Laminated Film

The laminated film with an acid-modified polyolefin and hydrophobic oxide particles addresses adhesion and repellency issues, providing durable and transparent water and oil repellency.

JP7563376B2Active Publication Date: 2024-10-08TOYOBO CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2021503937
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-08-11
Filing Date
2021-01-05
Publication Date
2024-10-08
Estimated Expiration
2041-01-05

AI Technical Summary

Technical Problem

Existing laminated films face issues with low adhesion between the base film and coating layer, leading to poor durability and difficulty in maintaining transparency while achieving water and oil repellency.

Method used

A laminated film configuration with a coating layer containing acid-modified polyolefin and hydrophobic oxide particles, where the acid-modified polyolefin has an acid value of 1 mgKOH/g to 60 mgKOH/g and hydrophobic oxide particles have an average primary particle diameter of 5 nm to 300 nm, ensuring strong adhesion and excellent water and oil repellency.

Benefits of technology

The laminated film achieves excellent water and oil repellency with strong adhesion to the base film, maintaining high transparency and durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007563376000001
    Figure 0007563376000001
  • Figure 0007563376000002
    Figure 0007563376000002
  • Figure 0007563376000003
    Figure 0007563376000003
Patent Text Reader

Abstract

The present invention addresses the problem of providing a laminated film showing excellent water and oil repellency and having good adhesion between a base film and a coating layer. To solve the problem, a laminated film is formed by laminating at least one coating layer on a base film, wherein: the coating layer contains an acid-modified polyolefin and hydrophobic oxide particles; and the acid-modified polyolefin has an acid value of 1-60 mgKOH / g. Preferably, a laminated film, in which the surface of the coating layer has a contact angle with respect to water of at least 100 degrees, is provided as a solution.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a laminated film, and more particularly to a coated laminated film having water- and oil-repellent properties. [Background technology]

[0002] Materials that exhibit water- and oil-repellent properties on their surfaces are industrially important in fields where antifouling is required. To achieve antifouling, it is necessary to reduce the interaction between contaminants and the material surface, which is usually achieved by making the material surface water- and oil-repellent.

[0003] Conventionally, known water-repellent treatment methods for achieving water repellency include a method of applying a fluorine-based resin or a silicone-based resin, which has a lower surface energy than water, to the film surface, and a method of forming fine irregularities on the film surface in addition to the above (see, for example, Patent Documents 1 to 4).

[0004] However, in general, coating methods for imparting water repellency to a film surface have the problem that the adhesion to the substrate is low and the coating layer easily falls off. In addition, even if a film with a water-repellent and oil-repellent surface can be formed, the film's transparency is generally not maintained, and the film's properties as a film material are not necessarily sufficient. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2000-284102 A [Patent Document 2] JP 2002-113805 A [Patent Document 3] JP 2018-103534 A [Patent Document 4] JP 2007-138027 A Summary of the Invention [Problem to be solved by the invention]

[0006] The present invention has been made in view of the problems in the conventional technology. That is, an object of the present invention is to provide a laminated film that exhibits excellent water and oil repellency and has good adhesion between a substrate film and a coating layer. [Means for solving the problem]

[0007] As a result of extensive investigations, the present inventors have found that the above problems can be solved by the means described below, and have arrived at the present invention. That is, the present invention has the following configuration. 1. A laminated film having at least one coating layer laminated on a base film, the coating layer comprising an acid-modified polyolefin and hydrophobic oxide particles, the acid value of the acid-modified polyolefin being 1 mgKOH / g or more and 60 mgKOH / g or less. 2. The laminate film according to the above item 1, wherein the hydrophobic oxide particles have an average primary particle diameter of 5 nm to 300 nm. 3. The laminate film according to the above 1 or 2, wherein the solid content of the hydrophobic oxide particles relative to the solid content of the coating layer is 10 to 90 mass %. 4. The laminated film according to any one of the above items 1 to 3, wherein the acid-modified polyolefin is an acid-modified polypropylene. 5. The laminate film according to any one of the above items 1 to 4, wherein the contact angle of the surface of the coating layer with water is 100 degrees or more. 6. The laminate film according to any one of the above items 1 to 5, wherein the base film is a polyethylene terephthalate film, a polyethylene naphthalate film, or a polyimide film. Effect of the Invention

