Block copolymer, composition, heat-shrinkable film, sheet, and molded article of the sheet

The block copolymer with a specific composition and synthesis method addresses the issues of gel foreign substances and impact resistance in heat-shrinkable films and sheets, enhancing mechanical strength and appearance through optimized molecular structure and processing.

JP7564199B2Active Publication Date: 2024-10-08DENKA CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2022522070
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-12-06
Filing Date
2022-03-18
Publication Date
2024-10-08
Estimated Expiration
2042-03-18

AI Technical Summary

Technical Problem

Existing block copolymers used in heat-shrinkable films and sheets suffer from issues such as gel foreign substances (fish eyes) and inadequate impact resistance, which affect their mechanical strength and appearance quality.

Method used

A block copolymer comprising a first and second vinyl aromatic block, and a copolymer block with a specific composition and molecular weight range, along with a composition containing this copolymer, which is synthesized through living anionic polymerization and optimized for dynamic viscoelasticity and tensile elongation.

Benefits of technology

The solution provides block copolymers with improved tensile elongation, impact resistance, and reduced gel foreign matter, resulting in films and sheets with enhanced mechanical strength and appearance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007564199000001
    Figure 0007564199000001
  • Figure 0007564199000002
    Figure 0007564199000002
Patent Text Reader

Abstract

The present invention provides, as a block copolymer having a high tensile elongation value and less foreign gel substances, a block copolymer which comprises a first vinyl aromatic block that is substantially configured only from the vinyl aromatic monomer unit, a second vinyl aromatic block that is substantially configured only from the vinyl aromatic monomer unit, and a copolymer block. With respect to this block copolymer, the second vinyl aromatic block has a weight average molecular weight that is not more than the weight average molecular weight of the first vinyl aromatic block; the copolymer block is substantially configured only from the vinyl aromatic monomer unit and the conjugated diene monomer unit; the content ratio of the conjugated diene monomer unit in the copolymer block is 55% by mass to 82% by mass; the proportion of the first vinyl aromatic block is 50% by mass to 85% by mass if the total mass of the first vinyl aromatic block and the second vinyl aromatic block is taken as 100% by mass; the content ratio of the copolymer block in the block copolymer is 38% by mass to 60% by mass; and the loss tangent value (tanδ) has at least one peak within the range from -70°C to -35°C if dynamic viscoelasticity measurement is carried out under specific conditions.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a block copolymer, a composition, a heat shrinkable film, a sheet, and a molded article of the sheet. [Background technology]

[0002] Heat-shrinkable films using block copolymers obtained by polymerizing vinyl aromatic compounds and conjugated diene compounds are excellent in heat shrinkability and finish after shrinkage, and can be adapted to various shapes and installation methods of packaged objects, and are therefore widely used for shrink packaging. Another advantage is that they do not cause environmental pollution problems when disposed of, unlike polyvinyl chloride. For example, Patent Document 1 discloses a heat-shrinkable film using a composition containing a block copolymer of styrene and butadiene.

[0003] The block copolymer is also used in sheets and molded articles thereof. For example, in the case of molded articles such as food containers, a technique of adding the block copolymer to polystyrene resin or poly(styrene-methyl methacrylate) copolymer resin is widely used for the purpose of improving impact resistance when dropped. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 11-158241 Summary of the Invention [Problem to be solved by the invention]

[0005] For heat-shrinkable films and sheets, and molded products thereof, impact resistance and break resistance are important properties, and the tensile elongation of the raw material block copolymer or a composition containing the block copolymer is used as an index of these properties. However, block copolymers and compositions thereof with good tensile elongation have a problem in that they are prone to generate gel foreign matter (fish eyes are likely to occur when the block copolymers are made into films or sheets). Therefore, it has been desired to achieve both good tensile elongation and a small amount of gel foreign matter.

[0006] The present invention has been made in view of the above problems, and aims to provide a block copolymer having a high tensile elongation value, which is an index of mechanical strength and appearance quality, and containing little gel foreign matter. Another aim of the present invention is to provide a composition containing the block copolymer, and to provide a sheet, film, or heat-shrinkable film using the composition as a raw material, which has high impact strength and tensile elongation, has few fisheyes, and is excellent in appearance. [Means for solving the problem]

[0007] According to the present invention, there is provided a block copolymer having a first vinyl aromatic block (S1), a second vinyl aromatic block (S2), and a copolymer block (B / S), in which the first vinyl aromatic block (S1) is substantially composed of only vinyl aromatic monomer units, the second vinyl aromatic block (S2) is substantially composed of only vinyl aromatic monomer units, and has a weight average molecular weight equal to or less than that of the first vinyl aromatic block, the copolymer block (B / S) is substantially composed of only vinyl aromatic monomer units and conjugated diene monomer units, and the conjugated diene monomer units in the copolymer block are the content of the copolymer block in the block copolymer is 38% by mass or more and 60% by mass or less, and the loss tangent value (tan δ) has at least one peak in the range of -70°C or more and -35°C or less when dynamic viscoelasticity measurement is performed under conditions of a heating rate of 4°C / min, a frequency of 1 Hz, and a strain of 0.02% according to ISO6721-1.

