable of forming the structure of formula (1); R 1 , R 4 , R 5 , R 6 are each a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, a phenyl group, or the like, and these alkyl groups and phenyl groups may be substituted with the groups shown below. Examples of the substitutable groups include a hydroxy group, an amide group, an ester group, an alkoxy group, a phenoxy group, a naphthoxy group, a thioalkoxy group, a thiophenoxy group, a cycloalkyl group, a trialkylammonium alkyl group, a cyano group, and halogens. R 3 Examples of the alkyl group include a methylene group, an ethylene group, and a propylene group. 1 , R 4 , R 5 , R 6 are preferably hydrogen or a methyl group. The number average molecular weight is preferably in the range of 5,000 to 100,000, more preferably in the range of 10,000 to 50,000, and even more preferably in the range of 20,000 to 40,000. The number average molecular weight is a molecular weight measured by gel permeation chromatography (GPC).

[0025] In the case of a polymer having the constituent element represented by the above formula (1) as a repeating unit, it is preferable that the polymer is copolymerized with another repeating unit from the viewpoint of increasing compatibility with other materials and improving the transparency of the obtained anti-fogging resin layer, etc. Examples of the other repeating units include alkyl acrylates such as methyl acrylate, ethyl acrylate, propyl acrylate, and butyl acrylate; alkyl methacrylates such as methyl methacrylate, ethyl methacrylate, propyl methacrylate, and butyl methacrylate; and acrylamides such as n-methylolacrylamide.

[0026] X in the above formula (1) - can be appropriately selected within the scope of the present invention. Examples of the cation include halogen ions, sulfonates, phosphates, nitrates, alkylsulfonates, and carboxylates.

[0027] (D) Crosslinking agent A crosslinking agent may be used in the anti-fogging resin composition of the present invention for the purpose of improving the durability of the anti-fogging resin layer when immersed in water. As the crosslinking agent, various known crosslinking agents can be used, for example, oxazoline compounds, epoxy compounds, melamine compounds, isocyanate compounds, carbodiimide compounds, silane coupling compounds, etc. Among these, oxazoline compounds or epoxy compounds are preferred from the viewpoint of improving durability when immersed in water.

[0028] From the viewpoint of obtaining antifogging properties while improving the durability of the coating film, the amount of reactive functional groups in the crosslinking agent is preferably in the range of 0.5 to 17 mmol / g, more preferably 1 to 13 mmol / g, even more preferably 2 to 10 mmol / g, and particularly preferably 3 to 8 mmol / g. Examples of the reactive functional group include an oxazoline group of an oxazoline compound, a glycidyl group of an epoxy compound, an imino group of a melamine compound, an alkylol group, an alkoxyalkyl group, an isocyanate group of an isocyanate compound, a carbodiimide group of a carbodiimide compound, and a silyl group of a silane coupling compound.

[0029] (Oxazoline compounds) The oxazoline compound is a compound having an oxazoline group in the molecule, and is preferably a polymer containing an oxazoline group. The oxazoline compound can be prepared by polymerization of an addition-polymerizable oxazoline group-containing monomer alone or with other monomers. Examples of the addition-polymerizable oxazoline group-containing monomer include 2-vinyl-2-oxazoline, 2-vinyl-4-methyl-2-oxazoline, 2-vinyl-5-methyl-2-oxazoline, 2-isopropenyl-2-oxazoline, 2-isopropenyl-4-methyl-2-oxazoline, and 2-isopropenyl-5-ethyl-2-oxazoline, and one or a mixture of two or more of these can be used. Among these, 2-isopropenyl-2-oxazoline is suitable because it is easily available industrially.

[0030] The other monomer is not limited as long as it is a monomer that can be copolymerized with the addition-polymerizable oxazoline group-containing monomer, and examples thereof include (meth)acrylic acid esters such as alkyl (meth)acrylates (alkyl groups include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, t-butyl, 2-ethylhexyl, and cyclohexyl groups); unsaturated carboxylic acids such as acrylic acid, methacrylic acid, itaconic acid, maleic acid, fumaric acid, crotonic acid, styrenesulfonic acid, and salts thereof (sodium salts, potassium salts, ammonium salts, tertiary amine salts, etc.); unsaturated nitriles such as acrylonitrile and methacrylonitrile; (meth)acrylamide, N-alkyl Examples of the monomer include unsaturated amides such as (meth)acrylamide and N,N-dialkyl(meth)acrylamide (alkyl groups include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, t-butyl, 2-ethylhexyl, and cyclohexyl groups); vinyl esters such as vinyl acetate and vinyl propionate; vinyl ethers such as methyl vinyl ether and ethyl vinyl ether; α-olefins such as ethylene and propylene; halogen-containing α,β-unsaturated monomers such as vinyl chloride and vinylidene chloride; and α,β-unsaturated aromatic monomers such as styrene and α-methylstyrene. One or more of these monomers can be used.

[0031] (Epoxy compounds) The epoxy compound is a compound having an epoxy group in the molecule, and examples thereof include condensates of epichlorohydrin, ethylene glycol, polyethylene glycol, glycerin, polyglycerin, bisphenol A, etc. with hydroxyl groups or amino groups, polyepoxy compounds, diepoxy compounds, monoepoxy compounds, and glycidylamine compounds. Examples of polyepoxy compounds include sorbitol polyglycidyl ether, polyglycerol polyglycidyl ether, pentaerythritol polyglycidyl ether, diglycerol polyglycidyl ether, triglycidyl tris(2-hydroxyethyl)isocyanate, glycerol polyglycidyl ether, and trimethylolpropane polyglycidyl ether; examples of diepoxy compounds include neopentyl glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether, resorcinol diglycidyl ether, ethylene glycol ... Cole diglycidyl ether, polyethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether and polytetramethylene glycol diglycidyl ether; monoepoxy compounds include, for example, allyl glycidyl ether, 2-ethylhexyl glycidyl ether and phenyl glycidyl ether; glycidylamine compounds include, for example, N,N,N',N'-tetraglycidyl-m-xylylenediamine and 1,3-bis(N,N-diglycidylamino)cyclohexane. From the viewpoint of improving adhesion, polyether-based epoxy compounds are preferred. In addition, the amount of epoxy groups is preferably a polyepoxy compound having a functionality of 3 or more than a functionality of 2.

[0032] (Melamine compounds) The melamine compound is a compound having a melamine skeleton in the compound, and for example, an alkylolated melamine derivative, a compound partially or completely etherified by reacting an alkylolated melamine derivative with an alcohol, and a mixture thereof can be used. As the alcohol used for etherification, methanol, ethanol, isopropanol, n-butanol, isobutanol, etc. are preferably used. In addition, the melamine compound may be either a monomer or a dimer or higher polymer, or a mixture thereof may be used. Furthermore, a product obtained by co-condensing a part of melamine with urea or the like can also be used, and a catalyst can be used to increase the reactivity of the melamine compound.

[0033] (Isocyanate compounds) The isocyanate compound is a compound having an isocyanate or an isocyanate derivative structure, such as a blocked isocyanate. Examples of the isocyanate include aromatic isocyanates such as tolylene diisocyanate, xylylene diisocyanate, methylene diphenyl diisocyanate, phenylene diisocyanate, and naphthalene diisocyanate; aliphatic isocyanates having an aromatic ring such as α,α,α',α'-tetramethyl xylylene diisocyanate; aliphatic isocyanates such as methylene diisocyanate, propylene diisocyanate, lysine diisocyanate, trimethylhexamethylene diisocyanate, and hexamethylene diisocyanate; and alicyclic isocyanates such as cyclohexane diisocyanate, methylcyclohexane diisocyanate, isophorone diisocyanate, methylene bis(4-cyclohexyl isocyanate), and isopropylidenedicyclohexyl diisocyanate. In addition, polymers and derivatives such as biuretized products, isocyanurate products, uretdione products, and carbodiimide modified products of these isocyanates are also included. These may be used alone or in combination. Among the above isocyanates, aliphatic isocyanates or alicyclic isocyanates are more preferable than aromatic isocyanates in order to prevent yellowing due to ultraviolet rays.

[0034] When used in the form of a blocked isocyanate, examples of the blocking agent include phenolic compounds such as bisulfites, phenol, cresol, and ethylphenol; alcohol compounds such as propylene glycol monomethyl ether, ethylene glycol, benzyl alcohol, methanol, and ethanol; active methylene compounds such as methyl isobutanoylacetate, dimethyl malonate, diethyl malonate, methyl acetoacetate, ethyl acetoacetate, and acetylacetone; mercaptan compounds such as butyl mercaptan and dodecyl mercaptan; lactam compounds such as ε-caprolactam and δ-valerolactam; amine compounds such as diphenylaniline, aniline, and ethyleneimine; acid amide compounds such as acetanilide and acetic acid amide; and oxime compounds such as formaldehyde, acetaldoxime, acetoneoxime, methyl ethyl ketoneoxime, and cyclohexanoneoxime, which may be used alone or in combination of two or more.

