Chabazite-type zeolite and its manufacturing method
A chabazite-type zeolite with controlled silica-to-alumina ratio and silanol content, along with specific crystal characteristics, addresses the structural collapse issue of larger crystals, ensuring high heat resistance and effective nitrogen oxide reduction.
Patent Information
- Application Number
- JP2023175562
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2017-02-22
- Filing Date
- 2023-10-10
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2038-02-16
AI Technical Summary
Conventional chabazite-type zeolites with larger crystal sizes face challenges in coating and handling, leading to difficulties in use as catalysts due to skeletal structure collapse under high temperature and humidity, limiting their heat resistance improvement.
A chabazite-type zeolite with a silica-to-alumina molar ratio of 15 or more, average crystal diameter of 0.5 to 1.5 μm, and controlled silanol content, along with specific crystal shapes and XRD peaks, is synthesized without increasing crystal size, enhancing heat resistance and nitrogen oxide reduction properties.
The synthesized zeolite maintains high heat resistance and nitrogen oxide reduction capabilities even under high temperature and humidity conditions, particularly below 200°C, without the drawbacks of larger crystal sizes.
Smart Images

Figure 0007563551000010 
Figure 0007563551000011 
Figure 0007563551000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a chabazite-type zeolite. [Background technology]
[0002] Chabazite-type zeolite is a zeolite having a three-dimensional pore structure containing an eight-membered oxygen ring forming a pore of 3.8 x 3.8 Å. Chabazite-type zeolite also exists in nature, but only artificially synthesized chabazite-type zeolites with a high molar ratio of silica to alumina (hereinafter also referred to as "SiO2 / Al2O3 ratio") have been found (for example, Patent Documents 1 to 3, Non-Patent Documents 1 and 2).
[0003] Patent Documents 1 and 2 disclose SSZ-13 as a chabazite-type zeolite having a SiO2 / Al2O3 ratio of 5 or more. Furthermore, Non-Patent Documents 1 and 2 disclose SSZ-13 in the form of aggregated particles in which crystal particles are chemically bonded to each other. Patent Document 3 discloses SSZ-62, a chabazite-type zeolite having the same crystal structure as SSZ-13, a SiO2 / Al2O3 ratio of more than 10, and a crystal diameter of 0.5 μm or less.
[0004] These chabazite-type zeolites are used as various catalysts including cracking catalysts and nitrogen oxide reduction catalysts, and among catalytic applications, they are widely used as nitrogen oxide reduction catalysts by selective catalytic reduction (Patent Documents 4 to 6). On the other hand, the skeletal structure of SSZ-13 and SSZ-62 is easily destroyed when exposed to a high-temperature, high-humidity atmosphere. For this reason, chabazite-type zeolites that can withstand use as nitrogen oxide reduction catalysts by selective catalytic reduction have been studied.
[0005] As a chabazite-type zeolite characterized by its skeletal structure not easily collapsing even when exposed to a high-temperature, high-humidity atmosphere, i.e., having high heat resistance, for example, a chabazite-type zeolite having an average crystal size of 1.5 μm or more and a SiO2 / Al2O3 ratio of 15 or more has been studied (Patent Document 7). In addition, a chabazite-type zeolite having a crystal size of more than 0.5 μm and a SiO2 / Al2O3 ratio of 5 to 15 has been disclosed by crystallizing a raw material that does not contain a structure-directing agent. The chabazite-type zeolite has a wide crystal particle size distribution and contains crystal particles with a crystal size of more than 0.5 μm to about 3 μm, and a scanning electron microscope photograph of these particles in an aggregated state has been specifically disclosed (Patent Document 8). [Prior art documents] [Patent documents]
[0006] [Patent Document 1] U.S. Patent No. 4,544,538 [Patent Document 2] U.S. Patent No. 4,665,110 [Patent Document 3] U.S. Patent Publication No. 2003 / 0069449 [Patent Document 4] US Patent Publication No. 2011 / 0182790 [Patent Document 5] U.S. Patent Publication No. 2008 / 0202107 [Patent Document 6] US Patent Publication No. 2010 / 0092362 [Patent Document 7] U.S. Patent Publication No. 2011 / 0251048 [Patent Document 8] U.S. Patent Publication No. 2012 / 0269719 [Non-patent literature]
[0007] [Non-Patent Document 1] J.Phys.Chem.C,114(2010)1633-1640 [Non-Patent Document 2] ZEOLITES, Vol. 8 (1988) 166-174 Summary of the Invention [Problem to be solved by the invention]
[0008] As disclosed in Patent Documents 7 and 8, in the past, in order to improve the heat resistance of chabazite-type zeolite, it was necessary to increase the crystal size. However, if the crystal size becomes too large, it becomes difficult to coat filters and the like, and it becomes difficult to use it as a catalyst. Therefore, there is a limit to how much heat resistance can be improved by increasing the crystal size.
[0009] In view of these problems, the present invention aims to provide a chabazite-type zeolite having high heat resistance without a large crystal size. Another aim of the present invention is to provide a catalyst that contains such a chabazite-type zeolite and exhibits high nitrogen oxide reduction properties, particularly high nitrogen oxide reduction properties in the low temperature range below 200°C, even after exposure to high temperature and high humidity. [Means for solving the problem]
[0010] The present inventors have investigated a catalyst for selective catalytic reduction of nitrogen oxides and a chabazite-type zeolite suitable as a substrate thereof. As a result, the present inventors have found that by focusing on the crystalline state of chabazite-type zeolite, the heat resistance of chabazite-type zeolite can be improved without necessarily requiring a large crystal size.
[0011] That is, the gist of the present invention is as follows. [1] The molar ratio of silica to alumina is 15 or more, and the molar ratio of silanol groups to silicon is 1.6 × 10 -2 The chabazite-type zeolite has an average crystal size of 0.5 μm or more and less than 1.5 μm, and a ratio of a 50% volume diameter to a 10% volume diameter of 3.2 or less. [2] The chabazite-type zeolite according to the above [1], having an average crystal size of 0.5 μm or more and 1.3 μm or less. [3] The chabazite-type zeolite according to the above [1] or [2], having a 50% volume diameter of 5.0 μm or less. [4] The chabazite-type zeolite according to any one of the above [1] to [3], wherein the crystal particles have at least one shape selected from the group consisting of cubes, rhombohedrons and approximately spherical shapes. [5] The chabazite-type zeolite according to any one of [1] to [4] above, having at least the XRD peaks shown in the table below in its XRD pattern.
[0012] [Table 1]
[0013] [6] In the IR spectrum, the wavelength range is at least 1800 cm -1 over 1930cm -1 Absorption peaks in the range of 3550cm -1 More than 3700cm -1 Absorption peaks in the following ranges and at 3710 cm -1 More than 3745cm -1 The chabazite-type zeolite according to any one of [1] to [5] above, having an absorption peak in the following range: [7] The chabazite-type zeolite according to any one of [1] to [6] above, which contains at least one of copper and iron. [8] The chabazite-type zeolite according to the above [7], wherein the ratio of at least one of copper and iron to alumina is 0.1 or more and 1.0 or less. [9] A method for producing a chabazite-type zeolite according to any one of [1] to [8] above, comprising a crystallization step of crystallizing a composition containing a silica source, an aluminum source, an alkali source, a structure directing agent, and water, wherein the composition has a molar ratio of sodium to silica greater than 0, a molar ratio of potassium to sodium less than 1.0, a molar ratio of the structure directing agent to silica less than 0.1, a molar ratio of water to silica less than 20, and a molar ratio of silica to alumina of 27.5 or more and less than 50.0.
[10] The method according to the above [9], wherein the structure directing agent is at least one selected from the group consisting of N,N,N-trialkyladamantanammonium cation, N,N,N-trimethylbenzylammonium cation, N-alkyl-3-quinuclidinol cation and N,N,N-trialkylexoaminonorbornane cation.
[11] The method according to [9] or
[10] above, wherein the molar ratio of the structure directing agent to silica is 0.06 or more and less than 0.1.
[12] The method according to any one of [9] to
[11] above, wherein the molar ratio of potassium to sodium is 0 or more and 0.6 or less.
[13] The method according to any one of [9] to
[12] above, wherein the composition does not contain fluorine.
[14] A catalyst comprising the chabazite-type zeolite according to any one of [1] to [8] above.
[15] A method for reducing nitrogen oxides, comprising using the chabazite-type zeolite according to any one of [1] to [8] above. Effect of the Invention
[0014] According to the present invention, it is possible to provide a chabazite-type zeolite having high heat resistance without having a large crystal size. Furthermore, the present invention can provide a catalyst containing such a chabazite-type zeolite. The catalyst is suitable for a nitrogen oxide reduction catalyst, particularly a nitrogen oxide reduction catalyst by selective catalytic reduction. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Hereinafter, the chabazite-type zeolite according to the embodiment of the present invention will be described.
[0016] The present invention relates to a chabazite-type zeolite, and further to a synthesized chabazite-type zeolite. The chabazite-type zeolite is a crystalline aluminosilicate having a CHA structure. The CHA structure is a crystal structure defined by the IUPAC structure code (hereinafter also simply referred to as the "structure code") defined by the International Zeolite Association (IZA). The crystal structure of a zeolite can be identified by comparing it with any of the powder X-ray diffraction (hereinafter also referred to as "XRD") patterns described in Collection of simulated XRD powder patterns for zeolites, Fifth revised edition (2007) and the XRD patterns described in Zeolite Framework Types on the IZA Structure Committee's homepage http: / / www.iza-structure.org / databases / .
