Solid Electrolytic Capacitors
The use of a porous layer filled with insulating inorganic particles in solid electrolytic capacitors addresses issues of heat-induced expansion and moisture absorption, enhancing durability and longevity by minimizing internal pressure and conductive polymer volume.
Patent Information
- Application Number
- JP2023546879
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-09-07
- Filing Date
- 2022-08-25
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2042-08-25
AI Technical Summary
Solid electrolytic capacitors are prone to destruction and deterioration due to heat expansion of air bubbles and moisture absorption, leading to internal pressure increases and potential delamination.
A solid electrolytic capacitor structure is designed with a porous layer filled with insulating inorganic particles, reducing residual air bubbles and minimizing the volume of conductive polymer, thereby preventing pressure breakdown and thermal deterioration.
The structure effectively suppresses destruction and deterioration caused by external heat, extending the lifespan of the capacitor by reducing internal stress and maintaining electrical integrity.
Smart Images

Figure 0007563617000005 
Figure 0007563617000006 
Figure 0007563617000007
Abstract
Description
[Technical field]
[0001] The present invention relates to a solid electrolytic capacitor. [Background technology]
[0002] Conventionally, solid electrolytic capacitors have a structure in which an anode is formed from aluminum via a metal, a conductive polymer is attached to the oxide film on the aluminum surface, and a cathode is formed by drawing an electrode from this conductive polymer.
[0003] Conductive polymers and carbon are used as a method for drawing out the cathode, and the conductive polymers and carbon are electrically connected to a good conductive electrode such as copper. The reason for using conductive polymers and carbon as electrode leads is due to the difference in work function of the materials and the defect rate of the oxide formed on the aluminum surface, and is to prevent unnecessary conduction and electrical barriers from occurring in the connection to the good conductive electrode.
[0004] A solid electrolytic capacitor has a large surface area obtained by making the aluminum surface porous, oxidizing the porous aluminum surface to form a dielectric layer made of oxide, and disposing a conductive polymer on the surface of the dielectric layer, which results in a solid electrolytic capacitor with a large capacitance. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2008-130722 A Summary of the Invention [Problem to be solved by the invention]
[0006] In solid electrolytic capacitors, there are spaces (voids) on the surface of porous aluminum. It is difficult to fill these spaces, and air bubbles tend to remain in the spaces. For this reason, when a solid electrolytic capacitor is sealed, the air bubbles remaining in the spaces expand due to heat applied from the outside, which can lead to pressure destruction. For these reasons, solid electrolytic capacitors are vulnerable to heat. In addition, the conductive polymers used tend to absorb water easily, and are prone to expansion and contraction due to the humidity of the outside air. Furthermore, this absorbed moisture evaporates into water vapor due to heat applied from the outside, which can increase the internal pressure of the solid electrolytic capacitor and lead to the destruction of the solid electrolytic capacitor.
[0007] In addition, conductive polymers are highly hygroscopic, and expand and contract due to moisture absorption and release. This expansion and contraction generates internal stress, which can cause cracks and delamination, especially near the surface of porous aluminum.
[0008] The present invention has been made in consideration of the above circumstances, and has an object to provide a solid electrolytic capacitor having a structure that suppresses damage and deterioration of the solid electrolytic capacitor due to external heat and makes it less likely that the life of the solid electrolytic capacitor will be shortened. [Means for solving the problem]
[0009] The solid electrolytic capacitor of the present invention comprises a valve metal base, a porous layer provided on at least one main surface of the valve metal base, a dielectric layer provided on the surface of the porous layer, and a solid electrolyte layer provided on the surface of the dielectric layer, the porous layer having pores which are filled with insulating inorganic particles. Effect of the Invention
[0010] According to the present invention, it is possible to provide a solid electrolytic capacitor having a structure that prevents damage and deterioration of the solid electrolytic capacitor due to external heat and makes it difficult for the life of the solid electrolytic capacitor to decrease. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a cross-sectional view that illustrates a schematic internal structure of a solid electrolytic capacitor. [Figure 2A] FIG. 2A is a process diagram showing a process for producing a solid electrolytic capacitor. [Figure 2B] FIG. 2B is a process diagram showing a process for producing a solid electrolytic capacitor. [Figure 2C] FIG. 2C is a process diagram showing a process for producing a solid electrolytic capacitor. [Figure 2D] FIG. 2D is a process diagram showing a process for producing a solid electrolytic capacitor. [Figure 2E] FIG. 2E is a process diagram showing a process for producing a solid electrolytic capacitor. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The solid electrolytic capacitor of the present invention will now be described. However, the present invention is not limited to the following configurations, and can be appropriately modified and applied within the scope of the present invention. Note that the present invention also includes a combination of two or more of the individual preferable configurations of the present invention described below.