[0008] The weight average molecular weight of the first vinyl aromatic block (S1) is preferably 30,000 or more and 100,000 or less.

[0009] When the total mass of the vinyl aromatic monomer units and the conjugated diene monomer units in the block copolymer is taken as 100 mass%, the ratio of the vinyl aromatic monomer units in the block copolymer is preferably 64 mass% or more and 75 mass% or less.

[0010] Various embodiments of the present invention will be described below. The embodiments described below can be combined with each other. Preferably, the copolymer block (B / S) is a random copolymer block of vinyl aromatic monomer units and conjugated diene monomer units. Preferably, it is linear, and the arrangement of polymer blocks is (S1)-(B / S)-(S2) or (S2)-(B / S)-(S1).

[0011] According to another aspect of the present invention, there is provided a composition comprising the block copolymer and further comprising a polymer different from the block copolymer. Preferably, the content of the block copolymer is 15% by mass or more and 85% by mass or less.

[0012] According to another aspect of the present invention, there is provided a heat shrinkable film comprising a layer constituted by the above composition.

[0013] According to another aspect of the present invention, there is provided a sheet comprising a layer constituted by the above-mentioned composition.

[0014] According to another aspect of the present invention, there is provided a molded article obtained by molding the above-mentioned sheet. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] Hereinafter, embodiments of the present invention will be described. Various features shown in the following embodiments can be combined with each other. Also, each feature can be an invention independently.

[0016] 1-1.Block copolymer A block copolymer according to one embodiment of the present invention has a first vinyl aromatic block (S1), a second vinyl aromatic block (S2), and a copolymer block (B / S).

[0017] The block copolymer is preferably a linear block copolymer. The linear block copolymer preferably has a first vinyl aromatic block (S1) at one end and a second vinyl aromatic block (S2) at the other end. The linear block copolymer preferably has a polymer block sequence represented by (S1)-(B / S)-(S2) or (S2)-(B / S)-(S1), in which the blocks are bonded in the order of the first vinyl aromatic block-copolymer block-second vinyl aromatic block or in the reverse order.

[0018] When the total mass of the first vinyl aromatic block and the second vinyl aromatic block contained in the block copolymer is 100% by mass, the ratio of the first vinyl aromatic block (mass of the first vinyl aromatic block / (mass of the first vinyl aromatic block+mass of the second vinyl aromatic block)×100) is 50-85% by mass. In other words, the ratio of the second vinyl aromatic block (mass of the second vinyl aromatic block / (mass of the first vinyl aromatic block+mass of the second vinyl aromatic block)×100) is 15-50% by mass. When the ratio of the first vinyl aromatic block is in such a range, the tensile elongation tends to be good, and the impact resistance and heat shrinkage rate tend to be good when used as a raw material for a heat shrinkable film. In addition, when the weight average molecular weight of the two vinyl aromatic blocks is the same (they cannot be distinguished after the copolymerization block of the block copolymer is decomposed and the blocks are separated), they can be treated as 50% by mass (the mass ratio of the two blocks is 50 / 50).

[0019] The content of the copolymer block in the block copolymer is 38% by mass or more and 60% by mass or less, and preferably 40% by mass or more and 55% by mass or less. When the content of the copolymer block is in such a range, the balance between tensile elongation and suppression of gel foreign matter generation (fisheye) tends to be good, and impact resistance tends to be good when used as a raw material for heat shrinkable films.

[0020] When the total mass of the vinyl aromatic monomer units and the conjugated diene monomer units in the block copolymer is taken as 100 mass%, the ratio of the vinyl aromatic monomer units in the block copolymer is preferably 64 to 75 mass%, more preferably 68 to 72 mass%. When the ratio of the vinyl aromatic monomer units in the block copolymer is within such a range, the balance between tensile elongation and suppression of gel foreign matter generation (fisheye) tends to be good, and impact resistance and blocking resistance tend to be good when used as a raw material for heat shrinkable films.

[0021] The weight average molecular weight of the block copolymer is preferably from 100,000 to 200,000. This tends to ensure good physical properties such as tensile elongation while also improving moldability when forming a film or sheet.