[0017] The chabazite-type zeolite in the embodiment of the present invention has a molar ratio of silica to alumina (hereinafter also referred to as "SiO2 / Al2O3 ratio") of 15 or more. If the SiO2 / Al2O3 molar ratio is less than 15, the durability becomes too low when used in applications where the material is exposed to high temperature and high humidity. The higher the SiO2 / Al2O3 ratio, the higher the heat resistance tends to be. However, the chabazite-type zeolite in the embodiment of the present invention may have a SiO2 / Al2O3 ratio of 15 or more and less than 50, preferably 20 or more and 35 or less, more preferably 25 or more and 35 or less, and even more preferably 26 or more and less than 31.
[0018] Preferably, the chabazite-type zeolite in the embodiment of the present invention is a crystalline aluminosilicate. The crystalline aluminosilicate has a three-dimensional network structure in which aluminum (Al) and silicon (Si) are skeletal metals (hereinafter also referred to as "T atoms") and the T atoms are bonded via oxygen (O). Furthermore, a conceptual crystalline aluminosilicate is composed only of a network structure. In contrast, a crystalline aluminosilicate that actually exists contains irregular parts in the skeletal structure, such as broken Si-O-Si bonds, missing T atoms, or siloxy defects. Such parts become the ends of the network structure or the ends in the network structure (hereinafter, these are collectively referred to as "skeletal ends"), and the skeletal ends become silanol groups (Si-OH). Therefore, the skeleton of a realistic crystalline aluminosilicate contains silanol groups.
[0019] Zeolite, which is a crystalline aluminosilicate, tends to have a larger amount of silanol groups (hereinafter referred to as "silanol amount") contained in the skeleton of the zeolite as the amount of silicon contained therein increases. Therefore, zeolite having a SiO2 / Al2O3 ratio of less than 5 (hereinafter also referred to as "low-silica zeolite") tends to have a smaller amount of silanol than zeolite having a SiO2 / Al2O3 ratio of more than 5 (hereinafter also referred to as "high-silica zeolite"). However, since the SiO2 / Al2O3 ratio of low-silica zeolite is too low, it has lower heat resistance than high-silica zeolite and is not suitable for applications exposed to high-temperature and high-humidity atmospheres. The chabazite-type zeolite in the embodiment of the present invention has a small amount of silanol despite being a high-silica zeolite. This makes the skeleton structure less likely to collapse, so that the chabazite-type zeolite in the embodiment of the present invention has high crystallinity even after being exposed to high temperatures, and even after being exposed to high-temperature and high-humidity atmospheres.
[0020] In the embodiment of the present invention, the chabazite-type zeolite has a molar ratio of silanol groups to silicon (hereinafter also referred to as the "SiOH / Si ratio") of 1.6 × 10 -2 is less than or equal to 1.5 x 10 -2 Below, 1.3×10-2 The SiOH / Si ratio of the chabazite-type zeolite of the present invention is preferably more than 0 and is preferably 0.5×10 -2 Above, and further 0.7×10 -2 More than this, and even 1.1×10 -2 Preferably, the SiOH / Si ratio of the chabazite-type zeolite in the embodiment of the present invention is 1.05×10 -2 Above 1.60 x 10 -2 is less than or equal to 1.10 x 10 -2 Above 1.50 x 10 -2 The following is the result.
[0021] The chabazite-type zeolite in the embodiment of the present invention has such a SiO2 / Al2O3 ratio and a SiOH / Si ratio, and therefore exhibits high heat resistance even if the crystal grain size is not large, and the collapse of the framework structure is unlikely to progress even when exposed to high temperature and high humidity.
[0022] The SiOH / Si ratio can be calculated from the amount of silanol determined from the 1H MAS NMR spectrum relative to the silicon content of the chabazite-type zeolite.
[0023] The silicon content of chabazite-type zeolite can be determined by fluorescent X-ray analysis and other compositional analyses. A method for measuring the silicon content by fluorescent X-ray analysis can be a calibration curve method. The calibration curve used in the calibration curve method can be prepared by measuring the intensity of the fluorescent X-ray peak corresponding to silicon (Si) for 8 to 15 silicon-containing compounds whose silicon content is known, and drawing a calibration curve using the intensity-silicon content. The silicon content of chabazite-type zeolite can be measured by measuring the intensity of the fluorescent X-ray peak corresponding to silicon (Si) in the fluorescent X-ray pattern of the chabazite-type zeolite, which is a measurement sample, and comparing the intensity with the calibration curve.
[0024] The amount of silanol can be determined from the 1H MAS NMR spectrum. For example, the amount of silanol can be determined by measuring the dehydrated chabazite-type zeolite by 1H MAS NMR and calculating the amount of silanol from the obtained 1H MAS NMR spectrum by a calibration curve method.
[0025] A more specific method for measuring the amount of silanol is to dehydrate the chabazite-type zeolite by holding it at 350 to 400°C for 5±2 hours under vacuum evacuation, and then to collect and weigh the dehydrated chabazite-type zeolite under a nitrogen atmosphere and measure it by 1H MAS NMR. The amount of silanol in the chabazite-type zeolite is determined by a calibration curve method from the area intensity of the peak (peak at 2.0±0.5 ppm) assigned to the silanol group in the 1H MAS NMR spectrum obtained by the measurement.
[0026] The silanol content of the chabazite-type zeolite in the embodiment of the present invention is not limited as long as it has the above-mentioned SiO2 / Al2O3 ratio and SiOH / Si ratio. The silanol content of the chabazite-type zeolite in the embodiment of the present invention is 1.5×10 20 pieces / g or less (2.49×10 4 mol / g or less), and even 1.4×10 20 pieces / g or less (2.32×10 4 mol / g or less), or even 1.3×10 20 pieces / g or less (2.16×10 4 The silanol amount of the chabazite-type zeolite in the embodiment of the present invention is more than 0 silanol / g.
[0027] As shown in FIG. 1(a), the crystal particles of chabazite-type zeolite in the embodiment of the present invention are crystal particles in which each primary particle grows independently, and the primary particles and the crystal particles have the same shape, that is, at least one shape selected from the group of cubes, rhombohedrons, and approximately spherical shapes. Therefore, most of the chabazite-type zeolite in the embodiment of the present invention are crystal particles that can be considered as primary particles. In contrast, as shown in FIG. 1(b), in chabazite-type zeolite, crystal particles may be formed by chemically bonding and aggregating primary particles. Crystal particles consisting of aggregate particles (aggregates) formed by chemically bonding such primary particles are particles having a polyhedral or amorphous shape, and even if they have cubic or rhombohedral edges, they cannot be considered as primary particles.
[0028] The chabazite-type zeolite in the embodiment of the present invention has an average crystal size of 0.5 μm or more and less than 1.5 μm, preferably 0.5 μm or more and 1.3 μm or less, and more preferably more than 0.5 μm and 1.3 μm or less. Crystal particles with an average crystal size of less than 0.5 μm have low durability when used as an adsorbent or catalyst carrier. On the other hand, when the average crystal size is 1.5 μm or more, the chabazite-type zeolite is likely to contain coarse particles, and when coated on a honeycomb carrier, coating defects such as clogging and peeling are likely to occur, and when molded, it is difficult to form a molded body with high compressive strength.
[0029] The average crystal size of chabazite-type zeolite in the embodiment of the present invention means the average particle size of primary particles based on SEM observation. The average crystal size based on SEM observation is the average value of the particle size (primary particle size) of primary particles measured from an image observed by a scanning electron microscope (SEM). More specifically, it refers to the average value of the crystal particle size of chabazite-type zeolite present in the field of view of an SEM observation image observed at any magnification at which crystal particles consisting of 150 or more primary particles can be observed.
[0030] The average crystal size based on SEM observation can be measured by arithmetically averaging the particle sizes of 150 or more crystal particles consisting of primary particles selected arbitrarily in one or more observation fields photographed at a magnification of 5,000 times, measured in an arbitrary fixed direction. The conditions for SEM observation are not particularly limited as long as the shape and number of crystal particles consisting of primary particles can be clearly observed, but examples thereof include SEM observation at a magnification of 3,000 to 15,000 times.
[0031] One of the characteristics of the crystal particles of the chabazite-type zeolite in the embodiment of the present invention is that there are few agglomerated particles (agglomerates) in which primary particles are physically aggregated together, that is, so-called secondary particles. The agglomerated state of the primary particles can be measured by particle size measurement based on volume distribution.
[0032] The chabazite-type zeolite in the embodiment of the present invention has a 50% volume diameter of 5.8 μm or less, further 5.0 μm or less, and further 4.5 μm or less. Thus, the chabazite-type zeolite in the embodiment of the present invention, although having relatively small crystal particles, is less likely to form aggregated particles than the chabazite-type zeolite having a small particle diameter and a similar crystal particle diameter that has been reported in the past.
[0033] The chabazite-type zeolite according to the embodiment of the present invention has few aggregated particles, and as one of its characteristics, the 50% volume diameter to the 10% volume diameter (hereinafter also referred to as the "volume particle diameter ratio") is 3.2 or less, preferably 3.0 or less, and more preferably 2.8 or less. In order to facilitate operability (handling) during production, the volume particle diameter ratio is preferably 1.0 or more, more preferably 1.3 or more, and even more preferably 2.0 or more. The range of the volume particle diameter ratio can be 1.0 or more and 3.2 or less, or even 1.3 or more and 2.8 or less.
