Release film for photosensitive resin, photosensitive resin laminated film, and photosensitive resin structure

The release film with an acid-modified polyolefin resin layer addresses mechanical weakness and blocking issues, ensuring effective mold releasability and precise pattern formation for photosensitive resins.

JP7563722B2Active Publication Date: 2024-10-08UNITIKA LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2020054476
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-09-30
Filing Date
2020-03-25
Publication Date
2024-10-08
Estimated Expiration
2040-03-25

AI Technical Summary

Technical Problem

Existing release films for photosensitive resins suffer from mechanical weakness leading to lifting during half-cutting or punching, and can cause blocking due to residual solvent in high temperature environments, failing to form fine resist patterns without defects.

Method used

A release film with a resin layer composed of acid-modified polyolefin resin, crosslinking agent, and hydrophilic polymer, ensuring a thickness of 30 μm or more and parallel light transmittance of 80% or more, which includes a propylene-rich olefin component and specific acid components for improved adhesion and mold releasability.

Benefits of technology

The film provides excellent mold releasability, prevents blocking in high humidity environments, and enables sharp, dense dot-like pattern formation with reduced lifting and defects during processing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007563722000001
    Figure 0007563722000001
  • Figure 0007563722000002
    Figure 0007563722000002
Patent Text Reader

Abstract

To provide a release film for a photosensitive resin which enables processing without causing floating in half cut and punching in a state of being laminated on a photosensitive resin layer, emits light in a state where a release film is laminated on the photosensitive resin layer, enables formation of a photosensitive resin layer having a dot-like dense pattern, and is excellent in releasability with the photosensitive resin layer.SOLUTION: There is provided a release film for a photosensitive resin in which a resin layer containing an acid-modified polyolefin resin and a crosslinking agent is laminated on at least one surface of a base material film.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a release film for a photosensitive resin. [Background technology]

[0002] A method for forming circuits such as printed wiring boards, semiconductor packages, and flexible substrates is known in which a photosensitive resin composition is exposed to light in a pattern on a substrate, the exposed areas are polymerized and cured, and the unexposed areas are removed to form a resist pattern on the substrate. In recent years, the miniaturization of electronic devices and the integration of circuits have led to a miniaturization of multilayer electronic components mounted on electronic devices. This has led to a demand for finer resist patterns, and methods for forming photosensitive resin layers with high resolution have been developed. One such method involves laminating a release film onto a photosensitive resin, masking the base surface of the release film that does not face the photosensitive resin with a photomask, and then exposing the film to light to form a pattern (for example, Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2018-161829 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, when the release film described in Patent Document 1 is subjected to half-cutting or punching processing while being laminated on a photosensitive resin layer, the release film may float due to insufficient mechanical strength, which may result in defective products. In addition, in applications in which a photosensitive resin composition is provided on a substrate film to form a photosensitive resin layer, an organic solvent may be used as a solvent for the photosensitive resin composition. However, when the photosensitive resin substrate film described in Patent Document 1 is used, the film may be exposed to residual solvent in the photosensitive resin layer due to long-term storage in a high-temperature environment after being wound into a roll, and blocking may occur. There is also a demand for forming patterns without omissions even in the case of minute dot-shaped exposure patterns.

[0005] In other words, in consideration of these problems, the present invention aims to provide a release film for photosensitive resin that has excellent releasability from a photosensitive resin layer, and further, does not float when half-cut or punched while laminated to a photosensitive resin layer, and does not cause blocking even when wound up into a roll and stored for a long period of time in a high-temperature environment. Another object of the present invention is to provide a release film which, when laminated on a photosensitive resin layer, can be irradiated with light to form a sharp, dense dot-like pattern of photosensitive resin. [Means for solving the problem]

[0006] Means for Solving the Problems The present inventors conducted extensive research to find that a release film having a resin layer of a specific composition can solve the problems described above, and thus arrived at the present invention.

[0007] That is, the gist of the present invention is the following (1) to (13). (1) A release film for photosensitive resins, comprising a base film and a resin layer containing an acid-modified polyolefin resin and a crosslinking agent laminated on at least one surface of the base film. (2) The release film for photosensitive resins according to (1), which has a thickness of 30 μm or more and a parallel light transmittance of 80% or more. (3) A release film for photosensitive resins according to (1) or (2), in which the olefin component of the acid-modified polyolefin resin contains propylene. (4) The release film for photosensitive resins according to (3), wherein the propylene content in the olefin component of the acid-modified polyolefin resin is 90% by mass or more. (5) The release film for photosensitive resins according to any one of (1) to (4), wherein the resin layer further contains a hydrophilic polymer. (6) A release film for a photosensitive resin according to (5), wherein the hydrophilic polymer is polyvinyl alcohol and / or polyvinylpyrrolidone. (7) The release film for photosensitive resins according to any one of (1) to (6), wherein the content of the crosslinking agent is 5 to 35 parts by mass per 100 parts by mass of the acid-modified polyolefin resin. (8) The release film for photosensitive resins according to any one of (1) to (6), wherein the content of the crosslinking agent is 15 to 25 parts by mass per 100 parts by mass of the acid-modified polyolefin resin. (9) The release film for a photosensitive resin according to any one of (1) to (8), wherein the base film is a polyester film. (10) The release film for a photosensitive resin according to any one of (1) to (9), wherein the base film is a multilayer film having two or more layers. (11) A photosensitive resin laminate film in which a protective layer, a photosensitive resin layer, and a release film for photosensitive resin according to any one of (1) to (10) are laminated in this order, such that the resin layer of the release film for photosensitive resin is adjacent to the photosensitive resin layer. (12) A photosensitive resin structure comprising a substrate, a photosensitive resin layer, and a release film for photosensitive resin according to any one of (1) to (10) laminated in this order such that the resin layer of the release film for photosensitive resin is adjacent to the photosensitive resin layer. (13) The photosensitive resin structure according to (12), wherein at least a part of the photosensitive resin layer is cured. Effect of the Invention

[0008] The release film for photosensitive resin of the present invention is excellent in releasability from a photosensitive resin layer and can suppress blocking even when stored for a long period of time under a high humidity environment. In addition, by irradiating light onto the photosensitive resin layer, a dense dot-like pattern of photosensitive resin can be sharply formed on the substrate, and floating can be suppressed even when punching processes such as half cutting are performed with the photosensitive resin layer laminated. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The release film for photosensitive resin of the present invention (hereinafter sometimes abbreviated as "release film") has a resin layer on at least one side of the base film, and the resin layer must contain an acid-modified polyolefin resin and a crosslinking agent.