[0035] The isocyanate compound may be used alone or as a mixture or bond with various polymers. In terms of improving the dispersibility and crosslinking property of the isocyanate compound, it is preferable to use a mixture or bond with a polyester resin or a urethane resin.

[0036] (Carbodiimide compounds) A carbodiimide compound is a compound having a carbodiimide structure, and is a compound having one or more carbodiimide structures in the molecule. For better adhesion, etc., a polycarbodiimide compound having two or more carbodiimide structures in the molecule is more preferred.

[0037] Carbodiimide compounds can be synthesized by conventionally known techniques, and generally, condensation reaction of diisocyanate compounds is used. The diisocyanate compounds are not particularly limited, and both aromatic and aliphatic compounds can be used, and specific examples thereof include tolylene diisocyanate, xylene diisocyanate, diphenylmethane diisocyanate, phenylene diisocyanate, naphthalene diisocyanate, hexamethylene diisocyanate, trimethylhexamethylene diisocyanate, cyclohexane diisocyanate, methylcyclohexane diisocyanate, isophorone diisocyanate, dicyclohexyl diisocyanate, and dicyclohexylmethane diisocyanate.

[0038] The content of carbodiimide groups contained in the carbodiimide compound, in terms of carbodiimide equivalent (weight [g] of the carbodiimide compound required to provide 1 mol of carbodiimide groups), is usually in the range of 100 to 1000, preferably 250 to 800, and more preferably 300 to 700. By using within the above range, the durability of the coating film is improved.

[0039] Furthermore, within the scope of the present invention, in order to improve the water solubility or water dispersibility of the polycarbodiimide compound, a surfactant may be added, or a hydrophilic monomer such as a polyalkylene oxide, a quaternary ammonium salt of a dialkylamino alcohol, or a hydroxyalkylsulfonate may be added.

[0040] ((E) Other optional components) When forming the anti-fogging resin layer, in order to improve the coating appearance, transparency, film-forming properties, etc., it is also possible to use various conventionally known polymers as binders, such as polyester resins, acrylic resins, urethane resins, etc., in combination with the anti-fogging resin composition. Furthermore, within the scope of the present invention, particles for improving blocking properties or slipping properties, materials having antibacterial properties for antibacterial or antiviral properties, and ultraviolet absorbers for weather resistance may be used in combination. Among these, it is preferable to use a material having antibacterial properties in view of hygiene.

[0041] The antibacterial material is an agent that has an MIC (minimum inhibitory concentration) against bacteria and fungi, and includes inorganic antibacterial agents and organic antibacterial agents. Among these, organic antibacterial agents are preferred from the viewpoint of good compatibility with the resin layer and good transparency of the antifogging resin layer.

[0042] Examples of inorganic antibacterial agents include silver-based antibacterial agents, zinc-based antibacterial agents, and copper-based antibacterial agents. These are inorganic compounds in which one or more selected from silver ions, zinc ions, and copper ions are supported, and examples of inorganic compounds include zeolite, glass, talc, silica gel, silicate, mica, and sepiolite. When using a plurality of ion species, each ion may be supported by the same inorganic compound. Specifically, an inorganic antibacterial agent in which silver ions and zinc ions are supported by glass may be used. In addition, when using a plurality of ion species, each ion may be supported by a different inorganic compound. Specifically, an inorganic antibacterial agent in which silver ions are supported by glass and an inorganic antibacterial agent in which zinc ions are supported by zeolite may be used.

[0043] The organic antibacterial agent is not particularly limited, but examples thereof include biguanide antibacterial agents such as the above-mentioned ammonium base-containing compounds, chlorhexidine gluconate, chlorhexidine hydrochloride, polybiguanide hydrochloride, polyaminopropyl biguanide hydrochloride, and polyhexamethylene biguanide; pyridine antibacterial agents such as zinc pyrithione (bis(2-pyridithio-1-oxide) zinc), densil (2,3,5,6,-tetrachloro-4-(methylsulfonyl)pyridine), and copper pyrithione (bis(2-pyridithio-1-oxide) copper); Thiazoline antibacterial agents such as T (2-n-octyl-4-isothiazolin-3-one), MIT (2-methyl-4-isothiazolin-3-one), CMI (5-chloro-2-methyl-4-isothiazolin-3-one), BIT (1,2-benzisothiazolone), and n-butylBIT (Nn-butyl-1,2-benzisothiazolone-3); triazine antibacterial agents such as hexahydro-1,3,5-trimethyl-1,3,5-triazine and 2,4-dichloro-6-methoxy-1,3,5-triazine; thiabendazole (2-(4-thiazolyl)-benzyl) imidazole antibacterial agents such as benzimidazole (methyl-2-benzimidazole carbamate) and carbendazim (methyl-2-benzimidazole carbamate); triazole antibacterial agents such as tebuconazole ((±)-α-[2-(4-chlorophenyl)ethyl]-α-(1,1-dimethylethyl)-1H-1,2,4-triazole-1-ethanol); iodine antibacterial agents such as diiodomethyl-paratolyl sulfone, polyvinylpyrrolidone iodine, and 3-iodo-2-propynyl butylcarbamate; arsenic antibacterial agents such as 10,10'-oxybis-10H-phenoxyarsine; Ether-based antibacterial agents such as losan; organic chlorine-based antibacterial agents such as triclocarban (3,4,4'-trichlorocarbanilide), halocarban (4,4-dichloro-3-(3-fluoromethyl)-carbanilide), chlorothalonil (2,4,5,6-tetrachloroisophthalonitrile), dichloroisocyanuric acid, and trichloroisocyanuric acid; sulfamide-based antibacterial agents such as dichlofluanid and trifluanid; quaternary ammonium chlorine-based antibacterial agents such as benzothonium chloride, cetylpyridinium chloride, and diallyldimethylammonium chloride;Examples of such antibacterial agents include aldehyde-based antibacterial agents such as BCA (α-bromocinnamaldehyde); carboxylic acid-based antibacterial agents such as magnesium dihydrogen bismonoperoxyphthalate and zinc undecylenate; ester-based antibacterial agents such as lauricidin (glycerol laurate); phenol-based antibacterial agents such as butylparaben (butyl-p-hydroxybenzoate) and sodium orthophenylphenol; and carbamate-based antibacterial agents such as sodium N-methyldithiocarbamate. Among these, biguanide-based antibacterial agents such as polyaminopropyl biguanide hydrochloride and polyhexamethylene biguanide are preferred from the viewpoints of safety and the fact that they are effective in small amounts. When an antibacterial agent is added, its content in the total non-volatile components of the antifogging resin layer composition is 0 to 10 mass%, preferably 0.03 to 8 mass%, and more preferably 0.5 to 5 mass%. If it is equal to or more than the lower limit, sufficient antibacterial performance is obtained, and if it is equal to or less than the upper limit, there is no effect such as skin sensitization.

[0044] The anti-fogging resin layer described below is composed of the above-mentioned anti-fogging resin composition, but it can be assumed that unreacted compounds of the various compounds in the anti-fogging resin composition, reacted compounds, or a mixture thereof are present.

[0045] The proportion of the (A) PVA-based resin in the total non-volatile components in the anti-fogging resin layer composition is usually 40 to 99 mass%, preferably 60 to 99 mass%, and more preferably 70 to 99 mass%. When the (A) PVA-based resin content is equal to or less than the upper limit, the strength and transparency of the anti-fogging resin layer are good, while when it is equal to or more than the lower limit, sufficient anti-fogging performance is obtained.

[0046] The proportion of the (B) acid catalyst in the total non-volatile components in the anti-fogging resin layer composition is usually 10% by mass or less, preferably 5% by mass or less, and more preferably 3% by mass or less. If the proportion of the (B) acid catalyst is below the upper limit, sufficient anti-fogging properties are obtained and the appearance of the anti-fogging resin layer becomes good. On the other hand, when the (B) acid catalyst is used, it is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, and even more preferably 1% by mass or more. If it is above the lower limit, sufficient anti-fogging properties are obtained.

[0047] The proportion of the ammonium base-containing compound (C) in the total non-volatile components in the anti-fogging resin layer composition is usually 50% by mass or less, preferably 30% by mass or less, and more preferably 20% by mass or less. When the proportion of the ammonium base-containing compound (C) is below the upper limit, the proportions of the other components are sufficient, and anti-fogging properties and film-forming properties are good. On the other hand, when the component (C) is used, it is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 15% by mass or more. When it is above the lower limit, sufficient anti-fogging properties are obtained and antibacterial properties are good.