[0013] FIG. 1 is a cross-sectional view that illustrates a schematic internal structure of a solid electrolytic capacitor. In a solid electrolytic capacitor 10 shown in FIG. 1, a porous layer 2 is provided on at least one main surface of a valve metal substrate 1 . A dielectric layer 3 is provided on the surface of the porous layer 2, and a solid electrolyte layer 4 is provided on the surface of the dielectric layer 3. The porous layer 2 has pores 5 , and the pores 5 are filled with insulating inorganic particles 6 . Moreover, a solid electrolyte layer 7 (inorganic particle coating layer 7) is further provided on the surface of the insulating inorganic particle 6, so that the insulating inorganic particle becomes a solid electrolyte-coated inorganic particle 8.
[0014] The valve metal substrate is made of a valve metal that exhibits a so-called valve action. Examples of the valve metal include simple metals such as aluminum, tantalum, niobium, titanium, and zirconium, and alloys containing these metals. Among these, aluminum or an aluminum alloy is preferred. The valve metal substrate is preferably in the form of a flat plate, more preferably in the form of a foil.
[0015] The porous layer may be an etched layer formed by etching a valve metal substrate. The porous layer has pores, the average pore size of which is preferably 10 nm or more and 600 nm or less, and more preferably 200 nm or more and 300 nm or less. The pore diameter of the pores is determined by taking a cross-sectional photograph of the solid electrolytic capacitor and measuring the diameter of the pores on the surface of the porous layer. The average pore diameter of the pores is calculated by averaging the pore diameters of the pores in the cross-sectional photograph. The hole diameter of the hole is the dimension at the position defined by the double-headed arrow W in the cross section shown in FIG. In order to obtain a large electrostatic capacitance, it is preferable that the average pore size is within the above range. If the average pore size is too small, it is not preferable because it becomes difficult for the conductive polymer and insulating inorganic particles to enter the pores.
[0016] The dielectric layer is provided on the surface of the porous layer and is preferably made of an oxide film of the valve metal. For example, when an aluminum foil is used as the valve metal substrate, an aluminum oxide film can be formed by oxidizing the aluminum foil in an aqueous solution containing boric acid, phosphoric acid, adipic acid, or their sodium salts, ammonium salts, or the like.
[0017] A solid electrolyte layer is provided on the surface of the dielectric layer. Examples of materials constituting the solid electrolyte layer include conductive polymers having a skeleton of pyrroles, thiophenes, anilines, etc. Examples of conductive polymers having a skeleton of thiophenes include PEDOT [poly(3,4-ethylenedioxythiophene)], which may be PEDOT / PSS composited with polystyrene sulfonic acid (PSS) as a dopant. The solid electrolyte layer provided on the surface of the dielectric layer is provided in a film-like form, and pores still remain in the porous layer after the film-like solid electrolyte layer is provided.
[0018] The pores remaining in the porous layer after the solid electrolyte layer is provided are filled with insulating inorganic particles. The term "insulating inorganic particles" refers to a concept that does not include metal or carbon particles, which are inorganic particles having electrical conductivity, and particles of metal oxides (metals include silicon) can be preferably used. As the insulating inorganic particles, at least one type of fine particles selected from the group consisting of silica and alumina can be suitably used. In this specification, the insulating inorganic particles may be simply referred to as inorganic particles.