[0034] The 10% volume diameter and the 50% volume diameter are particle diameters whose volume fractions are 10% and 50%, respectively, in particle diameter measurement by volume distribution. The conditions for particle diameter measurement by volume distribution include the following conditions. Measurement method: Laser diffraction scattering method Refractive index: Measurement powder 1.66, dispersion medium 1.33 Measurement sample: Slurry consisting of 1% by weight of measurement powder and 99% by weight of dispersion medium Dispersion medium: Pure water Pretreatment conditions: Treat the measurement sample (slurry) with an ultrasonic homogenizer for 2 minutes.
[0035] The chabazite-type zeolite according to the embodiment of the present invention has the above-mentioned SiO2 / Al2O3 ratio and SiOH / Si ratio, and therefore is less susceptible to deterioration, i.e., collapse of the framework structure, when exposed to high temperature and high humidity even if the average crystal size is not large. Thus, the chabazite-type zeolite according to the embodiment of the present invention exhibits high heat resistance because the crystallinity is less likely to decrease.
[0036] When evaluating the heat resistance, the zeolite can be exposed to high temperature and high humidity by hydrothermal durability treatment. The following conditions can be exemplified as the conditions for the hydrothermal durability treatment. Treatment atmosphere: Air containing 10% water vapor by volume Space velocity: 6,000hr -1 Processing temperature: 900±5℃ Processing time: 1 hour to 24 hours
[0037] The collapse of the zeolite framework is more affected by the treatment temperature than by the treatment time of the hydrothermal durability treatment, and the collapse of the zeolite framework progresses significantly as the treatment temperature increases. For example, the collapse of the zeolite framework progresses more rapidly in a hydrothermal durability treatment at a treatment temperature of 900°C and a treatment time of 1 hour than in a hydrothermal durability treatment at a treatment temperature of 700°C and a treatment time of 24 hours.
[0038] The heat resistance can be evaluated by comparing the change in crystallinity before and after exposing the zeolite to high temperature and humidity. In chabazite-type zeolite, the intensity of the peak at 2θ=21±1° in the XRD pattern is used as an index of crystallinity, and by comparing the crystallinity of zeolite samples that have been subjected to hydrothermal durability treatment, the degree of crystallinity of each zeolite can be compared. The higher the intensity after hydrothermal durability treatment, the higher the heat resistance.
[0039] Preferably, the chabazite-type zeolite in the embodiment of the present invention has at least the XRD peaks shown in the table below in its XRD pattern.
[0040] [Table 2]
[0041] The XRD measurement conditions in the embodiment of the present invention are as follows. Radiation source: CuKα radiation (λ=1.5405Å) Measurement mode: Step scan Scan condition: 0.04° / sec Measurement time: 3 seconds Measurement range: 2θ=4° to 44°
[0042] In an embodiment of the present invention, the chabazite-type zeolite has a wavelength of at least 1800 cm in the IR spectrum. -1 over 1930cm -1 Absorption peaks in the following range (hereinafter also referred to as "peak 1"): 3550 cm -1 More than 3700cm -1 Absorption peaks in the following range (hereinafter also referred to as “Peak 2”) and 3710 cm -1 More than 3745cm -1 It is preferable that the absorption peak (hereinafter also referred to as "peak 3") is in the following range.
[0043] In an embodiment of the present invention, the chabazite-type zeolite has a molecular weight of 3450 cm-1 More than 3545cm -1 It may have an absorption peak (hereinafter also referred to as "peak 4") in the following range.
[0044] Peak 1 is 1850cm -1 over 1890cm -1 The absorption peaks in the following ranges are preferred: Peak 2 is 3665 cm -1 More than 3695cm -1 The absorption peaks in the following ranges are preferred: Peak 3 is 3720 cm -1 More than 3740cm -1 The absorption peak is preferably in the following range:
[0045] The chabazite-type zeolite according to the embodiment of the present invention has a ratio of the maximum intensity of peak 2 to the maximum intensity of peak 1 (hereinafter referred to as "IR ratio"). P2 / P1 ") is preferably 0.1 or more and 1.5 or less, and more preferably 0.5 or more and 1.0 or less.
[0046] The chabazite-type zeolite according to the embodiment of the present invention has a ratio of the maximum intensity of peak 3 to the maximum intensity of peak 1 (hereinafter referred to as "IR ratio"). P3 / P1 ") is preferably 1.5 or more and 2.5 or less, and more preferably 1.6 or more and 2.0 or less.
[0047] The chabazite-type zeolite according to the embodiment of the present invention has a ratio of the maximum intensity of peak 4 to the maximum intensity of peak 1 (hereinafter referred to as "IR ratio"). P4 / P1 ") is preferably 0 or more and 1.0 or less, and more preferably 0 or more and 0.1 or less.
[0048] In the embodiment of the present invention, the chabazite-type zeolite has a peak 2 of 3665 cm -1 More than 3695cm -1 Absorption peak in the following range and IR ratio P2 / P1 is 0.1 or more and 1.5 or less and IR ratio P3 / P1It is more preferable that the ratio satisfies the range of 1.5 to 2.5.
[0049] The measurement conditions for IR spectrum in the embodiment of the present invention are as follows. Measurement method: Diffuse reflection method Measurement wavelength range: 400~4000cm -1 Resolution: 4cm -1 Number of times: 128
[0050] The IR spectrum and XRD pattern of the above chabazite-type zeolite are those in a state in which no organic structure directing agent is contained.
[0051] The chabazite-type zeolite in the embodiment of the present invention preferably contains a transition metal, more preferably contains at least one of iron (Fe) or copper (Cu), and even more preferably contains copper. This results in a chabazite-type zeolite that not only has high heat resistance but also exhibits high nitrogen oxide reduction properties. Therefore, the chabazite-type zeolite in the embodiment of the present invention that contains a transition metal (hereinafter also referred to as "the present metal-containing chabazite-type zeolite") can be used as a catalyst, further as a nitrogen oxide reduction catalyst, and further as a nitrogen oxide reduction catalyst that exhibits high nitrogen oxide reduction properties.
[0052] In the present metal-containing chabazite-type zeolite, the metal is preferably contained in the pores, on the surface, or elsewhere other than as a T atom.
[0053] When the present metal-containing chabazite-type zeolite contains copper, the molar ratio of copper to alumina (hereinafter also referred to as the "Cu / Al2O3 ratio" or "Cu / Al2 ratio") is preferably 0.1 or more and 1.0 or less, more preferably 0.4 or more and 0.8 or less.
[0054] After being exposed to high temperature and high humidity, the present metal-containing chabazite-type zeolite exhibits particularly high nitrogen oxide reduction properties in a temperature range of less than 200° C. One of the reasons for this is that the chabazite-type zeolite according to the embodiment of the present invention has high heat resistance.
[0055] Because the framework structure of the present metal-containing chabazite-type zeolite is resistant to collapse, it exhibits higher nitrogen oxide reduction properties than conventional metal-containing chabazite-type zeolites even after exposure to high temperature and high humidity, and exhibits particularly high nitrogen oxide reduction properties in the low temperature range below 200° C. The nitrogen oxide reduction properties of the present metal-containing chabazite-type zeolite are particularly high in the temperature range of 100° C. to 250° C., preferably in the temperature range of 100° C. to 200° C., and more preferably in the temperature range of 150° C. to 200° C.
[0056] Next, a method for producing chabazite-type zeolite according to an embodiment of the present invention will be described.
[0057] The chabazite-type zeolite of the present invention can be produced by a production method including a crystallization step of crystallizing a composition (hereinafter also referred to as a "raw material composition") containing a silica source, an aluminum source, an alkali source, a structure-directing agent, and water, wherein the composition has a molar ratio of sodium to silica greater than 0, a molar ratio of potassium to sodium less than 1.0, a molar ratio of structure-directing agent to silica less than 0.1, a molar ratio of water to silica less than 20, and a molar ratio of silica to alumina of 27.5 or more and less than 50.0.
[0058] The manufacturing method according to an embodiment of the present invention relates to a method for manufacturing chabazite-type zeolite by crystallizing a raw material composition containing a structure directing agent (hereinafter also referred to as "SDA"). When a composition not containing SDA is crystallized, even if chabazite-type zeolite particles having a crystal size exceeding 0.5 μm are obtained, the particles are particles in which primary particles are strongly bonded to each other by chemical bonds. Such particles are aggregates consisting of an assembly of primary particles that have grown into crystals while being oriented without regularity. The aggregated particles are not only bulky because it is difficult to break up the aggregates in a treatment after crystallization, but also the crystals themselves collapse when physical forces such as crushing are applied. Therefore, chabazite-type zeolite consisting of aggregated particles (aggregates) is not suitable for use as a catalyst or catalyst support.
[0059] Furthermore, the manufacturing method in the embodiment of the present invention crystallizes a raw material composition having a molar ratio of sodium to silica exceeding 0, and relates to a manufacturing method for chabazite-type zeolite by crystallizing a raw material composition containing at least sodium. By containing SDA and sodium, crystal growth due to chemical bonds between primary particles is suppressed, and crystal growth of each primary particle is likely to proceed without being affected by other primary particles. As a result, crystal particles in which each primary particle has grown independently are obtained. As a result, each crystal particle has at least one of a particle shape having a shape reflecting the shape of the primary particle or a substantially spherical particle shape. Furthermore, such crystal particles are unlikely to form aggregated particles (agglomerates) formed by physical aggregation, and chabazite-type zeolite consisting of crystal particles in a state in which the primary particles are dispersed is obtained. That is, the manufacturing method of the present invention is unlikely to generate either physical aggregated particles (agglomerates) or chemical aggregated particles (aggregates), and crystal particles consisting of highly dispersible primary particles are obtained. That is, by the production method according to the embodiment of the present invention, it is possible to obtain chabazite-type zeolite having particles with a crystal grain size that is not too large and a small volume-to-grain size ratio.
