Water-based composition, cured product and laminate

The aqueous compositions with specific poly(meth)acrylate and conductive polymers address the issues of antistatic properties and storage stability, achieving enhanced performance and stability in water-based applications.

JP7563400B2Active Publication Date: 2024-10-08ARAKAWA CHEM IND LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2022020916
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-03-02
Filing Date
2022-02-15
Publication Date
2024-10-08
Estimated Expiration
2042-02-15

AI Technical Summary

Technical Problem

Existing water-based compositions with poly(meth)acrylate and surfactants lack adequate antistatic properties and storage stability.

Method used

Aqueous compositions comprising poly(meth)acrylate with a hydroxyl value of 60 mgKOH/g or less, a π-conjugated conductive polymer, and an aqueous solvent with 80% water content, including components like polythiophenes and polyanilines, enhance antistatic performance and storage stability.

Benefits of technology

The compositions exhibit improved antistatic properties and storage stability, maintaining emulsion stability and providing effective scratch resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007563400000001
    Figure 0007563400000001
  • Figure 0007563400000002
    Figure 0007563400000002
  • Figure 0007563400000003
    Figure 0007563400000003
Patent Text Reader

Abstract

To provide an aqueous composition, a cured material and a laminate having improved anti-static property and excellent storage stability.SOLUTION: The present disclosure relates to an aqueous composition that includes a poly(meth)acrylate (A) having a hydroxyl value of 60 mgKOH / g or less, a surfactant (B), a π-conjugated conductive polymer (C), and an aqueous solvent (D), and among 100 mass% of the (D) component, 80 mass% or more is water.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a water-based composition, a cured product, and a laminate. [Background technology]

[0002] Compositions in which poly(meth)acrylate is made aqueous with a surfactant are widely used in water-based paints for construction, adhesives, coating agents for plastic films, etc. As an example, Patent Document 1 discloses a composition characterized by being obtained by dispersing (meth)acrylate in an aqueous solvent in the presence of a surfactant. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2008-303258 A Summary of the Invention [Problem to be solved by the invention]

[0004] Patent Document 1 has a problem with respect to antistatic properties. An object of the present invention is to provide an aqueous composition, a cured product, and a laminate that have improved antistatic properties and good storage stability. [Means for solving the problem]

[0005] As a result of intensive research, the present inventors have found that the above-mentioned problems can be solved by a specific aqueous composition. The present invention has been made to solve at least a part of the above-mentioned problems, and can be realized as the following aspects or application examples.

[0006] The present disclosure provides the following: (Item 1) A poly(meth)acrylate (A) having a hydroxyl value of 60 mgKOH / g or less; Surfactant (B), π-conjugated conductive polymer (C) and Contains water-based solvent (D) (D) 80% by mass or more of 100% by mass of the component is water; Water-based composition. (Item 2) 2. The aqueous composition according to item 1, wherein the component (A) has at least three (meth)acryloyl groups. (Item 3) 3. The aqueous composition according to item 1 or 2, wherein the component (C) is one or more selected from polythiophenes and / or polyanilines. (Item 4) A cured product of the aqueous composition according to any one of items 1 to 3. (Item 5) A laminate having the cured product according to item 4 on at least one surface of a substrate. Effect of the Invention

[0007] The aqueous composition provided by the present disclosure has good antistatic performance and storage stability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] Throughout the present disclosure, the range of the values ​​of each physical property, content, etc. may be set appropriately (for example, by selecting from the upper and lower limit values ​​described in each item below). Specifically, when A1, A2, A3, etc. are exemplified as the lower limit of the value α and B1, B2, B3, etc. are exemplified as the upper limit of the value α, the range of the value α is exemplified as A1 or more, A2 or more, A3 or more, B1 or less, B2 or less, B3 or less, A1 to B1, A1 to B2, A1 to B3, A2 to B1, A2 to B2, A2 to B3, A3 to B1, A3 to B2, A3 to B3, etc. In addition, in the present disclosure, "to" is used to mean that the values ​​described before and after it are included as the lower limit and upper limit. Hereinafter, each component of the aqueous composition provided in the present disclosure, the cured product, the laminate, etc. will be described in detail.

[0009] <Poly(meth)acrylate (A) having a hydroxyl value of 60 mgKOH / g or less> Poly(meth)acrylate (A) (also referred to as "component (A)" in this disclosure) having a hydroxyl value of 60 mgKOH / g or less may be (meth)acrylate having two or more (meth)acryloyl groups, the average hydroxyl value of which is 60 mgKOH / g or less. In this disclosure, (meth)acrylate refers to acrylate and / or methacrylate, and (meth)acryloyl group refers to acryloyl group and / or methacryloyl group. Component (A) does not include component (B).

[0010] The component (A) contains a poly(meth)acrylate (a1) having a hydroxyl group (also referred to as the "component (a1)" in the present disclosure). The component (A) may contain a poly(meth)acrylate (a2) having no hydroxyl group (also referred to as the "component (a2)" in the present disclosure) as necessary.

[0011] Examples of the (a1) component include 2-hydroxy-3-(meth)acryloyloxypropyl (meth)acrylate, bis((meth)acryloyloxy)propanol, glycerol di(meth)acrylate, trimethylolpropane di(meth)acrylate, sorbitol di(meth)acrylate, sorbitol tri(meth)acrylate, sorbitol tetra(meth)acrylate, sorbitol penta(meth)acrylate, pentaerythritol di(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol di(meth)acrylate, dipentaerythritol tri(meth)acrylate, dipentaerythritol tetra(meth)acrylate, and dipentaerythritol penta(meth)acrylate.

[0012] Other components (A) include: (1) A reaction product of a component having a hydroxyl group with a component having a functional group reactive with a hydroxyl group and a (meth)acryloyl group, (2) One or more types selected from the group consisting of reaction products of a component having a hydroxyl group and a (meth)acryloyl group, and a component having a functional group reactive with a hydroxyl group, are also exemplified. Examples of components having hydroxyl groups include polyether polyols, polyester polyols, polycarbonate polyols, acrylic polyols, polyolefin polyols, neopentyl glycol, 3-methyl-1,5-pentanediol, ethylene glycol, propylene glycol, 1,4-butanediol, 1,6-hexanediol, trimethylolpropane, pentaerythritol, tricyclodecane dimethylol, bis-[hydroxymethyl]-cyclohexane, and sorbitol. Examples of components having a functional group reactive with a hydroxyl group and a (meth)acryloyl group include 2-isocyanatoethyl (meth)acrylate, 2-(2-(meth)acryloyloxyethyloxy)ethyl isocyanate, 1,1-(bis(meth)acryloyloxymethyl)ethyl isocyanate, 2-acryloyloxyethyl succinic acid, 2-acryloyloxyethyl hexahydrophthalic acid, 2-acryloyloxyethyl phthalic acid, and 2-acryloyloxyethyl acid phosphate. An example of the component having a hydroxyl group and a (meth)acryloyl group is the above-mentioned component (a1). An example of a component having a functional group that reacts with a hydroxyl group is polyisocyanate. Examples of polyisocyanates include polyisocyanates containing a chain hydrocarbon group, polyisocyanates containing an alicyclic hydrocarbon group, and polyisocyanates containing an aromatic hydrocarbon group. Examples of polyisocyanates containing a chain hydrocarbon group include hexamethylene diisocyanate. Examples of polyisocyanates containing an alicyclic hydrocarbon group include isophorone diisocyanate and dicyclohexylmethane diisocyanate. Examples of polyisocyanates containing an aromatic hydrocarbon group include tolylene diisocyanate, xylene diisocyanate, diphenylmethane-4,4'-diisocyanate, and 3-methyldiphenylmethane diisocyanate. Examples of other polyisocyanates include adducts of the polyisocyanates exemplified above and various known polyisocyanates, and polymers of these isocyanates. Examples of such polyisocyanates include biurets, nurates, adducts, allophanates, and the like. Examples of polyisocyanate biurets include products named "Duranate 24A-100", "Duranate 22A-75P", and "Duranate 21S-75E" (all manufactured by Asahi Kasei Corporation). Examples of polyisocyanate nurates include products named "Coronate HK" and "Coronate HXR" (all manufactured by Tosoh Corporation). Examples of polyisocyanate adducts include products named "Duranate P301-75E" (manufactured by Asahi Kasei Corporation). Examples of polyisocyanate allophanates include products named "Coronate 2770" (manufactured by Tosoh Corporation). The polyisocyanates of the present disclosure may have an average number of isocyanate groups of about 3 or more and 10 or less. The average number of isocyanate groups can be calculated by the following formula: Average number of isocyanate groups = (number average molecular weight (Mn) x isocyanate group concentration (%)) / (42.02 x 100), where the isocyanate group concentration (%) is a value measured by the method described in JIS K 1603-1:2007.

