Wiring Board
The wiring board design addresses crack issues in alumite-coated substrates by forming the oxide film layer away from edges and using multiple metal thin films, ensuring insulation and enhanced heat dissipation for high-brightness LEDs and other components.
Patent Information
- Application Number
- JP2021040129
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-12
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2041-03-12
AI Technical Summary
Conventional alumite-coated aluminum substrates used in high-brightness LEDs for vehicle displays face issues with heat resistance and crack formation due to uneven oxide film thickness and stress concentration at edges, leading to insulation failures.
A wiring board design with an oxide film layer formed inside the periphery of the main surface, avoiding edges and corners, and omitting film formation on side and back surfaces, combined with a conductive wiring section of multiple metal thin films, to prevent crack formation and enhance heat dissipation.
The design effectively suppresses crack formation, maintains insulation, and improves heat dissipation, suitable for high-density mounting of high-brightness LEDs and other heat-generating components.
Smart Images

Figure 0007564025000001 
Figure 0007564025000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a wiring board. [Background technology]
[0002] Conventionally, wiring boards with high heat dissipation properties have been used as wiring boards on which elements that generate a lot of heat, such as LEDs (light emitting diodes) and power semiconductors, are mounted. As a wiring board with high heat dissipation properties, a technology has been proposed in which an aluminum substrate is coated with an alumite film to be used as an electronic substrate (hereinafter also referred to as an alumite substrate) (see, for example, Patent Documents 1 and 2). An alumite substrate can maintain the thermal conductivity and thermal diffusivity of an aluminum substrate while providing insulation, and therefore can achieve high heat dissipation. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2012-124324 A [Patent Document 2] JP 2012-201891 A Summary of the Invention [Problem to be solved by the invention]
[0004] Next-generation automobiles will use high-brightness LEDs for many of their exterior displays (lights). The number of LEDs used in vehicles will increase dramatically, requiring higher density, and high output for daytime running lights. As the number of LEDs used increases and the output of LEDs increases, there is a demand for even higher heat dissipation from the wiring boards on which the LEDs are mounted.
[0005] Therefore, anodized aluminum substrates have been considered as wiring substrates with high heat dissipation. However, since anodized aluminum coatings have low heat resistance and cracks are likely to occur on the anodized aluminum surface when heated, there is a problem that it is difficult to ensure insulation. Patent Document 1 proposes a technology to suppress the occurrence of cracks during the wiring electrode formation process by increasing the thickness of the aluminum substrate in the portion where the wiring electrode is formed and thinning the anodized aluminum layer in that portion, thereby making it easier to dissipate heat generated during the wiring electrode formation process to the aluminum substrate. Patent Document 2 proposes a technology to realize high-temperature crack resistance by appropriately defining the chemical composition of the aluminum alloy used as the base material and the size and number of intermetallic compounds present in the anodized film, and by forming a composite film structure in which at least a part of the anodized film is coated with an insulator or surface-modified.
[0006] However, even with the above-mentioned conventional techniques, there is still a risk of cracks occurring.
[0007] The present invention has been made to solve the above-mentioned problems, and aims to provide another technology for suppressing the occurrence of cracks in an oxide film layer in a wiring board having a base material made of a metal material mainly composed of aluminum and an oxide film layer formed on the surface of the base material. [Means for solving the problem]
[0008] The present invention has been made to solve the above-mentioned problems, and can be realized in the following forms.
[0009] (1) According to one aspect of the present invention, there is provided a wiring board comprising: a base material having a first main surface and made of a metal material mainly composed of aluminum (Al), an oxide coating layer which is an anodized coating of the metal material and is formed on the first main surface of the base material, and a conductive wiring portion formed on the oxide coating layer, wherein, in a plan view of the first main surface, the oxide coating layer is formed inside a periphery of the first main surface at a distance from the periphery.
[0010] If an oxide coating layer is formed on the edges, corners, etc. of the substrate, the thickness of the oxide coating layer becomes non-uniform, making it prone to cracks. In contrast, with the wiring board of this embodiment, the oxide coating layer is formed inside the periphery of the first main surface at a distance from the periphery in a plan view of the first main surface of the substrate, so that the oxide coating layer is not formed on the edges or corners of the substrate. This makes it possible to suppress the occurrence of cracks in the oxide coating layer.