[0008] The laminated film of the present invention comprises at least a substrate layer and a coating layer, and has good adhesion to the substrate film by containing an acid-modified polyolefin in the coating layer. In addition, the coating layer contains hydrophobic oxide particles or an acid-modified polyolefin having a specific low acid value, so that the coating layer surface of the laminated film has good water and oil repellency. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The present invention will be described in detail below. The present invention provides a useful laminate film having excellent water- and oil-repellency and excellent antifouling properties. That is, the laminate film has a coating layer laminated on a substrate film, and the coating layer is a coating layer containing an acid-modified polyolefin having an acid value of 1 mgKOH / g to 60 mgKOH / g and hydrophobic oxide particles, so that the outermost surface of the film exhibits excellent water- and oil-repellency, is capable of strong adhesion to the substrate film, and has high transparency.

[0010] (Base film) The laminated film in the present invention has a base film. The material of this base film is not particularly limited, but it is preferably a resin film from the viewpoint of handling such as flexibility. Examples of resins constituting the resin film include polyolefins such as polyethylene, polypropylene, polystyrene, and diene polymers, polyesters such as polyethylene terephthalate, polypropylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate, polyamides such as nylon 6, nylon 6,6, nylon 6,10, and nylon 12, acrylate resins such as polymethyl methacrylate, polymethacrylic acid esters, polymethyl acrylate, and polyacrylic acid esters, polyacrylic acid resins, polymethacrylic acid resins, and polyurethane resins. Examples of the resin include cellulose resins such as cellulose acetate and ethyl cellulose, polyarylates, aramids, polycarbonates, polyphenylene sulfides, polyphenylene oxides, polysulfones, polyethersulfones, polyetheretherketones, polyetherimides, polyimides, polyamideimides, aromatic hydrocarbon polymers such as polybenzimidazole, polybenzoxazole, and polybenzothiazole, fluorine resins such as polytetrafluoroethylene and polyvinylidene fluoride, epoxy resins, phenolic resins, novolac resins, and benzoxazine resins. Among these, from the viewpoint of transparency and dimensional stability, a film made of a polyester resin or an acrylate resin is preferable. Specific examples of polyester resins include polyethylene terephthalate, polypropylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate. Among these, from the viewpoint of physical properties, polyethylene terephthalate, polyethylene naphthalate, and polyimides are preferable, and from the viewpoint of balance between physical properties and cost, polyethylene terephthalate is particularly preferable.

[0011] The substrate film may be a single layer, or may have two or more layers laminated thereon. When two or more layers are laminated, the same or different films may be laminated. A resin composition may also be laminated on the substrate film. Furthermore, various additives may be contained in the substrate film as necessary within the range in which the effects of the present invention are achieved. Examples of additives include antioxidants, light resistance agents, gelation inhibitors, organic wetting agents, antistatic agents, ultraviolet absorbers, and surfactants. When the substrate film is composed of two or more layers, additives may also be contained according to the function of each layer. In order to improve the handling properties, such as the slipperiness and windability, of the substrate film, inactive particles may be contained in the substrate film.

[0012] In the present invention, the thickness of the substrate film is not particularly limited, but is preferably 5 μm to 300 μm. More preferably, it is 10 μm to 280 μm, and even more preferably, it is 12 μm to 260 μm. If it is 5 μm or more, it is easy to apply the coating layer when laminating it, and if it is 300 μm or less, it is advantageous in terms of cost.

[0013] The surface of the base film may be untreated, or may be surface-treated to improve adhesion to the coating layer. Specifically, the base film may be provided with an anchor coat layer or may be surface-treated by plasma treatment, corona treatment, flame treatment, or the like.

[0014] (Hydrophobic oxide particles) The coating layer of the laminated film in the present invention contains hydrophobic oxide particles. The hydrophobic oxide particles are not particularly limited as long as they are hydrophobic, and may be, for example, hydrophilic oxide particles that have been hydrophobized by surface treatment. That is, hydrophilic oxide particles that have been surface-treated with any reagent such as a silane coupling agent and have their surfaces hydrophobized can be used.

