Laminated lid material and packaging container
A laminated lid material with a specific adhesive layer composition and structure addresses the challenge of resisting benzoic acid and retort heat sterilization, ensuring durable sealing and leak prevention.
Patent Information
- Application Number
- JP2020213780
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-12-23
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2040-12-23
AI Technical Summary
Existing laminated lid materials for contact lens storage solutions fail to provide sufficient resistance to both benzoic acid and retort heat sterilization at 120°C, leading to delamination and potential leaks.
A laminated lid material structure comprising a base material layer, an aluminum layer, an adhesive layer made of maleic anhydride graft polymerized polypropylene with a specific molecular weight range, and an easy peel layer, which enhances resistance to benzoic acid and maintains integrity during retort sterilization.
The laminated lid material achieves robust adhesion and prevents delamination, ensuring effective sealing and resistance to benzoic acid even under retort heat sterilization conditions, maintaining a strong seal and preventing leaks.
Smart Images

Figure 0007563166000002 
Figure 0007563166000003 
Figure 0007563166000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a laminated lid material and a packaging container which are resistant to retort sterilization and exhibit excellent resistance to contents in a contact lens storage solution containing benzoic acid as a preservative. [Background technology]
[0002] As one mode of distribution of sanitary materials such as disposable contact lenses, they are provided in a container immersed in a storage solution, and are opened and removed from the storage solution when used. Since contact lenses require sterilization, the container containing the storage solution and contact lenses may be sterilized by retort treatment after being sealed. Such laminated films are required to have retort resistance, that is, not to undergo delamination (peeling of laminated layers) even when subjected to high-temperature sterilization treatment such as retort treatment.
[0003] In addition, as the lid material for such containers, laminated films having gas barrier properties that block the intrusion of water vapor, oxygen, and other gases that can deteriorate the contents are used in order to prevent deterioration or spoilage of the contents and to maintain their functions and properties.
[0004] In the manufacture of laminated films with gas barrier properties, even for applications such as resistant packaging materials for retort heat sterilization, urethane two-component curing type dry lamination adhesives are generally used as adhesives to form adhesive layers. However, many of the contents packed in the packaging materials contain alkaline substances, fragrances, surfactants, high boiling point organic solvents, etc., and packaging these contents can have a detrimental effect on the dry lamination adhesive layer, leading to a decrease in the lamination strength of the laminate or peeling. Content resistance to the extent that delamination due to these contents does not occur is also required.
[0005] In order to cope with such circumstances, various improvements have been made to the adhesives used in lamination, and adhesives with alcohol resistance have been proposed (see Patent Document 1).
[0006] In addition, as an adhesive layer, a laminated film using maleic anhydride graft-polymerized polypropylene with a maleic anhydride graft ratio of 0.1 Wt% or more and 1 Wt% or less has been proposed as a film that has excellent adhesion to a wide variety of transparent barrier films and aluminum foils and has excellent retort resistance and content resistance (see Patent Document 2). [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Patent No. 5915710 [Patent Document 2] JP 2020-49896 A Summary of the Invention [Problem to be solved by the invention]
[0008] In addition to alcohol, benzoic acid is sometimes used as a preservative in preservative solutions for sanitary materials. However, since benzoic acid has a strong attack on adhesives, when using sanitary materials that use such preservative solutions, it is necessary to consider resistance to benzoic acid in addition to retort processing.
[0009] For this reason, in the case of a contact lens covering material, both resistance to the contents of the storage solution containing benzoic acid and resistance to retort heat sterilization are required. However, in the dry lamination of the above-mentioned Patent Document 1, when the contents are benzoic acid, the lamination strength between the aluminum layer and the sealant layer decreases over time, resulting in delamination (peeling). Furthermore, a laminate obtained using an anchor coating agent as in Patent Document 2 has resistance to contents, but has the problem of insufficient resistance to retort heat sterilization in a 120°C environment.