[0013] Commercially available products may be used as component (A). Examples of such products include trimethylolpropane tri(meth)acrylate (product name: Miramer M300, manufactured by MIWON, hydroxyl value: 10 mg KOH / g), glycerin propoxy tri(meth)acrylate (product name: Miramer M320, manufactured by MIWON, hydroxyl value: 25 mg KOH / g), pentaerythritol EO-modified tetra(meth)acrylate (product name: Miramer M4004, manufactured by MIWON, hydroxyl value: 20 mg KOH / g), ditrimethylolpropane tetra(meth)acrylate (product name: Miramer M410, manufactured by MIWON, hydroxyl value: 10 mg KOH / g), and dipentaerythritol hexa(meth)acrylate (product name: Miramer M410, manufactured by MIWON, hydroxyl value: 10 mg KOH / g). Examples include dipentaerythritol poly(meth)acrylate (product name "A-DPH", manufactured by Shin-Nakamura Chemical Co., Ltd., hydroxyl value 10 mgKOH / g), (product name "A-9550", manufactured by Shin-Nakamura Chemical Co., Ltd., hydroxyl value 50 mgKOH / g), and EO-modified dipentaerythritol poly(meth)acrylate (product name "A-DPH-12EL", manufactured by Shin-Nakamura Chemical Co., Ltd., hydroxyl value 30 mgKOH / g).

[0014] The substances exemplified as the component (A) and the known substances as the component (A) can be used alone or in combination of two or more kinds. The component (A) is preferably a poly(meth)acrylate containing erythritol in its structure, and more preferably one or more selected from pentaerythritol poly(meth)acrylate, dipentaerythritol poly(meth)acrylate, tripentaerythritol poly(meth)acrylate, and urethane poly(meth)acrylate containing erythritol in its structure.

[0015] Examples of upper limits for the number of (meth)acryloyl groups in component (A) are 15, 14, 13, 12, 11, 10, 9, 8, 7, 6, 5, 4, 3, etc., and examples of lower limits are 14, 13, 12, 11, 10, 9, 8, 7, 6, 5, 4, 3, 2, etc. In one embodiment, the number of (meth)acryloyl groups in component (A) is preferably about 2 to 15, and more preferably about 3 to 12. The more (meth)acryloyl groups in component (A), the better the scratch resistance, and therefore this is preferred.

[0016] The upper limit of the hydroxyl value (mgKOH / g) of the component (A) is 60, 55, 50, 45, 40, 35, 30, 25, 20, 15, 10, 5, 1, 0.5, 0.1, etc., and the lower limit is 55, 50, 45, 40, 35, 30, 25, 20, 15, 10, 5, 1, 0.5, 0.1, 0.05, etc. In one embodiment, the hydroxyl value (mgKOH / g) of the component (A) is 60 or less, and preferably about 0.05 to 60. It is considered that the lower the hydroxyl value of the component (A), the more excellent the storage stability and scratch resistance tend to be. If the hydroxyl value of the component (A) exceeds 60 mgKOH / g, it is not preferable because the storage stability of the emulsion particle size is poor and the particle size is enlarged. A cured product or laminate using a component (A) with a high hydroxyl value exhibits better antistatic properties than a cured product or laminate using a component (A) with a low hydroxyl value, and therefore the value is preferably equal to or greater than the above lower limit. In addition, as a method for measuring the hydroxyl value in the present disclosure, the method described in JIS K 0070 1992 is exemplified, and in particular, the neutralization titration method is exemplified.

[0017] The upper limit of the molecular weight of the (A) component is exemplified as 20,000, 10,000, 5,000, 1,000, 500, 250, etc., and the lower limit is exemplified as 10,000, 5,000, 1,000, 500, 250, 100, etc. In one embodiment, the molecular weight of the (A) component is preferably about 100 to 20,000, more preferably 500 to 10,000. In the present disclosure, the term "molecular weight" simply refers to a numerical value calculated based on the atomic weight.

[0018] The upper limit of the weight average molecular weight of the component (A) is exemplified as 20,000, 10,000, 5,000, 1,000, 500, 250, etc., and the lower limit is exemplified as 10,000, 5,000, 1,000, 500, 250, 100, etc. In one embodiment, the weight average molecular weight of the component (A) is preferably about 100 to 20,000, more preferably 500 to 10,000. In the present disclosure, the weight average molecular weight is a polystyrene-equivalent value measured by gel permeation chromatography.

[0019] Examples of upper limits for the content (solid content) of component (A) relative to 100% by mass of the total amount of components (A), (B), and (C) of the present disclosure are 99.9, 99.5, 99, 98, 97, 96, 95, 94, 93, 92, 91, 90, 85, 80, and 75% by mass, and examples of lower limits are 99.5, 99, 98, 97, 96, 95, 94, 93, 92, 91, 90, 85, 80, 75, and 70% by mass. In one embodiment, the content of component (A) (converted into solid content) relative to the total amount of components (A), (B), and (C) of the present disclosure (100% by mass), in order to satisfactorily exhibit the effects of the present disclosure, is preferably about 70 to 99.9% by mass, more preferably 80 to 99.5% by mass, even more preferably 85 to 99.5% by mass, and particularly preferably 90 to 99% by mass.

[0020] <Surfactant (B)> The aqueous composition of the present disclosure contains a surfactant (B) (also referred to as "component (B)" in the present disclosure). Examples of component (B) include cationic surfactants, anionic surfactants, nonionic surfactants, reactive surfactants, etc. Component (B) does not include component (A).

[0021] Examples of cationic surfactants include quaternary ammonium type and aliphatic tertiary amidoamine type. Examples of quaternary ammonium type include cetyltrimethylammonium chloride, alkyltrimethylammonium chloride, lauryltrimethylammonium chloride, benzalkonium chloride, stearyltrimethylammonium chloride, cetyltrimethylammonium bromide, stearyltrimethylammonium bromide, etc. Examples of aliphatic tertiary amidoamine type include stearic acid diethylaminoethylamide, stearic acid dimethylaminopropylamide, etc. As the cationic surfactant, commercially available products may be used. Examples of such products include product names "Catiogen H" and "Catiogen L" (manufactured by Daiichi Kogyo Seiyaku Co., Ltd.), product names "Cortamin 24P", "Cortamin 86P Conc", "Cortamin 60W", and "Cortamin 86W" (manufactured by Kao Corporation), etc.