[0015] The type of oxide is not particularly limited. For example, at least one of silica (silicon dioxide), alumina, titania, zirconia, etc. can be used. These may be synthesized via any compound, and known or commercially available oxides may be used. In particular, silica (silicon dioxide) particles are preferred because they can be easily hydrophobized as described below.

[0016] As a method for hydrophobizing oxide particles, such as silica particles, surface treatment with various known reagents, such as silicone oil, silane coupling agents, and silazane, is preferably used. In particular, from the viewpoint of exhibiting excellent water and oil repellency, it is more preferable to introduce fluorine-based functional groups, such as 1H,1H,2H,2H-perfluorooctyl group, 1H,1H,2H,2H-perfluorodecyl group, 1H,1H,2H,2H-perfluorohexyl group, and 3,3,3-trifluoropropyl group, alkyl groups, such as methyl group, ethyl group, n-propyl group, isopropyl group, n-butyl group, isobutyl group, sec-butyl group, tert-butyl group, and octyl group, alkenyl group, alkynyl group, vinyl group, cyclohexyl group, styryl group, phenyl group, and trimethylsilyl group, to the surface. Among these, hydrophobic oxide particles having trimethylsilyl groups introduced therein are preferred, and hydrophobic silica having trimethylsilyl groups introduced therein is particularly preferred, as they exhibit superior water and oil repellency. Commercially available products corresponding to these include the aforementioned "AEROSIL (registered trademark) R812" and "AEROSIL (registered trademark) R812S" (both manufactured by Evonik Degussa).

[0017] The size of the hydrophobic oxide particles in the present invention is preferably 5 nm or more and 300 nm or less in terms of the average primary particle diameter, more preferably 5 nm or more and 200 nm or less, even more preferably 5 nm or more and 150 nm or less, particularly preferably 5 nm or more and 100 nm or less, and most preferably 5 nm or more and 75 nm or less. By setting the average primary particle diameter in the above range, even when a coating layer is laminated on the substrate film, the transparency of the laminated film is maintained, which is preferable. In addition, in the present invention, a mixture of multiple types of hydrophobic oxide particles having different particle diameters may be used. In addition, in the present invention, the size of the average primary particle diameter can be determined as a result of morphological observation by a microscope using a scanning electron microscope or a transmission electron microscope. Specifically, the average diameter of the diameters of 20 particles arbitrarily selected in these microscope observations is taken as the average primary particle diameter. The average primary particle diameter of particles of an indefinite shape can be calculated as the circle equivalent diameter. The circle equivalent diameter is a value obtained by dividing the area of ​​the observed particles by π, calculating the square root, and multiplying it by two.

[0018] In the present invention, the measurement results obtained by an X-ray photoelectron spectroscopy (ESCA) can be used as an index of the modification rate of the hydrophobic oxide particle surface by the functional group having water- and oil-repellency. Specifically, the atomic composition ratio can be obtained in a depth region of about 10 nm, and the ratio of specific atoms constituting the functional group having water- and oil-repellency, for example, carbon atoms, can be compared. In the present invention, from the viewpoint of exhibiting excellent water- and oil-repellency, for example, in the case of hydrophobic silica into which trimethylsilyl groups have been introduced, the ratio of carbon atoms is preferably 8 at% or more.

[0019] (Acid-modified polyolefin) The acid-modified polyolefin in the present invention is not particularly limited, and preferred precursor polyolefins include polyethylene such as LDPE (low density polyethylene), HDPE (high density polyethylene), and LDPE (low density polyethylene), polypropylene, a propylene-ethylene block copolymer, and a propylene-α-olefin block copolymer.

[0020] At least a part of the polyolefin as described above is a polyolefin or an unsaturated carboxylic acid modified polyolefin, preferably an acid modified polypropylene or an acid modified polyethylene, more preferably an unsaturated carboxylic acid modified polypropylene or an unsaturated carboxylic acid modified polyethylene. The unsaturated carboxylic acid modified polyolefin is a polyolefin modified by grafting a polyolefin with an unsaturated carboxylic acid, and examples thereof include maleic anhydride modified polypropylene and maleic anhydride modified polyethylene. Examples of the unsaturated carboxylic acid include maleic acid, fumaric acid, acrylic acid, methacrylic acid, and anhydrides thereof, among which maleic anhydride and maleic acid are preferred. The acid value of the acid modified polyolefin is preferably 1 mgKOH / g or more and 60 mgKOH / g or less, more preferably 1 mgKOH / g or more and 35 mgKOH / g or less, even more preferably 1 mgKOH / g or more and 25 mgKOH / g or less, and particularly preferably 1 mgKOH / g or more and 20 mgKOH / g or less. By using an acid modified polyolefin satisfying the above acid value, it is possible to ensure appropriate hydrophobicity while maintaining the coatability on the substrate film.