[0048] When a crosslinking agent (D) is used in combination, the proportion of the crosslinking agent in the total non-volatile components in the anti-fogging resin layer composition is usually 30% by mass or less, preferably 20% by mass or less, and particularly preferably 15% by mass or less. By satisfying the above range, good water resistance can be obtained and the strength of the anti-fogging resin layer is improved. On the other hand, when the component (D) is used, the proportion is preferably 1% by mass or more, more preferably 5% by mass or more, and even more preferably 8% by mass or more. When the proportion is equal to or more than the above lower limit, sufficient anti-fogging properties are obtained and antibacterial properties are good.

[0049] [Laminated film] The laminated film of the present invention has an anti-fog resin layer on at least one surface of a substrate film, and the anti-fog resin layer is formed from the above-mentioned anti-fog resin composition of the present invention. The anti-fog resin layer may be formed by applying the anti-fog resin composition and drying it or by curing it.

[0050] <Base film> The base film is not particularly limited as long as it can achieve the effects of the present invention, but a polyester film having excellent properties such as mechanical strength, dimensional stability, flatness, heat resistance, chemical resistance, and optical properties is preferred. The polyester film constituting the base film may be a single-layer structure or a multi-layer structure. In the case of a multi-layer structure, it may be a two-layer structure, a three-layer structure, or a four-layer structure or more, as long as it does not deviate from the gist of the present invention, and the number of layers is not particularly limited. In addition, as the polyester film, a non-stretched film or a polyester film stretched at least in one direction is preferable, a biaxially stretched polyester film or a non-stretched polyester film is more preferable, and a biaxially stretched film is even more preferable.

[0051] The polyester used may be either a homopolyester or a copolymer polyester. In the case of a homopolyester, it is preferable to use one obtained by polycondensation of an aromatic dicarboxylic acid and an aliphatic glycol. Examples of the aromatic dicarboxylic acid include terephthalic acid and 2,6-naphthalenedicarboxylic acid, and examples of the aliphatic glycol include ethylene glycol, diethylene glycol, and 1,4-cyclohexanedimethanol. A representative polyester is polyethylene terephthalate. On the other hand, examples of the dicarboxylic acid component of the copolymer polyester include one or more of isophthalic acid, phthalic acid, terephthalic acid, 2,6-naphthalenedicarboxylic acid, adipic acid, sebacic acid, and oxycarboxylic acid, and examples of the glycol component include one or more of ethylene glycol, diethylene glycol, propylene glycol, butanediol, 4-cyclohexanedimethanol, and neopentyl glycol.

[0052] The polyester polymerization catalyst is not particularly limited, and any conventionally known compound can be used, such as titanium compounds, germanium compounds, antimony compounds, manganese compounds, aluminum compounds, magnesium compounds, and calcium compounds.

[0053] In order to suppress the amount of oligomer component precipitation, the film may be produced using a polyester with a low content of oligomer component as a raw material. As a method for producing a polyester with a low content of oligomer component, various known methods can be used, for example, a method of performing solid-phase polymerization after polyester production. In addition, the amount of oligomer component precipitation may be suppressed by forming a polyester film with a three-layer or more structure and making the outermost layer of the polyester film a layer using a polyester raw material with a low content of oligomer component. The polyester may also be obtained by carrying out esterification or transesterification, followed by melt polycondensation at a higher reaction temperature under reduced pressure.

[0054] In order to improve the weather resistance of the polyester film, an ultraviolet absorbing agent may be contained in the polyester film. The ultraviolet absorbing agent is a compound that absorbs ultraviolet light and is not particularly limited as long as it can withstand the heat applied during the production process of the polyester film.

[0055] As the ultraviolet absorbing agent, there are organic ultraviolet absorbing agents and inorganic ultraviolet absorbing agents, and from the viewpoint of transparency, organic ultraviolet absorbing agents are preferred.As the organic ultraviolet absorbing agent, there are no particular limitations, but for example, cyclic imino esters, benzotriazoles, benzophenones, etc. are mentioned.From the viewpoint of durability, cyclic imino esters and benzotriazoles are more preferred.In addition, it is also possible to use two or more kinds of ultraviolet absorbing agents in combination.

[0056] Particles can be blended into the polyester layer of the film mainly for the purpose of imparting easy slippage and preventing scratches during each process. The type of particles to be blended is not particularly limited as long as it is a particle capable of imparting easy slippage, and specific examples include inorganic particles such as silica, calcium carbonate, magnesium carbonate, barium carbonate, calcium sulfate, calcium phosphate, magnesium phosphate, kaolin, aluminum oxide, and titanium oxide; organic particles such as acrylic resin, styrene resin, urea resin, phenolic resin, epoxy resin, and benzoguanamine resin. Furthermore, precipitated particles obtained by precipitating and finely dispersing a part of a metal compound such as a catalyst during the polyester production process can also be used.

[0057] On the other hand, the shape of the particles to be used is not particularly limited, and any of spherical, blocky, rod-like, flat, etc. may be used. In addition, there is no particular limit to the hardness, specific gravity, color, etc. Two or more kinds of these particles may be used in combination as necessary.

[0058] The average particle size of the particles used is usually 5 μm or less, preferably in the range of 0.01 to 3 μm. If the average particle size is 5 μm or less, the surface roughness of the film is not too rough, and no problems occur when various surface functional layers are formed in a post-process. In addition, the transparency of the film is good.

[0059] Furthermore, the particle content in the polyester layer is usually less than 5% by mass, preferably in the range of 0.0003 to 3% by mass. When there are no particles or when there are only a few particles, the film becomes highly transparent, resulting in a good film in terms of transparency. On the other hand, when the particles are contained in the above range, the film also becomes good in terms of slipperiness.

[0060] The method of adding particles to the polyester layer is not particularly limited, and any conventionally known method can be used. For example, the particles can be added at any stage in the production of the polyester constituting each layer, but it is preferable to add the particles after the completion of the esterification or transesterification reaction.

[0061] In addition to the above-mentioned particles, conventionally known antioxidants, antistatic agents, heat stabilizers, lubricants, dyes, pigments, etc. may be added to the polyester film as necessary.

[0062] The thickness of the substrate film is not particularly limited as long as it is within a range that allows formation of a film, but is usually in the range of 25 to 1000 μm, preferably 30 to 800 μm, more preferably 35 to 600 μm, and further preferably 40 to 400 μm.

[0063] Next, examples of the production of polyester films will be specifically described, but the production is not limited to the following examples.

[0064] (Non-oriented polyester film) A method is preferred in which the above-mentioned polyester raw material is dried, pelletized, and extruded from a die of an extruder as a molten sheet, and then cooled and solidified with a cooling roll to obtain an unstretched sheet. In this case, it is preferred to increase the adhesion between the sheet and the rotating cooling drum in order to improve the flatness of the sheet, and an electrostatic application adhesion method and / or a liquid application adhesion method are preferably used. In this way, an unstretched polyester film is obtained.

[0065] (Stretched polyester film) The unstretched sheet obtained by the above method is then stretched uniaxially and further biaxially. In this case, the unstretched sheet is first stretched in one direction by a roll or tenter type stretching machine. The stretching temperature is usually 70 to 120°C, preferably 80 to 110°C, and the stretching ratio is usually 2.5 to 7 times, preferably 3 to 6 times. Next, the sheet is stretched in a direction perpendicular to the first-stage stretching direction, in which the stretching temperature is usually 70 to 170°C, and the stretching ratio is usually 3 to 7 times, preferably 3.5 to 6 times. Then, the sheet is subsequently heat-treated under tension or relaxation of 30% or less at a temperature of 180 to 270°C to obtain a biaxially oriented film. In the above stretching, a method of stretching in one direction in two or more stages can also be adopted. In this case, it is preferable to perform the stretching so that the final stretching ratios in both directions are each within the above range.

[0066] In addition, a simultaneous biaxial stretching method can also be adopted for the production of polyester films. The simultaneous biaxial stretching method is a method in which the unstretched sheet is simultaneously stretched and oriented in the machine direction and the width direction under a temperature controlled condition usually at 70 to 120°C, preferably 80 to 110°C, and the stretching ratio is 4 to 50 times, preferably 7 to 35 times, more preferably 10 to 25 times in terms of area ratio. Then, the sheet is subsequently heat-treated under tension or relaxation of 30% or less at a temperature of 170 to 250°C to obtain a stretch-oriented film. As for the simultaneous biaxial stretching device adopting the above-mentioned stretching method, a conventionally known stretching method such as a screw method, a pantograph method, and a linear drive method can be adopted.