[0010] In addition, when sealing the container and lid, it is necessary to make the seal strong to prevent leaks. However, by making the seal strong, the seal layer becomes thin, and it cannot withstand the internal pressure during retort sterilization, causing the aluminum layer / adhesive layer to peel off, resulting in leaks.
[0011] In view of the above circumstances, the present invention aims to provide a laminated lid material and a packaging container that have resistance to contents containing benzoic acid and resistance to retort heat sterilization in a 120°C environment. [Means for solving the problem]
[0012] In order to solve the above problems, the present invention provides a film-forming material having a base layer, an aluminum layer, an adhesive layer, and an easy-peel layer laminated in this order from the surface layer, the adhesive layer has a layer containing maleic anhydride graft-polymerized polypropylene as a main component, The maleic anhydride graft-polymerized polypropylene has a weight average molecular weight of 300,000 to 350,000.
[0013] As an adhesive layer between the aluminum layer and the sealant layer, which is affected by the contents, maleic anhydride grafted polypropylene is used, and by adjusting the graft ratio, it is possible to provide resistance to the contents and retort. In addition, by designing the resin with a small weight average molecular weight, it is easier to increase the crystallinity of the resin, and by increasing heat resistance, it is possible to achieve sufficient adhesive strength even in a 120℃ environment.
[0014] The invention described in claim 2 is the laminated covering material described in claim 1, characterized in that the maleic anhydride graft rate of the maleic anhydride graft-polymerized polypropylene is 0.1 wt % or more and 1 wt % or less.
[0015] In addition, the invention described in claim 3 is a laminated covering material described in either claim 1 or claim 2, characterized in that the laminate strength between the aluminum layer and the adhesive layer measured in accordance with JIS-K6854 in an environment of 120°C is 2.0 N / 15 mm or more.
[0016] The invention described in claim 4 is a packaging container comprising a resin container body and the laminated lid material described in any one of claims 1 to 3 that is joined to the container body to seal the container body. Effect of the Invention
[0017] The laminated lid material of the present invention has sufficient resistance to retort treatment and benzoic acid. [Brief description of the drawings]
[0018] [Figure 1] 1 is a schematic cross-sectional view showing a packaging container provided with a laminated lid material according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic cross-sectional view of the laminated lid material. [Diagram 3] 1 is a schematic cross-sectional view of a laminated film according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] An embodiment of the present invention will be described with reference to Figs. 1 and 2. Fig. 1 is a cross-sectional view that shows a packaging container 100 equipped with a laminated lid material 1 of this embodiment. The packaging container 100 includes a resin container body 101 and a laminated lid material 1 that seals the upper opening of the container body 101. The container body 101 is filled with a preservative (contents), and a contact lens is immersed in the preservative. The preservative contains benzoic acid as a preservative. The packaging container 100 is sealed with the laminated lid material 1 and then retorted, thereby sterilizing the preservative and contact lens contained in the container body.
[0020] 2 shows a schematic cross-sectional view of the laminated lid material 1. The laminated lid material 1 comprises a base layer 2, an aluminum layer 3, an adhesive layer 7, and an easy-peel layer 4.
[0021] <Base material layer> For example, a resin film can be used as the base layer 2. As the resin forming the resin film, polyester is suitable from the viewpoint of heat resistance and suitability for various processes, but is not limited thereto. For example, polyolefin resins such as polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polyethylene-2,6-naphthalate, polybutylene terephthalate, and copolymers thereof; polyolefin resins such as polyethylene and polypropylene; polyamide resins such as nylon-6, nylon-66, and nylon-12; hydroxyl group-containing polymers such as polyvinyl alcohol and ethylene-vinyl alcohol copolymers, and the like can also be used. These resins may be used alone or in combination of two or more.
[0022] The substrate layer 2 may be a stretched film or an unstretched film. Among them, a uniaxially stretched film or a biaxially stretched film is preferable, and a biaxially stretched film is more preferable, from the viewpoint of excellent mechanical strength and dimensional stability. The substrate layer 2 may be a single layer structure made of one substrate film, or a multilayer structure in which two or more substrate films are laminated.