[0021] (Ingredients in the coating layer) The coating layer in the present invention may contain components other than the hydrophobic oxide particles, such as binder components, antioxidants, light resistance agents, gelling inhibitors, organic wetting agents, antistatic agents, ultraviolet absorbers, surfactants, etc., and these components may be appropriately contained as necessary.

[0022] The binder component is not particularly limited as long as it is a component that can be well bonded to the base film. For example, it is preferable to use polyester resin, polypropylene resin, polyurethane resin, epoxy resin, acrylic resin, etc. Of course, it is a particularly preferable embodiment that an acid-modified polyolefin is included as one of the binder components.

[0023] The hydrophobic oxide particles in the coating layer can be used in any ratio that allows the laminate film to exhibit water- and oil-repellency, but the solid content is preferably 10 to 90 mass% of the coating layer, more preferably 20 to 80 mass%, and particularly preferably 30 to 70 mass%. By using the hydrophobic oxide particles in the above ratio, the laminate film can exhibit excellent water- and oil-repellency.

[0024] (Coating liquid) In the present invention, a coating layer is laminated on a substrate film directly or via another layer to obtain a laminated film. The coating liquid for forming the coating layer can be used as is when the dispersion of hydrophobic oxide particles contains an acid-modified polyolefin, but may also contain various components for forming the coating layer, such as other binder components, and / or suitable solvents.

[0025] (Laminated film manufacturing process) In the production of the laminated film of the present invention, the coating method is not particularly limited. For example, it can be produced according to known methods such as roll coating, gravure coating, bar coating, doctor blade coating, spin coating, spray coating, and brush coating. The solvent used when coating is performed by these methods is not particularly limited, and for example, organic solvents such as water, alcohols, ketones, normal hexane, cyclohexane, toluene, butyl acetate, and glycols can be appropriately selected and used. These solvents may be used alone or in combination. The amount of hydrophobic oxide particles dispersed in the solvent can be selected at any ratio that provides a uniform dispersion. The method of drying after coating may be either natural drying or heat drying, but heat drying is more preferable from the viewpoint of industrial production. The drying temperature is not particularly limited as long as it does not affect the components contained in the base film or the coating layer, but is usually preferably 200 ° C or less, and more preferably 50 ° C or more and 160 ° C or less. The drying method is not particularly limited, and known methods for drying films such as hot plates and hot air ovens can be used. The drying time is appropriately selected depending on other conditions such as the drying temperature, but may be within a range that does not affect the components contained in the base film or coating layer.

[0026] (Water and oil repellency) The water and oil repellency of the laminated film according to the present invention can be evaluated by a known method. Specifically, the water repellency can be evaluated by contact angle measurement using water, and the oil repellency can be evaluated by contact angle measurement using diiodomethane. The preferred range of the contact angle with water in the present invention is 100 degrees or more, more preferably 120 degrees or more. A contact angle with water of 100 degrees or more is preferable because it shows excellent water repellency, and a contact angle of 120 degrees or more is more preferable because it shows water repellency equal to or higher than that of conventional fluorine-based resin sheets represented by polytetrafluoroethylene (PTFE). The upper limit of the contact angle with water is related to the contact angle with diiodomethane below, and is preferably 180 degrees or less. In addition, the preferred range of the contact angle with diiodomethane in the present invention is 60 degrees or more, more preferably 90 degrees or more. A contact angle with diiodomethane of 60 degrees or more is preferable from the viewpoint of imparting oil repellency capable of suppressing oil stains, and a contact angle of 90 degrees or more is more preferable because it shows oil repellency equal to or higher than that of conventional fluorine-based resin sheets. The upper limit is related to the degree of the contact angle with water, and is preferably 180 degrees or less. EXAMPLES

[0027] The present invention will be further described below with reference to specific examples, but the present invention is not limited to these examples. First, the evaluation methods employed in the present invention will be described.