[0067] <Anti-fogging resin layer> The antifogging resin layer is a layer formed from the above-mentioned antifogging resin composition. The thickness of the anti-fogging resin layer (after drying) is preferably 0.01 μm to 1 μm, more preferably 0.02 μm to 0.5 μm, even more preferably 0.03 μm to 0.1 μm, and particularly preferably 0.03 μm to 0.08 μm. If the thickness of the anti-fogging resin layer is within the above range, good anti-fogging properties can be imparted.

[0068] The method for forming the anti-fogging resin layer is not particularly limited, and may be in-line coating, off-line coating, or the like. It is preferable to form the layer by in-line coating, which treats the surface of the polyester film during the film-forming process.

[0069] In-line coating is a method of coating within the polyester film production process, specifically, a method of coating at any stage from melt extrusion of polyester to stretching, heat setting and winding up. Usually, coating is performed on any of the following: an unstretched sheet obtained by melting and quenching, a stretched uniaxially stretched film, a biaxially stretched film before heat setting, or a film after heat setting and before winding up. Although not limited to the following, for example, in the case of sequential biaxial stretching, a method in which a uniaxially stretched film stretched in the longitudinal direction (machine direction) is coated and then stretched in the transverse direction is particularly advantageous. This method has the advantage of being able to simultaneously form the film and the anti-fogging resin layer, and is advantageous in terms of production costs. In addition, since stretching is performed after coating, the thickness of the anti-fogging resin layer can be changed by the stretching ratio, and thin film coating can be performed more easily than with an off-line coated film.

[0070] In addition, by providing an anti-fog resin layer on the film before stretching, the anti-fog resin layer can be stretched together with the polyester film, and the anti-fog resin layer can be firmly attached to the polyester film. Furthermore, in the production of biaxially stretched polyester film, the film can be restrained in the longitudinal and lateral directions by stretching while holding the film ends with clips or the like, and high temperatures can be applied in the heat fixing step without wrinkles or the like and while maintaining flatness. Therefore, the heat treatment performed after coating can be performed at a high temperature that cannot be achieved by other methods, so that the film-forming properties of the anti-fog resin layer are improved, the anti-fog resin layer and the polyester film can be more firmly attached to each other, and a strong anti-fog resin layer can be obtained.

[0071] When the anti-fogging resin layer is provided by in-line coating, it is preferable to prepare a laminated film by coating an anti-fogging resin layer composition, which is prepared by preparing an aqueous solution or water dispersion of the above-mentioned series of compounds so that the solid content concentration is adjusted to about 0.1 to 50 mass%, on a polyester film. Within the scope of the present invention, the anti-fogging resin composition may contain a small amount of organic solvent for the purpose of improving dispersibility in water, improving film-forming properties, etc. Only one type of organic solvent may be used, or two or more types may be used as appropriate.

[0072] The anti-fogging resin layer can be provided by a conventional coating method such as reverse gravure coating, direct gravure coating, roll coating, die coating, bar coating, curtain coating, or the like.

[0073] The drying and curing conditions when forming an anti-fogging resin layer on a polyester film are not particularly limited. For example, when the anti-fogging resin layer is provided by offline coating, the heat treatment is usually performed at 80 to 200°C for 3 to 40 seconds, preferably at 100 to 180°C for 3 to 40 seconds. On the other hand, when the anti-fogging resin layer is provided by in-line coating, it is usually preferable to carry out heat treatment at 70 to 280° C. for 3 to 200 seconds as a guideline.

[0074] Regardless of whether off-line coating or in-line coating is used, heat treatment and irradiation with active energy rays such as ultraviolet light may be used in combination as necessary. The polyester film (substrate film) constituting the laminated polyester film of the present invention may be previously subjected to a surface treatment such as a corona treatment or a plasma treatment.

[0075] The components in the anti-fogging resin layer can be analyzed by, for example, TOF-SIMS, ESCA, fluorescent X-ray analysis, or the like.

[0076] <Functional layer> The laminated film of the present invention is characterized in that it has an anti-fogging resin layer on at least one side of the substrate film. The anti-fogging resin layer may be provided on one side or both sides of the substrate film. Alternatively, the anti-fogging resin layer may be formed on one side of the substrate film, and a different functional layer may be provided on the other side. Examples of the functional layer include a visibility improving layer having functions such as low reflection and improved transmittance, a hard coat layer for preventing scratches, and an antibacterial layer for maintaining cleanliness. The functional layer may be formed by preparing a functional layer-forming composition (resin layer-forming composition) and applying it to the substrate film.

[0077] <Visibility improvement layer> The visibility improving layer is a layer designed for low reflectance, and is a functional layer that can improve total light transmittance. By designing the functional layer for low reflectance, it is possible to prevent light and objects from being reflected. Furthermore, reflectance and total light transmittance are mutually related properties, and in a polyester film that has low light absorption and high transparency, a low reflectance can be used to show high total light transmittance and improve visibility.

[0078] The visibility improving layer has one minimum absolute reflectance value in the wavelength range of 300 to 800 nm, and the minimum value is preferably 3.0% or less. The wavelength of the minimum value is more preferably in the range of 400 to 700 nm, and further preferably in the range of 450 to 650 nm. The minimum value is preferably 2.5% or less, and further preferably 2.0% or less.

[0079] The visibility improving layer preferably contains a resin having a low refractive index, such as a fluorine-containing compound or an acrylic resin.

[0080] (Fluorine-containing compounds) The fluorine-containing compound is preferably a fluorine-containing resin from the viewpoint of increasing the strength of the coating film.Specific examples of the fluorine-containing resin include fluoroolefin copolymer resins with vinyl fluoride, vinylidene fluoride, tetrafluoroethylene, hexafluoropropylene, chlorotrifluoroethylene, etc. as monomers; fluorine-containing copolymer resins obtained by polymerizing polyalkylene ether groups in which some or all of hydrogen atoms such as fluoromethylene ether groups, difluoromethylene ether groups, fluoroethylene ether groups, difluoroethylene ether groups, tetrafluoroethylene ether groups, hexafluoropropylene ether groups, etc. are substituted with fluorine atoms and other monomers; fluorine-containing copolymer resins obtained by graft polymerization of hydroxyl group-containing fluororesin copolymers and (meth)acrylic acid ester compounds or other monomers; vinyl polymers having perfluoroalkyl groups, etc. Among these, from the viewpoint of having a low refractive index and being able to more effectively suppress reflection and improve transmittance, fluoroolefin-based copolymer resins and fluororesin copolymers containing polyalkylene ether groups in which some or all of the hydrogen atoms are fluorinated are preferred.

[0081] Examples of fluorine-based copolymer resins obtained by polymerizing a polyalkylene ether in which some or all of the hydrogen atoms have been substituted with fluorine atoms with other monomers include urethane resins having a polyfluoroalkylene ether group, polyester resins having a polyfluoroalkylene ether group, and acrylic resins having a polyfluoroalkylene ether group. Other monomers constituting the urethane resin having a polyfluoroalkylene ether group include isocyanate compounds. Examples of isocyanate compounds include aromatic diisocyanates such as tolylene diisocyanate, xylylene diisocyanate, methylene diphenyl diisocyanate, phenylene diisocyanate, naphthalene diisocyanate, and tolidine diisocyanate; aliphatic diisocyanates having an aromatic ring such as α,α,α',α'-tetramethyl xylylene diisocyanate; aliphatic diisocyanates such as methylene diisocyanate, propylene diisocyanate, lysine diisocyanate, trimethylhexamethylene diisocyanate, and hexamethylene diisocyanate; and alicyclic diisocyanates such as cyclohexane diisocyanate, methylcyclohexane diisocyanate, isophorone diisocyanate, dicyclohexylmethane diisocyanate, and isopropylidenedicyclohexyl diisocyanate.

[0082] Other monomers constituting the urethane resin include polyols not containing fluorine atoms, and polyols having a carboxy group such as dimethylolpropanoic acid, dimethylolbutanoic acid, bis-(2-hydroxyethyl)propionic acid, and bis-(2-hydroxyethyl)butanoic acid. Among these, it is preferable to include a polyol having a carboxy group from the viewpoint of self-emulsification when water is used as the dispersion solvent, and among these, dimethylolpropanoic acid is more preferable.

[0083] The visibility improving layer is preferably formed from a resin layer forming composition containing a fluorine-containing compound. The resin layer forming composition may be composed of a fluorine-containing compound as a non-volatile component, or may contain other components. In addition, the visibility improving layer is more preferably formed by curing a resin layer forming composition containing a fluorine-containing compound and a crosslinking agent. By curing the resin layer forming composition containing a crosslinking agent in this manner, the strength of the visibility improving layer is improved. The details of the crosslinking agent are as described below. The content of the fluorine-containing compound in the visibility improving layer forming composition is preferably 30 to 100 mass %, more preferably 40 to 98 mass %, and even more preferably 50 to 95 mass %, based on the non-volatile components in the resin layer forming composition. By making it 30 mass % or more, it becomes possible to effectively lower the refractive index of the visibility improving layer, suppress the reflectance, and improve the total light transmittance.