[0022] Examples of anionic surfactants include carboxylates, sulfates, sulfonates, and phosphates. Examples of carboxylates include rosinates, fatty acid salts, and acylated sarcosinates. Examples of rosinates include potassium rosinate and sodium rosinate. Examples of fatty acid salts include potassium oleate, potassium laurate, sodium laurate, sodium stearate, potassium stearate, coconut oil fatty acid triethanolamine, and triethanolamine laurate. Examples of acylated sarcosinates include sodium lauroyl sarcosinate. Examples of sulfate ester salts include alkyl sulfate salts, alkyl ether sulfate salts, and amide ether sulfate. Examples of alkyl sulfate salts include sodium lauryl sulfate, ammonium lauryl sulfate, and triethanolamine lauryl sulfate. Examples of alkyl ether sulfate salts include polyoxyethylene alkyl ether sulfate salts. Examples of amide ether sulfate salts include polyoxyethylene coconut oil fatty acid monoethanolamide sodium sulfate. Examples of sulfonate include alkyl allyl sulfonate, sulfosuccinic acid diester salt, sulfosuccinic acid ester salt, etc. Examples of alkyl allyl sulfonate include triethanolamine dodecylbenzenesulfonate, etc. Examples of sulfosuccinic acid diester salt include dioctyl sulfosuccinate, etc. Examples of sulfosuccinic acid ester salt include polyoxyethylene lauryl sulfosuccinate disodium, lauryl sulfosuccinate disodium, etc. Examples of phosphate ester salt include alkyl phosphate ester, alkyl ether phosphate ester, etc. Examples of alkyl phosphate ester include lauryl phosphoric acid, etc. Examples of alkyl ether phosphate ester include polyoxyethylene lauryl ether phosphate, polyoxyethylene oleyl ether phosphate, etc.

[0023] Examples of nonionic surfactants include ether type, ester type, ester-ether type, aminoether type, alkanolamide type, etc. Examples of ether type include polyoxyethylene alkyl ether, polyoxyethylene polyoxypropylene alkyl ether, etc. Examples of ester type include polyethylene glycol alkyl ester, sorbitan fatty acid ester, etc. Examples of ester-ether type include polyoxyethylene sorbitan aliphatic ester, etc. Examples of aminoether type include polyoxyethylene alkylamine, etc. Examples of alkanolamide type include aliphatic monoethanolamide, aliphatic diethanolamide, etc.

[0024] The reactive surfactant may be a commercially available product. Examples of the product include those under the product names "Latemul S-180A", "Latemul PD-104", "Latemul PD-105", "Latemul PD-420", and "Latemul PD-430" (manufactured by Kao Corporation), those under the product name "Eleminol JS-2" (manufactured by Sanyo Chemical Industries, Ltd.), those under the product names "Aqualon KH-10", "Aqualon BC-20", "Aqualon RN-20", "Aqualon RN-30", and "Aqualon RN-50" (manufactured by Daiichi Kogyo Seiyaku Co., Ltd.), those under the product names "ADEKA REASOAP SE-10N", "ADEKA REASOAP SR-10N" (manufactured by ADEKA Corporation), those under the product names "Antox MS-60", "Aminoion RE-1000L" (manufactured by Nippon Nyukazai Co., Ltd.), and those under the product name "Surfmer FP-120" (manufactured by Toho Chemical Industry Co., Ltd.).

[0025] The substances exemplified as the component (B) and those known as the component (B) can be used alone or in combination of two or more kinds.

[0026] The upper limit of the content ratio of component (A) to component (B) (mass ratio, solid content equivalent, [component (A) / component (B)]) is 99.9 / 0.1, 99.8 / 0.2, 99.7 / 0.3, 99.6 / 0.4, 99.5 / 0.5, 99.4 / 0.6, 99.3 / 0.7, 99.2 / 0.8, 99.1 / 0.9, 99 / 1, 98 / 2, 97 / 3, 96 / 4, 95 / 5, 94 / 6, 93 / 7, 92 / 8, Examples of the ratio are 91 / 9, 90 / 10, and 85 / 15, and examples of the lower limit are 99.8 / 0.2, 99.7 / 0.3, 99.6 / 0.4, 99.5 / 0.5, 99.4 / 0.6, 99.3 / 0.7, 99.2 / 0.8, 99.1 / 0.9, 99 / 1, 98 / 2, 97 / 3, 96 / 4, 95 / 5, 94 / 6, 93 / 7, 92 / 8, 91 / 9, 90 / 10, 85 / 15, and 80 / 20. In one embodiment, the content ratio of the (A) component to the (B) component (mass ratio, solid content equivalent, [(A) component / (B) component]) is preferably about 80 / 20 to 99.9 / 0.1, since the effects of the present disclosure are satisfactorily exhibited.

[0027] The upper limit of the content (solid content) of the (B) component in 100% by mass of the total of the (A), (B), and (C) components of the present disclosure is 20, 15, 10, 5, 1, 0.5, 0.1% by mass, and the lower limit is 15, 10, 5, 1, 0.5, 0.1, 0.05% by mass. In one embodiment, the content (solid content) of the (B) component in 100% by mass of the total of the (A), (B), and (C) components of the present disclosure is preferably about 0.05 to 20% by mass. By being equal to or greater than the above lower limit, the aqueous system (emulsion) can be favorably formed.

[0028] <π-conjugated conductive polymer (C)> The aqueous composition of the present disclosure contains a π-conjugated conductive polymer (C) (also referred to as "component (C)" in the present disclosure). By containing component (C) in the aqueous composition of the present disclosure, the desired effects of the present disclosure, particularly excellent storage stability and antistatic properties, are achieved compared to other antistatic agents. Examples of component (C) include at least one selected from the group consisting of polythiophenes, polyanilines, polythiophene vinylenes, polypyrroles, polyfurans, and the like. Note that component (C) does not contain component (A).

[0029] Examples of polythiophenes include polythiophene, poly(alkylthiophenes), poly(monoalkoxythiophenes), poly(dialkoxythiophenes), and poly(alkylenedioxythiophenes). The polythiophenes are preferably alkylenedioxypoly(thiophenes) doped with polystyrenesulfonic acid (PSS), and more preferably a complex of poly3,4-ethylenedioxythiophene (PEDOT) and PSS (also referred to as "PEDOT / PSS" in the present disclosure). PEDOT / PSS can be obtained, for example, by polymerizing 3,4-ethylenedioxythiophene (EDOT) as a monomer in an aqueous phase in the presence of polystyrenesulfonic acid (PSS) as a dopant using an oxidizing agent. Examples of commercially available PEDOT / PSS include the product name "Clevios P" (manufactured by Heraeus Co., Ltd.) and the product name "Orgacon ICP1010" (manufactured by Agfa Materials Japan, Inc.).

[0030] Examples of polyanilines include polyaniline, poly(2-methylaniline), poly(3-isobutylaniline), poly(2-anilinesulfonic acid), and poly(3-anilinesulfonic acid).