[0010] In the present invention, the acid-modified polyolefin resin constituting the resin layer is a resin containing an olefin component as a main component and modified with an acid component. Examples of the olefin component include alkenes having 2 to 6 carbon atoms, such as ethylene, propylene, isobutylene, 2-butene, 1-butene, 1-pentene, and 1-hexene, and mixtures thereof may also be used. In the present invention, the olefin component preferably contains a propylene component from the viewpoint of improving releasability from the photosensitive resin. From the viewpoint of reducing parallel light transmittance, it is preferable that the olefin component does not contain butene. It is also preferable that the olefin component contains a propylene component. The propylene component content is preferably 90% by mass or more, more preferably 95% by mass or more, and even more preferably 98% by mass or more.

[0011] The acid component constituting the acid-modified polyolefin resin includes unsaturated carboxylic acid components, specifically acrylic acid, methacrylic acid, maleic acid, maleic anhydride, itaconic acid, itaconic anhydride, fumaric acid, crotonic acid, etc., as well as half esters and half amides of unsaturated dicarboxylic acids. Among them, in order to stably disperse the resin in the aqueous dispersion of the resin described later, acrylic acid, methacrylic acid, maleic acid, and maleic anhydride are preferred, and acrylic acid, methacrylic acid, and maleic anhydride are particularly preferred. Two or more of these acid components may be contained in the acid-modified polyolefin resin.

[0012] The proportion of the acid component in the acid-modified polyolefin resin is not particularly limited, but is preferably 1 to 10% by mass. If the acid component is less than 1% by mass, the resin layer tends not to have sufficient adhesion to the base film, and may contaminate the adherend released from the resin layer, whereas if the acid component ratio exceeds 10% by mass, the releasability from the adherend tends to decrease.

[0013] The acid-modified polyolefin resin may contain an ethylenically unsaturated component containing an oxygen atom in the side chain. Examples of ethylenically unsaturated components containing oxygen atoms in the side chain include esters of (meth)acrylic acid and alcohols having 1 to 30 carbon atoms, and among these, from the viewpoint of availability, esters of (meth)acrylic acid and alcohols having 1 to 20 carbon atoms are preferred. Specific examples of such compounds include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, hexyl (meth)acrylate, octyl (meth)acrylate, decyl (meth)acrylate, lauryl (meth)acrylate, dodecyl (meth)acrylate, and stearyl (meth)acrylate. A mixture of these may be used. Among these, from the viewpoint of adhesion to polyester film, methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, hexyl acrylate, and octyl acrylate are more preferred, ethyl acrylate and butyl acrylate are even more preferred, and ethyl acrylate is particularly preferred. "(meth)acrylic acid" means "acrylic acid or methacrylic acid". The proportion of ethylenically unsaturated components containing oxygen atoms in the side chains in the acid-modified polyolefin resin is not particularly limited, but is preferably 1 to 40% by mass.

[0014] In the present invention, the resin layer must contain a crosslinking agent in addition to the acid-modified polyolefin resin, which can inhibit migration of the resin layer to the adherend.

[0015] The content of the crosslinking agent is preferably 5 to 35 parts by mass, more preferably 10 to 35 parts by mass, even more preferably 15 to 25 parts by mass, and most preferably 21 to 25 parts by mass, relative to 100 parts by mass of the acid-modified polyolefin resin, from the viewpoint of releasability from the photosensitive resin. If the content of the crosslinking agent is less than 5 parts by mass, the resin layer tends to have poor releasability from the photosensitive resin, poor adhesion to the substrate film due to weakened cohesive force, and tends to be easily transferred to the adherend. On the other hand, if the content exceeds 35 parts by mass, the liquid material for forming the resin layer may thicken and the stability may decrease, and the obtained resin layer may have poor releasability from the photosensitive resin.

[0016] As the crosslinking agent, a compound having a plurality of functional groups in the molecule that react with a carboxyl group can be used, and examples thereof include polyfunctional epoxy compounds; polyfunctional isocyanate compounds; polyfunctional aziridine compounds; carbodiimide group-containing compounds; oxazoline group-containing compounds; phenolic resins; and amino resins such as urea compounds, melamine resins, and benzoguanamine resins. One of these may be used, or two or more may be used in combination. Among these, polyfunctional isocyanate compounds, melamine compounds, urea compounds, polyfunctional epoxy compounds, carbodiimide group-containing compounds, and oxazoline group-containing compounds are preferred, carbodiimide group-containing compounds and oxazoline group-containing compounds are more preferred, and oxazoline group-containing compounds are even more preferred. By using an oxazoline group-containing compound, it is possible to obtain a release film that is excellent in releasability from the adherend and blocking resistance. These crosslinking agents may also be used in combination.

[0017] In the present invention, the resin layer preferably contains a hydrophilic polymer. The content of the hydrophilic polymer is preferably 1 to 1000 parts by mass, more preferably 1 to 600 parts by mass, further preferably 10 to 600 parts by mass, and most preferably 100 to 600 parts by mass, relative to 100 parts by mass of the acid-modified polyolefin resin.