[0084] (Acrylic resin) The acrylic resin is a polymer made of polymerizable monomers including acrylic and methacrylic monomers. These may be homopolymers or copolymers, or copolymers with polymerizable monomers other than acrylic and methacrylic monomers. The acrylic resin may also be copolymerized with other polymers (such as polyesters, polyurethanes, etc.). For example, block copolymers and graft copolymers. Alternatively, the acrylic resin may also be polymerized with a polymerizable monomer in a polyester solution or polyester dispersion (or a mixture of polymers in some cases). Similarly, the acrylic resin may also be polymerized with a polymerizable monomer in a polyurethane solution or polyurethane dispersion (or a mixture of polymers in some cases). Similarly, the acrylic resin may also be polymerized with a polymerizable monomer in another polymer solution or dispersion (or a mixture of polymers in some cases). In order to further improve adhesion to the substrate, the acrylic resin may also contain a hydroxyl group or an amino group.

[0085] The polymerizable monomer is not particularly limited, but particularly representative compounds include various carboxyl group-containing monomers such as acrylic acid, methacrylic acid, crotonic acid, itaconic acid, fumaric acid, maleic acid, and citraconic acid, and salts thereof; various hydroxyl group-containing monomers such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, monobutyl hydroxyl fumarate, and monobutyl hydroxy itaconate; methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, hexyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate. Examples of the monomers include various (meth)acrylic acid esters such as cyclohexyl (meth)acrylate and lauryl (meth)acrylate; various nitrogen-containing compounds such as (meth)acrylamide, diacetone acrylamide, N-methylol acrylamide and (meth)acrylonitrile; various styrene derivatives such as styrene, α-methylstyrene, divinylbenzene and vinyl toluene; various vinyl esters such as vinyl propionate; various silicon-containing polymerizable monomers such as γ-methacryloxypropyltrimethoxysilane and vinyltrimethoxysilane; phosphorus-containing vinyl monomers; various vinyl halides such as vinyl chloride and vinylidene chloride; and various conjugated dienes such as butadiene.

[0086] <Hard coat layer> The hard coat layer preferably has a pencil hardness of F or more. With a pencil hardness of F or more, the surface of the laminated film can be protected from scratches, stains, etc. From the above viewpoints, the pencil hardness is more preferably H or more, and further preferably 2H or more. The hard coat layer can be made of various hard coat agents, and is not limited as long as it can obtain the above-mentioned pencil hardness. For example, a layer formed using a hard coat agent containing an active energy ray-curable resin composition or a thermosetting resin composition can be mentioned. Specifically, the composition may contain a polymerizable monomer or oligomer that forms a cured product upon irradiation with active energy rays.

[0087] The polymerizable monomer may be a (meth)acrylate monomer having a radically polymerizable unsaturated group in the molecule, or a (meth)acrylate oligomer having a radically polymerizable unsaturated group in the molecule. More specifically, the (meth)acrylic derivatives of polyfunctional alcohols such as dipentaerythritol hexa(meth)acrylate, tetramethylolmethane tetra(meth)acrylate, tetramethylolmethane tri(meth)acrylate, trimethylolpropane tri(meth)acrylate, 1,6-hexanediol di(meth)acrylate, and 1,6-bis(3-acryloyloxy-2-hydroxypropyloxy)hexane; and monomers or oligomers such as urethane(meth)acrylate, polyester(meth)acrylate, epoxy(meth)acrylate, melamine(meth)acrylate, polyfluoroalkyl(meth)acrylate, and silicone(meth)acrylate may be used alone or in combination of two or more of these polymerizable monomers or oligomers. Among them, the (meth)acrylic derivatives of polyfunctional alcohols and urethane(meth)acrylate are preferred in that they provide high surface hardness.

[0088] <Antibacterial layer> The antibacterial layer is a functional layer having an inhibitory effect against bacteria and fungi, and suppresses the proliferation of bacteria on the surface of the antibacterial layer, thereby keeping the film clean. The antibacterial layer may be a layer containing an antibacterial agent such as the inorganic antibacterial agent or the organic antibacterial agent described above, and may have the same composition as the antifogging resin layer or a different composition.

[0089] The antibacterial layer preferably uses various polymers in combination to hold the antibacterial agent on the film surface. Specific examples of the polymer include polyester resin, acrylic resin, urethane resin, polyvinyl (polyvinyl alcohol, vinyl chloride vinyl acetate copolymer, etc.), polyalkylene glycol, polyalkyleneimine, methyl cellulose, hydroxy cellulose, starch, etc. Among these, polyester resin and urethane resin are preferred, and polyester resin is more preferred, in terms of excellent adhesion to polyester film.

[0090] (polyester resin) The polyester resin may be composed of, for example, the following polyvalent carboxylic acid and polyvalent hydroxy compound as main components. That is, as the polyvalent carboxylic acid, terephthalic acid, isophthalic acid, orthophthalic acid, phthalic acid, 4,4'-diphenyldicarboxylic acid, 2,5-naphthalenedicarboxylic acid, 1,5-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 2,7-naphthalenedicarboxylic acid, 1,4-cyclohexanedicarboxylic acid, 2-potassium sulfoterephthalic acid, 5-sodium sulfoisophthalic acid, adipic acid, azelaic acid, sebacic acid, dodecanedicarboxylic acid, glutaric acid, succinic acid, trimellitic acid, trimesic acid, pyromellitic acid, trimellitic anhydride, phthalic anhydride, p-hydroxybenzoic acid, trimellitic acid monopotassium salt, and ester-forming derivatives thereof may be used; Examples of the oxy compound include ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, 1,6-hexanediol, 2-methyl-1,5-pentanediol, neopentyl glycol, 1,4-cyclohexanedimethanol, p-xylylene glycol, bisphenol A-ethylene glycol adduct, diethylene glycol, triethylene glycol, polyethylene glycol, polypropylene glycol, polytetramethylene glycol, polytetramethylene oxide glycol, dimethylolpropionic acid, glycerin, trimethylolpropane, sodium dimethylolethylsulfonate, and potassium dimethylolpropionate. One or more of these compounds may be appropriately selected and a polyester resin may be synthesized by a conventional polycondensation reaction.

[0091] (Crosslinking agent) The functional layer-forming composition may further contain a crosslinking agent from the viewpoint of improving the strength of the coating film. As the crosslinking agent, various known crosslinking agents can be used, for example, melamine compounds, oxazoline compounds, epoxy compounds, isocyanate compounds, carbodiimide compounds, silane coupling compounds, etc. are listed. Among these, melamine compounds are preferably used from the viewpoint of improving the durability of the resin layer. The crosslinking agent may be used alone or in combination of two or more.

[0092] The melamine compound is a compound having a melamine skeleton in the compound, and for example, an alkylolated melamine derivative, a compound obtained by reacting an alkylolated melamine derivative with an alcohol to partially or completely etherify it, and a mixture thereof can be used. Examples of alkylolation include methylolation, ethylolation, isopropylolation, n-butyrolation, isobutyrolation, etc. Among these, methylolation is preferred from the viewpoint of reactivity. As the alcohol used for etherification, methyl alcohol, ethyl alcohol, isopropyl alcohol, n-butanol, isobutanol, etc. are preferably used, and among these, methyl alcohol is more preferred. The melamine compound may be either a monomer or a dimer or higher polymer, or a mixture of these may be used. Furthermore, a product obtained by co-condensing melamine with urea or the like may also be used. Furthermore, in order to increase the reactivity of the melamine compound, a catalyst may be further blended into the resin layer-forming composition.

[0093] The above-mentioned crosslinking agent may be designed to react during the drying process or film-forming process to improve the performance of the resin layer. It is presumed that the formed resin layer contains unreacted crosslinking agent, reacted compound, or a mixture thereof.

[0094] The content of the crosslinking agent in the functional layer is preferably 1 to 50% by mass, more preferably 5 to 40% by mass, and even more preferably 8 to 30% by mass, based on the non-volatile components in the functional layer-forming composition. By making it 1% by mass or more, the effect of blending the crosslinking agent can be easily exhibited. Also, by making it 50% by mass or less, the refractive index can be kept low, and transparency can be maintained.

[0095] The thickness of the functional layer (after drying) is preferably 0.04 μm to 0.15 μm, more preferably 0.06 μm to 0.13 μm. If the thickness of the functional layer is within the above range, the total light transmittance is high and visibility can be improved.

[0096] The method for providing the functional layer is the same as that for forming the antifogging resin layer, and any conventionally known coating method such as reverse gravure coating, direct gravure coating, roll coating, die coating, bar coating, curtain coating, etc. can be used.