[0031] Examples of polythiophene vinylenes include poly(thiophene vinylene), alkylenedioxy group-substituted poly(thiophene vinylene), alkoxy group-substituted poly(thiophene vinylene), alkyl group-substituted poly(thiophene vinylene), carboxyl group-substituted poly(thiophene vinylene), hydroxy group-substituted poly(thiophene vinylene), phenyl group-substituted poly(thiophene vinylene), cyano group-substituted poly(thiophene vinylene), halogen-substituted poly(thiophene vinylene), etc. Examples of alkylenedioxy group-substituted poly(thiophene vinylene)s include poly(3,4-ethylenedioxythiophene vinylene), poly(3,4-propylenedioxythiophene vinylene), poly(3,4-butenedioxythiophene vinylene), etc. Alkoxy group-substituted poly(thiophene vinylene)s include poly(3-methoxythiophene vinylene), poly(3-ethoxythiophene vinylene), poly(3-butoxythiophene vinylene), poly(3-hexyloxythiophene vinylene), poly(3-heptyloxythiophene vinylene), poly(3-octyloxythiophene vinylene), poly(3-decyloxythiophene vinylene), poly(3-dodecyloxythiophene vinylene), poly(3-octadecyloxythiophene vinylene), poly(3,4-dimethoxythiophene vinylene), poly(3, Examples of the thiophene vinylene include poly(3,4-diethoxythiophene vinylene), poly(3,4-dipropoxythiophene vinylene), poly(3,4-dibutoxythiophene vinylene), poly(3,4-dihexyloxythiophene vinylene), poly(3,4-diheptyloxythiophene vinylene), poly(3,4-dioctyloxythiophene vinylene), poly(3,4-didecyloxythiophene vinylene), poly(3,4-didodecyloxythiophene vinylene), poly(3-methyl-4-methoxythiophene vinylene), and poly(3-methyl-4-ethoxythiophene vinylene).Examples of alkyl group-substituted poly(thiophene vinylene)s include poly(3-methylthiophene vinylene), poly(3-ethylthiophene vinylene), poly(3-propylthiophene vinylene), poly(3-butylthiophene vinylene), poly(3-hexylthiophene vinylene), poly(3-heptylthiophene vinylene), poly(3-octylthiophene vinylene), poly(3-decylthiophene vinylene), poly(3-dodecylthiophene vinylene), poly(3-octadecylthiophene vinylene), poly(3,4-dimethylthiophene vinylene), and poly(3,4-dibutylthiophene vinylene). Examples of carboxyl group-substituted poly(thiophene vinylene)s include poly(3-carboxythiophene vinylene), poly(3-methyl-4-carboxythiophene vinylene), poly(3-methyl-4-carboxyethylthiophene vinylene), and poly(3-methyl-4-carboxybutylthiophene vinylene). Examples of hydroxyl group-substituted poly(thiophene vinylene)s include poly(3-hydroxythiophene vinylene), poly(3,4-dihydroxythiophene vinylene). Examples of phenyl group-substituted poly(thiophene vinylene)s include poly(3-phenylthiophene vinylene). Examples of cyano group-substituted poly(thiophene vinylene)s include poly(3-cyanothiophene vinylene). Examples of halogen-substituted poly(thiophene vinylene)s include poly(3-bromothiophene vinylene), poly(3-chlorothiophene vinylene), and poly(3-iodothiophene vinylene).

[0032] Examples of polypyrroles include poly(pyrrole), alkoxy group-substituted poly(pyrroles), alkyl group-substituted poly(pyrroles), carboxyl group-substituted poly(pyrroles), and hydroxy group-substituted poly(pyrroles). Examples of alkoxy group-substituted poly(pyrroles) include poly(3-methoxypyrrole), poly(3-ethoxypyrrole), poly(3-butoxypyrrole), poly(3-hexyloxypyrrole), and poly(3-methyl-4-hexyloxypyrrole). Examples of alkyl group-substituted poly(pyrroles) include poly(3-methylpyrrole), poly(3-ethylpyrrole), poly(3-n-propylpyrrole), poly(3-butylpyrrole), poly(3-octylpyrrole), poly(3-decylpyrrole), poly(3-dodecylpyrrole), poly(3,4-dimethylpyrrole), and poly(3,4-dibutylpyrrole). Examples of carboxyl group-substituted poly(pyrroles) include poly(3-carboxypyrrole), poly(3-methyl-4-carboxypyrrole), poly(3-methyl-4-carboxyethylpyrrole), poly(3-methyl-4-carboxybutylpyrrole), etc. Examples of hydroxyl group-substituted poly(pyrroles) include poly(3-hydroxypyrrole).

[0033] Examples of polyfurans include polyfuran, alkoxy group-substituted polyfurans, alkyl group-substituted polyfurans, carboxyl group-substituted polyfurans, and hydroxy group-substituted polyfurans. Examples of alkoxy group-substituted polyfurans include poly(3-methoxyfuran), poly(3-ethoxyfuran), poly(3-butoxyfuran), poly(3-hexyloxyfuran), and poly(3-methyl-4-hexyloxyfuran). Examples of alkyl group-substituted polyfurans include poly(3-methylfuran), poly(3-ethylfuran), poly(3-n-propylfuran), poly(3-butylfuran), poly(3-octylfuran), poly(3-decylfuran), poly(3-dodecylfuran), poly(3,4-dimethylfuran), and poly(3,4-dibutylfuran). Examples of carboxyl-substituted polyfurans include poly(3-carboxyfuran), poly(3-methyl-4-carboxyfuran), poly(3-methyl-4-carboxyethylfuran), poly(3-methyl-4-carboxybutylfuran), etc. Examples of hydroxyl-substituted polyfurans include poly(3-hydroxyfuran), etc.

[0034] The substances exemplified as the component (C) and known substances as the component (C) can be used alone or in combination of two or more. From the viewpoint of the antistatic property and transparency of the cured product of the aqueous composition, the component (C) is preferably a polythiophene and / or a polyaniline, more preferably a polythiophene, and even more preferably PEDOT / PSS.

[0035] The upper limit of the content ratio of component (A) to component (C) (mass ratio, solid content equivalent, [component (A) / component (C)]) is 99.9 / 0.1, 99.8 / 0.2, 99.7 / 0.3, 99.6 / 0.4, 99.5 / 0.5, 99.4 / 0.6, 99.3 / 0.7, 99.2 / 0.8, 99.1 / 0.9, 99 / 1, 98 / 2, 97 / 3 Examples of the upper limit include 99.8 / 0.2, 99.7 / 0.3, 99.6 / 0.4, 99.5 / 0.5, 99.4 / 0.6, 99.3 / 0.7, 99.2 / 0.8, 99.1 / 0.9, 99 / 1, 98 / 2, 97 / 3, 96 / 4, 95 / 5, 90 / 10, 85 / 15, etc. In one embodiment, the content ratio of the (A) component to the (C) component (mass ratio, solid content equivalent, [(A) component / (C) component]) is preferably about 85 / 15 to 99.9 / 0.1, since the effects of the present disclosure are satisfactorily exhibited.

[0036] Examples of upper limits of the content ratio of the (B) component to the (C) component (mass ratio, calculated as solid content, [(B) component / (C) component]) are 80 / 20, 75 / 25, 70 / 30, 65 / 35, 60 / 40, 55 / 45, 50 / 50, 45 / 55, 40 / 60, 35 / 65, 30 / 70, and 25 / 75, while examples of lower limits include 75 / 25, 70 / 30, 65 / 35, 60 / 40, 55 / 45, 50 / 50, 45 / 55, 40 / 60, 35 / 65, 30 / 70, 25 / 75, and 20 / 80. In one embodiment, the content ratio of the (B) component to the (C) component (mass ratio, solid content equivalent, [(B) component / (C) component]) is preferably about 20 / 80 to 80 / 20, in order to satisfactorily exhibit the effects of the present disclosure.