[0019] By filling the pores remaining in the porous layer after the solid electrolyte layer is provided with insulating inorganic particles, it is possible to reduce the amount of residual air bubbles in the pores and prevent pressure breakdown due to the expansion of the air bubbles. In addition, the volume ratio of the conductive polymer that forms the solid electrolyte layer in the pores can be reduced, which makes it possible to prevent thermal deterioration and destruction that would otherwise occur if a large amount of conductive polymer were present in the pores.
[0020] It is also preferable that the solid electrolyte layer is further provided on the surface of the insulating inorganic particles. 1 shows a solid electrolyte-coated inorganic particle 8 in which a solid electrolyte layer 7 is provided on the surface of an insulating inorganic particle 6. In this specification, the solid electrolyte layer provided on the surface of the insulating inorganic particle is also referred to as an inorganic particle-coated layer to distinguish it from a solid electrolyte layer provided on the surface of a dielectric layer. To describe the embodiment shown in FIG. 1 in more detail, it can be said that solid electrolyte-coated inorganic particles 8 are filled in pores 5 so as to be in contact with solid electrolyte layer 4 provided on the surface of dielectric layer 3.
[0021] Since the inorganic particles such as silica that fill the pores are insulating inorganic particles, filling the pores with inorganic particles increases the resistance of the conductive part from the anode to the cathode. If the resistance of this part is high, a series resistance component is introduced into the capacitor, and the loss as a capacitor increases. For this reason, it is necessary to reduce the resistance of the material that fills the pores.
[0022] The conductive polymer used to form the solid electrolyte layer is a resin with high conductivity, and in order to achieve high conductivity, it is preferable that the conductive polymer particles are appropriately dispersed. If the conductive polymer particles aggregate or clump, the conductivity will be hindered. Therefore, primary particles of the conductive polymer are attached to the surface of the insulating inorganic particles, and the insulating inorganic particles are coated with the conductive polymer. Then, the solid electrolyte-coated inorganic particles, in which the insulating inorganic particles are coated with the conductive polymer, are filled into the pores of the porous layer. In this way, the resistance of the material filled in the voids is reduced, thereby reducing loss as a capacitor, and the volume ratio of the conductive polymer filled in the voids is reduced, thereby preventing thermal degradation and destruction that would result from the presence of a large amount of conductive polymer in the voids. In addition, the conductive polymer PEDOT / PSS is a material that undergoes moisture absorption and expansion, and the expansion pressure can be reduced by reducing the amount of conductive polymer.
[0023] As the conductive polymer used to form the inorganic particle coating layer, the conductive polymers listed as materials constituting the solid electrolyte layer provided on the surface of the dielectric layer can be used.
[0024] The average particle size of the insulating inorganic particles is preferably 10 nm or more and 100 nm or less, and more preferably 30 nm or more and 60 nm or less. If the average particle size of the insulating inorganic particles is too small, the insulating inorganic particles will adhere to the surface of the conductive polymer, resulting in the conductive polymer being covered with the insulating inorganic particles. As a result, it may not be possible to obtain solid electrolyte-coated inorganic particles in which the insulating inorganic particles are coated with the conductive polymer. Also, if the average particle size of the insulating inorganic particles is too large, the insulating inorganic particles may not be able to fill the inside of the pores of the porous layer. The average particle size of the insulating inorganic particles is determined by taking a cross-sectional photograph of the solid electrolytic capacitor and averaging the particle sizes of a plurality of insulating inorganic particles in the cross-sectional photograph. Furthermore, when solid electrolyte-coated inorganic particles are used, the preferred range of average particle size of the insulating inorganic particles is determined as the average particle size of the insulating inorganic particle portion without taking into consideration the thickness of the inorganic particle coating layer.
[0025] FIG. 1 shows that a solid electrolyte-coated inorganic particle layer 9, which is a layer of solid electrolyte-coated inorganic particles 8, is present on the porous layer 2 (parts of the surface of the porous layer that are not pores). Then, a conductive layer 13 is provided on the solid electrolyte-coated inorganic particle layer 9. FIG. 1 shows an example in which a carbon layer 11 and a metal layer 12 are provided as examples of the conductive layer.