[0023] The thickness of the base layer 2 is not particularly limited, but may be, for example, 3 to 200 μm, and preferably 6 to 30 μm. The base layer 2 has a printed layer 5 on one surface. The printed layer 5 may appropriately include information about the contents, various patterns, and the like. In FIG. 2, the printed layer 5 is formed on the surface on the container body 101 side, but it may be formed on the opposite surface, or on both surfaces. Furthermore, the printed layer 5 may be omitted.
[0024] <Aluminum layer> The aluminum layer 3 has a gas barrier function. As the aluminum layer 3, aluminum foil, an aluminum vapor deposition layer, or the like can be used. In this embodiment, the aluminum layer 3 is formed by bonding the aluminum foil to the printed layer 5 with an adhesive layer 6. As the adhesive layer 6, various types of adhesives for dry lamination can be used, and examples thereof include a two-component adhesive consisting of a polyol component and an isocyanate component.
[0025] <Easy peel layer> The easy peel layer 4 bonds the laminated lid material 1 and the container body 101 to maintain the sealed state of the packaging container 100 and facilitate the opening operation. As the easy peel layer 4, various known easy peel sealant films (polypropylene-based, etc.) can be appropriately selected and used. The easy peel layer 4 is bonded to the aluminum layer 3 by an adhesive layer 7. The bonding method of the easy peel layer 4 can be extrusion lamination, in which the resin that becomes the adhesive layer 7 is extruded as a single layer or co-extruded.
[0026] <Adhesive layer> The adhesive layer 7 mainly contains maleic anhydride graft-polymerized polypropylene (hereinafter referred to as "modified PP") on the side in contact with the aluminum layer 3. The adhesive layer 7 may be a single layer, or may have another layer on the side of the easy-peel layer 4. An example of the material of the other layer is unmodified polypropylene. Modified PP is polypropylene graft-modified with maleic anhydride. Propylene. Examples of the polypropylene in the modified PP include homopolypropylene, block polypropylene, random polypropylene, propylene-α-olefin copolymer, etc. Examples of the α-olefin include ethylene, 1-butene, etc.
[0027] It has been found that in order to construct a laminated lid material that is highly resistant to retort treatment and benzoic acid, it is preferable to use modified PP for the adhesive layer 7, and that the effect is more pronounced when the maleic anhydride graft rate of the modified PP is 0.1 weight percent (wt%) or more and 1 wt% or less and the weight average molecular weight is 300,000 to 350,000.
[0028] If the maleic anhydride grafting rate is less than 0.1% by weight, sufficient adhesive strength with the aluminum layer 3 cannot be obtained, and there is a high possibility that delamination may occur during sterilization, etc. On the other hand, if the maleic anhydride grafting rate exceeds 1% by weight, the resin properties become unstable. Specifically, the reaction catalyst used during grafting promotes the decomposition of the PP resin itself, resulting in a smaller molecular weight and an extremely increased melt flow rate (MFR), which causes the film-forming suitability to be lost. As a result, the film strength of the formed adhesive layer decreases, and there is a possibility that a defect of insufficient adhesive strength cannot be obtained occurs.
[0029] In addition, the weight average molecular weight of the modified PP is preferably 300,000 to 350,000. By designing the resin with a small weight average molecular weight, it becomes easier to increase the crystallinity of the resin, and by increasing the heat resistance, sufficient adhesive strength can be obtained even in a 120°C environment. If it is less than 300,000, the film forming suitability is poor, and if it exceeds 350,000, it becomes difficult to increase the crystallinity. The adhesive layer 7 may contain other resins as long as it is mainly composed of modified PP. An example of a resin other than modified PP used in the adhesive layer 7 is unmodified polypropylene.
[0030] The resin forming the container body 101 may be any resin that can bond the easy peel layer 4, and a resin of the same type as the easy peel layer 4 can be selected in accordance with the easy peel layer 4.