[0028] (Contact angle measurement) The contact angle of the coating layer surface of the laminated film produced was measured with respect to the solvent. A fully automatic contact angle meter DM-701 manufactured by Kyowa Interface Science Co., Ltd. was used to measure the contact angle. Pure water and diiodomethane were used as the measurement solvents. The contact angle of water (hereinafter sometimes abbreviated as WCA) was measured after 60 seconds from a 1.8 μL water droplet being dropped. The contact angle of diiodomethane (hereinafter sometimes abbreviated as DCA) was measured after 30 seconds from a 0.9 μL diiodomethane droplet being dropped.

[0029] (Adhesion measurement) The adhesion between the film and the coating layer was confirmed by measuring the peel strength. The peel strength was measured using a JSV-H1000 made by Japan Measurement Systems Co., Ltd. (unit: N / cm). In the examples of the present invention, a peel strength of 2 N / cm or more was considered acceptable.

[0030] (Measurement of the average diameter of primary particles) The average primary particle diameter of hydrophobic oxide particles was determined as a result of observation using a scanning electron microscope or a transmission electron microscope. Specifically, the average diameter of 20 particles randomly selected in these microscope observations was taken as the average primary particle diameter. The average primary particle diameter of irregular particles can be calculated as the equivalent circle diameter. The equivalent circle diameter is calculated by dividing the area of ​​the observed particles by π, calculating the square root, and multiplying it by two.

[0031] (Method of measuring acid value) The acid value (mgKOH / g-resin) in the present invention refers to the amount of KOH required to neutralize 1g of acid-modified polyolefin, and was measured in accordance with the test method of JIS K0070 (1992). Specifically, 1g of acid-modified polyolefin was dissolved in 100g of xylene adjusted to 100°C, and then titrated with 0.1mol / L potassium hydroxide ethanol solution [product name "0.1mol / L ethanolic potassium hydroxide solution", manufactured by Wako Pure Chemical Industries, Ltd.] at the same temperature using phenolphthalein as an indicator. At this time, the amount of potassium hydroxide required for titration was converted to mg to calculate the acid value (mgKOH / g).

[0032] (ESCA measurement of hydrophobic oxide particles) The hydrophobic oxide particle dispersion was dropped onto a clean aluminum foil and dried to form a thin film of hydrophobic oxide particles on the aluminum foil. At this time, the aluminum foil was quickly dried to prevent surface contamination as much as possible, and immediately sampled for surface composition analysis. The device is K-Alpha +(Thermo Fisher Scientific) was used. Details of the measurement conditions are shown below. During the analysis, background removal was performed using the Shirley method. The surface composition ratio was the average value of the measurement results from three or more locations where Al was not detected on the substrate. Measurement conditions Excitation X-ray: Monochrome AlKα line X-ray output: 12kV, 6mA Photoelectron escape angle: 90 degrees Spot size: 400μmΦ Pass energy: 50eV Step: 0.1eV

[0033] <Production Example of Maleic Anhydride Modified Polypropylene A-1> Manufacturing Example 1 In a 1L autoclave, 100 parts by mass of polypropylene, 150 parts by mass of toluene, 3 parts by mass of maleic anhydride, and 1 part by mass of di-tert-butyl peroxide were added, and the mixture was heated to 140°C and further stirred for 1 hour. After the reaction was completed, the reaction liquid was poured into a large amount of methyl ethyl ketone to precipitate a resin. This resin was further washed several times with methyl ethyl ketone to remove unreacted maleic anhydride. The obtained resin was dried under reduced pressure to obtain maleic anhydride-modified polypropylene (acid value 6 mgKOH / g, weight average molecular weight 60,000, Tm 80°C), which is an acid-modified polyolefin.