[0026] The conductive layer is preferably a carbon layer, a graphene layer, or a metal layer such as a copper layer or a silver layer formed by applying a conductive paste such as a carbon paste, a graphene paste, a copper paste, a silver paste, etc. Alternatively, the conductive layer may be a composite layer in which a metal layer is provided on a carbon layer or a graphene layer, or a mixed layer in which a carbon paste or a graphene paste is mixed with a metal paste.
[0027] In addition, when inorganic particles that are not covered with a solid electrolyte layer are used as insulating inorganic particles, the inorganic particles themselves are insulating, so providing a layer of insulating inorganic particles between the porous layer and the conductive layer increases the resistance value. Therefore, it is preferable to not provide a layer of insulating inorganic particles and to enable electrical connection between the solid electrolyte layer provided on the surface of the dielectric layer and the conductive layer.
[0028] Next, an example of a method for producing the solid electrolytic capacitor of the present invention will be described. First, a mixed dispersion ink and a conductive resin paste that can be used in the production of the solid electrolytic capacitor of the present invention, as well as methods for producing them, will be described.
[0029] The mixed dispersion ink is an ink obtained by mixing and dispersing a dispersion of a conductive polymer and a dispersion of insulating inorganic particles. The conductive polymer dispersion is preferably a dispersion of a conductive polymer dispersed in water, and the solid content of the conductive polymer is preferably 2% by weight or less. If the solid content of the conductive polymer is high, the intermolecular distance becomes short, which may cause aggregation of the conductive polymer.
[0030] The insulating inorganic particles contained in the dispersion of insulating inorganic particles are preferably treated to be hydrophilic, because PEDOT / PSS, which is preferably used as a conductive polymer, is hydrophilic, and therefore, if the insulating inorganic particles are hydrophilic, the conductive polymer will adhere favorably to the surfaces of the insulating inorganic particles. The hydrophilic treatment is a treatment for reducing surface tension, and examples of the treatment include surface treatment with a coupling agent, and treatment with OH groups introduced by activation in air, such as UV irradiation treatment, plasma treatment, and corona discharge treatment. The dispersion of insulating inorganic particles is preferably a dispersion dispersed in isopropyl alcohol. Because water and isopropyl alcohol have a high affinity, a dispersion of a conductive polymer dispersed in water and a dispersion of insulating inorganic particles dispersed in isopropyl alcohol are suitably mixed.
[0031] When obtaining a mixed dispersion ink, for example, a dispersion of insulating inorganic particles is dropped into a conductive polymer dispersion while stirring the conductive polymer dispersion, thereby diffusing the insulating inorganic particles into the conductive polymer. When stirring the conductive polymer dispersion, it is preferable to apply high vibration, and it is preferable to use a dispersing machine that applies ultrasonic vibration as a device for applying high vibration. Specifically, a device such as an ultrasonic homogenizer can be used.
[0032] The manner in which the insulating inorganic particles and the conductive polymer adhere to each other varies depending on the size of the insulating inorganic particles. When the insulating inorganic particles are too small, particularly when the average particle size of the insulating inorganic particles is less than 10 nm, the insulating inorganic particles adhere to the surface of the conductive polymer, resulting in a form in which the conductive polymer is coated with the insulating inorganic particles, and as a result, it may not be possible to obtain solid electrolyte-coated inorganic particles in which the insulating inorganic particles are coated with the conductive polymer. When the size of the insulating inorganic particles is relatively large, particularly when the average particle size of the insulating inorganic particles is 30 nm or more, the conductive polymer adheres to the periphery of the insulating inorganic particles, and solid electrolyte-coated inorganic particles in which the insulating inorganic particles are coated with the conductive polymer can be suitably obtained.
[0033] From the above viewpoints, the insulating inorganic particles are preferably hydrophilically treated particles having an average particle size of 30 nm to 100 nm, and more preferably hydrophilically treated silica particles having an average particle size of 30 nm to 100 nm. The dispersion of insulating inorganic particles is preferably a dispersion in which silica particles are dispersed in isopropyl alcohol.