[0097] The drying and curing conditions when forming a functional layer on a polyester film are the same as those for forming an anti-fogging resin layer. For example, when providing a functional layer by offline coating, heat treatment is usually performed at 80 to 200°C for 3 to 40 seconds, preferably at 100 to 180°C for 3 to 40 seconds. On the other hand, when the functional layer is provided by in-line coating, it is usually preferable to carry out the heat treatment at 70 to 280° C. for 3 to 200 seconds as a guideline.

[0098] In addition, regardless of whether offline coating or in-line coating is used, heat treatment and irradiation with active energy rays such as ultraviolet light may be used in combination as necessary, and the polyester film constituting the base film may be previously subjected to a surface treatment such as a corona treatment or a plasma treatment, as in the case of forming an anti-fogging resin layer.

[0099] The analysis of various components in the functional layer can be carried out by, for example, TOF-SIMS, ESCA, fluorescent X-ray analysis, etc., in the same manner as the analysis of the anti-fogging resin layer.

[0100] [Characteristics of laminated film] 1) Difference between water drop contact angle and advancing expansion angle The laminate film of the present invention has a difference (advancing contact angle - waterdrop contact angle) of 1° or more between the average waterdrop contact angle 20 to 60 seconds after a water droplet is dropped on the anti-fog resin layer surface and the average advancing contact angle 20 to 60 seconds after liquid is discharged by the expansion method. More specifically, the difference between the average water droplet contact angle 20 to 60 seconds after the drop of water and the average advancing contact angle 20 to 60 seconds after the liquid is ejected by the expansion method, measured using an automatic contact angle meter (DataPhysics, model OCA20), is 1° or more, preferably 3° or more, more preferably 4° or more, and even more preferably 5° or more. It is considered that when a water droplet contacts the surface of the anti-fogging resin layer, a part of the components derived from the anti-fogging resin layer dissolves into the water droplet from the surface of the resin layer and spreads over the surface of the resin layer. Therefore, when the difference between the advancing contact angle and the water droplet contact angle is smaller than 1°, the newly contacted water droplet spreads over the surface of the anti-fogging resin layer faster than the rate at which the anti-fogging resin layer components dissolve into the water droplet, so that the difference in viscosity of the water film formed on the surface of the resin layer becomes large depending on the position of the landed water droplet, causing bleeding, and it is presumed that even if you try to see the scenery on the other side through the film, the visibility is poor and visibility is reduced.

[0101] 2) Water droplet contact angle In the laminate film of the present invention, it is preferable that a contact angle of water dropped on the surface of the anti-fogging resin layer after 60 seconds has elapsed is 35° or less. More specifically, the anti-fog resin layer in the laminate film of the present invention preferably has a contact angle of 35° or less, more preferably 30° or less, even more preferably 25° or less, and particularly preferably 20° or less, 60 seconds after a water droplet is dropped on the anti-fog resin layer, as measured using an automatic contact angle meter (DataPhysics, Model OCA20). When the contact angle is within the above range, the anti-fog performance is excellent.

[0102] 3) Thickness of the anti-fogging resin layer The surface of the anti-fogging resin layer was stained with RuO4 and embedded in epoxy resin. Then, sections prepared by ultra-thin sectioning were stained with RuO4, and the cross section of the anti-fogging resin layer was measured using a transmission electron microscope (TEM) (Hitachi High-Technologies Corporation, H-7650, accelerating voltage 100 kV).

[0103] 4) Anti-fog properties (initial stage) The laminate film of the present invention preferably has an anti-fogging evaluation of rank 2 or higher after exposing the anti-fogging resin layer to a water bath at 40° C. for 1 minute. The rank is based on the following criteria, and the higher the value, the better the result. (Judgment criteria) Rank 1: Water droplets formed on the film surface, causing it to become cloudy and reducing visibility through the film. Rank 2: The water film formed on the film surface was smudged, but had no effect on visibility through the film. Rank 3: No obvious changes were observed on the film surface, and visibility through the film was good.

[0104] 5) Anti-fogging properties after water immersion treatment The laminated film of the present invention preferably has an anti-fogging property evaluation of rank 2 or higher after immersion in water at 23° C. for 1 minute. The ranks are the same as those described above.

[0105] 6) Residual rate of anti-fogging resin layer In the laminate film of the present invention, after immersion in water at 23° C. for 1 hour, the coating film remaining rate of the anti-fogging resin layer is preferably 70% or less, more preferably 55% or less, even more preferably 50% or less, and particularly preferably 45% or less. The smaller the remaining rate of the anti-fogging film, the higher the recyclability. After immersion in water at 23°C for 1 hour, the thickness of the anti-fogging resin layer after immersion was measured in the same manner as in 3) Thickness of the anti-fogging resin layer above. The coating film remaining rate was calculated from the thicknesses of the anti-fogging resin layer before and after immersion. The smaller the coating film remaining rate, the easier it is to remove the anti-fogging resin layer, and the better the recyclability.

[0106] 7) Total light transmittance Measurement was performed in accordance with JIS K 7361 using a haze meter HM-150 manufactured by Murakami Color Research Laboratory Co., Ltd. The total light transmittance is preferably 90% or more, more preferably 93% or more, and further preferably 95% or more.

[0107] [Recycling laminated film] The laminate film of the present invention is characterized by being designed with recycling in mind, that is, to be reused after completing its role after a certain period of use. That is, the laminate film of the present invention is used in a method of reusing the base film (laminate film) by dissolving the anti-fogging resin layer or the functional layer in addition to the anti-fogging resin layer in a solvent or the like, or by peeling it off. More specifically, the anti-fogging resin layer or the functional layer constituting the laminated film is removed using a cleaning agent. Examples of the removal method include an immersion method in which the film is immersed in a cleaning tank containing water or a solvent, a coating method in which water or a solvent is applied, and a spraying method in which vaporized water or a solvent is sprayed. Among these, the immersion method is preferred because of the permeability of water or a solvent to the functional layer. From the viewpoint of ease of handling, the cleaning agent is preferably an aqueous solution, and the solvent is preferably an alcohol.

[0108] Examples of the alcohols include monohydric alcohols such as methyl alcohol, ethyl alcohol, propyl alcohol, butyl alcohol, benzyl alcohol, ethylene glycol monomethyl ether, propylene glycol monomethyl ether, and propylene glycol monoethyl ether; dihydric alcohols such as ethylene glycol, diethylene glycol, and propylene glycol; and polyhydric alcohols such as glycerin. From the viewpoint of cleaning properties, methyl alcohol, ethyl alcohol, propyl alcohol, and benzyl alcohol are more preferable.

[0109] From the viewpoint of cleaning properties, the acidity constant (pKa) of the alcohol is preferably in the range of 10.0 or more and 20.0 or less, more preferably 10.0 or more and 18.0 or less, even more preferably 12.0 or more and 16.0 or less, particularly preferably 14.0 or more and 15.6 or less, and most preferably 14.0 or more and 15.4 or less. The acidity constants (pKa) of some alcohols are as follows: benzyl alcohol (pKa = 15.4), methanol (pKa = 15.5), ethanol (pKa = 16.0), 1-propanol (pKa = 16.1), 2-propanol (pKa = 17.1), 1-butanol (pKa = 16.1), tert-butanol (pKa = 18.0). From the values ​​of the acidity constants (pKa) of alcohols shown above, it can be said that alcohols with an acidity constant (pKa) of 15.4 or less are alcohols with an acidity constant (pKa) smaller than that of methanol.

[0110] The temperature of the solvent in the immersion method is preferably room temperature (20°C) or higher. At room temperature (20°C) or higher, the viscosity of the solvent is low and it is easy to penetrate into the functional layer, so good cleaning properties can be obtained. From the above viewpoints, the temperature of the cleaning agent in the immersion method is more preferably 40°C or higher, even more preferably 50°C or higher, and particularly preferably 60°C or higher. The upper limit of the solvent temperature is preferably a temperature equal to or lower than the boiling point when the cleaning agent is used in a solution state. In the case of an aqueous cleaning agent, which is a preferred embodiment of the present application, the upper limit is preferably 100° C. or lower, and more preferably 80° C. or lower.

[0111] When the laminate film is composed of only an anti-fogging resin layer, water or hot water can be used. When the laminate film is composed of an anti-fogging resin layer and a functional layer, the anti-fogging resin layer or the functional layer can be efficiently removed by appropriately using water or an alcohol solvent, such as using only an alcohol or a combination of water and an alcohol.

[0112] <Explanation of terms> In this specification, when "X to Y" (X and Y are any numbers) is expressed, unless otherwise specified, it includes the meaning of "X or more and Y or less", as well as "preferably greater than X" or "preferably smaller than Y". In addition, when "X or more" (X is any number) or "Y or less" (Y is any number) is expressed, it also includes the meaning of "preferably greater than X" or "preferably less than Y". EXAMPLES

[0113] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples within the scope of the present invention. The measurement and evaluation methods used in the present invention are as follows.