[0060] The silica source is a compound containing silicon (Si), and can be at least one selected from the group consisting of colloidal silica, precipitated silica, amorphous silica, sodium silicate, tetraethyl orthosilicate, and amorphous aluminosilicate, and can further include amorphous aluminosilicate.
[0061] The alumina source is a compound containing aluminum (Al), and can include at least one selected from the group consisting of aluminum sulfate, sodium aluminate, aluminum hydroxide, aluminum chloride, and amorphous aluminosilicates, and further includes amorphous aluminosilicates.
[0062] The silica source and alumina source are preferably in a form that allows them to be mixed sufficiently uniformly with other raw materials, and are preferably amorphous aluminosilicates.
[0063] The alkali source is a compound containing an alkali metal. The alkali source in the production method according to the embodiment of the present invention is a compound containing at least sodium, and is preferably a compound containing at least one selected from the group consisting of potassium, rubidium, and cesium, and a compound containing sodium. The compound containing an alkali metal may be at least one selected from the group consisting of hydroxides, fluorides, bromides, iodides, sulfates, nitrates, and carbonates of alkali metals.
[0064] When other raw materials contained in the raw material composition, such as a silica source or an alumina source, contain at least one selected from the group consisting of sodium, potassium, rubidium, and cesium, these other raw materials can also be used as an alkali source.
[0065] The water contained in the raw material composition may be pure water, but when other raw materials contained in the raw material composition contain water, such as aqueous solutions, the moisture of these other raw materials can also be considered as the water in the raw material composition.
[0066] In an embodiment of the present invention, the SDA is preferably an organic structure directing agent, more preferably at least one selected from the group consisting of N,N,N-trialkyladamantan ammonium cation, N,N,N-trimethylbenzyl ammonium cation, N-alkyl-3-quinuclidinol cation and N,N,N-trialkylexoaminonorbornane cation, and further preferably at least one of N,N,N-trialkyladamantan ammonium cation and N,N,N-trimethylbenzyl ammonium cation. The SDA is preferably an organic structure directing agent, more preferably at least one selected from the group consisting of N,N,N-trialkyladamantan ammonium cation, N,N,N-trimethylbenzyl ammonium cation and N,N,N-trialkyladamantan ammonium cation (hereinafter referred to as "TAAD + It is even more preferable that the TAAD is + As the ammonium salt, N,N,N-trimethyladamantanate (hereinafter referred to as "TMAD + " ) can be mentioned as examples.
[0067] SDA may be contained in the raw material composition in the form of a salt, and is preferably at least one selected from the group consisting of hydroxide, bromide, iodide, carbonate, methyl carbonate salt, and sulfate containing any of the above cations, more preferably at least one selected from the group consisting of hydroxide, bromide, and iodide, and even more preferably hydroxide.
[0068] For example, SDA is TMAD + If so, TMAD +The salt may be at least one selected from the group consisting of N,N,N-trimethyladamantan ammonium hydroxide, N,N,N-trimethyladamantan ammonium fluoride, N,N,N-trimethyladamantan ammonium bromide, N,N,N-trimethyladamantan ammonium iodide, N,N,N-trimethyladamantan ammonium carbonate, N,N,N-trimethyladamantan ammonium methyl carbonate salt, and N,N,N-trimethyladamantan ammonium sulfate. At least one of N,N,N-trimethyladamantan ammonium hydroxide and N,N,N-trimethyladamantan ammonium halide is preferred, and N,N,N-trimethyladamantan ammonium hydroxide (hereinafter also referred to as "TMADOH") is more preferred. In an embodiment of the present invention, the organic structure directing agent contained in the raw material composition is TMAD. + It is preferable that only
[0069] When the raw material composition contains chlorine or fluorine, it is necessary to use a corrosion-resistant manufacturing device due to their corrosiveness, which tends to increase the manufacturing cost. Therefore, the raw material composition preferably does not contain fluorine, more preferably does not contain at least one of chlorine or fluorine, and preferably does not contain chlorine or fluorine. Considering measurement errors, etc., the chlorine content and fluorine content of the raw material composition are preferably 6000 ppm or less, and further preferably 1000 ppm or less, respectively.
[0070] The molar ratio of silica to alumina in the raw material composition (SiO2 / Al2O3 ratio) is 27.5 or more and less than 50.0, preferably 27.8 or more and less than 50.0. In the crystallization step, the SiO2 / Al2O3 ratio of the obtained chabazite-type zeolite tends to be lower than the SiO2 / Al2O3 ratio of the raw material composition. If the SiO2 / Al2O3 ratio is less than 27.5, the chabazite-type zeolite having the SiO2 / Al2O3 ratio of the present invention tends to be difficult to crystallize, and the physical aggregation of the obtained chabazite-type zeolite tends to be strong. If the SiO2 / Al2O3 ratio is too high, zeolites other than chabazite-type zeolite are generated, making it difficult to obtain a single-phase chabazite-type zeolite. Therefore, the SiO2 / Al2O3 ratio is less than 50.0, preferably 40.0 or less. A particularly preferable range of the SiO2 / Al2O3 ratio is 27.5 or more and 40.0 or less, and furthermore 30.0 or more and 35.0 or less.
[0071] The raw material composition has a molar ratio of SDA to silica (hereinafter also referred to as "SDA / SiO2 ratio") of less than 0.1, preferably 0.095 or less, and more preferably 0.085 or less. If the raw material composition has a molar ratio of water to silica (hereinafter also referred to as "H2O / SiO2 ratio") described below and the SDA / SiO2 ratio is 0.1 or more, the resulting chabazite-type zeolite will be too fine. Since SDA is expensive, the production cost will be high if the SDA / SiO2 ratio is 0.1 or more.
[0072] Since the raw material composition contains SDA, the SDA / SiO2 ratio exceeds 0, but the SDA / SiO2 ratio is 0.05 or more, and further 0.06 or more, to promote the crystallization of chabazite-type zeolite. This makes it difficult for crystallization of zeolites other than chabazite-type zeolite and crystallization of a mixture of zeolites other than chabazite-type zeolite and chabazite-type zeolite to occur, and tends to make it easier to obtain single-phase chabazite-type zeolite. From the viewpoint of obtaining a crystallization time suitable for industrial production, the SDA / SiO2 ratio is preferably 0.06 or more and less than 0.1, and further preferably 0.07 or more and 0.09 or less.
[0073] The raw material composition has a molar ratio of water (H2O) to silica (H2O / SiO2 ratio) of less than 20 and preferably 19 or less. By having the above-mentioned SDA / SiO2 ratio and an H2O / SiO2 ratio of less than 20, the obtained chabazite-type zeolite is less likely to be fine. In addition, if the H2O / SiO2 ratio is 20 or more, the crystallization of the chabazite-type zeolite of the present invention does not proceed in the range of the OH / SiO2 ratio described later. On the other hand, since the raw material composition contains water, the H2O / SiO2 ratio exceeds 0, but by making the H2O / SiO2 ratio 5 or more, or even 9 or more, the raw material composition can be given an appropriate fluidity, and the composition of the raw material composition is easily made uniform. More preferable H2O / SiO2 ratios include 10 or more and less than 20, and even 11 or more and 19 or less. Particularly preferable H2O / SiO2 ratios include 11 or more and 18 or less, and even 11 or more and 16 or less.
[0074] The raw material composition has a molar ratio of sodium to silica (hereinafter also referred to as "Na / SiO2 ratio") exceeding 0, and contains at least sodium. The Na / SiO2 ratio is preferably 0.02 or more, and more preferably 0.04 or more. The Na / SiO2 ratio is preferably 0.1 or less, and more preferably 0.08 or less. When the Na / SiO2 ratio is within this range, dissolution of the silica source is promoted in the raw material composition having the SiO2 / Al2O3 ratio, SDA / SiO2 ratio, and H2O / SiO2 ratio of the present invention, and crystallization of the chabazite-type zeolite is likely to occur efficiently.
[0075] The molar ratio of potassium to sodium in the raw material composition (hereinafter also referred to as "K / Na ratio") is preferably less than 1.0 and less than 0.6. The raw material composition may not contain potassium, but may contain potassium (that is, the K / Na ratio may be 0 or more). However, when the raw material composition contains potassium in addition to sodium, the production of zeolites other than chabazite-type zeolite is further suppressed. On the other hand, when the amount of potassium is greater than that of sodium, the crystal particles tend to become too large, or the crystal particles tend to physically aggregate with each other and form aggregated particles (agglomerates). Therefore, when the raw material composition contains potassium, the preferable K / Na ratio can be 0 or more and less than 1.0, further 0.1 or more and less than 1.0, further 0 or more and less than 0.6, further 0 or more and less than 0.3, and further 0.2 or more and less than 0.6.
[0076] The molar ratio of hydroxide ions to silica in the raw material composition (hereinafter also referred to as "OH / SiO2 ratio") is preferably 0.1 or more and less than 0.9, and more preferably 0.15 or more and 0.5 or less. When the OH / SiO2 ratio is 0.1 or more, the crystallization of chabazite-type zeolite is likely to proceed. When the OH / SiO2 ratio is 0.9 or more, the dissolution of the silica source is promoted, so that it tends to be difficult to obtain a chabazite-type zeolite that is a single phase of the CHA structure and has both the SiO2 / Al2O3 ratio and the SiOH / Si ratio in the embodiment of the present invention.