[0018] Examples of hydrophilic polymers include sodium polyacrylate, carboxyvinyl polymer, polyacrylic acid amide, acrylamide / acrylate copolymer, polyvinyl alcohol, polyvinylpyrrolidone, copolymers thereof, etc. Among these, polyvinyl alcohol or polyvinylpyrrolidone, which are vinyl-based hydrophilic polymers, are preferred. The resin layer of the release film of the present invention contains polyvinyl alcohol, which improves the releasability from the photosensitive resin. In addition, the resin layer contains polyvinylpyrrolidone, which improves the coatability and the adhesion between the base film and the resin layer, and tends to suppress the transfer of the resin layer to the adherend (photosensitive resin layer). In the resin layer, polyvinylpyrrolidone is dispersed in the acid-modified polyolefin resin, so that the obtained aqueous dispersion has excellent coatability and can form a coating film in which the occurrence of streak-like defects described below is suppressed, and the formed coating film has excellent adhesion to the base film. In addition, the aqueous dispersion can form a resin layer that shows excellent releasability even when the amount of heat applied to the coating film in the coating film formation process changes.

[0019] When polyvinyl alcohol is used as the hydrophilic polymer, its content is preferably 10 to 1000 parts by mass, more preferably 10 to 600 parts by mass, and most preferably 100 to 600 parts by mass, relative to 100 parts by mass of the acid-modified polyolefin resin. If the content of polyvinyl alcohol exceeds 1000 parts by mass, the resin layer is likely to transfer to the adherend (photosensitive resin layer).

[0020] The saponification rate of polyvinyl alcohol is preferably 80% or more, and more preferably 90% or more. If the saponification rate of polyvinyl alcohol is less than 80%, the stability of the coating agent tends to deteriorate.

[0021] In the present invention, commercially available polyvinyl alcohols can be used, such as "JP-15", "JT-05", "JF-05", "JL-05E", "JM-17" and "VC-10" of "J-Poval" manufactured by Japan Vinyl Acetate & Poval Corporation, and "PVA-CST", "PVA-624", "PVA-203", "PVA-220" and "PVA-405" of "Kuraray Poval" manufactured by Kuraray Co., Ltd.

[0022] When polyvinylpyrrolidone is used as the hydrophilic polymer, the content is preferably 1 to 1000 parts by mass, more preferably 1 to 600 parts by mass, further preferably 2 to 500 parts by mass, particularly preferably 2 to 300 parts by mass, and most preferably 2 to 200 parts by mass, relative to 100 parts by mass of the acid-modified polyolefin resin. If the content of polyvinylpyrrolidone exceeds 1000 parts by mass, the releasability from the photosensitive resin and the parallel light transmittance tend to deteriorate.

[0023] The weight average molecular weight of polyvinylpyrrolidone is not particularly limited, but is preferably 10,000 to 1,100,000, more preferably 30,000 to 1,000,000, and even more preferably 100,000 to 800,000. If the weight average molecular weight of polyvinylpyrrolidone is less than 10,000, the resin layer tends to have poor releasability. On the other hand, if the weight average molecular weight of polyvinylpyrrolidone is more than 1,100,000, the aqueous dispersion has a high viscosity, which reduces the handling property in the work process, reduces the coatability, and tends to cause streak-like defects to be described later on the surface of the formed resin layer.

[0024] In the present invention, commercially available polyvinylpyrrolidone can be used, such as "K-30L", "K-60L", "K-90L", and "V-7154" of "Pitzcol" manufactured by Daiichi Kogyo Seiyaku Co., Ltd., and "K-30", "K-85", and "K-90" of "Polyvinylpyrrolidone" manufactured by Nippon Shokubai Co., Ltd.

[0025] When polyvinyl alcohol and polyvinylpyrrolidone are used in combination as the hydrophilic polymer, the content thereof is preferably 10 to 1,000 parts by mass, more preferably 10 to 600 parts by mass, and most preferably 100 to 600 parts by mass, per 100 parts by mass of the acid-modified polyolefin resin.

[0026] The thickness of the resin layer in the release film of the present invention is preferably 0.01 to 2 μm, more preferably 0.01 to 1 μm, and even more preferably 0.01 to 0.5 μm. If the thickness of the resin layer is less than 0.01 μm, sufficient releasability from the adherend cannot be obtained, and if it exceeds 1 μm, it is likely to transfer to the adherend and costs will increase, which is not preferable.

[0027] The base film constituting the release film of the present invention is preferably a polyester film that is not affected by the curing shrinkage before and after the UV irradiation process of the photosensitive resin and has excellent dimensional stability and mechanical strength. Specific examples of polyester include polyethylene terephthalate, polybutylene terephthalate, polyethylene isophthalate, polyethylene-2,6-naphthalenedicarboxylate, etc., and also include copolymers thereof or blends thereof with small proportions of other resins.

[0028] If necessary, the base film may contain, for example, an antioxidant, a heat stabilizer, an antistatic agent, a pinning agent, etc. Examples of the antioxidant include hindered phenol compounds and hindered amine compounds, and examples of the heat stabilizer include phosphorus compounds.

[0029] The release film of the present invention preferably has a thickness of 30 μm or more from the viewpoint of suitability for punching processing such as half cutting. Among them, from the viewpoint of balance with parallel light transmittance, 30 to 100 μm is more preferable, 30 to 65 μm is even more preferable, and more than 30 μm to 65 μm or less is particularly preferable. If it is less than 30 μm, sufficient mechanical strength is insufficient for punching processing such as half cutting, and dimensional stability may not be obtained, such as affecting the curing shrinkage of the photosensitive resin.

[0030] The substrate film may be a single layer or a multilayer, but is preferably a multilayer film having two or more layers. The multilayer film can be produced, for example, by melting the resins constituting each layer separately, extruding them using a multilayer die, laminating and fusing them before solidification, and then biaxially stretching and heat fixing them, or by melting and extruding two or more resins separately to form films, and laminating and fusing them in an unstretched state or after stretching them. From the viewpoint of process simplicity, it is preferable to use a multilayer die and laminate and fusing them before solidification.