[0022] The block copolymer may be a mixture of two or more types of block copolymers that satisfy the above requirements, and may contain other components within a range that does not impair the effects of the present invention. Examples of other components include heat-deactivated products and coupling products generated during the production of the block copolymer, and additives.

[0023] 1-2. First vinyl aromatic block The first vinyl aromatic block is substantially composed of only vinyl aromatic monomer units. "Substantially composed of only vinyl aromatic monomer units" means that, when the weight of the first vinyl aromatic block is 100% by mass, 98% by mass or more of the block is vinyl aromatic monomer units, and 2% by mass or less of unintended monomer units may be present. Hereinafter, when "substantially composed of ..." is used, the same meaning is intended. When the weight of the first vinyl aromatic block is 100% by mass, more preferably 99% by mass or more of the block is vinyl aromatic monomer units, and even more preferably 100% by mass of the block is vinyl aromatic monomer units.

[0024] The vinyl aromatic monomer unit is a unit derived from the vinyl aromatic monomer used in the polymerization. The vinyl aromatic monomer is a monomer in which a vinyl group is bonded to an aromatic ring. Examples of the vinyl aromatic monomer include vinyl aromatic hydrocarbon monomers such as styrene, o-methylstyrene, p-methylstyrene, p-tert-butylstyrene, 2,4-dimethylstyrene, 2,5-dimethylstyrene, α-methylstyrene, vinylnaphthalene, and vinylanthracene. In one embodiment, the vinyl aromatic monomer is preferably styrene. These monomers may be used alone or in combination of two or more.

[0025] The weight average molecular weight of the first vinyl aromatic block is preferably 30,000 or more and 100,000 or less, and more preferably 35,000 or more and 70,000 or less. The weight average molecular weight of the first vinyl aromatic block is equal to or greater than that of the second vinyl aromatic block. This tends to result in good transparency when used as a raw material for heat shrinkable films and sheets.

[0026] 1-3. Second vinyl aromatic block The second vinyl aromatic block is substantially composed of only vinyl aromatic monomer units. When the weight of the second vinyl aromatic block is taken as 100% by mass, the second vinyl aromatic block is more preferably 99% by mass or more of vinyl aromatic monomer units, and even more preferably 100% by mass of vinyl aromatic monomer units. The vinyl aromatic monomer units are the same as those of the first aromatic vinyl block. The weight average molecular weight of the second vinyl aromatic block is equal to or less than that of the first vinyl aromatic block.

[0027] 1-4. Copolymer block The copolymer block is substantially composed of only vinyl aromatic monomer units and conjugated diene monomer units. When the weight of the copolymer block is taken as 100 mass%, the copolymer block is more preferably composed of 99 mass% or more of vinyl aromatic monomer units and conjugated diene monomer units, and even more preferably 100 mass% of vinyl aromatic monomer units and conjugated diene monomer units.

[0028] The content of the conjugated diene monomer unit in the copolymer block is 55% by mass or more and 82% by mass or less, and preferably 60% by mass or more and 80% by mass or less, when the total mass of the monomer units constituting the copolymer block is taken as 100% by mass. When the content of the conjugated diene monomer unit is within such a range, a good balance between tensile elongation and suppression of gel foreign matter generation (fisheye) is likely to be achieved, and impact resistance and blocking resistance when used as a raw material for a heat-shrinkable film are likely to be good.

[0029] The copolymer block may be of a tapered type in which the composition of the vinyl aromatic monomer unit and the conjugated diene monomer unit changes continuously, or of a random type in which the composition of the vinyl aromatic monomer unit and the conjugated diene monomer unit is almost constant. In the present invention, however, the random copolymer block is preferable. The random copolymer block is formed, for example, by continuously adding the vinyl aromatic monomer unit and the conjugated diene monomer unit to the polymerization system at a constant weight ratio. Since the composition of the vinyl aromatic monomer unit and the conjugated diene monomer unit is almost constant in the random copolymer block, there is no region where the composition ratio of the conjugated diene monomer unit is locally high, and the generation of fish eyes can be suppressed more than in the tapered type. In addition, since there is no region where the composition ratio of the conjugated diene monomer unit is locally low, the conjugated diene monomer unit can efficiently contribute to the impact resistance and the break resistance, and the balance of these physical properties is good.

[0030] The conjugated diene monomer unit is a unit derived from the conjugated diene monomer used in the polymerization. The conjugated diene monomer is a monomer having a chemical structure represented by C=CC=C. Examples of the conjugated diene monomer include conjugated diene monomers such as 1,3-butadiene, 2-methyl-1,3-butadiene (isoprene), 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, and 1,3-hexadiene. In one embodiment, the conjugated diene monomer is preferably 1,3-butadiene. These monomers may be used alone or in combination of two or more.