[0114] (1) Intrinsic viscosity of polyester 1 g of polyester from which components incompatible with the polyester had been removed was precisely weighed, dissolved in 100 ml of a mixed solvent of phenol / tetrachloroethane = 50 / 50 (mass ratio), and measured at 30°C.

[0115] (2) Average particle size The coating layer was observed using a TEM (Hitachi H-7650, accelerating voltage 100 V), and the average particle size of 10 particles was determined as the average particle size.

[0116] (3) Thickness of the anti-fogging resin layer The surface of the anti-fogging resin layer was stained with RuO4 and embedded in epoxy resin. Then, sections prepared by ultra-thin sectioning were stained with RuO4, and the cross section of the anti-fogging resin layer was measured using a transmission electron microscope (TEM) (Hitachi High-Technologies Corporation, H-7650, accelerating voltage 100 kV).

[0117] (4) Water droplet contact angle The contact angle of the anti-fog layer surface of a film sample that had been conditioned for more than 24 hours in an environment of 23°C and 50% RH was measured using an automatic contact angle meter (DataPhysics, model OCA20) by contacting a 2 μL water droplet with the anti-fog layer surface, measuring the water droplet contact angle after 60 seconds and the average water droplet contact angle after 20 to 60 seconds.

[0118] (5) Advancing contact angle by the extended method The contact angle of the anti-fog layer surface of a film sample that had been conditioned for more than 24 hours in an environment of 23°C and 50% RH was measured using an automatic contact angle meter (DataPhysics, model OCA20) by contacting a 2 μL water droplet with the anti-fog layer surface, then contacting the tip of a water supply syringe with the center of the resulting droplet and supplying water at a flow rate of 0.06 μL / sec., and measuring the average advancing contact angle of the water droplet after 20 to 60 seconds.

[0119] (6) Anti-fog properties (initial) The anti-fogging resin layer was exposed to a water bath at 40° C. for 1 minute, and then the anti-fogging properties were evaluated according to the following criteria. (Judgment criteria) Rank 1: Water droplets formed and clouded the view through the film. Rank 2: A water film formed and blurred the image, but visibility through the film was good. Rank 3: Visibility through the film was not affected.

[0120] (7) Anti-fogging evaluation after water immersion treatment The sample film was immersed in water at 23° C. for 1 minute, and then evaluated according to the same criteria as for anti-fogging property (initial).

[0121] (8) Residual rate of anti-fogging resin layer After immersion in water at 23° C. for 1 hour, the thickness of the anti-fogging resin layer after immersion was measured in the same manner as in (3) Film Thickness of the Anti-Fogging Resin Layer. The smaller the coating film remaining rate, the easier it is to remove the anti-fogging resin layer, and the better the recyclability.

[0122] (9) Film Haze The haze of the laminated film was measured in accordance with JIS K 7361 using a haze meter HM-150 manufactured by Murakami Color Research Laboratory Co., Ltd.

[0123] (10) Total light transmittance The total light transmittance of the laminated film was measured in accordance with JIS K 7361 using a haze meter HM-150 manufactured by Murakami Color Research Laboratory Co., Ltd. The evaluation criteria were as follows: ◎: Total light transmittance is 95% or more 〇: Total light transmittance is 93% or more but less than 95% △: Total light transmittance is 90% or more but less than 93% ×: Total light transmittance is less than 90%

[0124] (11) Method for measuring absolute minimum reflectance from functional layer First, black tape (Vinyl tape VT-50 manufactured by Nichiban Co., Ltd.) was applied to the back surface of the functional layer to be measured (the surface of the anti-fogging resin layer), and the absolute reflectance of the functional layer surface in the wavelength range of 300 to 800 nm was measured using a spectrophotometer (UV-Visible Spectrophotometer V-670 manufactured by JASCO Corporation and Automatic Absolute Reflectance Measurement Device ARMN-735) in synchronous mode, with an incident angle of 5°, N polarization, Fast response, data collection interval of 1.0 nm, bandwidth of 10 nm, and scanning speed of 1000 m / min, and the wavelength at the minimum value (bottom wavelength) and absolute reflectance were evaluated.

[0125] (12) Antibacterial performance The antibacterial activity values ​​against Escherichia coli and Staphylococcus aureus after 24-hour incubation were measured in accordance with JIS Z 2801. The untreated test specimen used for calculating the antibacterial activity value was a biaxially stretched polyester film that had not been subjected to a surface treatment (a film prepared in the same manner as in Example 1 except that no antifogging resin layer was applied).

[0126] (13) Overall rating The anti-fogging properties (initial and after water immersion treatment) and the remaining rate of the anti-fogging resin layer were evaluated comprehensively. A: Anti-fogging performance is rank 3, and the remaining coating rate is 30% or less. B: Anti-fogging property (initial) is rank 3, anti-fogging property (after water immersion treatment) is rank 2, and the coating film remaining rate is 30% or less. C: Anti-fogging properties are both rank 2, and the coating film remaining rate is 30% or less, or the anti-fogging property (initial) is rank 3, the anti-fogging property (after water immersion treatment) is rank 2, and the coating film remaining rate is more than 30%. D: Anti-fogging performance is rank 2, and the coating film remaining rate is greater than 30%. E: At least one of the anti-fog properties is rank 1

[0127] The polyester raw materials used in the examples and comparative examples are as follows:

[0128] <Production method of polyester (1)> 100 parts by mass of dimethyl terephthalate and 55 parts by mass of ethylene glycol were used as starting materials, and 0.04 parts by mass of magnesium acetate tetrahydrate was added to the reactor as a catalyst. The reaction was started at 150°C, and the reaction temperature was gradually increased as methanol was distilled off, reaching 230°C after 3 hours. After 4 hours, the transesterification reaction was essentially completed. 0.02 parts by mass of ethyl acid phosphate was added to this reaction mixture, and then 0.04 parts by mass of antimony trioxide was added, and the polycondensation reaction was carried out for 4 hours. The temperature was gradually increased from 230°C to 280°C. Meanwhile, the pressure was gradually reduced from normal pressure, and finally reached 0.3 mmHg. After the start of the reaction, the reaction was stopped at the point corresponding to an intrinsic viscosity of 0.65 due to a change in the stirring power of the reaction vessel, and the polymer was discharged under nitrogen pressure to obtain polyester (1) with an intrinsic viscosity of 0.65.

[0129] <Production method of polyester (2)> 100 parts by mass of dimethyl terephthalate and 45 parts by mass of ethylene glycol were used as starting materials, and 0.06 parts by mass of magnesium acetate tetrahydrate was added to the reactor as a catalyst. The reaction was started at 150°C, and the reaction temperature was gradually increased as methanol was distilled off, reaching 230°C after 3 hours. After 4 hours, the transesterification reaction was essentially completed. 0.03 parts by mass of ethyl acid phosphate was added to this reaction mixture, and then 0.3 parts by mass of silica particles with an average particle size of 2.7 μm dispersed in ethylene glycol and 0.03 parts by mass of antimony trioxide were added, and the polycondensation reaction was carried out for 4 hours. The temperature was gradually increased from 230°C to 280°C. Meanwhile, the pressure was gradually reduced from normal pressure, and finally reached 0.3 mmHg. After the start of the reaction, the reaction was stopped at the point corresponding to an intrinsic viscosity of 0.65 due to changes in the stirring power of the reaction vessel, and the polymer was discharged under nitrogen pressure to obtain polyester (2) with an intrinsic viscosity of 0.65.

[0130] The following composition was used as the anti-fogging resin layer composition. (A) Polyvinyl alcohol resin (including modified polyvinyl alcohol resin) A1: PVA (PVA-based resin) with a saponification degree of 88 mol% and an average polymerization degree of 600 A2: PVA having a polyethylene oxide group with a saponification degree of 50 mol% and an average polymerization degree of 200 (modified PVA resin) (B) Acid catalyst 2-Sulfobenzoic anhydride (C) Ammonium base-containing compounds Poly(trimethylammonium ethyl methacrylate methanesulfonate), number average molecular weight 30000 (D) Crosslinking agent D1: Oxazoline compound: Acrylic polymer containing oxazoline groups (oxazoline group amount 4.5 mmol / g) D2: Epoxy crosslinker: Water-soluble polyglycerol polyglycidyl ether (glycidyl group amount 6.5 mmol / g) D3: Melamine compound: Partially etherified melamine having methylol, methoxy and imino groups (total functional amount of methylol, methoxy and imino groups: 19.8 mmol / g) (E) Other ingredients E1: Polyaminopropyl biguanide hydrochloride (organic antibacterial agent) E2: Sucrose fatty acid ester (Rikemal A, manufactured by Riken Vitamin Co., Ltd.)