[0031] An example of a method for producing a polyester film will be described. First, a sufficiently dried polyester is fed into an extruder, melted at a temperature at which it is sufficiently plasticized and exhibits fluidity, passed through a filter selected as necessary, and then extruded into a sheet through a T-die. This sheet is brought into close contact with a cooling drum whose temperature is adjusted to below the glass transition temperature (Tg) of the polyester, to obtain an unstretched film. The unstretched film thus obtained is uniaxially oriented by a uniaxial stretching method, or biaxially oriented by a biaxial stretching method. The biaxial stretching method is not particularly limited, but may be a sequential biaxial stretching method or a simultaneous biaxial stretching method.

[0032] The release film of the present invention can be easily produced industrially by a method in which a liquid containing an acid-modified polyolefin resin and a crosslinking agent in a liquid medium is applied to a base film, and the base film to which the liquid has been applied is dried, stretched, and heat-treated to form a resin layer.

[0033] The surface shape of the release film of the present invention is not particularly limited, and may be smooth or, for example, matte.

[0034] In the present invention, the liquid medium constituting the resin layer-forming liquid material is preferably an aqueous medium. The aqueous medium means a solvent containing water and an amphipathic organic solvent and having a water content of 2% by mass or more, or may be water alone. An amphipathic organic solvent refers to an organic solvent in which the solubility of water in the organic solvent at 20°C is 5 mass% or more (the solubility of water in organic solvents at 20°C is described in literature such as "Solvent Handbook" (Kodansha Scientific, 10th edition, 1990)). Specific examples of amphipathic organic solvents include alcohols such as methanol, ethanol, n-propanol, and isopropanol; ethers such as tetrahydrofuran and 1,4-dioxane; ketones such as acetone and methyl ethyl ketone; esters such as methyl acetate, n-propyl acetate, isopropyl acetate, methyl propionate, ethyl propionate, and dimethyl carbonate; ethylene glycol derivatives such as ethylene glycol n-butyl ether; organic amine compounds containing ammonia such as diethylamine, triethylamine, diethanolamine, triethanolamine, N,N-dimethylethanolamine, and N,N-diethylethanolamine; and lactams such as 2-pyrrolidone and N-methyl-2-pyrrolidone.

[0035] In the present invention, the resin layer on the substrate film can be formed by coating, transfer, lamination, etc. Considering the ease of forming the resin layer, it is preferable to form the resin layer by coating. Known methods such as gravure roll coating, reverse roll coating, wire bar coating, lip coating, air knife coating, curtain flow coating, spray coating, dip coating, brush coating, etc. can be used.

[0036] The method for forming the resin layer by coating may be either an in-line coating method carried out within the film production process, or an off-line coating method in which coating is carried out outside the system on a film that has already been produced.

[0037] In the production of the release film of the present invention, it is preferable to adopt an in-line coating method. That is, it is preferable to include a step of applying a liquid material for forming a resin layer during the production process of a base film, and a step of drying, orientation stretching, and heat fixing treatment together with the base film. By applying during the production process, the resin layer can be formed in a state where the degree of orientation crystallization of the surface of the base film is small, so that the adhesion between the base film and the resin layer is improved. In addition, since the resin layer can be heat-treated at a higher temperature while the base film is in a tensed state, it is possible to improve the releasability and residual adhesive strength without deteriorating the quality of the base film. Furthermore, compared with offline coating, not only can the production process be simplified, but it is also advantageous in terms of cost due to the thinning of the resin layer. In addition, when the sequential biaxial stretching method is adopted, it is preferable from the viewpoint of simplicity and operation to apply the liquid material to a base film stretched in a uniaxial direction, dry the base film coated with the liquid material, and then further stretch the base film in a direction perpendicular to the direction and heat treat it.

[0038] The release film of the present invention can be used as a protective film for a photosensitive resin layer by applying a photosensitive resin onto the resin layer formed on one side of the base film by the above-mentioned method, drying it, and laminating it. Also, a photosensitive resin formed in a sheet shape can be laminated onto the resin layer of the release film.

[0039] As the photosensitive resin, a known one can be used. As the photosensitive resin for the dry film resist, a negative photosensitive resin is used, which is mainly composed of a composition containing a monomer having a polymerizable unsaturated group, a polymer, a photopolymerization initiator, etc. Photosensitive resins are generally alkaline water-soluble, and in the dry film resist processing step, the exposed portion forms a circuit (image) by development, and the unexposed portion is dissolved and removed by the developer.

[0040] The photosensitive resin is not particularly limited, but examples thereof include polymers made of acrylic or methacrylic polymerizable monomers. The photosensitive resin may be either a homopolymer or a copolymer. Examples of the polymerizable monomer include carboxyl group-containing monomers such as acrylic acid, methacrylic acid, crotonic acid, maleic acid, fumaric acid, and itaconic acid, or their anhydrides and half esters, (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, cyclohexyl (meth)acrylate, benzyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, and glycidyl (meth)acrylate, acrylamide, methacrylamide, acrylonitrile, methacrylonitrile, styrene, α-methylstyrene, vinyl acetate, and alkyl vinyl ether.

[0041] Additives such as thermal polymerization inhibitors, plasticizers, dyes, discolorants, adhesion promoters, antioxidants, solvents, surface tension modifiers, stabilizers, chain transfer agents, antifoaming agents, and flame retardants may be appropriately added to the photosensitive resin layer, as necessary.

[0042] The photosensitive resin layer can be formed by applying a coating liquid prepared by dissolving or dispersing the above-mentioned polymer, crosslinkable monomer, photopolymerization initiator, etc. in a solvent by a wet coating method, and then drying and, if necessary, curing the coating liquid.

[0043] Examples of the wet coating method include reverse coating, spray coating, bar coating, gravure coating, rod coating, die coating, spin coating, extrusion coating, and curtain coating.

[0044] When a photosensitive resin layer is laminated on the resin layer of a release film, an organic solvent may be mixed so that the photosensitive resin has a predetermined concentration. Examples of organic solvents include acetone, methyl ethyl ketone, methanol, ethanol, isopropyl alcohol, toluene, propylene glycol monoethyl ether, propylene glycol monomethyl ether acetate, ethyl acetate, and butyl acetate. These may be used alone or in combination of two or more. A coating liquid containing a photosensitive resin is uniformly applied to the resin layer of a release film by a roll coater method, a bar coater method, or the like, and then dried to form a photosensitive resin layer.