[0034] It is preferable to mix the insulating inorganic particles in such an amount that the inorganic particle solid content is 10% by weight or more and 100% by weight or less relative to the conductive polymer dispersion. If the above ratio exceeds 100% by weight, the ratio of the insulating inorganic particles is too high, resulting in a decrease in conductivity and an increase in resistance. If the above ratio is less than 10% by weight, the ratio of the conductive polymer is too high, making it difficult to obtain the effect of using the insulating inorganic particles.
[0035] The viscosity of the mixed dispersion ink is preferably 2 mPa·s or more and 10 mPa·s or less. When the viscosity of the ink is in the above range, it is suitable for forming a solid electrolyte layer by inkjet printing.
[0036] Next, the conductive resin paste will be described. The conductive resin paste is a paste obtained by mixing and dispersing the above-mentioned mixed dispersion ink into a water or alcohol dispersion of a high-concentration conductive polymer. It is preferable that the paste be obtained by mixing the mixed dispersion ink in a ratio of 10% by weight or more and 50% by weight or less with a water or alcohol dispersion of a high-concentration conductive polymer.
[0037] The water or alcohol dispersion of the high-concentration conductive polymer contains the conductive polymer at a solid concentration of 20% by weight or more. This means that the solid concentration of the conductive polymer is higher than the solid concentration of the conductive polymer contained in the conductive polymer dispersion used to obtain the mixed dispersion ink.
[0038] Although the water or alcohol dispersion of the high-concentration conductive polymer becomes gel-like and difficult to handle, by mixing it with the mixed dispersion ink, the mixed dispersion ink acts as a dispersant and reduces the viscosity of the water or alcohol dispersion of the high-concentration conductive polymer. Therefore, the conductivity of the conductive resin paste is not impaired, but rather improved. This makes the paste suitable for forming a solid electrolyte layer by screen printing.
[0039] The viscosity of the conductive resin paste is preferably 50 mPa·s or more and 1000 mPa·s or less. When the viscosity of the conductive resin paste is in the above range, it is suitable for forming a solid electrolyte layer by screen printing.
[0040] The process of using a solid electrolytic capacitor by using the mixed dispersion ink or the conductive resin paste will be described below. 2A, 2B, 2C, 2D, and 2E are process diagrams showing steps for producing a solid electrolytic capacitor.
[0041] FIG. 2A shows a state in which a porous layer 2 is formed on the main surface of a valve metal substrate 1 and a dielectric layer 3 is formed on the surface of the porous layer 2. The porous layer can be formed by etching, and the dielectric layer can be formed by chemical conversion treatment.
[0042] Chemical conversion is a process in which an oxide film is formed on the surface of a porous layer of a valve metal substrate made of a metal such as aluminum, and this is used as a dielectric layer. Adipic acid is preferably used for the chemical conversion, and an oxide film can be formed by applying a voltage of, for example, 3V. The higher the applied voltage, the thicker the oxide film becomes, and the higher the breakdown voltage. However, a thicker oxide film reduces the capacitance. On the other hand, a lower voltage results in a thinner oxide film, and the capacitance increases. However, if the oxide film becomes too thin, the probability of defects in the oxide film increases, so it is desirable to apply a voltage of 3V or more.
[0043] 2B shows the state after the insulating layer 14 is formed. The insulating layer is formed in the position where the solid electrolyte layer is not to be formed. By providing the insulating layer, the anode and the cathode are insulated from each other. The insulating layer can be made of a resin, and examples of the resin that can be used to form the insulating layer include epoxy resin, phenol resin, polyimide resin, silicone resin, polyamide resin, and liquid crystal polymer.
[0044] FIG. 2C shows a state in which a solid electrolyte layer 4 is formed on the surface of the dielectric layer 3. The solid electrolyte layer 4 can be formed by a process of printing and drying a dispersion liquid of a conductive polymer. It is preferable to repeat the printing and drying of the dispersion liquid of the conductive polymer several times. The printing of the conductive polymer dispersion can be carried out by a method such as sponge transfer, screen printing, spray coating, dispenser, or inkjet printing.