[0131] (Functional layer forming composition 12) A composition of fluorine-containing compound:melamine compound=80:20 (mass%) Fluorine-containing compound: Water dispersion of fluorine-based polyether urethane resin, in which isophorone diisocyanate / dimethylolpropanoic acid / perfluoroether glycol (copolymer of difluoroethylene oxide: difluoromethylene oxide: tetrafluoroethylene oxide = 5: 43: 52 (mol%)) = 49 / 28 / 23 (mol%)

[0132] Example 1 A blend of polyester (1) and polyester (2) in a mass ratio of 92 / 8 was used as the raw material for layer A, and polyester (1) alone was used as the raw material for layer B. The layers were fed into an extruder, heated and melted at 285°C, and the layer A was divided into two parts to form a layer structure of two types of three layers (A / B / A) with layer B as the middle layer, and the layer structure was co-extruded under extrusion conditions with a thickness composition ratio of A / B / A=5 / 90 / 5. The film was cooled and solidified while being in close contact with a mirror-finished cooling drum with a surface temperature of 40-50°C to produce an unstretched polyethylene terephthalate film. The film was stretched 3.7 times in the longitudinal direction while passing through a group of heating rolls at 85°C to produce a uniaxially oriented film. The anti-fog resin layer composition 1 shown in Table 1 below was applied to one side of this uniaxially stretched film, and then the film was introduced into a tenter stretching machine and stretched 4.3 times in the width direction at 100°C. After further heat treatment at 230°C, a 2% relaxation treatment was performed in the width direction to obtain a 50 μm thick biaxially oriented polyester film having an anti-fog resin layer with a film thickness (after drying) of 0.07 μm.

[0133] Examples 2 to 10 and Comparative Example 1 The same procedure as in Example 1 was carried out except that the anti-fogging resin composition was changed as shown in Tables 1 and 2, to obtain a laminated film.

[0134] Example 11 In Example 1, anti-fogging resin composition 4 shown in Table 1 below was applied to one side of the uniaxially stretched film to obtain a uniaxially oriented polyester film having a thickness of 50 μm and an anti-fogging resin layer having a thickness (after drying) of 0.07 μm.

[0135] Example 12 In Example 1, the anti-fog resin layer composition 4 was applied to one side of the uniaxially stretched film, and the anti-fog resin composition 4 was also applied to the other side of the uniaxially stretched film so that the film thickness (after drying) was 0.09 μm. The film was then introduced into a tenter stretching machine, stretched 4.3 times in the width direction at 100°C, and further heat-treated at 230°C, followed by a 2% relaxation treatment in the width direction to obtain a biaxially oriented polyester film having an anti-fog resin layer with a thickness (after drying) of 0.07 μm and an anti-fog resin layer with a thickness (after drying) of 0.09 μm on the other side.

[0136] Example 13 In Example 1, anti-fog resin composition 4 shown in Table 1 below was applied to one side of an unstretched polyethylene terephthalate film, and resin composition 12 described above was applied to the other side to obtain an unstretched polyester film having a thickness of 250 μm and an anti-fog resin layer having a thickness (after drying) of 0.07 μm and a functional layer (visibility improving layer) having a thickness (after drying) of 0.09 μm on the other side.

[0137] Reference example 1 A laminated film was obtained in the same manner as in Example 1, except that anti-fog resin composition 11 was used instead of anti-fog resin composition 1 in Example 1.

[0138] [Table 1]

[0139] [Table 2]

[0140] The anti-fogging resin composition and laminated film of the present invention maintain good anti-fogging performance and have good recyclability. For example, they are suitable for various applications requiring anti-fogging properties, such as agricultural, medical, and packaging applications. Among these, they are particularly suitable for face shields. Furthermore, they are particularly suitable for disposable applications, and can be collected and recycled.

Claims

1. An anti-fogging resin composition comprising (A) a polyvinyl alcohol-based resin having a degree of saponification of 50 to 99 mol% and an average degree of polymerization of 200 or more and 1,800 or less, and (C) an ammonium base-containing compound, wherein the content of the ammonium base-containing compound (C) is 50% by mass or less and 5% by mass or more, as a proportion of all non-volatile components in the anti-fogging resin composition.

2. An anti-fogging resin composition as described in claim 1, wherein the polyvinyl alcohol-based resin includes a modified polyvinyl alcohol-based resin.

3. The anti-fogging resin composition according to claim 1 or 2, further comprising (D) a crosslinking agent.

4. An anti-fogging resin composition as described in claim 3, wherein the content of the (D) crosslinking agent is 20 mass% or less as a proportion of all non-volatile components in the anti-fogging resin composition.

5. A laminated film comprising an anti-fogging resin layer formed on at least one surface of a substrate film from the anti-fogging resin composition according to any one of claims 1 to 4.

6. A laminated film having an anti-fog resin layer formed on at least one surface of a base film from an anti-fog resin composition, the anti-fog resin composition comprising (A) a polyvinyl alcohol-based resin having a degree of saponification of 50 to 99 mol% and an average degree of polymerization of 200 or more and 1,800 or less, and (C) an ammonium base-containing compound, and the anti-fog resin layer has a thickness (after drying) of 0.01 μm to 1 μm.

7. A laminated film as described in claim 5 or 6, in which the difference (advancing contact angle - water droplet contact angle) between the average water droplet contact angle 20 to 60 seconds after a water droplet is dropped on the surface of the anti-fogging resin layer and the average advancing contact angle 20 to 60 seconds after liquid is ejected by the expansion method is 1° or more.

8. 8. The laminate film according to claim 5, wherein a contact angle of water dropped on a surface of the anti-fogging resin layer after 60 seconds is 35° or less.

9. The laminate film according to any one of claims 5 to 8, wherein the anti-fogging resin layer is exposed to a water bath at 40°C for 1 minute and then evaluated for anti-fogging properties as rank 2 or higher. Rank 2: A water film formed and blurred the image, but visibility through the film was good.

10. The laminate film according to any one of claims 5 to 9, which has an anti-fogging property evaluation of rank 2 or higher after a water immersion treatment (immersion at 23°C for 1 minute). Rank 2: A water film formed and blurred the image, but visibility through the film was good.

11. The laminate film according to any one of claims 5 to 10, wherein after immersion in water at 23°C for 1 hour, the coating remaining rate (%) of the anti-fogging resin layer is 55% or less.

12. The laminate film according to any one of claims 5 to 11, wherein the base film is a polyester film.

13. The laminate film according to any one of claims 5 to 12, wherein the base film is a polyester film that is unstretched or stretched at least uniaxially.

14. The laminate film according to any one of claims 5 to 13, wherein the anti-fogging resin layer has a thickness (after drying) of 0.01 µm to 1 µm.

15. The laminate film according to any one of claims 5 to 14, further comprising a functional layer on the opposite side of the anti-fogging resin layer.

16. The laminate film according to claim 15 , wherein the functional layer is a visibility improving layer.

17. The laminate film according to claim 16, wherein the visibility improving layer is a resin layer obtained by curing a resin composition containing a fluorine-containing compound and a crosslinking agent.

18. A method for using a laminate film according to any one of claims 5 to 17, comprising treating the laminate film with water and / or an alcohol-based solvent and then reusing the laminate film.

19. A method for using a laminated film, comprising treating the laminated film having an anti-fog resin layer formed from an anti-fog resin composition on at least one surface of a base film with water and / or an alcohol-based solvent and then reusing the laminated film, wherein the anti-fog resin composition contains (A) a polyvinyl alcohol-based resin having a saponification degree of 50 to 99 mol% and an average polymerization degree of 200 or more and 1,800 or less, and also contains at least one selected from (B) an acid catalyst and (C) an ammonium base-containing compound.

20. A method for using the laminated film described in claim 19, wherein the content of the (B) acid catalyst is 0.1 mass% or more and 10 mass% or less, and the content of the (C) ammonium base-containing compound is 5 mass% or more and 50 mass% or less, as a proportion of all non-volatile components in the anti-fogging resin composition.

21. The anti-fogging resin composition according to any one of claims 1 to 4, which is for a face shield.

22. The laminate film according to any one of claims 5 to 17, which is for a face shield.

23. A method for using the laminate film according to any one of claims 18 to 20 as a face shield.

Citation Information

Patent Citations

  • JP1974070885A

  • Easy-to-adhere polyester film and method for producing the same

    JP1993310976A

  • Hygroscopic Anti-fogging film and method of manufacturing the same

    JP2001145982A

  • Hydrophilic material, hydrophilic member, method for manufacturing them, and hydrophilic coating agent set

    JP2002355916A

  • Needle-shaped silica coating to enhance hydrophilicity / transmittance

    JP2011530401A