[0045] The thickness of the photosensitive resin layer can be appropriately selected depending on the purpose, and is, for example, in the range of 0.1 to 100 μm. The number of photosensitive resin layers is not particularly limited and can be appropriately selected depending on the purpose, and may be, for example, one layer or two or more layers.

[0046] The photosensitive resin laminate film of the present invention will now be described. The photosensitive resin laminate film is formed by laminating a protective layer, a photosensitive resin layer, and a release film in this order, where the photosensitive resin layer is adjacent to the resin layer of the release film.

[0047] The protective layer is formed for the purpose of protecting the photosensitive resin layer from dust and scratches. From the viewpoint of winding the photosensitive resin laminate film in a roll, the protective layer is preferably a thermoplastic resin film. Examples of the thermoplastic resin film include polyolefin films such as polyethylene films and polypropylene films, nylon films, and polyester films, and from the viewpoints of economy, versatility, and bending resistance, polyolefin films are more preferable, and polypropylene films are even more preferable.

[0048] The photosensitive resin construct in the present invention will be described below. The photosensitive resin structure is a laminate of a substrate, a photosensitive resin layer, and a release film in this order, where the photosensitive resin layer is adjacent to the resin layer of the release film.

[0049] The substrate is not particularly limited, and known substrates such as a glass substrate and a copper foil substrate can be used.

[0050] An example of a method for producing a circuit board using a photosensitive resin laminate film will be described. The roll-shaped photosensitive resin laminate film is unwound, and then the protective layer of the photosensitive resin laminate film is peeled off, and the copper foil substrate is pressed and bonded to the photosensitive resin layer. Then, a photomask with an exposure pattern formed on the base film surface of the release film is vacuum-adhered, and ultraviolet light is applied from the photomask side to harden the exposed portion of the photosensitive resin. Then, the release film is peeled off from the photosensitive resin layer, and the uncured (unexposed portion) photosensitive resin is dissolved and removed with a developer. When dried, a circuit board can be obtained in which a pattern of the cured photosensitive resin is formed on the copper foil substrate.

[0051] Examples of ultraviolet light sources for exposing and curing at least a portion of the photosensitive resin layer include high-pressure mercury lamps, ultraviolet fluorescent lamps, carbon arc lamps, xenon lamps, sunlight, etc. In the case of ultraviolet irradiation, the amount of irradiation light is 50 mJ to 1500 mJ / cm. 2 degree is preferred.

[0052] Examples of the developer that dissolves and removes the uncured (unexposed) photosensitive resin include an alkaline aqueous solution and a water-soluble organic solvent, and a mixture of these may also be used. Examples of the alkaline substance that can be used to compose the alkaline aqueous solution include sodium borate, sodium hydroxide, sodium carbonate, sodium phosphate, and sodium silicate. The water-soluble organic solvent may have a water solubility sufficient to form a homogeneous system when contained in an amount of 0.1 to 50 parts by mass relative to 100 parts by mass of water, and may be, for example, ethers, alcohols, etc. Examples of ethers include octylphenoxy polyoxy ether, and examples of alcohols include methanol, ethanol, etc. The developer may contain additives such as surfactants, antifoaming agents, dispersants, emulsifiers, corrosion inhibitors, putrefactive agents, and pH adjusters. EXAMPLES

[0053] The present invention will be specifically described below with reference to examples, but is not limited to these. The various properties described below were measured or evaluated by the following methods.

[0054] (1) Thickness Based on JIS K 7130 (1999), the thickness of the release film is measured at 10 random points using a thickness meter MT-12B manufactured by HEIDENHAIN Corporation, and the average value is regarded as the thickness of the release film.

[0055] (2) Measurement of the haze value of release film Based on JIS K 7136 (2000), the haze value of the release film was measured using a turbidity meter "NDH-4000" manufactured by Nippon Denshoku Industries Co., Ltd. During the measurement, the release film was positioned so that light was incident on the surface of the resin layer.

[0056] (3) Measurement of parallel light transmittance of release film As in (2) above, the parallel light transmittance of the release film was measured using a turbidity meter "NDH-4000" manufactured by Nippon Denshoku Industries Co., Ltd. During the measurement, the release film was positioned so that light was incident on the surface of the resin layer.

[0057] (4) Releasability from photosensitive resin layer A photosensitive resin composition having the following composition was applied to the resin layer of the release film produced in the Examples and Comparative Examples, and dried at 110°C for 3 minutes to form a 40 μm photosensitive resin layer. A copper foil substrate was laminated onto the obtained photosensitive resin layer, and pressed to produce a photosensitive resin structure laminated in the order of copper foil substrate / photosensitive resin layer / release film. Next, using a photosensitive resin relief plate making machine Takano Processor A3-PRINTER model manufactured by Takano Machinery Manufacturing Co., Ltd., an ultraviolet low-pressure mercury lamp of 40 W was used to irradiate about 500 mJ / cm from the release film side of the photosensitive resin structure. 2 The exposure was performed at . The photosensitive resin construct with the photosensitive resin layer cured by exposure was cut into a width of 10 mm and a length of 150 mm (MD direction) to prepare a sample for measuring peel strength. The peel strength between the photosensitive resin layer and the release film of the sample for measuring peel strength was measured in a thermostatic chamber at 23°C using a tensile tester (Shimadzu Corporation Autograph AGS-100B) at a peel angle of 180° and a peel speed of 300 mm / min. The evaluation was performed with n=3, and the average value was calculated. The evaluation of the releasability is preferably 1.0 N / cm or less, more preferably 0.7 N / cm or less, and most preferably 0.4 N / cm or less. (Photosensitive resin composition) As the monomer having a polymerizable unsaturated group, 30 parts by mass of ethylene oxide modified bisphenol A dimethacrylate, in which the number of ethylene oxide repeats is 17 (total number of repeating units), 10 parts by mass of propylene glycol diglycidyl ether diacrylate, and 10 parts by mass of trimethylolpropane triacrylate were used. As the polymer, 25 parts by mass of a polymer having a weight average molecular weight of 170,000 polymerized in a ratio of methyl methacrylate / n-butyl methacrylate / styrene / methacrylic acid = 45 / 15 / 15 / 25 (mass ratio), styrene / acrylic acid = 75 / 25 (mass ratio), and The mixture consisted of 25 parts by mass of a polymer having a weight-average molecular weight of 20,000 polymerized in a ratio of 1:1, 2 parts by mass of 2,2-dimethoxy-1,2-diphenylethan-1-one and 0.4 parts by mass of (2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1 as photopolymerization initiators, and 75 parts by mass of methyl ethyl ketone and 25 parts by mass of isopropyl alcohol as solvents. The weight-average molecular weight of the polymer was measured using a GPC (gel permeation chromatography) device and a THF (tetrahydrofuran) solution of the dried polymer against polystyrene standards.