[0037] The upper limit of the content (solid content) of the (C) component in 100% by mass of the total of the (A), (B) and (C) components of the present disclosure is 15, 10, 9, 7, 5, 3, 1, 0.9, 0.7, 0.5, 0.3, 0.1% by mass, and the lower limit is 10, 9, 7, 5, 3, 1, 0.9, 0.7, 0.5, 0.3, 0.1, 0.05% by mass, etc. In one embodiment, the content (solid content) of the (C) component in 100% by mass of the total of the (A), (B) and (C) components of the present disclosure is preferably about 0.05 to 15% by mass, more preferably 0.05 to 10% by mass, even more preferably 0.1 to 10% by mass, particularly preferably 0.5 to 3% by mass, and even more particularly preferably 0.5 to 1% by mass. By being equal to or more than the above lower limit, it is possible to exhibit good antistatic properties, while by being equal to or less than the above upper limit, compatibility with other components is good, and the transparency of the cured product of the present disclosure is excellent.

[0038] <Water-based solvent (D)> The aqueous composition of the present disclosure contains an aqueous solvent (D) (also referred to as "component (D)" in the present disclosure), and 80 mass % or more of 100 mass % of component (D) is water.

[0039] The component (D) is a solvent consisting of only water, or a solvent consisting of a mixture of water and a water-soluble organic solvent. The type of the water-soluble organic solvent is not particularly limited as long as it is an organic solvent that is soluble in water. Examples of the water-soluble organic solvent include alcohols and ethers. Examples of the alcohols include methanol, ethanol, n-propyl alcohol, i-propyl alcohol, n-butyl alcohol, sec-butyl alcohol, t-butyl alcohol, isobutyl alcohol, n-hexyl alcohol, n-octyl alcohol, ethylene glycol, propylene glycol, diethylene glycol, triethylene glycol, and diacetone alcohol. Examples of the ethers include ethylene glycol monobutyl ether, propylene glycol monomethyl ether, and propylene glycol monoethyl ether.

[0040] When a mixture of water and a water-soluble organic solvent is used as the component (D), the upper limit of the proportion of water used is, for example, 100, 95, 90, or 85% by mass, relative to 100% by mass of the component (D), and the lower limit is, for example, 95, 90, 85, or 80% by mass. In one embodiment, when a mixture of water and a water-soluble organic solvent is used as the component (D), the proportion of water used is preferably about 80 to 100% by mass, relative to 100% by mass of the component (D). The higher the proportion of water used as the component (D), the smaller the impact on the environment, the more suppressed the collapse of micelles in the resin emulsion, and the better the stability of the dispersed state (emulsion stability), and the greater the particle size (D) of the resin emulsion measured using a laser diffraction / scattering particle size measuring device (e.g., Microtrac MT3000, etc.) in accordance with JIS Z8825:2013. 50 Or D 90 It is most preferred because the molecular weight distribution (Mg / mol) of the water-based composition of the present disclosure is small and the dispersibility is good. It is also preferred that the water-based composition of the present disclosure does not contain any solvent other than the component (D).

[0041] The substances exemplified as the solvent and known solvents can be used alone or in combination of two or more kinds.

[0042] The upper limit of the content ratio of the aqueous solvent to the solid content of the aqueous composition of the present disclosure (mass ratio, [solid content of the aqueous composition of the present disclosure / aqueous solvent]) is 99 / 1, 95 / 5, 90 / 10, 80 / 20, 70 / 30, 60 / 40, 50 / 50, 40 / 60, 30 / 70, 20 / 80, 10 / 90, 5 / 95, etc., and the lower limit is 95 / 5, 90 / 10, 80 / 20, 70 / 30, 60 / 40, 50 / 50, 40 / 60, 30 / 70, 20 / 80, 10 / 90, 5 / 95, 1 / 99, etc. As one embodiment, the content ratio of the aqueous solvent to the solid content of the aqueous composition of the present disclosure (mass ratio, [solid content of the aqueous composition of the present disclosure / aqueous solvent]) is preferably about 1 / 99 to 99 / 1. By reducing the amount of the aqueous solvent, the thickness of the cured product of the aqueous composition of the present disclosure can be increased.

[0043] <Polymerization initiator (E)> The aqueous composition of the present disclosure may contain a polymerization initiator (E) (also referred to as "component (E)" in the present disclosure). Examples of the polymerization initiator include a photopolymerization initiator and a thermal polymerization initiator.

[0044] Examples of the photopolymerization initiator include radical photopolymerization initiators, cationic photopolymerization initiators, and anionic photopolymerization initiators. Examples of the radical photopolymerization initiator include alkylphenone-type photopolymerization initiators, acylphosphine oxide-type photopolymerization initiators, hydrogen abstraction-type photopolymerization initiators, and oxime ester-type photopolymerization initiators. Examples of the alkylphenone-type photopolymerization initiator include benzyl dimethyl ketals such as 2,2-dimethoxy-1,2-diphenylethane-1-one, α-hydroxyalkylphenones such as 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one, and 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]phenyl}-2-methyl-propan-1-one, and α-aminoalkylphenones such as 2-methyl-1-(4-methylthiophenyl)-2-morpholinopropan-1-one. Examples of acylphosphine oxide type photopolymerization initiators include 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide and bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide. Examples of hydrogen abstraction type photopolymerization initiators include phenylglyoxylic acid methyl ester. Examples of oxime ester type photopolymerization initiators include 1,2-octanedione, 1-[4-(phenylthio)-, 2-(O-benzoyloxime)], ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-, 1-(O-acetyloxime). Examples of cationic photopolymerization initiators include a mixture of iodonium, (4-methylphenyl)]4-(2-methylpropyl)phenyl]-hexafluorophosphate(1-) and propylene carbonate, triarylsulfonium hexafluorophosphate, triarylsulfonium tetrakis-(pentafluorophenyl)borate, etc. Examples of anionic photopolymerization initiators include cobalt amine complexes, o-nitrobenzyl alcohol carbamic acid esters, oxime esters, etc.

[0045] Examples of the thermal polymerization initiator include organic peroxides and azo compounds. Examples of the organic peroxides include 1,1-bis(t-butylperoxy)2-methylcyclohexane, 1,1-bis(t-hexylperoxy)-3,3,5-trimethylcyclohexane, 1,1-bis(t-hexylperoxy)cyclohexane, 1,1-bis(t-butylperoxy)-3,3,5-trimethylcyclohexane, and 1,1-bis(t-butylperoxy)cyclohexane. Examples of the azo compounds include 1,1'-azobis(cyclohexane-1-carbonitrile), 2-(carbamoylazo)isobutyronitrile, 2-phenylazo-4-methoxy-2,4-dimethylvaleronitrile, azodi-t-octane, and azodi-t-butane.

[0046] The substances exemplified as the polymerization initiator and those known as the polymerization initiator can be used alone or in combination of two or more kinds.

[0047] The upper limit of the content (solid content) of the component (E) based on 100% by mass of the aqueous composition of the present disclosure in terms of solid content is, for example, 20, 15, 10, 8, 6, 4, 2, 1, 0.5% by mass, and the lower limit is, for example, 15, 10, 8, 6, 4, 2, 1, 0.5, 0.1, 0% by mass. In one embodiment, the content (solid content) of the component (E) based on 100% by mass of the aqueous composition of the present disclosure in terms of solid content is preferably about 0 to 20% by mass.