[0011] (2) In the wiring board of the above embodiment, the oxide coating layer may be rectangular with chamfered corners in a plan view of the first main surface. In this way, the oxide coating layer does not have corners at which stress is concentrated, thereby making it possible to suppress the occurrence of cracks.
[0012] (3) In the wiring board of the above embodiment, the base material is plate-shaped and includes a second main surface that is the reverse side of the first main surface, and a side surface that connects the first main surface and the second main surface, and the side surface may not be provided with the oxide coating layer. In this way, heat dissipation can be improved compared to when an oxide coating layer is provided on the side surface.
[0013] The present invention can be realized in various forms, for example, in the form of a product including a wiring board, a method for manufacturing a wiring board, and a method for manufacturing a product including a wiring board. [Brief description of the drawings]
[0014] [Figure 1] FIG. 2 is an explanatory diagram illustrating a schematic planar configuration of a wiring board. [Diagram 2] FIG. 2 is an explanatory diagram illustrating a schematic cross-sectional configuration of a wiring board. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] <Embodiment> FIG. 1 is an explanatory diagram that shows a schematic planar configuration of a wiring board 100 according to an embodiment of the present invention, and FIG. 2 is an explanatory diagram that shows a schematic cross-sectional configuration of the wiring board 100. FIG. 1(B) shows a first main surface 11 of a base material 10, and FIG. 1(A) shows a side surface 13 on the left side of the plan view shown in FIG. 1(B), and FIG. 1(C) shows a side surface 13 on the right side of the plan view. FIG. 2 shows a cross section AA in FIG. 1. The wiring board 100 includes a base material 10 that is a flat plate having a substantially square planar shape, an oxide coating layer 20 formed on the first main surface 11 of the base material 10, and a wiring portion 30 formed on the oxide coating layer 20.
[0016] The substrate 10 is made of a metal material mainly composed of aluminum (Al). Since the substrate 10 is made of a metal material mainly composed of aluminum, it has high thermal conductivity and thermal diffusivity. In this embodiment, the main component is the component with the highest mass percentage.
[0017] As shown in Fig. 2, the substrate 10 is flat and includes a first main surface 11, a second main surface 12 which is the back side of the first main surface 11, and a side surface 13 which connects the first main surface 11 and the second main surface 12. In this embodiment, an oxide coating layer 20 is formed on the first main surface 11 of the substrate 10, and the oxide coating layer 20 is not formed on the second main surface 12 and the side surface 13. In Fig. 1, the side surface 13 on the upper side and the side surface 13 on the lower side of the plane of the plan view shown in Fig. 1(B) are not shown, but the oxide coating layer 20 is not formed on them as with the side surface 13 shown in Figs. 1(A) and (C). The second main surface 12 and the side surface 13 of the substrate 10 are exposed.
[0018] The oxide coating layer 20 is an oxide coating (anodized aluminum) formed by anodizing a flat plate (hereinafter also referred to as "original plate") made of a metal material mainly composed of aluminum to modify the surface. That is, in this embodiment, the oxide coating portion formed by anodizing the original plate is the oxide coating layer 20, and the unmodified base portion is the substrate 10. The oxide coating layer 20 has insulating properties.
[0019] As shown in FIG. 1B, the oxide coating layer 20 has a planar shape of a square with rounded corners, in other words, a square shape with rounded corners. In a plan view of the first main surface 11 of the substrate 10, the oxide coating layer 20 is formed inside the periphery of the first main surface 11 at a distance from the periphery. In other words, the oxide coating layer 20 is not formed on the periphery of the first main surface 11 of the substrate 10, and the substrate 10 is exposed. The oxide coating layer 20 is anodized aluminum, which is prone to cracks due to vibration, heating, and the like. In the wiring board 100 of this embodiment, the oxide coating layer 20 is formed away from the end (edge, corner) of the substrate 10, which is likely to become the starting point of cracks due to heating or impact, and therefore cracks in the oxide coating layer 20 can be suppressed.
[0020] A conductive wiring section 30 is formed on the oxide film layer 20, and the oxide film layer 20 is an area on which electronic components are mounted (hereinafter also referred to as a product area).