[0031] The molecular weight of each block can be calculated based on the weight average molecular weight of the block copolymer and the amount of each monomer charged, or may be calculated based on the weight average molecular weight of the block copolymer and the weight average molecular weight after decomposition of the block copolymer.

[0032] The block copolymer can be decomposed, for example, by the ozone decomposition method described in a known document (Y.TANAKA, et.al., "RUBBER CHEMISTRY AND TECHNOLOGY", p. 16 (1985)). The first vinyl aromatic block and the second vinyl aromatic block, which are composed only of vinyl aromatic monomers, are not decomposed, and the molecular weights of the first vinyl aromatic block and the second vinyl aromatic block can be measured after decomposition, and their contents can be calculated. The weight average molecular weight and content of the copolymer block can be calculated by subtracting the weight average molecular weights of the first vinyl aromatic block and the second vinyl aromatic block from the weight average molecular weight of the block copolymer before decomposition.

[0033] 1-5.Composition The composition according to one embodiment of the present invention preferably further contains, in addition to the block copolymer, a polymer (resin) different from the block copolymer. Examples of the polymer different from the block copolymer include a styrene-butadiene block copolymer different from the block copolymer, polystyrene, and poly(styrene-methyl methacrylate) copolymer. The block copolymer of the present invention is excellent in balance of impact resistance, break resistance, and fisheye suppression when used as a raw material for heat-shrinkable films and sheets, and by forming a composition with, for example, a styrene-butadiene block copolymer having an excellent heat shrinkage rate of a heat-shrinkable film, or polystyrene having excellent rigidity, a heat-shrinkable film or sheet having an even better balance of these physical properties can be obtained.

[0034] The content of the block copolymer in the composition is preferably 15% by mass or more and 85% by mass or less, more preferably 30% by mass or more and 70% by mass or less. The content of the polymer different from the block copolymer in the composition is not particularly limited, but is, for example, 15% by mass or more and 85% by mass or less, preferably 30% by mass or more and 70% by mass or less.

[0035] 1-6. Physical properties of block copolymers and compositions According to ISO6721-1, the block copolymer is subjected to dynamic viscoelasticity measurement under conditions of a heating rate of 4°C / min, a frequency of 1Hz, and a strain of 0.02%, and the loss tangent value (tan δ) has at least one peak in the range of -70 to -35°C. When the copolymer block is a random copolymer block and the content of the conjugated diene monomer unit in the copolymer block is within the above range, tan δ tends to be within the above range, and the balance of impact resistance, break resistance, and blocking resistance is good, and the occurrence of fish eyes is easily suppressed. In addition, the composition containing the block copolymer preferably has at least one peak in the same range.

[0036] 1-7. Manufacturing method

[0037] The block copolymer according to one embodiment of the present invention can be synthesized by various methods, but can be obtained by a living anionic polymerization reaction in an organic solvent using an organolithium compound as a polymerization initiator.

[0038] Examples of the organic solvent include aliphatic hydrocarbons such as butane, pentane, hexane, isopentane, heptane, octane, and isooctane, alicyclic hydrocarbons such as cyclopentane, methylcyclopentane, cyclohexane, methylcyclohexane, and ethylcyclohexane, and aromatic hydrocarbons such as benzene, toluene, ethylbenzene, and xylene. Cyclohexane is particularly preferred.

[0039] An organolithium compound is a compound in which one or more lithium atoms are bonded in the molecule. Examples of organolithium compounds include monofunctional organolithium compounds such as ethyllithium, n-propyllithium, isopropyllithium, n-butyllithium, sec-butyllithium, and tert-butyllithium, and polyfunctional organolithium compounds such as hexamethylenedilithium, butadienyldilithium, and isoprenyldilithium. In particular, it is preferable to use n-butyllithium.

[0040] In living anionic polymerization, a block copolymer having any primary structure can be obtained by changing the amount and method of addition of monomers (vinyl aromatic monomer and conjugated diene monomer). For example, there is a method in which only vinyl aromatic monomer is added, and after the vinyl aromatic monomer is completely consumed, vinyl aromatic monomer and conjugated diene monomer are added simultaneously at a predetermined rate, and after these are completely consumed, only vinyl aromatic monomer is added again to polymerize.

[0041] By changing the amount and method of addition, it is possible to control the physical properties of the block copolymer. For example, the molecular weight can be controlled by changing the ratio of the organolithium compound to the monomer, and the storage modulus and loss tangent (tan δ) can be controlled by changing the ratio of the vinyl aromatic monomer unit and the conjugated diene monomer unit in each block chain.