[0048] <Other agents that can be used>

[0043] The aqueous composition of the present disclosure may further contain various additives, such as a binder resin, an antifoaming agent, a leveling agent, a preservative, an antioxidant, a conductivity improver, organic particles, inorganic particles, a thickener, a foaming agent, a plasticizer, an ultraviolet absorber, a colorant, and a polymerization inhibitor, in addition to the components exemplified above, as necessary.

[0049] Examples of the polymerization inhibitor include p-methoxyphenol and phenothiazine. Commercially available products may be used as the polymerization inhibitor. Examples of such products include those with the product names "IRGANOX1010" and "IRGANOX1035" (manufactured by BASF Japan Ltd.), those with the product name "Sumilizer GA-80" (manufactured by Sumitomo Chemical Co., Ltd.), those with the product names "Kinopower QS-30" and "Kinopower QS-W10" (manufactured by Kawasaki Chemical Industries, Ltd.). These may be used alone or in combination of two or more kinds.

[0050] <Method of producing aqueous composition> The aqueous composition of the present disclosure may be obtained by watering an emulsion containing the (A) and (B) components to obtain an emulsion, and then adding the (C) component to the emulsion. The (D) component may be added at any stage of the above-mentioned production method, but it is preferable to mix the (A) and (B) components and then add the (D) component to disperse them. Furthermore, the (E) component, which is added as necessary, may also be added at any stage of the above-mentioned production method. As the emulsification method, either a forced emulsification method or a phase inversion emulsification method may be adopted. The emulsification conditions are not particularly limited, and for example, the temperature is usually about 5 to 70°C, preferably about 10 to 50°C. The time is usually about 1 to 24 hours, preferably about 1 to 12 hours. Note that a mixture of the (A) and (B) components may be pre-emulsified before emulsification.

[0051] Examples of equipment used for emulsification include a propeller mixer, a turbine mixer, a homomixer, a disperser mixer, an ultra mixer, a colloid mill, a high-pressure homogenizer, an ultrasonic wave, etc. These equipment may be used alone or in combination as appropriate.

[0052] <Laminate> The present disclosure provides a laminate having a substrate and a cured product of the aqueous composition of the present disclosure. The present disclosure also provides a method for producing the laminate, the method including a step of curing the aqueous composition of the present disclosure applied to at least one surface of the substrate with active energy rays and / or heat.

[0053] Examples of substrates to which the aqueous composition of the present disclosure is applied include glass substrates, metal substrates, and plastic substrates. Examples of plastic substrates include thermoplastic plastic substrates and thermosetting plastic substrates. Examples of thermoplastic plastic substrates include general-purpose plastic substrates and engineering plastic substrates. Examples of general-purpose plastic substrates include olefin-based, polyester-based, acrylic-based, vinyl-based, and polystyrene-based substrates. Examples of olefin-based substrates include polyethylene, polypropylene, and norbornene. Examples of polyester-based substrates include polyethylene terephthalate (PET) and polyethylene naphthalate (PEN). Examples of acrylic-based substrates include polymethyl methacrylate (PMMA). Examples of vinyl-based substrates include polyvinyl chloride, polyvinylidene chloride, and polyvinyl alcohol. Examples of polystyrene-based substrates include polystyrene (PS) resin, styrene-acrylonitrile (AS) resin, and styrene-butadiene-acrylonitrile (ABS) resin. Examples of engineering plastic substrates include general-purpose engineering plastics and super engineering plastics. Examples of general-purpose engineering plastics include polycarbonate and polyamide (nylon). Examples of super engineering plastics include polyether ether ketone (PEEK). Examples of thermosetting plastic substrates include polyimide, epoxy resin, melamine resin, and the like. Examples of other plastic substrates include triacetyl cellulose resin. The plastic substrate may be a copolymer of the above-mentioned plastics. The substrate of the present disclosure may be a multilayer including a plurality of the above-mentioned substrates. The substrate may be surface-treated (corona discharge, etc.). The substrate may have other layers (e.g., an easy-adhesion layer, an anchor layer, etc.) between the layer formed by the aqueous composition of the present disclosure and one or both sides of the substrate. The substrate is preferably a polyester-based substrate, more preferably a polyethylene terephthalate film, because it is excellent in transparency, dimensional stability, mechanical properties, chemical resistance, and the like. The substrate is preferably a polyimide, because it is excellent in heat resistance, dimensional stability, mechanical properties, and the like.Examples of the upper limit of the thickness of the substrate include 300, 275, 250, 225, 200, 175, 150, 125, 100, 75, 50, 25, and 10 μm, and examples of the lower limit include 275, 250, 225, 200, 175, 150, 125, 100, 75, 50, 25, 10, and 1 μm. In one embodiment, the thickness of the substrate is preferably 1 to 300 μm, more preferably 25 to 250 μm, even more preferably 50 to 200 μm, particularly preferably 50 to 150 μm, and even more particularly preferably 75 to 125 μm.

[0054] The plastic substrate may be an unstretched resin film formed from a resin, which is a raw material for plastic, in a sheet shape, or a stretched resin film formed by stretching this unstretched resin film.

[0055] The unstretched resin film is obtained by forming a resin material into a sheet shape, for example, by melt extrusion, melt dripping, calendaring, etc. The forming method is preferably melt extrusion. Examples of forming devices used in melt extrusion include single-screw extruders and twin-screw extruders. The melting conditions are not particularly limited, and for example, the temperature is usually about 200°C to 300°C.

[0056] The stretched resin film can be obtained by stretching the unstretched resin film in the longitudinal direction (machine direction) or transverse direction. The stretched resin film is preferably an unstretched resin film stretched in the longitudinal direction (machine direction).

[0057] The method for stretching the unstretched resin film in the longitudinal direction is not particularly limited, and examples thereof include a method of stretching the film 2 to 5 times using a preheated roll, etc. The roll temperature is not particularly limited, and is usually about 80 to 120°C, and preferably about 80 to 100°C.

[0058] The method for stretching the unstretched resin film in the short direction is not particularly limited, and examples thereof include a method in which the end portions are held by clipping or the like, and the film is guided to a hot air zone and stretched 2.5 to 5 times. The temperature of the hot air zone is not particularly limited, and is usually about 70 to 140°C, and preferably about 80 to 120°C.

[0059] Examples of methods for coating the aqueous composition of the present disclosure on a substrate include roll coater coating, reverse roll coater coating, bar coater coating, Mayer bar coating, air knife coating, gravure coating, reverse gravure coating, offset printing, flexographic printing, screen printing, etc. The amount of coating is not particularly limited, but is usually 0.01 to 20 g / m2 in terms of the mass after drying. 2 The range is preferably 0.025 to 10 g / m 2 and more preferably 0.05 to 5 g / m 2 The upper limit of the thickness of the cured product is 50, 45, 40, 35, 30, 25, 20, 15, 10, 5, 4, 3, 2, 1, 0.5, 0.1, 0.05, 0.02 μm, and the like, and the lower limit is 45, 40, 35, 30, 25, 20, 15, 10, 5, 4, 3, 2, 1, 0.5, 0.1, 0.05, 0.02, 0.01 μm, and the like. The thickness of the cured product is preferably 0.01 to 50 μm, more preferably 0.01 to 10 μm, even more preferably 0.01 to 1 μm, and particularly preferably 0.02 to 1 μm.