[0045] 2D shows a state in which insulating inorganic particles (solid electrolyte-coated inorganic particles 8) are filled in the pores 5. The insulating inorganic particles can be filled in the pores by printing the mixed dispersion ink or conductive resin paste described above and drying it. This printing and drying is preferably repeated multiple times. When the mixed dispersion ink is used, it is preferable to print the mixed dispersion ink by inkjet printing. Alternatively, the mixed dispersion ink may be printed by dropping the ink with a dispenser. This is because the mixed dispersion ink has a relatively low viscosity. When a conductive resin paste is used, it is preferable to print the conductive resin paste by screen printing. Since the conductive resin paste has a relatively high viscosity and has thixotropy, the fluidity of the paste increases during printing, and the paste easily penetrates into the pores. Screen printing is more preferable.
[0046] FIG. 2E shows a state in which a conductive layer 13 consisting of a carbon layer 11 and a metal layer 12 is provided. The conductive layer can be provided by forming a conductive paste, such as a carbon paste or a metal paste mainly composed of silver, copper or nickel, on the solid electrolyte layer by sponge transfer, screen printing, spray coating, dispenser, inkjet printing or the like. By the above steps, the solid electrolytic capacitor of the present invention can be manufactured. EXAMPLES
[0047] Examples in which the solid electrolytic capacitor of the present invention was evaluated are shown below, but the present invention is not limited to these examples.
[0048] Example 1 An aqueous dispersion of a conductive polymer (PEDOT / PSS) and a silica sol dispersion (isopropanol dispersion) were prepared. Silica sols with average particle sizes of 20 nm, 45 nm, and 80 nm were prepared and manufactured by Nissan Chemical Co., Ltd. The solid content concentration of each silica sol was 30% by weight. Furthermore, the silica sol with an average particle size of 20 nm had a D10 of 10 nm and a D90 of 30 nm, the silica sol with an average particle size of 45 nm had a D10 of 30 nm and a D90 of 60 nm, and the silica sol with an average particle size of 80 nm had a D10 of 60 nm and a D90 of 100 nm.
[0049] The silica sol of each particle size was converted into a solid content and weighed out to give 10 parts by weight, 30 parts by weight, 50 parts by weight, 70 parts by weight, and 100 parts by weight per 100 parts by weight of the conductive polymer dispersion. While stirring and dispersing the conductive polymer dispersion with an ultrasonic homogenizer at approximately 300 W, the silica sol dispersion was added dropwise at a rate of 1 g / min to disperse it. The viscosity after dispersion was low, about 3 mPa·s. The mixed dispersion ink thus obtained was applied to a glass substrate by spin coating to a thickness of 0.2 μm, and the resistivity was measured by the four-terminal method. The measurement results are shown in Table 1.
[0050] [Table 1]
[0051] The coating films (samples No. 2a and 3a) coated with the mixed dispersion ink obtained by dropping a silica sol dispersion having a silica sol with an average particle size of 20 nm into a dispersion of a conductive polymer had a resistance of 20 MΩ / □ or more and were insulating. On the other hand, when silica sol dispersions having average particle sizes of 45 nm and 80 nm were used, the resistivity increased depending on the amount added, but the increase in resistivity was about 1 to 10 times that of a conductive polymer dispersion that did not use silica sol dispersion. From these results, it can be seen that when the particle size of the silica sol contained in the mixed dispersion ink is relatively large (45 nm and 80 nm), desirable electrical conductivity can be maintained. In addition, since this test involved applying a mixed dispersion ink and measuring the resistivity, it does not mean that conductivity cannot be ensured when using a mixed dispersion ink containing silica sol with an average particle size of 20 nm in the manufacture of solid electrolytic capacitors.
[0052] Furthermore, the mixed dispersion ink obtained by mixing the conductive polymer dispersion and the silica sol dispersion showed a viscosity of less than 3 mPa·s and was suitable for spin coating and inkjet printing methods. Furthermore, the mixed dispersion ink was left at room temperature for two weeks, a coating was formed, and then the ink was examined under an optical microscope at a magnification of 3000 times. As a result, no aggregation was observed in the mixed dispersion ink.