[0077] In the crystallization step, the raw material composition is crystallized by hydrothermal treatment. Crystallization proceeds at 80°C or higher.
[0078] The raw material composition can be produced by crystallizing the raw material composition in a sealed pressure vessel at a temperature of 100 to 200°C for a sufficient period of time. A preferred crystallization temperature is 155°C to 185°C. The crystallization may be performed with the raw material composition left to stand, but is preferably performed with the raw material composition stirred and mixed. The crystallization time can be 1 hour to 100 hours, and more preferably 10 hours to 80 hours.
[0079] The method for producing chabazite-type zeolite in the embodiment of the present invention may include, after the crystallization step, one or more of a washing step, a drying step, an SDA removal step, or an ammonium treatment step.
[0080] In the washing step, the crystallized chabazite-type zeolite and the liquid phase are separated into a solid-liquid phase by a known method, and the chabazite-type zeolite obtained as a solid phase may be washed with pure water.
[0081] The drying step removes moisture from the chabazite-type zeolite. The conditions for the drying step are arbitrary, but examples include drying in the air at 50° C. or higher and 150° C. or lower, or even at 100° C. or higher and 150° C. or lower, for 2 hours or more, by leaving the zeolite to stand or by using a spray dryer.
[0082] The SDA removal step is carried out to remove SDA contained in the chabazite-type zeolite. Usually, the chabazite-type zeolite that has undergone the crystallization step contains SDA in its pores. Therefore, this can be removed as necessary.
[0083] The SDA removal step can be carried out by any method as long as the SDA can be removed. Examples of such removal methods include at least one selected from the group consisting of liquid phase treatment using an acidic aqueous solution, exchange treatment using a resin or the like, pyrolysis treatment, and calcination treatment. From the viewpoint of production efficiency, the SDA removal step is preferably either pyrolysis treatment or calcination treatment. Examples of the SDA removal step include a step of treating the chabazite-type zeolite in the air at 400°C or higher and 700°C or lower.
[0084] The ammonium treatment step is carried out to remove the alkali metal contained in the chabazite-type zeolite. The ammonium treatment step can be carried out by a general method. For example, the ammonium treatment step is carried out by contacting the chabazite-type zeolite with an aqueous solution containing ammonium ions.
[0085] When the chabazite-type zeolite in the embodiment of the present invention is a metal-containing chabazite-type zeolite, the production method in the embodiment of the present invention may include a metal-containing step of contacting the chabazite-type zeolite with a compound containing at least one of copper or iron (hereinafter also referred to as a "metal-containing compound").
[0086] In the metal-containing step, the chabazite-type zeolite is contacted with a metal-containing compound. This allows at least one of copper and iron to be contained in the pores of the chabazite-type zeolite. As long as at least one of copper and iron is contained in the chabazite-type zeolite, the method of contacting the chabazite-type zeolite with the metal-containing compound (hereinafter also referred to as the "metal-containing method") may be any method. As the metal-containing method, at least one selected from the group consisting of an ion exchange method, an impregnation support method, an evaporation to dryness method, a precipitation support method, and a physical mixing method can be mentioned. Since it is easy to control the amount of at least one of copper and iron contained in the chabazite-type zeolite, the metal-containing method is preferably the impregnation support method.
[0087] The metal-containing compound used in the metal-containing step is arbitrary, and may be at least one selected from the group consisting of nitrates, sulfates, acetates, chlorides, complex salts, oxides, and composite oxides containing at least one of copper and iron. In order to facilitate uniform incorporation of at least one of copper and iron into the chabazite-type zeolite, the metal-containing compound is preferably a water-soluble compound containing at least one of copper and iron, and is preferably at least one selected from the group consisting of nitrates, sulfates, and acetates containing at least one of copper and iron.
[0088] In the manufacturing method according to the embodiment of the present invention, it is preferable to have a calcination step of calcining the metal-containing chabazite-type zeolite obtained in the metal-containing step. Depending on the metal-containing method, impurities such as counter ions of metal compounds may remain, and such impurities are removed in the calcination step. In the calcination step, the metal-containing chabazite-type zeolite may be calcined under any conditions. Examples of the calcination conditions include air, a calcination temperature of 500°C to 700°C, and a calcination time of 0.5 hours to 5 hours.
[0089] The chabazite-type zeolite and metal-containing chabazite-type zeolite in the embodiment of the present invention (hereinafter also referred to as "the present chabazite-type zeolite, etc.") can be used as a catalyst. The catalyst containing the present chabazite-type zeolite, etc. (hereinafter also referred to as "the present catalyst") can be used in the form of either a powder or a molded body. When the present catalyst is used in the form of a powder, it may be applied or wash-coated to a substrate such as a honeycomb to form a catalyst member. When the present catalyst is used as a molded body, it may be in at least one shape selected from the group consisting of a sphere, an approximately sphere, an ellipse, a disk, a cylinder, a polyhedron, an irregular shape, and a petal shape, or any other shape suitable for the application.
[0090] When the present catalyst is formed into a molded body, it may contain, in addition to the present catalyst, at least one clay selected from the group consisting of silica, alumina, kaolin, attapulgite, montmorillonite, bentonite, allophane, and sepiolite.
[0091] In particular, the present catalyst is preferably used as a nitrogen oxide reduction catalyst, and more preferably as a nitrogen oxide reduction catalyst in the exhaust gas of an internal combustion engine.
[0092] The reduction of nitrogen oxides can be achieved by contacting the present catalyst with a nitrogen oxide-containing gas. The space velocity at which the nitrogen oxide-containing gas is contacted with the present catalyst is optional, and is generally within the range of 500 to 500,000 h on a volume basis. -1 , and further 2000~300,000hr -1 The following points can be mentioned.
[0093] Examples of nitrogen oxides reduced by the present catalyst include at least one selected from the group consisting of nitric oxide, nitrogen dioxide, dinitrogen trioxide, dinitrogen tetroxide, and dinitrogen monoxide, and examples of nitrogen oxides include at least one selected from the group consisting of nitric oxide, nitrogen dioxide, and dinitrogen monoxide.
[0094] The nitrogen oxide-containing gas may contain components other than nitrogen oxide, and examples of the nitrogen oxide-containing gas include gases containing nitrogen oxide and at least one selected from the group consisting of hydrocarbons, carbon monoxide, carbon dioxide, hydrogen, nitrogen, oxygen, sulfur oxides, and water.Specific examples of the nitrogen oxide-containing gas include exhaust gas from internal combustion engines, and further exhaust gas from diesel automobiles, gasoline automobiles, boilers, gas turbines, etc.
[0095] The method for reducing nitrogen oxides using the present catalyst is preferably a method for reducing nitrogen oxides in the presence of a reducing agent. The reducing agent may be at least one selected from the group consisting of ammonia, urea, organic amines, hydrocarbons, alcohols, ketones, carbon monoxide, and hydrogen. In order to further increase the efficiency of nitrogen oxide reduction, the reducing agent is more preferably at least one selected from the group consisting of ammonia, urea, and organic amines. In addition, when the nitrogen oxide-containing gas contains a reducing substance such as at least one selected from the group consisting of hydrocarbons, carbon monoxide, and hydrogen, this can also be considered as a reducing agent. [Brief description of the drawings]
[0096] [Figure 1] Schematic diagram showing the shape of crystal particles ((a) primary crystal particle, (b) aggregate) [Diagram 2] SEM observation of the chabazite-type zeolite of Comparative Example 6 (upper figure: magnification 15,000 times, lower figure: magnification 1,000 times) EXAMPLES
[0097] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples.
[0098] (Crystal Structure and Crystallinity) Using a general X-ray diffractometer (product name: MXP-3, manufactured by Mac Science), powder X-ray diffraction (hereinafter, referred to as "XRD") measurements of the samples were performed under the following conditions. Radiation source: CuKα radiation (λ=1.5405Å) Measurement mode: Step scan Scan condition: 0.04° / sec Measurement time: 3 seconds Measurement range: 2θ=4° to 44° The obtained XRD pattern was compared with the XRD pattern listed on the IZA Structure Committee website to identify the crystal structure of the sample. The height of the XRD peak (2θ=21±1°) corresponding to the lattice spacing (d)=4.25 in the XRD pattern was taken as the degree of crystallinity. (SiO2 / Al2O3 ratio) The composition of the samples was measured by X-ray fluorescence spectroscopy. The SiO2 / Al2O3 ratio was calculated from the X-ray intensity ratio of Si to Al using a calibration curve.
[0099] (Silanol group content) The silanol group content of chabazite-type zeolite was measured by 1H MAS NMR. The sample used was chabazite-type zeolite that had been treated at 600°C for 2 hours under air flow, ion-exchanged with a 20% aqueous ammonium chloride solution, and then dried overnight at 110°C in air. Prior to the measurement, the sample was pretreated by dehydrating it by holding it at 400°C for 5 hours under vacuum exhaust. After pretreatment, the sample was cooled to room temperature and collected under a nitrogen atmosphere and weighed. A general NMR measurement device (device name: VXR-300S, manufactured by Varian) was used as the measurement device. The measurement conditions were as follows: Resonance frequency: 300.0MHz Pulse width: π / 2 Measurement waiting time: 10 seconds Number of times: 32 Rotation frequency: 4kHz Shift criteria: TMS From the obtained 1H MAS NMR spectrum, the peak at 2.0±0.5 ppm was determined to be a peak attributable to silanol groups. The peak was subjected to waveform separation and its area intensity was calculated. The amount of silanol in the sample was calculated from the obtained area intensity by the calibration curve method.