[0021] The wiring section 30 is configured by laminating three kinds of metal thin films whose main components are different from each other. Specifically, a metal thin film whose main component is titanium (Ti), a metal thin film whose main component is platinum (Pt), and a metal thin film whose main component is gold (Au) are laminated in this order from the oxide film layer 20 side. Titanium has good adhesion to the oxide film layer 20, platinum has better adhesion to gold than titanium, and gold has high conductivity, anticorrosion properties, and good bondability. Therefore, according to this configuration, peeling of the wiring section 30 is suppressed, and a wiring layer that is highly conductive, anticorrosive, and has good bondability can be realized. Note that in FIG. 2, each thin film is not shown separately. The wiring section 30 can be formed by a known method such as vapor deposition or sputtering.
[0022] In the wiring board 100 of this embodiment, the oxide coating layer 20 is formed inside the periphery of the first main surface 11 of the substrate 10 at a distance from the periphery. As such, as a method for partially forming an oxide coating on the surface of the substrate 10, for example, a method (first method) can be used in which anodized aluminum is formed on the entire surface of the original sheet, and then unnecessary parts (parts that expose the surface of the substrate 10) are removed by wet chemical processing, laser processing, or the like. Also, for example, a method (second method) can be used in which anodized aluminum is formed on the unnecessary parts (parts that expose the surface of the substrate 10) on the surface of the original sheet after masking with photolithography, tape, or the like.
[0023] When the oxide coating layer 20 is formed by the first method, the thickness of the substrate 10 is approximately uniform and thinner than the thickness of the original sheet. On the other hand, when the oxide coating layer 20 is formed by the second method, the thickness of the substrate 10 at the portion where the first main surface 11 of the substrate 10 is exposed (the portion shown with diagonal hatching in FIG. 1) is approximately the same as the thickness of the original sheet, and the thickness of the substrate 10 at the portion where the oxide coating layer 20 is formed is thinner than the portion where the first main surface 11 of the substrate 10 is exposed. In other words, when the oxide coating layer 20 is formed by the second method, the thickness of the substrate 10 varies partially.
[0024] In general, when anodized aluminum is formed on protruding portions such as corners and edges of the substrate 10, the thickness of the oxide coating layer 20 is likely to be non-uniform. In addition, the corners and edges of the substrate 10 may have burrs. Therefore, when anodized aluminum is formed on the corners and edges of the substrate 10, cracks are likely to occur easily due to vibration or heating. In contrast, according to the wiring board 100 of this embodiment, the oxide coating layer 20 is not formed on the peripheral portion of the first main surface 11 of the substrate 10 (in other words, the oxide coating layer 20 is formed away from the edges of the substrate 10), so that the occurrence of cracks in the oxide coating layer 20 can be suppressed.
[0025] In addition, in the wiring board 100 of this embodiment, the oxide coating layer 20 is not formed on the peripheral portion of the first main surface 11 of the base material 10, the side surface 13, and the second main surface 12. Therefore, when the oxide coating layer 20 is formed by the above-mentioned second method, the portion where the oxide coating layer 20 is not formed is masked with a resist. When performing anodizing (anodic oxidation coating) after masking, if the end of the resist is placed on the edge or corner of the original plate, there is a risk that the resist will peel off. In contrast, in the wiring board 100 of this embodiment, the end of the resist is not placed on the edge or corner of the original plate, so that peeling of the resist is more suppressed, and unevenness in the thickness of the end of the oxide coating layer 20 can be suppressed, and defects can be suppressed. As a result, the occurrence of cracks in the oxide coating layer 20 can be suppressed.
[0026] Furthermore, in the wiring board 100, since the oxide coating layer 20 is not formed on the side surface 13 and the second main surface 12 of the base material 10, heat dissipation can be improved compared to when the oxide coating layer 20 is formed on the second main surface 12 and the side surface 13.
[0027] Furthermore, the planar shape of the oxide coating layer 20 is a square with rounded corners, and since there are no corners at which stress is concentrated, the occurrence of cracks can be suppressed.
[0028] According to the wiring board 100 of this embodiment, cracks in the product area can be suppressed, and high heat dissipation can be obtained by the base material 10, which is mainly composed of aluminum with high thermal conductivity, while ensuring insulation by the oxide coating layer 20. Therefore, for example, it can be used as a wiring board on which high-brightness LEDs that generate a large amount of heat are mounted in a high density. In addition, it can be applied to semiconductors such as CPUs (Central Processing Units), power devices, and solar cells, liquid crystals, etc.