[0034] <Production Example of Maleic Anhydride Modified Polypropylene B-1> In a 1L autoclave, 100 parts by mass of polypropylene, 150 parts by mass of toluene, 8.5 parts by mass of maleic anhydride, and 4 parts by mass of di-tert-butyl peroxide were added, and the mixture was heated to 140°C and further stirred for 1 hour. After the reaction was completed, the reaction liquid was poured into a large amount of methyl ethyl ketone to precipitate a resin. This resin was further washed several times with methyl ethyl ketone to remove unreacted maleic anhydride. The obtained resin was dried under reduced pressure to obtain maleic anhydride-modified polypropylene (acid value 12.7 mgKOH / g, weight average molecular weight 60,000, Tm 80°C), which is an acid-modified polyolefin.

[0035] <Production Example of Maleic Anhydride Modified Polypropylene C-1> In a 1L autoclave, 100 parts by mass of polypropylene, 150 parts by mass of toluene, 22 parts by mass of maleic anhydride, and 4 parts by mass of di-tert-butyl peroxide were added, and the mixture was heated to 140°C and further stirred for 1 hour. After the reaction was completed, the reaction liquid was poured into a large amount of methyl ethyl ketone to precipitate a resin. This resin was further washed several times with methyl ethyl ketone to remove unreacted maleic anhydride. The obtained resin was dried under reduced pressure to obtain maleic anhydride-modified polypropylene (acid value 22.9 mgKOH / g, weight average molecular weight 60,000, Tm 80°C), which is an acid-modified polyolefin.

[0036] <Production Examples of Maleic Anhydride Modified Polypropylene Solutions A-2, B-2, and C-2> 25 g of maleic anhydride-modified polypropylene A-1 was weighed out into a reaction vessel, 475 g of a mixed solvent of cyclohexane and methyl ethyl ketone (mixed mass ratio = 9:1) was added thereto, and the mixture was stirred for 1 hour or more to obtain maleic anhydride-modified polypropylene solution A-2 having a solid content concentration of 5 mass%. Similarly, maleic anhydride-modified polypropylene B-1 and C-1 were also prepared in the same manner to have a solid content concentration of 5 mass%, and these were named maleic anhydride-modified polypropylene solutions B-2 and C-2, respectively.

[0037] <Production Example of Silica Particle Dispersion D> As hydrophobic silica, commercially available AEROSIL (registered trademark) R812S (manufactured by Evonik, primary particle average diameter 7 nm) with trimethylsilyl groups on the surface was used. 25 g of R812S was weighed out into a reaction vessel, and 475 g of a mixed solvent of cyclohexane and methyl ethyl ketone (mixed mass ratio = 9:1) was added thereto and stirred for 12 hours or more. After that, an ultrasonic homogenizer was applied for 10 minutes to obtain silica particle dispersion D with a solid concentration of 5 mass%.

[0038] <Production Example of Silica Particle Dispersion E> As hydrophobic silica, commercially available silica particles AEROSIL (registered trademark) R972 (manufactured by Evonik, primary particle average diameter 60 nm) modified with dimethyldichlorosilane were used. 25 g of R972 was weighed out into a reaction vessel, 475 g of a mixed solvent of cyclohexane and methyl ethyl ketone (mixed mass ratio = 9:1) was added thereto, and the mixture was stirred for 12 hours or more. After that, an ultrasonic homogenizer was applied for 10 minutes to obtain silica particle dispersion E with a solid content concentration of 5 mass%.

[0039] <Production Example of Silica Particle Dispersion F> 100 parts by mass of tetraethoxysilane and 339 parts by mass of ethanol were mixed in a reaction vessel 1. 179 parts by mass of ethanol, 14 parts by mass of ammonia water (25%), and 125 parts by mass of deionized water were mixed in a reaction vessel 2, and then the contents of the reaction vessel 2 were transferred dropwise to the reaction vessel 1. At this time, the dropwise addition took 10 minutes to prevent a rapid reaction. After the dropwise addition, the reaction solution was left at 20°C for 48 hours. Then, ammonia and water were distilled off to prepare a silica particle dispersion (average primary particle diameter 260 nm). Then, 150 parts by mass of hexamethyldisilazane was added and heated at 65°C for 2 days to prepare a silica particle dispersion modified with a trimethylsilyl group. In order to confirm the solid content concentration of the silica particle dispersion, 5 grams of the silica particle dispersion was measured out in an aluminum cup (1.3 grams) and heated in an oven at 150°C for 24 hours or more to remove the residual solvent ethanol and water. The aluminum cup after removal was weighed to be 1.55 grams, so the solid content in 5 grams of silica microparticle dispersion was calculated to be 0.25 grams, and the solid content concentration of the silica microparticle dispersion was confirmed to be 5% by mass. After that, in order to prepare a coating liquid, the ethanol was removed from the silica microparticle dispersion, and the same amount of a mixed solvent of cyclohexane and methyl ethyl ketone (mixed mass ratio = 9:1) as the removed ethanol was added, obtaining silica particle dispersion F with a solid content concentration of 5% by mass using cyclohexane / methyl ethyl ketone = 9 / 1 as the solvent.