[0100] (SiOH / Si ratio) The silanol group content (mol / g) of the chabazite-type zeolite measured by 1H MAS NMR relative to the silicon content (mol / g) of the chabazite-type zeolite obtained by fluorescent X-ray analysis was calculated, and this was defined as the SiOH / Si ratio. (Cu / Al2O3 ratio) The copper content was measured by ICP method. The sample was dissolved in a mixed solution of hydrofluoric acid and nitric acid to prepare a measurement solution. A general ICP device (device name: Optima 5300DV, manufactured by Perkin Elmer) was used to measure the Al concentration, Cu concentration, Na concentration, and K concentration of the measurement solution. The Cu / Al2O3 ratio, Na / Al2O3 ratio, and K / Al2O3 ratio were calculated from the obtained concentrations.
[0101] (copper content) The copper content was calculated from the following formula using the measurement results of the SiO2 / Al2O3 ratio, the Cu / Al2O3 ratio, the Na / Al2O3 ratio, and the K / Al2O3 ratio. Copper content (wt%)=(d×M Cu ×100) / (M Al2O3 +a·M SiO2 +b / 2 M Na2O +c / 2·M K2O +d·M CuO ) In the above formula, a is the SiO2 / Al2O3 ratio (mol / mol), b is the Na / Al2O3 ratio (mol / mol), c is the K / Al2O3 ratio (mol / mol), d is the Cu / Al2O3 ratio (mol / mol), M Cu is the atomic weight of copper (63.5g / mol), M Al2O3 is the molecular weight of Al2O3 (102.0 g / mol), M SiO2 is the molecular weight of SiO2 (60.1g / mol), M Na2Ois the molecular weight of Na2O (62.0 g / mol), M K2O is the molecular weight of K2O (94.2 g / mol), and M CuO is the molecular weight of CuO (79.5 g / mol).
[0102] (Method of measuring average crystal size) The sample was observed with a scanning electron microscope (hereinafter referred to as "SEM") using a general scanning electron microscope (instrument name: JSM-6390LV, manufactured by JEOL Ltd.). The magnification for SEM observation was 10,000 times. From the SEM image of the sample obtained by SEM observation, 150 primary particles were randomly selected and their horizontal Feret diameter was measured. The average of the obtained measurements was calculated and used as the average crystal diameter of the sample. (Measurement of 10% volume diameter and 50% volume diameter) 1 g of the powder sample was mixed with 99 g of pure water to obtain a slurry, which was used as the measurement sample. The obtained slurry was treated with an ultrasonic homogenizer for 2 minutes to disperse the powder sample in the slurry. The volume diameter of the treated slurry was measured by a laser diffraction scattering method to measure the 10% volume diameter and the 50% volume diameter. The volume diameter ratio was calculated from the obtained 10% volume diameter and 50% volume diameter.
[0103] (Method of measuring nitrogen oxide reduction rate (%)) The sample was molded and crushed to obtain agglomerated particles with an aggregate diameter of 12 to 20 mesh. 1.5 mL of the agglomerated particle sample was filled into an atmospheric pressure fixed bed flow type reactor, and a nitrogen oxide-containing gas was passed through it at a specified temperature, and the nitrogen oxide concentrations at the inlet and outlet of the atmospheric pressure fixed bed flow type reactor were measured. The flow conditions for the nitrogen oxide-containing gas were as follows: Composition of nitrogen oxide-containing gas: NO 200ppm NH3 200ppm O210 capacity% H2O 3% by volume N2 remainder Flow rate of nitrogen oxide-containing gas: 1.5L / min Space velocity: 60,000hr -1 The nitrogen oxide reduction rate was calculated from the obtained nitrogen oxide concentration according to the following formula. Nitrogen oxide reduction rate (%) ={([NOx]in-[NOx]out) / [NOx]in}×100 [NOx]in is the nitrogen oxide concentration of the nitrogen oxide-containing gas at the inlet of the atmospheric pressure fixed-bed flow reactor, and [NOx]out is the nitrogen oxide concentration of the nitrogen oxide-containing gas at the outlet of the atmospheric pressure fixed-bed flow reactor.
[0104] Example 1 A 25% aqueous solution of N,N,N-trimethyladamantanammonium hydroxide (hereinafter also referred to as "25% aqueous solution of TMADAOH"), pure water, a 48% aqueous solution of sodium hydroxide, and amorphous aluminosilicate were added and mixed well to obtain a raw material composition having the following composition. SiO2 / Al2O3 ratio = 27.5 TMADA / SiO2 ratio = 0.081 Na / SiO2 ratio = 0.094 K / SiO2 ratio = 0 K / Na ratio = 0 H2O / SiO2 ratio = 12 OH / SiO2 ratio = 0.175
[0105] The raw material composition was sealed in a stainless steel autoclave and heated at 170°C for 70 hours while rotating at 55 rpm. The product after heating was subjected to solid-liquid separation, and the obtained solid phase was washed with a sufficient amount of pure water and dried at 110°C.
[0106] The product was a single phase of chabazite-type zeolite with a SiO2 / Al2O3 ratio of 26.2 and a SiOH / Si ratio of 1.1×10 -2 The average crystal size was 0.6 μm and the volume diameter ratio was 2.29.
[0107] Example 2 A 25% TMADAOH aqueous solution, pure water, a 48% sodium hydroxide aqueous solution, a 48% potassium hydroxide aqueous solution, and an amorphous aluminosilicate were mixed to obtain a raw material composition having the following composition, and a product was obtained in the same manner as in Example 1. This product was designated as the chabazite-type zeolite of this example. SiO2 / Al2O3 ratio = 32.3 TMADA / SiO2 ratio = 0.081 Na / SiO2 ratio = 0.140 K / SiO2 ratio = 0.029 K / Na ratio = 0.21 H2O / SiO2 ratio = 18 OH / SiO2 ratio = 0.250
[0108] The chabazite-type zeolite of this example is a single phase of chabazite-type zeolite, with a SiO2 / Al2O3 ratio of 30.2 and a SiOH / Si ratio of 1.2×10 -2 The average crystal size was 1.0 μm and the volume diameter ratio was 2.74.
[0109] The chabazite-type zeolite of this example has a peak at 1861 cm in the IR spectrum. -1 , 3683cm -1 and 3732 cm -1 From this, it was confirmed that the chabazite-type zeolite of this example has peaks 1, 2, and 3, but does not have peak 4. In addition, the ratio of each absorption spectrum is expressed as the IR ratio. P2 / P1 is 0.75, IR ratio P3 / P1 is 1.67 and IR ratio P4 / P1 was 0.
[0110] Example 3 A 25% TMADAOH aqueous solution, pure water, a 48% sodium hydroxide aqueous solution, a 48% potassium hydroxide aqueous solution, and an amorphous aluminosilicate were mixed to obtain a raw material composition having the following composition. A product was obtained in the same manner as in Example 1, and this product was designated as the chabazite-type zeolite of this example. SiO2 / Al2O3 ratio = 32.3 TMADA / SiO2 ratio = 0.081 Na / SiO2 ratio = 0.111 K / SiO2 ratio = 0.058 K / Na ratio = 0.52 H2O / SiO2 ratio = 18 OH / SiO2 ratio = 0.250
[0111] The chabazite-type zeolite of this example is a single-phase chabazite-type zeolite, with a SiO2 / Al2O3 ratio of 30.7 and a SiOH / Si ratio of 1.3×10 -2 The average crystal size was 0.5 μm and the volume diameter ratio was 2.63.
[0112] Example 4 A 25% TMADAOH aqueous solution, pure water, a 48% sodium hydroxide aqueous solution, a 48% potassium hydroxide aqueous solution, and an amorphous aluminosilicate were mixed to obtain a raw material composition having the following composition. A product was obtained in the same manner as in Example 1, and this product was designated as the chabazite-type zeolite of this example. SiO2 / Al2O3 ratio = 32.3 TMADA / SiO2 ratio = 0.081 Na / SiO2 ratio = 0.149 K / SiO2 ratio = 0.020 K / Na ratio = 0.13 H2O / SiO2 ratio = 18 OH / SiO2 ratio = 0.250
[0113] The chabazite-type zeolite of this example is a single phase of chabazite-type zeolite, with a SiO2 / Al2O3 ratio of 29.9 and a SiOH / Si ratio of 1.3×10 -2 The average crystal size was 1.3 μm and the volume diameter ratio was 2.19.
[0114] Example 5 A product was obtained in the same manner as in Example 1 except that 13.0 g of a 25% TMADAOH aqueous solution, 12.6 g of pure water, 0.4 g of a 48% sodium hydroxide aqueous solution, and 30.9 g of amorphous aluminosilicate were mixed to obtain a raw material composition having the following composition, and this product was designated as the chabazite-type zeolite of this example. SiO2 / Al2O3 ratio = 32.3 TMADA / SiO2 ratio = 0.081 Na / SiO2 ratio = 0.094 K / SiO2 ratio = 0 K / Na ratio = 0 H2O / SiO2 ratio = 12 OH / SiO2 ratio = 0.175
[0115] The chabazite-type zeolite of this example is a single phase of chabazite-type zeolite, with a SiO2 / Al2O3 ratio of 32.5 and a SiOH / Si ratio of 1.3×10 -2 The average crystal size was 1.0 μm and the volume diameter ratio was 2.06.