[0042] The block copolymer thus obtained is inactivated by adding a polymerization terminator such as water, alcohol, or carbon dioxide in an amount sufficient to inactivate the active terminals. The copolymer can be recovered from the resulting block copolymer solution by any method, such as (A) a method of precipitating with a poor solvent such as methanol, (B) a method of precipitating by evaporating the solvent with a heated roll or the like (drum dryer method), (C) a method of concentrating the solution with a concentrator and then removing the solvent with a vented extruder (devolatilizing extrusion method), or (D) a method of dispersing the solution in water, blowing in steam to heat and remove the solvent, and recovering the copolymer (steam stripping method). The devolatilizing extrusion method is particularly preferred.

[0043] A composition according to one embodiment of the present invention can be obtained by mixing the block copolymer obtained by the above-mentioned production method or the like with other block copolymers, polymers, or additives as necessary.

[0044] Examples of other additives include various stabilizers, lubricants, processing aids, antiblocking agents, antistatic agents, antifogging agents, light resistance improvers, softeners, plasticizers, pigments, etc. Each additive may be added to the block copolymer solution, or may be blended with the recovered copolymer and melt-mixed.

[0045] Examples of the stabilizer include phenol-based antioxidants such as 2-tert-butyl-6-(3-tert-butyl-2-hydroxy-5-methylbenzyl)-4-methylphenyl acrylate, 2-[1-(2-hydroxy-3,5-di-tert-pentylphenyl)ethyl]-4,6-di-tert-pentylphenyl acrylate, octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate and 2,6-di-tert-butyl-4-methylphenol, and phosphorus-based antioxidants such as trisnonylphenyl phosphite. Examples of the antiblocking agent, antistatic agent, and lubricant include fatty acid amide, ethylene bisstearic acid amide, sorbitan monostearate, saturated fatty acid ester of fatty alcohol, and pentaerythritol fatty acid ester. It is preferable to use these additives in an amount of 5% by mass or less based on the block copolymer.

[0046] The composition according to one embodiment of the present invention may contain a plurality of polymers, such as the block copolymer and other polymers, and known methods can be used to mix these polymers. For example, they may be dry-blended using a Henschel mixer, ribbon blender, super mixer, V blender, or the like, or may be melted and pelletized using an extruder. In one embodiment, melt mixing is preferred. Alternatively, a method of mixing polymer solutions together and then removing the solvent may be used.

[0047] 2.Heat-shrinkable film / sheet / molded sheet products A heat-shrinkable film or sheet according to one embodiment of the present invention comprises a layer constituted by the above-mentioned composition.

[0048] A sheet ("sheet" can also be called "film", but hereinafter it will be referred to as "sheet" to distinguish it from "heat shrinkable film") can be obtained by extruding the above composition using a known method, such as the T-die method or the tubular method.

[0049] The heat-shrinkable film can be obtained by stretching the extruded sheet uniaxially, biaxially or multiaxially, and in particular, the method of extruding the sheet by the T-die method and then stretching the sheet biaxially is preferred.

[0050] The heat-shrinkable film or sheet according to one embodiment of the present invention may have a structure including only a layer made of the above-mentioned composition, but can be made into a multi-layered heat-shrinkable film or sheet by laminating another resin layer on at least one surface of the layer. In order to make the heat-shrinkable film into a multi-layered structure, another resin layer may be laminated on the layer made of the above-mentioned composition after stretching, another resin layer may be laminated on an unstretched film obtained by forming the above-mentioned composition into a film and stretching it, or a multi-layered film in which the above-mentioned composition and another resin are laminated by multi-layer extrusion molding may be stretched. As the resin used for the other resin layer, a styrene-based resin is preferable.

[0051] Examples of uniaxial stretching include a method of stretching an extruded sheet in a direction perpendicular to the extrusion direction (TD) using a tenter, and a method of stretching an extruded tubular film in the circumferential direction.

[0052] Examples of biaxial stretching include a method in which an extruded sheet is stretched in the extrusion direction (MD) with a roll and then stretched in a direction perpendicular to the extrusion direction (TD) with a tenter or the like, and a method in which an extruded tubular sheet is stretched in the extrusion direction and the circumferential direction simultaneously or separately.

[0053] The stretching temperature is preferably, for example, 60 to 120°C. By setting the temperature to 60°C or higher, the sheet is less likely to break during stretching, and by setting the temperature to 120°C or lower, the heat shrinkage rate and thickness precision of the obtained film are likely to be good. The stretching ratio is not particularly limited, but is preferably 1.5 to 8 times. By setting the temperature to 1.5 times or higher, the heat shrinkability is likely to be good, and by setting the temperature to 8 times or lower, the sheet is less likely to break during stretching. When the heat shrinkable film is used as a heat shrinkable label or packaging material, the heat shrinkage rate is preferably 20% or more at 80°C. If it is less than 20%, a high temperature is required for shrinkage, which is not preferable as it adversely affects the article to be covered. The thickness of the film is preferably 10 to 300 μm.