[0040] <Example of coating liquid production> A coating solution was prepared by adding 40 parts by mass of maleic anhydride modified polypropylene solution A-2, 40 parts by mass of silica particle dispersion E, and 20 parts by mass of a mixed solvent of cyclohexane and methyl ethyl ketone (mixture mass ratio = 9:1) to a reaction vessel and stirring at room temperature for 1 hour.

[0041] <Preparation of coating film> Example 1 The coating liquid was applied to the corona-treated surface of Toyobo Ester (registered trademark) film (product number: E5100, thickness: 75 μm), which is a film made of polyethylene terephthalate (hereinafter, sometimes referred to as PET film), by a bar coat method using a bar coater #3, and then dried at 120° C. for 1 minute to obtain a coating film.

[0042] (Examples 2 to 12) The type and amount of the acid-modified polypropylene solution and the type and amount of the silica particle dispersion in the coating liquid were changed as shown in Table 1 below, to obtain coating films of Examples 2 to 12.

[0043] [Table 1]

[0044] Comparative Example 1 The maleic anhydride modified polypropylene solution A-2 (solid content 5% by mass) was applied to the corona-treated surface of the PET film E5100 using a bar coater #3, and then dried at 120° C. for 1 minute to obtain a coating film.

[0045] Comparative Example 2 A coating film was obtained in the same manner as in Example 1, except that the maleic anhydride-modified polypropylene solution A-2 in Example 1 was replaced with an unmodified polypropylene solution of the same concentration and no silica microparticle dispersion was added. The evaluation results of Comparative Examples 1 and 2 are shown in Table 2.

[0046] [Table 2]

[0047] Here, the results of ESCA analysis of the surfaces of the silica particles contained in the above silica particle dispersions D to F are shown in Table 3.

[0048] [Table 3] [Industrial Applicability]

[0049] The present invention provides a laminated film having excellent water and oil repellency and antifouling properties. The laminated film of the present invention is useful because it can be expected to be used in applications such as packaging, covering, and release materials.

Claims

1. A laminated film having at least one coating layer laminated on a base film, the coating layer comprising an acid-modified polyolefin and hydrophobic oxide particles, the hydrophobic oxide particles being hydrophobic silica particles having trimethylsilyl groups introduced onto their surfaces, the ratio of carbon atoms in a 10 nm depth region measured by an X-ray photoelectron spectroscopy (ESCA) being 8 at % or more, and the acid value of the acid-modified polyolefin being 1.0 mg KOH / g or more and 60 mg KOH / g or less.

2. 2. The laminated film according to claim 1, wherein the hydrophobic oxide particles have an average primary particle diameter of 5 nm to 300 nm.

3. 3. The laminate film according to claim 1, wherein the solid content of the hydrophobic oxide particles relative to the solid content of the coating layer is 10 to 90 mass %.

4. 4. The laminated film according to claim 1, wherein the acid-modified polyolefin is an acid-modified polypropylene.

5. 5. The laminated film according to claim 1, wherein the contact angle of the surface of the coating layer with water is 100 degrees or more.

6. 6. The laminate film according to claim 1, wherein the base film is a polyethylene terephthalate film, a polyethylene naphthalate film, or a polyimide film.

Citation Information

Patent Citations

  • Antireflection film and image display device

    JP2000284102A

  • Molded material having transparent water-repelling surface and its production

    JP2001131318A

  • Water repellant stainproof film

    JP2002113805A

  • Polyimide-based coating composition

    JP2007138027A

  • Gas barrier film

    JP2009221518A