[0029] <Modifications of this embodiment> The present invention is not limited to the above-described embodiment, and can be embodied in various forms without departing from the spirit and scope of the invention. For example, the following modifications are also possible.
[0030] The main components and configuration of the wiring section 30 are not limited to those in the above embodiment. For example, it may be formed of a single layer or a multi-layer structure of metals such as Al, Au, Pt, Ti, Cu, Pd, Rh, Ni, W, Mo, Cr, Ag, or alloys thereof. A conductive material such as ITO (Indium Tin Oxide) may also be used.
[0031] In the above embodiment, the wiring board 100 having one oxide layer 20 formed thereon has been exemplified, but two or more oxide layers 20 may be formed. The wiring board may be formed as a so-called multi-piece wiring board. Even when the wiring board has two or more oxide layers 20, it is sufficient that the oxide layers 20 are formed inside the periphery of the first main surface 11 at a distance from the periphery in a plan view of the first main surface 11 of the base material 10.
[0032] In the above embodiment, an example was shown in which the oxide coating layer 20 was not formed on the second main surface 12 of the base material 10, but the oxide coating layer 20 may also be formed on the second main surface 12. In this way, electronic components can be mounted on the second main surface 12 side of the base material 10 as well.
[0033] The planar shape of the oxide coating layer 20 is not limited to the above embodiment, and may be a rectangle with unchamfered corners. The planar shape of the oxide coating layer 20 may be a polygonal shape, such as a triangle, a square, a pentagon, or a hexagon, or a shape other than a polygon, such as a circle or an ellipse. In the case of a polygonal shape, the corners may or may not be chamfered. The chamfering may be rounded (also called R chamfering) or 45° chamfering (also called C chamfering).
[0034] The planar shape of the substrate 10 is not limited to the above embodiment. For example, it may be a polygonal shape such as a triangle, a rectangle, a pentagon, or a hexagon, or a shape other than a polygon such as a circle or an ellipse. In the case of a polygonal shape, the corners may or may not be chamfered. The chamfering may be rounded (also called R chamfer) or 45° chamfered (also called C chamfer).
[0035] In the above embodiment, an example has been shown in which the surface of the base material 10 is exposed in the portion where the oxide coating layer 20 is not formed, but the surface of the base material 10 does not have to be exposed. For example, some kind of coating may be applied to the portion where the oxide coating layer 20 is not formed. However, a configuration in which the surface of the base material 10 is exposed is preferable because it can improve heat dissipation properties.
[0036] The present invention has been described above based on the embodiments and modifications, but the above-mentioned embodiments of the invention are intended to facilitate understanding of the present invention and are not intended to limit the present invention. The present invention may be modified or improved without departing from the spirit and scope of the claims, and the present invention includes equivalents thereof. Furthermore, if a technical feature is not described as essential in this specification, it may be deleted as appropriate. [Explanation of symbols]
[0037] 10...Base material 11...First main surface 12...Second main surface 13...Side 20…Oxide film layer 30…Wiring section 100...Wiring board
Claims
1. A wiring board, A substrate having a first main surface and made of a metal material containing aluminum (Al) as a main component; an oxide coating layer which is an anodized coating of the metallic material and is formed on the first main surface of the base material; a wiring portion having electrical conductivity and formed on the oxide film layer; Equipped with In a plan view of the first main surface, the oxide coating layer is formed inside a periphery of the first main surface at a distance from the periphery, When viewed in plan on the first main surface, the oxide coating layer has a rectangular shape with chamfered corners. Wiring board.
2. 2. The wiring board according to claim 1, The substrate has a plate shape, A second main surface that is a back surface of the first main surface, and a side surface that connects the first main surface and the second main surface, The side surface is not formed with the oxide coating layer. Wiring board.
Citation Information
Patent Citations
Plasma treatment device and method of manufacturing electrostatic chuck
JP2004259745A
mounts for electrical circuits, specifically for power switches
JP2004527120A
Thin-film capacitor and wiring board
JP2006228907A
Printed circuit board having metal core
JP2007243194A
Circuit device and its manufacturing method
JP2008187144A