[0031] A storage solution and a contact lens are placed in the container body 101, and the laminated lid material 1 is placed with the easy-peel layer 4 facing the container body 101. Thereafter, when the contact area between the laminated lid material 1 and the container body 101 is heated and pressurized, the laminated lid material 1 is bonded to the container body, and the packaging container 100 with the inside of the container body 101 sealed is completed.
[0032] Since the laminated lid material 1 has the above-mentioned configuration, even when the preservative solution contains benzoic acid and the manufactured packaging container 100 is sterilized by retort treatment, the sealed state is suitably maintained and delamination (peeling) between the aluminum layer 3 and the easy-peel layer 4 is suitably suppressed. As a result, even in an environment of 120°C, which is almost the same temperature as during retort treatment, the laminate strength between the aluminum layer 3 and the adhesive layer 7 can be made 2.0 N / 15 mm or more. The laminated lid material 1 and the packaging container 100 provided with the same are suitable for packaging various sanitary materials that contain benzoic acid or require sterilization. In addition, since dry lamination is not required and the bonding strength increases with retort treatment, no curing step is required during production, and production efficiency is high.
[0033] The laminated lid material 1 and the packaging container 100 of the present invention will be further described using examples. The technical scope of the present invention should not be narrowly interpreted only by the following description. EXAMPLES
[0034] (Example) A polyester film (FE2001, manufactured by Futamura Chemical Co., Ltd.) having a thickness of 16 μm was prepared as the base layer 2. An aluminum foil (manufactured by Toyo Aluminum Co., Ltd.) having a thickness of 50 μm was bonded to one side of the base layer 2 by dry lamination using an adhesive consisting of an ester main chain base agent (A525, manufactured by Mitsui Chemical Co., Ltd.) and a curing agent (A52, manufactured by Mitsui Chemical Co., Ltd.), forming an adhesive layer 6 and an aluminum layer 3. An easy peel sealant film (9501H, manufactured by Toray Film Processing Co., Ltd.) having a thickness of 30 μm was used as the easy peel layer 4, and an adhesive layer 7 and an easy peel layer 4 were formed on the aluminum layer 3 by extrusion lamination. A modified PP (A) (melting point peak: 141° C., density: 0.90 g / cm 3 ) was used as the adhesive layer 7. 3 , MFR: 15g / 10min) and unmodified random polypropylene F329RA (melting point peak: 141°C, density: 0.91g / cm 3Two types of resins were used: modified PP (A) and modified PP (MFR: 25g / 10min). The thickness of each layer was 12μm, and the layer made of modified PP was laminated on the aluminum layer side. The laminated film was heated at 140°C for 15 seconds by being held by a heater roll to produce a laminated lid material. The weight average molecular weight (Mw) of the adhesive layer 7 using modified PP (A) was 326,000.
[0035] (Comparative Example) As a comparative example, different brands of modified PP for the adhesive layer were evaluated. Instead of modified PP (A), modified PP (B) (melting point peak: 103, 133 to 155 °C, density: 0.89 g / cm 3 A laminated film and a laminated lid material of Comparative Example 1 were produced in the same manner as in Example 1, except that modified PP (B) was used. The weight average molecular weight (Mw) of the adhesive layer 7 using modified PP (B) was 391,000.
[0036] FIG. 3 is a schematic cross-sectional view showing the configuration of the laminated films of the examples and comparative examples prepared as described above.
[0037] The laminated films and packaging containers of each of the Examples and Comparative Examples were used to carry out the following evaluations.
[0038] (Quantitative analysis of maleic anhydride graft ratio) The maleic anhydride graft ratio can be measured by the following method. The additives in the sample were removed, and the grafted maleic anhydride sites were methyl esterified, and then 1 H-NMR measurement was performed. 1 The amount of grafted maleic anhydride is calculated from the H-NMR spectrum.