[0054] The heat-shrinkable film can be used as a heat-shrinkable label, a heat-shrinkable cap seal, etc. In addition, it can be used as a packaging film, etc. By using such a heat-shrinkable film as a label, a container such as a PET bottle with a label attached thereto can be obtained.

[0055] Moreover, the molded article according to one embodiment of the present invention is a molded article obtained by molding a sheet into a desired shape. EXAMPLES

[0056] The present invention will be described in more detail below with reference to examples. Note that these are merely illustrative and do not limit the scope of the present invention.

[0057] [Production of block copolymers] Block copolymers P1 to P8 were produced as Examples 1 to 4 and Comparative Examples 1 to 4 by the following procedures (Table 1).

[0058] <Polymerization of Block Copolymer P1> (1) 500.0 kg of cyclohexane and 75.0 g of tetrahydrofuran (THF) were placed in a reaction vessel. (2) 2000 mL of a 10% by mass solution of n-butyllithium in cyclohexane was added thereto as a polymerization initiator solution, and the temperature was maintained at 30°C. (3) 20 kg of styrene was added and the styrene was polymerized anionically. The internal temperature rose to 42°C. (4) After the styrene was completely consumed, the internal temperature of the reaction system was raised to 80°C, and while maintaining the internal temperature, a total of 40 kg of styrene and a total of 60 kg of 1,3-butadiene were added simultaneously at constant addition rates of 40 kg / h and 60 kg / h, respectively. (5) After styrene and 1,3-butadiene were completely consumed, the internal temperature of the reaction system was lowered to 55°C, and 80 kg of styrene was added in one go to carry out anionic polymerization of styrene. The internal temperature rose to 93°C. (6) Finally, all of the polymerization active ends were deactivated with water to obtain a polymerization solution containing a block copolymer having a polystyrene block and a random block of styrene and butadiene. (7) The polymerization liquid was devolatilized and melt-pelletized in an extruder to obtain a block copolymer P1.

[0059] <Polymerization of block copolymer P2> (1) 500.0 kg of cyclohexane and 75.0 g of tetrahydrofuran (THF) were placed in a reaction vessel. (2) 2000 mL of a 10% by mass solution of n-butyllithium in cyclohexane was added thereto as a polymerization initiator solution, and the temperature was maintained at 30°C. (3) 25.6 kg of styrene was added and anionically polymerized. The internal temperature rose to 45°C. (4) After the styrene was completely consumed, the internal temperature of the reaction system was raised to 80°C, and while maintaining the internal temperature, a total of 34.4 kg of styrene and a total of 60 kg of 1,3-butadiene were added simultaneously at constant addition rates of 34.4 kg / h and 60 kg / h, respectively. (5) After styrene and 1,3-butadiene were completely consumed, the internal temperature of the reaction system was lowered to 55°C, and 80 kg of styrene was added in one go to carry out anionic polymerization of styrene. The internal temperature rose to 93°C. (6) Finally, all of the polymerization active ends were deactivated with water to obtain a polymerization solution containing a block copolymer having a polystyrene block and a random block of styrene and butadiene. (7) The polymerization liquid was devolatilized and melt-pelletized in an extruder to obtain a block copolymer P2.

[0060] <Polymerization of block copolymer P3> (1) 500.0 kg of cyclohexane and 75.0 g of tetrahydrofuran (THF) were placed in a reaction vessel. (2) 2000 mL of a 10% by mass solution of n-butyllithium in cyclohexane was added thereto as a polymerization initiator solution, and the temperature was maintained at 30°C. (3) 50 kg of styrene was added and the styrene was polymerized anionically. The internal temperature rose to 49°C. (4) After the styrene was completely consumed, the internal temperature of the reaction system was raised to 80°C, and while maintaining the internal temperature, a total of 40 kg of styrene and a total of 60 kg of 1,3-butadiene were added simultaneously at constant addition rates of 40 kg / h and 60 kg / h, respectively. (5) After styrene and 1,3-butadiene were completely consumed, the internal temperature of the reaction system was lowered to 60°C, 50 kg of styrene was added in one go, and styrene was polymerized anionically. The internal temperature rose to 81°C. (6) Finally, all of the polymerization active ends were deactivated with water to obtain a polymerization solution containing a block copolymer having a polystyrene block and a random block of styrene and butadiene. (7) The polymerization liquid was devolatilized and melt-pelletized in an extruder to obtain a block copolymer P3.