[0053] Example 2 A paste (water-based dispersion medium) of conductive polymer (PEDOT / PSS) with a high concentration (solid concentration 20% by weight) was prepared. 100 g of this paste was placed in a plastic container and shaken (60 Hz, amplitude 3 mm) to reduce the viscosity. Mixed dispersion ink No. 5a, 6a, or 8a prepared in Example 1 was dripped at a speed of 1 g / min in the ratios shown in Table 2. After dripping was completed, the paste was placed in a high dispersion mixer (Kakuhunter) and stirred for 30 minutes to obtain a conductive resin paste. Each conductive resin paste was printed to a thickness of about 30 μm by screen printing, and the resistivity was measured by a four-point probe method. The measurement results are shown in Table 2.
[0054] [Table 2]
[0055] The high-concentration conductive polymer paste gels violently and has strong thixotropy, so it was difficult to mix the mixed dispersion ink unless it was placed in a shaker. Furthermore, when only a shaker was used, the fluidity was insufficient and a gelled state remained, so the mixture was put into a high dispersion mixer (Kakuhunter) to obtain a conductive resin paste. In addition, when the ratio of the mixed dispersion ink was 30% by weight or less (samples No. 2b, 3b, 6b, 7b, 10b, and 11b), the viscosity increased over time and the life of the conductive resin paste was short. The conductive resin paste obtained under these conditions required high dispersion stirring treatment immediately before use.
[0056] Example 3 An aluminum substrate with a porous layer formed by surface processing was prepared, and then chemical conversion treatment was performed to form an oxide film on the surface of the porous layer. Epoxy resin was printed on this aluminum substrate in a pattern with an inner frame of 10 mm square and an outer frame of 15 mm square, and then cured. After this, a dispersion of a conductive polymer (PEDOT / PSS) was printed inside the epoxy resin frame using the inkjet method, and the process of drying at 160°C for 10 minutes was repeated five times, and the oxide film (dielectric layer) on the surface of the porous layer was coated with the dispersion of the conductive polymer to form a solid electrolyte layer.
[0057] Thereafter, the mixed dispersion inks No. 4a to 13a prepared in Example 1 were each printed by the inkjet method, and the process of drying at 180°C for 10 minutes was repeated multiple times until the thickness of the coating film was 5 μm or more and 20 μm or less from the surface of the porous layer.
[0058] In addition, a sample was prepared using the mixed dispersion ink No. 1a prepared in Example 1 as the mixed dispersion ink.
[0059] Thereafter, carbon paste was printed to a thickness of about 20 μm and dried at 180° C. for 30 minutes, after which copper electrode paste was printed and dried at 200° C. for 30 minutes to obtain a cathode. The electrical properties were evaluated between the back side of the porous layer of the aluminum substrate as the anode and the copper cathode. Using a commercially available LCR meter, the capacitance was measured at 1Vrms and 120Hz, and the ESR was measured at 1Vrms and 100KHz. A voltage of 2V was applied, and the current (leak current) was measured after 60 seconds. Furthermore, a pressure cooker test (high-temperature, high-humidity test) at 125°C and 85% RH was repeated for 100 hours three times to examine the changes in capacitance and ESR before and after the high-temperature, high-humidity test. The measurement results are shown in Table 3.
[0060] [Table 3]
[0061] As shown in Table 3, by printing the mixed dispersion ink and filling the pores of the porous layer with insulating inorganic particles, an increase in capacitance and a decrease in ESR were observed, and the leakage current was also improved. As an accelerated test, a high temperature and high humidity test was repeated three times. As a result, in the example in which the mixed dispersion ink was used, the fluctuation in both capacitance and ESR was suppressed. In the case where the mixed dispersion ink was not added, delamination was confirmed by observing the cross section by polishing.
[0062] Example 4 An aluminum substrate with a porous layer formed by surface processing was prepared, and then chemical conversion treatment was performed to form an oxide film on the surface of the porous layer. Epoxy resin was printed on this aluminum substrate in a pattern with an inner frame of 10 mm square and an outer frame of 15 mm square, and then cured. After this, a dispersion of a conductive polymer (PEDOT / PSS) was printed inside the epoxy resin frame using the inkjet method, and the process of drying at 160°C for 10 minutes was repeated five times, and the oxide film (dielectric layer) on the surface of the porous layer was coated with the dispersion of the conductive polymer to form a solid electrolyte layer.