[0039] [Measurement conditions] Equipment: JEOL EX-400 type Observation kernel: 1 H Solvent:ODCB / C6D6(4 / 1) Temperature: 130℃
[0040] (Measurement of weight average molecular weight) The polystyrene (PS) equivalent molecular weight distribution of each laminate film was calculated by gel permeation chromatography (GPC) under the following measurement conditions.
[0041] [Measurement conditions] Equipment: Agilent PL-GPC220 Column: Agilent PLgel Olexis 2 columns + Guard Dissolving solution: o-dichlorobenzene Temperature: 145℃ Concentration: 0.1wt / vol% Flow rate: 1.0ml / min Pretreatment: Hot filtration (0.5 μm pore size filter) Solubility: Completely soluble Detector: Differential refractive index system (RI)
[0042] (Laminate strength measurement) A test piece with a width of 15 mm was cut out from each laminate film. The laminate strength (between the aluminum layer and the easy peel layer) was measured using a tensile tester at room temperature (20°C, 30% RH) and at a speed of 300 mm / min in accordance with JIS-K6854.
[0043] (Leak test) A leak test was conducted as follows to evaluate the benzoic acid-containing contents and the sealing retention against retort treatment of each example. 0.6 mL of saturated benzoic acid aqueous solution was filled into the packaging container 100, and the laminated lid material 1 of each example was sealed to seal it. In this way, the packaging container 100 according to each example was produced. After the packaging container 100 of each example was subjected to retort sterilization treatment under conditions of 120°C and 30 minutes, a hole was made in the container body to remove the saturated benzoic acid aqueous solution, and ink was poured in, and the presence or absence of ink leakage at the joint between the laminated lid material 1 and the container body 101 was visually confirmed. The two-level evaluation was conducted: "○ (good)" for no leakage, and "× (bad)" for leakage.
[0044] The results are shown in Table 1.
[0045] [Table 1]
[0046] As shown in Table 1, in the example in which the weight average molecular weight (Mw) of the adhesive layer 7 was 326,000, the laminate strength between the aluminum layer 3 and the adhesive layer 7 in a 120°C environment was high, and leakage after retort treatment was prevented. On the other hand, in the comparative example in which the weight average molecular weight (Mw) of the adhesive layer 7 was 391,000, the laminate strength in a 120°C environment was insufficient. In addition, the adhesive layer 7 could not be kept sealed after retort treatment, and leakage occurred.
[0047] As described above, the present invention makes it possible to provide a laminated lid material and a packaging container that have resistance to contents containing benzoic acid and resistance to retort heat sterilization in a 120°C environment. [Explanation of symbols]
[0048] 1. Laminated lid material 2...Base material layer 3. Aluminum layer 4. Easy peel layer 5...printing layer 6...Adhesive layer 7...adhesive layer 100...Packaging containers 101... Container body
Claims
1. From the surface layer, a base layer, an aluminum layer, an adhesive layer, and an easy-peel layer are laminated in this order, the adhesive layer has a layer containing maleic anhydride graft-polymerized polypropylene as a main component, A laminated covering material characterized in that the weight average molecular weight of the maleic anhydride graft-polymerized polypropylene is 300,000 to 350,000.
2. 2. The laminated covering material according to claim 1, wherein the maleic anhydride grafted polypropylene has a maleic anhydride grafting rate of 0.1 wt % or more and 1 wt % or less.
3. The laminated lid material according to claim 1 or 2, characterized in that the laminate strength between the aluminum layer and the adhesive layer measured in accordance with JIS-K6854 in a 120°C environment is 2.0 N / 15 mm or more.
4. A resin container body; The laminated lid material according to any one of claims 1 to 3, which is joined to the container body to seal the container body; A packaging container comprising:
Citation Information
Patent Citations
Retort sterilizable hermetricall sealed package
JP1980012029A
Pulse combustion device
JP1984015710A
Multi-layer laminated material and its manufacture
JP1992189537A
Adhesive sealing member
JP2011213767A
Adhesive for packaging material, packaging material and method for producing packaging material
JP2019038950A