[0061] <Polymerization of block copolymer P4> (1) 500.0 kg of cyclohexane and 75.0 g of tetrahydrofuran (THF) were placed in a reaction vessel. (2) 2000 mL of a 10% by mass solution of n-butyllithium in cyclohexane was added thereto as a polymerization initiator solution, and the temperature was maintained at 30°C. (3) 60 kg of styrene was added and the styrene was polymerized anionically. The internal temperature rose to 56°C. (4) After the styrene was completely consumed, the internal temperature of the reaction system was raised to 80°C, and while maintaining the internal temperature, a total of 16 kg of styrene and a total of 64 kg of 1,3-butadiene were added simultaneously at constant addition rates of 16 kg / h and 64 kg / h, respectively. (5) After styrene and 1,3-butadiene were completely consumed, the internal temperature of the reaction system was lowered to 60°C, 60 kg of styrene was added in one go, and styrene was polymerized anionically. The internal temperature rose to 81°C. (6) Finally, all of the polymerization active ends were deactivated with water to obtain a polymerization solution containing a block copolymer having a polystyrene block and a random block of styrene and butadiene. (7) The polymerization liquid was devolatilized and melt-pelletized in an extruder to obtain block copolymer P4.

[0062] <Polymerization of block copolymer P5> (1) 500.0 kg of cyclohexane and 75.0 g of tetrahydrofuran (THF) were placed in a reaction vessel. (2) 2000 mL of a 10% by mass solution of n-butyllithium in cyclohexane was added thereto as a polymerization initiator solution, and the temperature was maintained at 30°C. (3) 4 kg of styrene was added and the styrene was polymerized anionically. The internal temperature rose to 35°C. (4) After the styrene was completely consumed, the internal temperature of the reaction system was raised to 80°C, and while maintaining the internal temperature, a total of 51 kg of styrene and a total of 7 kg of 1,3-butadiene were added simultaneously at constant addition rates of 153 kg / h and 21 kg / h, respectively. (5) After styrene and 1,3-butadiene were completely consumed, the internal temperature of the reaction system was lowered to 60°C, and 46 kg of 1,3-butadiene was added all at once to carry out anionic polymerization of 1,3-butadiene. The internal temperature rose to 94°C. (6) After 1,3-butadiene was completely consumed, the internal temperature of the reaction system was lowered to 65°C, and 34 kg of styrene was added in one go to carry out anionic polymerization of styrene. The internal temperature rose to 79°C. (7) Finally, all of the polymerization active ends were deactivated with water to obtain a polymerization solution containing a block copolymer having polystyrene blocks, polybutadiene blocks, and random blocks of styrene and butadiene. (8) The polymerization liquid was devolatilized and melt-pelletized in an extruder to obtain block copolymer P5.

[0063] <Polymerization of block copolymer P6> (1) 500.0 kg of cyclohexane and 75.0 g of tetrahydrofuran (THF) were placed in a reaction vessel. (2) 2000 mL of a 10% by mass solution of n-butyllithium in cyclohexane was added thereto as a polymerization initiator solution, and the temperature was maintained at 30°C. (3) 74 kg of styrene was added and anionically polymerized. The internal temperature rose to 66°C. (4) After the styrene was completely consumed, the internal temperature of the reaction system was lowered to 45°C, and 100 kg of 1,3-butadiene was added in one go to carry out anionic polymerization of 1,3-butadiene. The internal temperature rose to 112°C. (5) After 1,3-butadiene was completely consumed, the internal temperature of the reaction system was lowered to 70°C, and 26 kg of styrene was added in one go to carry out anionic polymerization of styrene. The internal temperature rose to 78°C. (6) Finally, all of the polymerization active ends were deactivated with water to obtain a polymerization solution containing a block copolymer having a polystyrene block and a polybutadiene block. (7) The polymerization liquid was devolatilized and melt-pelletized in an extruder to obtain block copolymer P6.

[0064] <Polymerization of block copolymer P7> (1) 500.0 kg of cyclohexane and 75.0 g of tetrahydrofuran (THF) were placed in a reaction vessel. (2) 2000 mL of a 10% by mass solution of n-butyllithium in cyclohexane was added thereto as a polymerization initiator solution, and the temperature was maintained at 30°C. (3) 65 kg of styrene was added and the styrene was polymerized anionically. The internal temperature rose to 54°C. (4) After the styrene was completely consumed, the internal temperature of the reaction system was raised to 80°C, and while maintaining the internal temperature, a total of 22 kg of styrene and a total of 48 kg of 1,3-butadiene were added simultaneously at constant addition rates of 22 kg / h and 48 kg / h, respectively. (5) After styrene and 1,3-butadiene were completely consumed, the internal temperature of the reaction system was lowered to 60°C, 65 kg of styrene was added in one go, and styrene was polymerized anionically. The internal temperature rose to 86°C. (6) Finally, all of the polymerization active ends were deactivated with water to obtain a polymerization solution containing a block copolymer having a polystyrene block and a random block of styrene and butadiene. (7) The polymerization liquid was devolatilized and melt-pelletized in an extruder to obtain block copolymer 7.