[0116] Comparative Example 1 Chabazite-type zeolite was synthesized by a method according to JP 2010-168269 A. That is, a 25% aqueous solution of TMADAOH, pure water, a 48% aqueous solution of sodium hydroxide, a 48% aqueous solution of potassium hydroxide, and an amorphous luminosilicate were mixed to obtain a raw material composition having the following composition. SiO2 / Al2O3 ratio = 32.3 TMADA / SiO2 ratio = 0.081 Na / SiO2 ratio = 0.084 K / SiO2 ratio = 0.084 K / Na ratio = 1.0 H2O / SiO2 ratio = 18 OH / SiO2 ratio = 0.249
[0117] A product was obtained in the same manner as in Example 1, except that the raw material composition was used and the heating temperature was 150° C., and this product was designated as the chabazite-type zeolite of this comparative example.
[0118] The chabazite-type zeolite of this comparative example is a single-phase chabazite-type zeolite, with a SiO2 / Al2O3 ratio of 31.0 and a SiOH / Si ratio of 1.7×10 -2 The average crystal size was 1.6 μm and the volume diameter ratio was 1.23. Thus, the chabazite-type zeolite of this comparative example had a large average particle size.
[0119] Comparative Example 2 A 25% TMADAOH aqueous solution, pure water, a 48% sodium hydroxide aqueous solution, a 48% potassium hydroxide aqueous solution, and an amorphous aluminosilicate were mixed to obtain a raw material composition having the following composition. A product was obtained in the same manner as in Example 1, and this product was designated as the chabazite-type zeolite of this example. SiO2 / Al2O3 ratio = 27.0 TMADA / SiO2 ratio = 0.081 Na / SiO2 ratio = 0.140 K / SiO2 ratio = 0.029 K / Na ratio = 0.21 H2O / SiO2 ratio = 18 OH / SiO2 ratio = 0.250
[0120] The chabazite-type zeolite of this example is a single phase of chabazite-type zeolite, with a SiO2 / Al2O3 ratio of 24.1 and a SiOH / Si ratio of 1.0×10 -2 The average crystal size was 0.5 μm and the volume diameter ratio was 3.47. Thus, the chabazite-type zeolite of this comparative example had a small average particle size and strong physical aggregation between the particles.
[0121] Comparative Example 3 A 25% TMADAOH aqueous solution, pure water, a 48% sodium hydroxide aqueous solution, a 48% potassium hydroxide aqueous solution, and an amorphous aluminosilicate were mixed to obtain a raw material composition having the following composition. A product was obtained in the same manner as in Example 1, and this product was designated as the chabazite-type zeolite of this comparative example. SiO2 / Al2O3 ratio = 23.3 TMADA / SiO2 ratio = 0.081 Na / SiO2 ratio = 0.140 K / SiO2 ratio = 0.029 K / Na ratio = 0.21 H2O / SiO2 ratio = 18 OH / SiO2 ratio = 0.250
[0122] The chabazite-type zeolite of this comparative example is a single-phase chabazite-type zeolite, with a SiO2 / Al2O3 ratio of 21.0 and a SiOH / Si ratio of 1.0×10 -2 The average crystal size was 0.3 μm and the volume diameter ratio was 3.12. Thus, the chabazite-type zeolite of this comparative example had a very small average particle size.
[0123] Comparative Example 4 A 25% TMADAOH aqueous solution, pure water, a 48% sodium hydroxide aqueous solution, a 48% potassium hydroxide aqueous solution, and an amorphous aluminosilicate were mixed to obtain a raw material composition having the following composition. A product was obtained in the same manner as in Example 1, and this product was designated as the chabazite-type zeolite of this comparative example. SiO2 / Al2O3 ratio = 14.7 TMADA / SiO2 ratio = 0.081 Na / SiO2 ratio = 0.140 K / SiO2 ratio = 0.029 K / Na ratio = 0.21 H2O / SiO2 ratio = 18 OH / SiO2 ratio = 0.250
[0124] The chabazite-type zeolite of this comparative example is a single-phase chabazite-type zeolite, with a SiO2 / Al2O3 ratio of 13.7 and a SiOH / Si ratio of 0.6×10 -2 The average crystal size was 0.5 μm and the volume diameter ratio was 1.67. Thus, the chabazite-type zeolite of this comparative example had a low SiO2 / Al2O3 ratio.
[0125] Comparative Example 5 A 25% TMADAOH aqueous solution, pure water, a 48% potassium hydroxide aqueous solution, and amorphous aluminosilicate were mixed to obtain a raw material composition having the following composition. A product was obtained in the same manner as in Example 1, and this product was designated as the chabazite-type zeolite of this comparative example. SiO2 / Al2O3 ratio = 29.5 TMADA / SiO2 ratio = 0.081 Na / SiO2 ratio = 0 K / SiO2 ratio = 0.169 K / Na ratio = ∞ H2O / SiO2 ratio = 18 OH / SiO2 ratio = 0.250
[0126] The chabazite-type zeolite of this comparative example was a single phase of chabazite-type zeolite, with a SiO2 / Al2O3 ratio of 26.9, an average crystal size of 1.5 μm, and a volume diameter ratio of 1.96.
[0127] Comparative Example 6 SSZ-13 was synthesized according to the method of Examples 1 and 5 of US Patent No. 4,665,110. That is, 17.5 g of 1-adamantanamine (Sigma-Aldrich) was dissolved in 105 ml of dimethyl formamide (Kishida Chemical). After dissolution, 50.8 g of tributylamine (Kishida Chemical) was added, and while stirring under ice cooling, 49.7 g of methyl iodide (Wako Pure Chemical) was slowly added dropwise.
[0128] After the dropwise addition of methyl iodide, the mixture was stirred for 5 days to react, yielding a white precipitate, which was washed 5 times with 100 mL of diethyl ether (Kishida Chemical) and dried under reduced pressure to obtain a white powder.
[0129] As a result of elemental analysis and NMR measurement of the obtained white powder, the white powder was identified as N,N,N-trimethyladamantammonium iodide (hereinafter referred to as "Template A").
[0130] 13.6g of Ludox AS-30 and 5.3g of Template A were mixed with water to obtain solution 1. 1.1g of Al2(SO4)3·18H2O and 2.91g of solid potassium hydroxide were mixed with water to obtain solution 2.
[0131] Solution 2 was added to solution 1 and mixed to obtain a uniform milky white solution. The mixed solution was filled into an 80 mL stainless steel reaction vessel and sealed, and the reaction vessel was heated at 150°C for 6 days while rotating at 30 rpm to obtain a product. The obtained product was washed with water, methanol, and acetone in this order, and dried at 110°C to obtain a white powder.
[0132] The obtained white powder was confirmed to be a single phase of SSZ-13. However, as shown in FIG. 2, the crystal morphology was an irregular aggregated particle (aggregate) that had grown while multiple crystals were irregularly chemically agglomerated, and cubic or rhombohedral edges were confirmed in some of the aggregated particles. However, in the chabazite-type zeolite of this comparative example, no independent primary particles were confirmed, and the average crystal size could not be evaluated. The SiO2 / Al2O3 ratio was 28.3. In addition, the volume diameter ratio was 3.97, confirming that the particles were significantly aggregated.
[0133] The evaluation results of the chabazite-type zeolites of the above Examples and Comparative Examples are shown in the table below.
[0134] [Table 3]
[0135] From these examples, the manufacturing method of this example is characterized in that the SiO2 / Al2O3 ratio is 15 or more and the SiOH / Si ratio is 1.6×10 -2 It was confirmed that a chabazite-type zeolite having an average crystal size of 0.5 μm or more and less than 1.5 μm and a volume particle size ratio of 3.2 or less could be produced, and thus a chabazite-type zeolite having characteristics different from those of the comparative examples could be obtained. In addition, the raw material composition did not contain compounds containing fluorine and chlorine, and the contents of chlorine and fluorine in the obtained chabazite-type zeolite were below the detection limit.
[0136] Comparative Example 1 and Example 5 both contain TMAD. +This is a synthetic chabazite-type zeolite obtained from a raw material composition containing only Al2O3 as an organic structure directing agent. Compared to the chabazite-type zeolite of Comparative Example 1, the chabazite-type zeolite of Example 5 has a high SiO2 / Al2O3 ratio but a low SiOH / Si ratio. This confirms that the chabazite-type zeolite of this example has a lower SiOH / Si ratio than conventional chabazite-type zeolite.
[0137] Although the chabazite-type zeolites of Example 3 and Comparative Example 2 have the same average crystal grain size, the volume particle size ratio of Comparative Example 2 exceeded 3.2. This confirmed that the chabazite-type zeolite of this example is less prone to physical aggregation than conventional chabazite-type zeolites.
[0138] The average crystal size of Examples 2 and 5 was equal and larger than that of Example 3. However, the volume particle size ratio of Example 3 was an intermediate value between Examples 2 and 5, and the 50% volume diameter of Examples 2 and 5 was different. From this, it was confirmed that there is no direct correlation between the average crystal size, the volume particle size ratio, and the 50% volume diameter. In addition, in the chabazite-type zeolite according to the embodiment of the present invention, it was confirmed that there is no direct relationship between the particle size of the primary particles and the ease of forming aggregated particles.