[0058] (5) Dot printing suitability (resolution accuracy) A photosensitive resin structure was prepared in the same manner as in (4) above. Next, a photomask film with a dot pattern was attached to the base surface side of the release film of the photosensitive resin structure in a vacuum using a photosensitive resin letterpress plate-making machine, Takano Processor A3-PRINTER model, manufactured by Takano Machinery Manufacturing Co., Ltd., and an irradiation dose of about 500 mJ / cm was applied using a 40 W low-pressure ultraviolet mercury lamp. 2 (The ultraviolet illuminometer used was model UV-M03A manufactured by Oak Manufacturing Co., Ltd.) ) The photomask film cut into a dot pattern is a film on which 100 circles of 2 mm in diameter (at a pitch of 3 mm) are depicted, and which is capable of blocking ultraviolet rays in areas other than the circles. Thereafter, the release film was peeled off from the photosensitive resin layer, and the uncured photosensitive resin (unexposed portion) was washed off with a developer (a mixture of 2 parts by mass of sodium borate, 2 parts by mass of octylphenoxy polyoxyether, and 100 parts by mass of water), and then dried. After drying, a dot-shaped photosensitive resin pattern (100 circles with a diameter of 2 mm) was formed on the copper foil substrate. A solvent ink (Process X Cyan manufactured by Toyo Ink Mfg. Co., Ltd.) was applied to the obtained photosensitive resin, and a dot pattern with a diameter of 2 mm was printed on the OPP film. The circular shape of the printed dot pattern was observed with a magnifying glass, and the number of defects (circle chipping or rubbing, circles larger than or smaller than 2 mm in diameter) was counted, and the dot printing suitability was evaluated according to the following evaluation criteria. In practical terms, it is preferable that the number of defects is 2 or less, and it is most preferable that the number of defects is 0.

[0059] (6) Punching suitability (half-cutting ability) The photosensitive resin composition described in (4) was applied onto the resin layer of the release film, and dried at 110°C for 3 minutes. An OPP film was laminated as a protective layer on the semi-cured photosensitive resin layer to produce a photosensitive resin laminate film. An incision was made from the OPP film side to the interface between the semi-cured photosensitive resin layer and the release film. By making an incision from the photosensitive resin layer side to the interface with the release film, the release film bends slightly, a small gap is generated at the interface, and a circular part where the release film is not in contact with the photosensitive resin layer is generated. This circular part where the release film is not in contact is called a "float" and is preferably as small as possible. The diameter of the float that was generated was measured from the release film side to evaluate the punchability as follows. ○: The width of the float is less than 2 mm △: Floating width is 2mm or more and less than 4mm ×: Floating width is 4mm or more

[0060] (7) Adhesion between the base film and the resin layer The adhesiveness of the resin layer side surface of the obtained release film was confirmed by the cross-cut method in accordance with JIS K-5600-5-6. In detail, an adhesive tape (TF-12 manufactured by Nichiban Co., Ltd.) was applied to the resin layer surface on which a lattice pattern of 100 sections was formed by cutting, and the tape was vigorously peeled off. "100 / 100" indicates the best state in which none of the 100 sections peeled off, and "0 / 100" indicates the worst state in which all of the 100 sections peeled off. In practical terms, it is preferable that 90 or more sections are not peeled off (90 / 100), more preferably 95 or more sections are not peeled off (95 / 100), and most preferably 100 sections are not peeled off at all (100 / 100).

[0061] (8) Blocking resistance The obtained release film was cut into a size of 100 mm x 100 mm, and the coated surface (resin layer) and the non-coated surface (biaxially stretched PET film) of the obtained release film were overlapped so that they were in contact with each other, and left for 24 hours at 70 ° C. with a load of 10 kPa applied. The load was removed and cooled to room temperature. Next, the film was cut into strips with a width of 10 mm, and the load (N) required to peel the two sheets was measured in a thermostatic chamber at 23 ° C. using a tensile tester (Shimadzu Corporation Autograph AGS-100B) under conditions of a peel angle of 180 degrees and a peel speed of 300 mm / min, and used as an index of blocking resistance. The number of evaluations n was n = 3, and the average value was calculated. The smaller the measured peel force value, the better the blocking resistance. Specifically, it is preferably less than 0.30 N / cm, and more preferably less than 0.10 N / cm.

[0062] (9) Coatability (suppression of streak-like defects in coating) The liquid for forming the resin layer was applied (offline coating) with a Mayer bar to the corona-treated surface of a biaxially oriented polyester film (Unitika Ltd., Emblet S-50, thickness 50 μm), and then dried at 120°C for 20 seconds to obtain a release film on which a resin layer of approximately 0.1 μm in thickness was formed. The resin layer side surface of the obtained release film was exposed to white light (100 lumens) from a fluorescent lamp at an angle of 5 to 45°, and the presence or absence of streaky interference was visually confirmed. Straight lines were drawn with a black oil-based pen in the width direction (TD) of the film at the following 10 points, and streaky defects intersecting the straight lines were observed across the entire width of the film, and the coatability was evaluated based on the occurrence of streaky defects. In evaluating coatability, practically speaking, the number of streak-like defects that occur is required to be 5 or less, preferably 3 or less, and most preferably no streak-like defects at any point. The points to be evaluated were 10 points in total: a point 1 m from one edge in the longitudinal direction of the release film, a point 1 m from the other edge, and a point dividing the area between these two points into 9 equal parts.