[0060] The method of curing by irradiation with active energy rays is to use a high-pressure mercury lamp, ultra-high-pressure mercury lamp, carbon arc lamp, metal halide lamp, xenon lamp, chemical lamp, electrodeless discharge lamp, LED, or the like that emits light in the wavelength range of 150 nm or more and 450 nm or less, at a dose of 10 mJ / cm. 2 More than 10,000mJ / cm 2The following irradiation methods are exemplified. Before the irradiation with active energy rays, the coating may be dried by heating as necessary. After the irradiation with active energy rays, the coating may be completely cured by heating as necessary. Heating conditions include, for example, about 60 to 150°C for about 30 seconds to 30 minutes, and preferably, 70 to 130°C for about 50 seconds to 10 minutes.

[0061] The conditions for the method of curing the aqueous composition of the present disclosure by heating include heating at 70 to 250°C for 1 to 100 minutes. The number of times of heating and the number of times of pressing with or without heating are not particularly limited. The heating method varies depending on the types and blending ratios of each component. Specific examples of the heating method include heating at 70 to 180°C for 1 to 15 minutes, followed by heat treatment at 180 to 250°C (preferably 200 to 250°C) for 5 to 90 minutes, and a cured product can be obtained by the heating.

[0062] The aqueous composition of the present disclosure may be used as follows (1) to (12): The aqueous composition of the present disclosure is preferably used as an antistatic hard coating agent, but may also be used in various applications in which the effects of the aqueous composition of the present disclosure can be exerted. (1) Cured product of the aqueous composition of the present disclosure, and substrate (2) Cured product of the aqueous composition of the present disclosure, primer layer, and substrate (3) Cured product of the aqueous composition of the present disclosure, substrate, and pressure-sensitive adhesive layer (4) Cured product of the aqueous composition of the present disclosure, primer layer, substrate, and pressure-sensitive adhesive layer (5) Antifouling layer, cured product of the aqueous composition of the present disclosure, and substrate (6) Antifouling layer, cured product of the aqueous composition of the present disclosure, primer layer, and substrate (7) Antifouling layer, cured product of the aqueous composition of the present disclosure, substrate, and pressure-sensitive adhesive layer (8) Antifouling layer, cured product of the aqueous composition of the present disclosure, primer layer, substrate, adhesive layer (9) Low refractive index layer, high refractive index layer, cured product of the aqueous composition of the present disclosure, substrate, (10) Low refractive index layer, high refractive index layer, cured product of the aqueous composition of the present disclosure, substrate, and pressure-sensitive adhesive layer (11) Low refractive index layer, high refractive index layer, cured product of the aqueous composition of the present disclosure, primer layer, and substrate (12) Low refractive index layer, high refractive index layer, cured product of the aqueous composition of the present disclosure, primer layer, substrate, and pressure-sensitive adhesive layer EXAMPLES

[0063] Specific examples of the present disclosure will be described below with reference to examples, but the present disclosure is not limited to these examples. In the examples, parts and percentages are all based on the solid content mass unless otherwise specified.

[0064] In the present examples, the weight average molecular weight (Mw) was measured by gel permeation chromatography (GPC) under the following conditions. (GPC measurement conditions) Model: Product name "HLC-8220" (manufactured by Tosoh Corporation) Column: Product name "TSKgel SuperHM-L" (Tosoh Corporation) x 3 Developing solvent: Tetrahydrofuran (hereinafter referred to as "THF")

[0065] <Synthesis Example 1: Synthesis of poly(meth)acrylate (A-1) having a hydroxyl value of 60 mgKOH / g or less> In a reaction vessel equipped with a thermometer, a stirrer, a cooling tube, a dropping funnel, and a nitrogen inlet tube, 200 g of an isocyanurate of isophorone diisocyanate, 0.2 g of tin octylate, and 268 g of pentaerythritol triacrylate (hereinafter also referred to as "PETA") were charged, and the temperature in the system was raised to about 80°C over about 1 hour. Next, the reaction system was maintained at the same temperature for 3 hours, and the isocyanate group was detected at 2250 cm -1 The reaction was continued until the infrared absorption spectrum of the compound disappeared, thereby obtaining a reaction product (hereinafter also referred to as "component (A-1)"). The component (A-1) had a (meth)acryloyl group equivalent of 173 g / eq and a weight average molecular weight of 1,560.

[0066] <Example 1: Preparation of aqueous composition (1)> A 300 mL four-neck flask equipped with a stirrer, a thermometer, a condenser, and a drying gas inlet tube was charged with 100 parts of (A-1) in terms of solids, 1.55 parts of surfactant (B-1) (product name "Aminoion RE-1000L", manufactured by Nippon Nyukazai Co., Ltd.) in terms of solids, and 0.9 parts of PEDOT / PSS (C-1) (product name "Orgacon ICP1010", manufactured by Agfa Materials Japan, Inc.) was added to the aqueous emulsion, which was then diluted with water to prepare an aqueous composition (1) with a non-volatile content of 30%.

[0067] <Examples 2 to 5 and Comparative Examples 1 to 6: Preparation of Aqueous Compositions (2) to (5) and (C1) to (C6)> Examples 2 to 5 and Comparative Examples 1 to 6 were carried out in the same manner as Example 1, except that the compositions were changed to those shown in Tables 1 and 2, to obtain aqueous compositions (2) to (5) and (C1) to (C6).

[0068] <Preparation of Laminate> The aqueous compositions described in each of the Examples and Comparative Examples were applied to a 100 μm-thick PET film (Cosmoshine A4100, manufactured by Toyobo Co., Ltd.) using a bar coater #3 so that the thickness of the film after curing would be 1 μm. The film was then dried at 80° C. for 2 minutes to evaporate the water, and then heat-treated at 200° C. to produce a thermoset film and obtain a laminate.

[0069] <Performance evaluation (1): Storage stability> The aqueous compositions of the Examples and Comparative Examples were stored in a 40° C. incubator, and the appearance of the compositions was observed to measure the number of days until the particle size increased. The number of days was evaluated according to the following criteria. AAA: No hypertrophy occurred for 90 days or more. AA: Enlarged within 30 to 90 days. A: The swelling occurred between 10 and 30 days. B: Enlarged in less than 10 days.

[0070] <Performance evaluation (2): Scratch resistance> The laminates of each Example and Comparative Example were set in a commercially available measuring device (product name: "Flat Abrasion Tester", manufactured by Daiei Scientific Instruments Co., Ltd.), and the cured surface was scratched 1000 times with a load of 1 kg using steel wool (number "#0000", grade "extra fine", manufactured by Nippon Steel Wool Co., Ltd.). The scratch resistance of the laminate was evaluated based on the number of scratches created, according to the following criteria. Each laminate was measured four times, and the average value was used for evaluation. AAA: 0 AA: More than 0 but less than 5 A: More than 5 but less than 10 B: More than 10 pieces and less than 20 pieces C: More than 20 pieces

[0071] <Performance evaluation (3): Surface resistance test> The surface resistance of the laminate was measured using a commercially available resistivity meter (manufactured by Mitsubishi Chemical Corporation, product name "Hiresta MCP-HT-450") at an applied voltage of 500 V in accordance with JIS K 6911. The measured values ​​were evaluated according to the following criteria. A: 1×10 10 Ω / □ or less B: 1×10 10 Ω / □Super

[0072] [Table 1]

[0073] [Table 2]