[0139] Measurement example 1 (heat resistance evaluation) The chabazite-type zeolites of Example 2 and Comparative Example 2 were each treated at 600°C for 2 hours under air flow, and then ion-exchanged with a 20% aqueous ammonium chloride solution. After the ion-exchange, the zeolites were dried overnight at 110°C in air to obtain chabazite-type zeolites with an NH4 cation type.
[0140] The main XRD peaks of the chabazite-type zeolite of Example 2 after treatment are shown in the table below.
[0141] [Table 4]
[0142] (Hydrothermal durability treatment) NH4-type chabazite-type zeolite was molded and pulverized to obtain aggregated particles with an aggregate diameter of 12 to 20 mesh. 3 mL of the aggregated particles of chabazite-type zeolite was packed into an atmospheric pressure fixed-bed flow-type reactor, and then air containing 10% by volume of moisture was passed through the reactor, and hydrothermal durability treatment was performed under the following conditions. Air flow rate: 300mL / min Processing temperature: 900℃ Processing time: 2 hours
[0143] (Measurement of crystallinity) The chabazite-type zeolite after the hydrothermal durability treatment was subjected to XRD measurement to determine the crystallinity. The crystallinity of the chabazite-type zeolite of Example 2 after the hydrothermal durability treatment was set to 100%, and the crystallinity measurement results are shown in the table below.
[0144] [Table 5]
[0145] From the above table, it can be seen that the chabazite-type zeolite of Example 2 has a higher crystallinity after hydrothermal durability treatment than the conventional chabazite-type zeolite. This confirms that the chabazite-type zeolite of the present invention has high heat resistance.
[0146] Example 6 The chabazite-type zeolite of Example 1 was calcined at 600°C for 2 hours under air flow, and then treated with a 20% ammonium chloride aqueous solution. The treated chabazite-type zeolite was dried overnight at 110°C in air to obtain chabazite-type zeolite with an ammonium cation type (NH4 type). A copper nitrate solution was added dropwise to 10 g of NH4 type chabazite-type zeolite and mixed in a mortar to impregnate and support copper in the chabazite-type zeolite. The copper nitrate aqueous solution was prepared by dissolving 1.1 g of copper nitrate trihydrate in 5.0 g of pure water.
[0147] After impregnation, the mixture was dried overnight at 110°C in air and then calcined for 2 hours at 550°C in air to obtain the copper-containing chabazite-type zeolite of this example. The copper-containing chabazite-type zeolite of this example had a copper content of 2.8% by weight and a Cu / Al2O3 ratio of 0.78.
[0148] Example 7 The copper-containing chabazite-type zeolite of this example was obtained in the same manner as in Example 6, except that the chabazite-type zeolite of Example 2 was used, and that a solution of 1.0 g of copper nitrate trihydrate dissolved in 5.0 g of pure water was used as the copper nitrate aqueous solution. The copper-containing chabazite-type zeolite of this example had a copper content of 2.6% by weight and a Cu / Al2O3 ratio of 0.78.
[0149] Example 8 The copper-containing chabazite-type zeolite of this example was obtained in the same manner as in Example 6, except that the chabazite-type zeolite of Example 5 was used, and that a copper nitrate aqueous solution obtained by dissolving 0.9 g of copper nitrate trihydrate in 5.0 g of pure water was used. The copper-containing chabazite-type zeolite of this example had a copper content of 2.5 wt % and a Cu / Al2O3 ratio of 0.81.
[0150] Comparative Example 7 The copper-containing chabazite-type zeolite of this comparative example was obtained in the same manner as in Example 6, except that the chabazite-type zeolite of Comparative Example 1 was used, and that a solution of 1.0 g of copper nitrate trihydrate dissolved in 5.0 g of pure water was used as the copper nitrate aqueous solution. The copper-containing chabazite-type zeolite of this comparative example had a copper content of 2.5% by weight and a Cu / Al2O3 ratio of 0.78.
[0151] Comparative Example 8 The copper-containing chabazite-type zeolite of this comparative example was obtained in the same manner as in Example 6, except that the chabazite-type zeolite of Comparative Example 2 was used, and that a solution of 1.2 g of copper nitrate trihydrate dissolved in 5.0 g of pure water was used as the copper nitrate aqueous solution. The copper-containing chabazite-type zeolite of this comparative example had a copper content of 3.1% by weight and a Cu / Al2O3 ratio of 0.77.
[0152] Comparative Example 9 The copper-containing chabazite-type zeolite of this comparative example was obtained in the same manner as in Example 6, except that the chabazite-type zeolite of Comparative Example 3 was used, and that a solution of 1.3 g of copper nitrate trihydrate dissolved in 4.3 g of pure water was used as the copper nitrate aqueous solution. The copper-containing chabazite-type zeolite of this comparative example had a copper content of 3.3 wt% and a Cu / Al2O3 ratio of 0.73.
[0153] Comparative Example 10 The copper-containing chabazite-type zeolite of this comparative example was obtained in the same manner as in Example 6, except that the chabazite-type zeolite of Comparative Example 4 was used, and that a solution of 1.2 g of copper nitrate trihydrate dissolved in 5.0 g of pure water was used as the copper nitrate aqueous solution. The copper-containing chabazite-type zeolite of this comparative example had a copper content of 2.7% by weight and a Cu / Al2O3 ratio of 0.47.
[0154] The evaluation results of the copper-containing chabazite-type zeolites of Examples 6 to 8 and Comparative Examples 7 to 10 are shown in the table below.
[0155] [Table 6]
[0156] Measurement example 2 (measurement of nitrogen oxide reduction rate) The copper-containing chabazite-type zeolites of Example 6, Comparative Example 7, and Comparative Example 10 were subjected to hydrothermal durability treatment in the same manner as in Measurement Example 1 to obtain samples (hereinafter also referred to as "durability-treated samples (2)"). The nitrogen oxide reduction rates of the obtained durability-treated samples (2) at 150°C were measured. The results are shown in the table below.
[0157] [Table 7]
[0158] Compared to Example 6, the copper-containing chabazite-type zeolite of Comparative Example 7 has the same Cu / Al2 ratio, but a higher SiO2 / Al2O3 ratio and a larger average crystal grain size. Despite this, the nitrogen oxide reduction rate of Comparative Example 7 was lower than that of Example 6. This confirmed that even when compared to conventional chabazite-type zeolites in which heat resistance was improved by increasing the crystal grain size, the copper-containing chabazite-type zeolite of this example has better heat resistance without increasing the crystal grain size, and has a higher nitrogen oxide reduction rate after exposure to high temperature and high humidity.
[0159] Furthermore, the copper-containing chabazite-type zeolites of Examples 6 to 8 and Comparative Examples 7 to 9 were subjected to hydrothermal durability treatment in the same manner as in Measurement Example 1, except that the treatment time was 3 hours, to obtain samples (hereinafter also referred to as "durability-treated samples (3)"). The nitrogen oxide reduction rates of the obtained durability-treated samples (3) at 150°C were measured. The results are shown in the table below.
[0160] [Table 8] A comparison between Examples 6 and 7 confirms that the nitrogen oxide reduction rate in the low temperature range after hydrothermal durability treatment increases as the crystal grain size and SiO2 / Al2O3 ratio increase. In contrast, in Comparative Example 7, the crystal grain size and SiO2 / Al2O3 ratio were larger than those of Example 7, but the nitrogen oxide reduction rate was about half that of Example 7. This confirms that the copper-containing chabazite-type zeolite of this example has a significantly higher nitrogen oxide reduction rate in the low temperature range than the conventional copper-containing chabazite-type zeolite. [Industrial Applicability]
[0161] The chabazite-type zeolite of the present invention can be used as an adsorbent or catalyst, particularly as an adsorbent or catalyst used under high temperatures. It can be used as a catalyst incorporated in an exhaust gas treatment system. In particular, the chabazite-type zeolite of the present invention can be used as an SCR catalyst, further an SCR catalyst integrated with a DPF, which reduces and removes nitrogen oxides in the exhaust gas of an automobile, particularly a diesel automobile, in the presence of a reducing agent.
Claims
1. The molar ratio of silica to alumina is 15 or more and less than 50, and the amount of silanol is 1.5×10 20 silanol groups / g or less, and the molar ratio of silanol groups to silicon is 0.7×10 -2 That's 1.6 x 10 -2 and a ratio of a 50% volume diameter to a 10% volume diameter is 2.8 or less.
2. 2. The nitrogen oxide reducing catalyst according to claim 1, wherein the 50% volume diameter of the chabazite-type zeolite is 5.0 μm or less.
3. 3. The nitrogen oxide reduction catalyst according to claim 1, wherein the average crystal size of the chabazite-type zeolite is 1.5 μm or less.
4. 3. The nitrogen oxide reducing catalyst according to claim 1, wherein the chabazite-type zeolite has at least the XRD peaks shown in the table below in an XRD pattern. [Table 1]
5. 3. The nitrogen oxide reducing catalyst according to claim 1, wherein the molar ratio of silica to alumina in the chabazite-type zeolite is 32.5 or less.
6. 3. The nitrogen oxide reducing catalyst according to claim 1, wherein the chabazite-type zeolite contains at least one of copper and iron.
Citation Information
Patent Citations
Chabazite-type zeolite and method for producing the same
JP2010168269A
High-silica chabazite for selective catalytic reduction, method for producing the same, and method for using the same.
JP2013514257A
Lev type zeolite and method of producing the same
JP2015155364A
Preparation of high-silica cha-type molecular sieves using mixed templates
JP2016529195A
Small crystallite zeolite CHA
US20030069449A1