[0063] In order to prepare a liquid material for forming a resin layer, an acid-modified polyolefin resin and an aqueous dispersion thereof were produced by the following method.

[0064] <Production of Acid-Modified Polyolefin Resin A-1> 280 g of propylene-butene-ethylene terpolymer (propylene / butene / ethylene=68.0 / 16.0 / 16.0 (mass ratio)) was heated and melted in a four-neck flask under a nitrogen atmosphere, and then 32.0 g of maleic anhydride as an unsaturated carboxylic acid and 6.0 g of dicumyl peroxide as a radical generator were added over 1 hour while stirring while maintaining the temperature in the system at 170°C, and then reacted for 1 hour. After the reaction was completed, the reaction product obtained was poured into a large amount of acetone to precipitate a resin. This resin was further washed several times with acetone to remove unreacted maleic anhydride, and then dried under reduced pressure in a vacuum dryer to obtain an acid-modified polyolefin resin A-1. The proportion of acid components in A-1 was 4.5% by mass.

[0065] <Production of Acid-Modified Polyolefin Resins A-2 and A-3> In the above-mentioned acid-modified polyolefin resin A-1, except that propylene-butene-ethylene terpolymer (propylene / butene / ethylene=68.0 / 16.0 / 16.0 (mass ratio)) was replaced with propylene-ethylene copolymer (propylene / ethylene=99 / 1 (mass ratio)), acid-modified polyolefin resin A-2 was obtained in the same manner. The proportion of acid component in A-2 was 4.2 mass%. In addition, acid-modified polyolefin resin A-3 was obtained in the same manner, except that the copolymer was changed to an ethylene-ethyl acrylate copolymer (ethylene / ethyl acrylate=93 / 7 (mass ratio)). The proportion of acid components in A-3 was 2.0 mass%.

[0066] <Production of Acid-Modified Polyolefin Resin Aqueous Dispersion E-1> Using a stirrer equipped with a sealable pressure-resistant 1-liter glass container with a heater, 60.0 g of the acid-modified polyolefin resin A-1 produced by the above method, 45.0 g of ethylene glycol-n-butyl ether (boiling point 171 ° C), 6.9 g of N,N-dimethylethanolamine (boiling point 134 ° C, 1.0 times equivalent to the carboxyl group of the maleic anhydride unit in the resin), and 188.1 g of distilled water were charged into the above glass container, and the stirring blade rotation speed was set to 300 rpm and stirred. No resin precipitation was observed at the bottom of the container, and it was confirmed that the resin was in a floating state. While maintaining this state, the heater was turned on after 10 minutes to heat, and the temperature in the system was kept at 140 ° C and stirred for another 60 minutes. After that, the mixture was cooled to room temperature (about 25 ° C) by air cooling while stirring at a rotation speed of 300 rpm. Further, pressure filtration (air pressure 0.2 MPa) was performed using a 300 mesh stainless steel filter (wire diameter 0.035 mm, plain weave) to obtain a uniform acid-modified polyolefin resin aqueous dispersion E-1 (solid content concentration 25 mass%). Note that there was almost no residual resin on the filter.

[0067] <Production of Acid-Modified Polyolefin Resin Aqueous Dispersions E-2 and E-3> Except for changing the acid-modified polyolefin resin A-1 to A-2 and A-3, acid-modified polyolefin resin aqueous dispersions E-2 and E-3 (solid content concentration 25% by mass) were obtained in the same manner as the production of the acid-modified polyolefin resin aqueous dispersion E-1 described above.

[0068] The following types of crosslinking agents were used: WS-700: Epocross WS-700 manufactured by Nippon Shokubai Co., Ltd., an aqueous solution of an oxazoline group-containing compound, solid content concentration 25% by mass EM-051R: Adeka Resin EM-051R manufactured by Adeka Corporation, an aqueous solution of an epoxy group-containing compound, solid content concentration 25% by mass SV-02: Carbodilite SV-02 manufactured by Nisshinbo Corporation, an aqueous solution of a compound containing a carbodiimide group, solid content concentration 25% by mass U-ban: U-ban 28-60 manufactured by Mitsui Chemicals, melamine compound, solids concentration 100% by mass

[0069] The polyvinyl alcohol used was JF-05 (JF-05 manufactured by Japan Vinyl Acetate & Poval Co., Ltd., saponification rate 94.5%, degree of polymerization 500, solid content concentration 8% by mass). The polyvinylpyrrolidone used was K-60L (Pitscol K-60L manufactured by Daiichi Kogyo Seiyaku Co., Ltd., weight average molecular weight 450,000, solid content concentration 20% by mass).

[0070] Example 1 <Preparation of Liquid for Forming Resin Layer> Acid-modified polyolefin resin aqueous dispersion E-1, WS-700, and JF-05 were mixed to obtain the solid content shown in Table 1, and the final solid concentration was adjusted to 6.0 mass% with water to obtain a liquid for forming a resin layer. <Production of release film> Polyethylene terephthalate B, which was prepared by adding 0.07% by mass of silica particles (particle diameter 2.3 μm) to polyethylene terephthalate A (polymerization catalyst: antimony trioxide, intrinsic viscosity: 0.62, glass transition temperature: 78°C, melting point: 255°C), was fed into extruder I (screw diameter: 50 mm), and polyethylene terephthalate A was fed into extruder II (screw diameter: 65 mm) and melted at 280°C, after which the melts were joined together in layers before reaching the outlet of the T-die. The layer thickness ratio (I / II) was adjusted to 4 / 6 and the total thickness was adjusted to 600 μm, and the mixture was extruded from the outlet of the T-die, rapidly cooled, and solidified to obtain an unstretched film. This unstretched film was stretched 3.5 times at 85° C. using a roll-type longitudinal stretching machine to obtain a longitudinally stretched film. Next, the resin layer-forming liquid material obtained in Example 1 was applied to the surface of the film layer of the longitudinally stretched film from the extruder II using a 120-mesh gravure roll at a rate of 5 g / m 2 After coating so as to give the desired result, the ends of the longitudinally stretched film were continuously held by the clips of a flat-type stretching machine and stretched horizontally to 4.5 times their original size at 100°C. Thereafter, the film was heat-treated at 243°C for 3 seconds with a relaxation rate of 3% in the horizontal direction to obtain a 50μm-thick release film having a 0.1μm-thick resin layer on one side of a base film made of two types of two-layer polyester film.