[0074] The meanings of the terms in Tables 1 and 2 are as follows. The values ​​in the tables are calculated based on the solid content. (A-1): Poly(meth)acrylate obtained in Synthesis Example 1 (hydroxyl value: 0.8 mg KOH / g, viscosity: 40,000, number of (meth)acryloyl groups: 10) (A-2): Dipentaerythritol hexaacrylate (product name: Miramer M600, manufactured by MIWON, hydroxyl value: 5 mg KOH / g, viscosity: 5,410, number of (meth)acryloyl groups: 5 to 6) (A-3): Dipentaerythritol poly(meth)acrylate (product name "NK Ester A-9550W", manufactured by Shin-Nakamura Chemical Co., Ltd., hydroxyl value: 44 mg KOH / g, viscosity: 6,820, number of (meth)acryloyl groups: 5 to 6) (A-C1): Dipentaerythritol poly(meth)acrylate (product name "NK Ester A-9570W", manufactured by Shin-Nakamura Chemical Co., Ltd., hydroxyl value: 98.5 mg KOH / g, viscosity: 6,990, number of (meth)acryloyl groups: 5 to 6) (A-C2): 2-hydroxy-3-phenoxypropyl acrylate (product name: "Epoxy Ester M-600A", manufactured by Kyoeisha Chemical Co., Ltd., viscosity: 150 to 200, number of (meth)acryloyl groups: 1) (B-1): Surfactant (product name: Aminoion RE-1000L, manufactured by Nippon Nyukazai Co., Ltd.) (C-1): PEDOT / PSS (product name: Orgacon ICP1010, manufactured by Agfa Materials Japan, Inc.) (C-C1): A polymer containing a quaternary ammonium salt structure obtained by Synthesis Example 2 below *1: Not dispersed and could not be measured.

[0075] <Synthesis Example 2: Synthesis of polymer containing quaternary ammonium salt structure> A reactor equipped with a stirrer and a cooling tube was charged with 130 parts of hydroxyethyl methacrylate, 1140 parts of ε-caprolactone, and 1.3 parts of tin octylate, and the temperature was raised to 150°C. After 6 hours of warming, the mixture was cooled to obtain a polyester structure-containing monofunctional vinyl monomer having a weight average molecular weight of 5500. A reactor equipped with a stirrer and a cooling tube was charged with 100 parts of methacryloyloxyethyl trimethylammonium chloride (DMC), 60 parts of the polyester structure-containing monofunctional vinyl monomer, 40 parts of tert-butyl methacrylate (t-BMA), and 800 parts of propylene glycol monomethyl ether (PGM), and the temperature was raised to 90°C. Next, 8 parts of 2,2'-azobis(methylbutyronitrile) (AMBN) and 32 parts of PGM were added to initiate the polymerization reaction, and the mixture was cooled after warming at 100°C for 6 hours to obtain a solution of a quaternary ammonium salt structure-containing polymer (non-volatile content 20%).

[0076] <Example 6: Preparation of aqueous composition (6)> As the aqueous composition of Example 6, the same aqueous composition as that of Example 1 was used.

[0077] <Example 7: Preparation of aqueous composition (7)> In a 300mL four-neck flask equipped with a stirrer, thermometer, cooler and dry gas inlet tube, 100 parts of (A-1), 1.55 parts of surfactant (B-1) (product name "Aminoion RE-1000L", manufactured by Nippon Nyukazai Co., Ltd.), 0.9 parts of PEDOT / PSS (C-1) (product name "Orgacon ICP1010", manufactured by Agfa Materials Japan Co., Ltd.) were mixed in terms of solids into the aqueous dispersion emulsion, and 2.05 parts of ethanol were mixed to prepare an aqueous composition with a non-volatile content of 30%. The content of water in the aqueous solvent was 98% by mass relative to 100% by mass of the aqueous solvent.

[0078] <Examples 8 to 9 and Comparative Example 7: Preparation of aqueous compositions (8) to (9) and (C7)> Examples 8 to 9 and Comparative Example 7 were prepared in the same manner as in Example 7, except that the content of water in the aqueous solvent was changed to 90 mass%, 81 mass%, and 67 mass%, respectively, relative to 100 mass% of the aqueous solvent, to obtain aqueous compositions (8) to (9) and (C7).

[0079] <Performance evaluation (4): Emulsion stability> The aqueous compositions were evaluated by observing the appearance of each of the aqueous compositions of Examples 6 to 9 and Comparative Example 7. The appearance was evaluated according to the following criteria. AA: The entire emulsion is dispersed. A: A small amount of the emulsion is oily, and the majority is emulsified and dispersed. B: Most of the emulsion is oily, with a small amount being emulsified and dispersed.

[0080] [Table 3]

Claims

1. Poly(meth)acrylate (A) having a hydroxyl value of 60 mgKOH / g or less; A surfactant (B), A π-conjugated conductive polymer (C), and Contains an aqueous solvent (D) The component (B) is represented by chemical formula (1): Of 100% by mass of the (D) component, 80% by mass or more is water, The mass ratio ((A) component / (B) component) is 95 / 5 to 99.3 / 0.7, The mass ratio ((A) component / (C) component) is 90 / 10 to 99.7 / 0.3, The mass ratio (component (B) / component (C)) is 40 / 60 to 70 / 30, The mass ratio (solid content of the aqueous composition / aqueous solvent (D)) is 20 / 80 to 40 / 60. Water-based composition. 【Chemistry 1】 In the chemical formula (1), R is a substituted or unsubstituted linear, branched, or cyclic alkyl group having 1 to 30 carbon atoms, a substituted or unsubstituted aryl group having 6 to 30 carbon atoms, or a substituted or unsubstituted arylalkyl group having 7 to 31 carbon atoms; A is a linear or branched alkylene group having 2 to 4 carbon atoms; n is the average number of repeating units of the oxyalkylene group (OA) of 2 to 50; Q is an ammonium ion having an ethylenically unsaturated bond, an imidazolium ion having an ethylenically unsaturated bond, a pyridinium ion having an ethylenically unsaturated bond, a pyrrolidinium ion having an ethylenically unsaturated bond, a pyrrolinium ion having an ethylenically unsaturated bond, a piperidinium ion having an ethylenically unsaturated bond, or a cyclic alkyl group having an ethylenically unsaturated bond. and at least one selected from the group consisting of a pyrazinium ion having an ethylenically unsaturated bond, a pyrazinium ion having an ethylenically unsaturated bond, a pyrimidinium ion having an ethylenically unsaturated bond, a triazolium ion having an ethylenically unsaturated bond, a triazinium ion having an ethylenically unsaturated bond, a quinolinium ion having an ethylenically unsaturated bond, an isoquinolinium ion having an ethylenically unsaturated bond, an indolinium ion having an ethylenically unsaturated bond, a quinoxalinium ion having an ethylenically unsaturated bond, a piperazinium ion having an ethylenically unsaturated bond, an oxazolinium ion having an ethylenically unsaturated bond, a thiazolinium ion having an ethylenically unsaturated bond, and a morpholinium ion having an ethylenically unsaturated bond.

2. 2. The aqueous composition according to claim 1, wherein the number of (meth)acryloyl groups contained in component (A) is at least 3.

3. 3. The aqueous composition according to claim 1, wherein the component (C) is at least one selected from the group consisting of polythiophenes and / or polyanilines.

4. A cured product of the aqueous composition according to any one of claims 1 to 3.

5. A laminate comprising the cured product of claim 4 on at least one surface of a substrate.

Citation Information

Patent Citations

  • Energy ray-curable oil-in-water drop type emulsion and water-based hard coating agent

    JP2005239803A

  • Active energy ray-curable emulsion composition and coating agent composition

    JP2008303258A

  • Polarizing film comprising antistatic coating layer

    JP2014222355A

  • Aqueous coating agent for in-line coat, cured film, and laminate

    JP2019167530A