[0063] Thereafter, the conductive resin pastes No. 2b to 13b prepared in Example 2 were printed by screen printing using a 10.5 mm square pattern to cover the solid electrolyte layer, and the process of drying at 180°C for 10 minutes was repeated twice.
[0064] In addition, a sample was prepared using the conductive resin paste No. 1b prepared in Example 2 as the conductive resin paste.
[0065] Thereafter, carbon paste was printed to a thickness of about 20 μm and dried at 180° C. for 30 minutes, after which copper electrode paste was printed and dried at 200° C. for 30 minutes to obtain a cathode.
[0066] The electrical characteristics were evaluated in the same manner as in Example 3. The measurement results are shown in Table 4.
[0067] [Table 4]
[0068] An increase in capacitance and a decrease in ESR were observed when the conductive resin paste was printed, similar to the case of printing the mixed dispersion ink in Example 3. Regarding the decrease in ESR, the ESR was higher than when the mixed dispersion ink was printed, but the conductive resin paste has the advantage that it can be screen-printed and the number of printing cycles can be reduced because it is in paste form. When a conductive resin paste without adding a mixed dispersion ink was used (sample No. 1b), a significant increase in ESR was observed in the high temperature and high humidity test, but no significant increase in ESR was observed in the other samples (samples No. 2b to 13b). When the cross section of sample No. 1b was polished and examined, delamination was confirmed. [Explanation of symbols]
[0069] 1 Valve metal substrate 2 Porous layer 3 Dielectric Layer 4. Solid electrolyte layer (solid electrolyte layer on the surface of the dielectric layer) 5 Hole 6. Insulating inorganic particles 7 Solid electrolyte layer (inorganic particle coating layer) 8 Solid electrolyte coated inorganic particles 9 Solid electrolyte coated inorganic particle layer 10 Solid electrolytic capacitor 11 Carbon layer 12 metal layer 13 Conductive layer 14 Insulating layer
Claims
1. a valve metal substrate; a porous layer provided on at least one of the main surfaces of the valve metal substrate; a dielectric layer provided on a surface of the porous layer; a solid electrolyte layer provided on a surface of the dielectric layer, the porous layer has pores, and the pores are filled with solid electrolyte-coated inorganic particles in which insulating inorganic particles are coated with a conductive polymer; The insulating inorganic particles have an average particle size of 10 nm or more and 100 nm or less.
2. 2. The solid electrolytic capacitor according to claim 1, wherein the insulating inorganic particles are at least one type selected from the group consisting of silica and alumina.
3. 3. The solid electrolytic capacitor according to claim 1, wherein the solid electrolyte layer is further provided on the surfaces of the insulating inorganic particles.
4. 3. The solid electrolytic capacitor according to claim 1, wherein the average pore size of the pores is 10 nm or more and 600 nm or less.
5. 3. The solid electrolytic capacitor according to claim 1, wherein the insulating inorganic particles have an average particle size of 30 nm or more and 60 nm or less.
6. 6. The solid electrolytic capacitor according to claim 5, wherein the average pore size of the pores is 200 nm or more and 300 nm or less.
7. 3. The solid electrolytic capacitor according to claim 1, wherein the insulating inorganic particles have an average particle size of 30 nm or more.
8. 3. The solid electrolytic capacitor according to claim 1, wherein the insulating inorganic particles have an average particle size of 45 nm or more.
Citation Information
Patent Citations
Solid electrolytic capacitor and its manufacturing method
JP2003163138A
Circuit board with built-in solid-state electrolytic capacitor, and its manufacturing method
JP2008130722A
High-conductive ionic liquid composition
JP2008177385A
Conductive polymer dispersion liquid for manufacturing solid electrolytic capacitor and solid electrolytic capacitor manufactured using the same
JP2013251359A
Sulfur complex with coating layer formed on surface of sulfur base
JP2015043300A