[0071] Examples 2 to 13 and 18 22、31~ 38, Reference Examples 23~30 Comparative Example 1 A liquid material for forming a resin layer was prepared so as to have the composition shown in Table 1. Moreover, a release film was obtained in the same manner as in Example 1, except that this liquid material was used.

[0072] [Table 1]

[0073] Examples 14 to 17 A release film was obtained in the same manner as in Example 2, except that the thickness of the release film was as shown in Table 2.

[0074] Comparative Example 2 A release film was obtained in the same manner as in Example 1, except that a liquid prepared by dissolving 10 parts by mass of a long-chain alkyl compound (Ashio Resin RA-80, manufactured by Ashio Sangyo Co., Ltd.) and 2 parts by mass of the melamine compound U-Van as a crosslinking agent in toluene was used as the liquid for forming the release layer.

[0075] Comparative Example 3 A release film was obtained in the same manner as in Comparative Example 2, except that the thickness of the release film was set as shown in Table 2.

[0076] Comparative Example 4 100 parts by mass of the acid-modified polyolefin resin of the acid-modified polyolefin resin aqueous dispersion E-2 were mixed with 20 parts by mass of a crosslinking agent (WS-700) as solid content and 25 parts by mass of colloidal silica (PL-3, secondary particle diameter 70 nm; manufactured by Fuso Chemical Co., Ltd.), and the mixture was stirred to prepare a liquid for forming a resin layer. A release film was obtained in the same manner as in Example 1.

[0077] The results of various evaluations of the release films obtained in the examples and comparative examples are shown in Table 2.

[0078] [Table 2]

[0079] In particular, the release films of Examples 9 to 13 had high parallel light transmittance and excellent dot printing suitability because the olefin component of the acid-modified polyolefin resin constituting the resin layer did not contain butene and had a high propylene ratio. Reference example The release film No. 23 contained the crosslinking agent and the hydrophilic polymer in the preferred amounts, and therefore had particularly excellent releasability from the photosensitive resin layer.

[0080] The release film of Comparative Example 1 had poor releasability from the photosensitive resin because the liquid material for forming the resin layer did not contain the crosslinking agent defined in the present invention. In addition, not only did the adhesion between the resin layer and the substrate tend to be poor, but the blocking resistance was also poor. The release films of Comparative Examples 2 and 3 did not contain the acid-modified polyolefin resin defined in the present invention in the liquid material for forming the resin layer, and therefore had poor releasability from the photosensitive resin and poor blocking resistance. In addition, the release film of Comparative Example 3 was thin and poor in punchability. The release film of Comparative Example 4 did not satisfy the parallel light transmittance specified in the present invention, and was therefore inferior in dot printing suitability.

Claims

1. A release film comprising a base film and a resin layer containing an acid-modified polyolefin resin and a crosslinking agent laminated on at least one surface of the base film, The olefin component of the acid-modified polyolefin resin contains 68% by mass or more of propylene, A release film for photosensitive resin used for separating the resin layer from the photosensitive resin that has been cured by exposure to light.

2. 2. The release film for photosensitive resins according to claim 1, which has a thickness of 30 μm or more and a parallel light transmittance of 80% or more.

3. 2. The release film for photosensitive resins according to claim 1, wherein the propylene content in the olefin component of the acid-modified polyolefin resin is 90% by mass or more.

4. 4. The release film for photosensitive resins according to claim 1, wherein the resin layer further contains a hydrophilic polymer.

5. 5. The release film for photosensitive resins according to claim 4, wherein the hydrophilic polymer is polyvinyl alcohol and / or polyvinylpyrrolidone.

6. 6. The release film for photosensitive resins according to claim 1, wherein the content of the crosslinking agent is 5 to 35 parts by mass per 100 parts by mass of the acid-modified polyolefin resin.

7. 6. The release film for photosensitive resins according to claim 1, wherein the content of the crosslinking agent is 15 to 25 parts by mass per 100 parts by mass of the acid-modified polyolefin resin.

8. 8. The release film for photosensitive resins according to claim 1, wherein the base film is a polyester film.

9. 9. The release film for photosensitive resins according to claim 1, wherein the base film is a multi-layer film having two or more layers.

10. A photosensitive resin laminate film in which a protective layer, a photosensitive resin layer, and the release film for photosensitive resin according to any one of claims 1 to 9 are laminated in this order such that the resin layer of the release film for photosensitive resin is adjacent to the photosensitive resin layer.

11. A photosensitive resin structure in which a substrate, a photosensitive resin layer, and the release film for photosensitive resin according to any one of claims 1 to 9 are laminated in this order such that the resin layer of the release film for photosensitive resin is adjacent to the photosensitive resin layer.

12. 12. The photosensitive resin structure according to claim 11, wherein at least a portion of the photosensitive resin layer is cured.

Citation Information

Patent Citations

  • Photosensitive resin structure for letterpress printing

    JP2010188693A

  • Base film for dry film resist and laminate using the same

    JP2013099907A

  • Photosensitive film laminate and cured product formed therewith

    JP2018136510A

  • Release film for photosensitive conductive layer transfer

    JP2018161829A