[0065] <Polymerization of block copolymer P8> (1) 500.0 kg of cyclohexane and 75.0 g of tetrahydrofuran (THF) were placed in a reaction vessel. (2) 2000 mL of a 10% by mass solution of n-butyllithium in cyclohexane was added thereto as a polymerization initiator solution, and the temperature was maintained at 30°C. (3) 10 kg of styrene was added and the styrene was polymerized anionically. The internal temperature rose to 36°C. (4) After the styrene was completely consumed, the internal temperature of the reaction system was raised to 80°C, and while maintaining the internal temperature, a total of 16 kg of styrene and a total of 64 kg of 1,3-butadiene were added simultaneously at constant addition rates of 16 kg / h and 64 kg / h, respectively. (5) After styrene and 1,3-butadiene were completely consumed, the internal temperature of the reaction system was lowered to 50°C, 110 kg of styrene was added in one go, and styrene was polymerized anionically. The internal temperature rose to 103°C. (6) Finally, all of the polymerization active ends were deactivated with water to obtain a polymerization solution containing a block copolymer having a polystyrene block and a random block of styrene and butadiene. (7) The polymerization liquid was devolatilized and melt-pelletized in an extruder to obtain block copolymer P8.

[0066] [Analysis of block copolymers] <Content of vinyl aromatic monomer units and conjugated diene monomer units> The content of vinyl aromatic monomer units (styrene) and conjugated diene monomer units (butadiene) in the block copolymer was measured and calculated by the halogen addition method described below. (A1) The sample was dissolved in a solvent (such as carbon tetrachloride) capable of completely dissolving the sample, and then an excess amount of iodine monochloride / carbon tetrachloride solution was added to react sufficiently. The unreacted iodine monochloride was titrated with a sodium thiosulfate / ethanol solution to calculate the amount of double bonds. (A2) Based on the amount of double bonds obtained by the method of (A1), the butadiene content (rubber content) was calculated. The styrene content was calculated by subtracting the butadiene content from the total content of the sample.

[0067] <Weight average molecular weight and content of each block> The weight average molecular weight of each block was calculated from the weight average molecular weight (M) of the block copolymer measured by GPC and the weight (W) [kg] of the monomer charged during polymerization of each block, according to the following formulas (1) to (3). The content of each block was calculated from the following formulas (B4) to (B6). (B1) (weight average molecular weight of first vinyl aromatic block)=M×W1 / (W1+W2+W3) (B2) (weight average molecular weight of second vinyl aromatic block)=M×W2 / (W1+W2+W3) (B3) (Weight average molecular weight of copolymer block) = M × W3 / (W1 + W2 + W3) (B4) (Content of first vinyl aromatic block) = W1 / (W1+W2+W3) x 100 [%] (B5) (content of second vinyl aromatic block) = W2 / (W1+W2+W3) x 100 [%] (B6) (Copolymer block content) = W3 / (W1+W2+W3) x 100 [%] (W1: Charge monomer weight of the first vinyl aromatic block [kg], W2: Charge monomer weight of the second vinyl aromatic block [kg], W3: Charge monomer weight of the copolymer block [kg])

[0068] Also, the weight average molecular weights of the first vinyl aromatic block and the second vinyl aromatic block can be measured by decomposing the conjugated diene monomer units by the ozonolysis method described in a known document (Y. TANAKA, et al., "RUBBER CHEMISTRY AND TECHNOLOGY", p16 (1985)) and then performing GPC measurement. In that case, the weight average molecular weight of the copolymer block is calculated by subtracting the weight average molecular weights of the first vinyl aromatic block and the second vinyl aromatic block from the weight average molecular weight of the block copolymer before decomposition measured by GPC measurement. <GPC measurement> The molecular weight of the block copolymer was measured using the following GPC measurement apparatus and conditions, and calculated as the polystyrene equivalent molecular weight by a calibration curve using standard polystyrene. Apparatus name: HLC-8220GPC (manufactured by Tosoh Corporation) Column: Four Shodex GPC KF-404 (manufactured by Showa Denko KK) columns connected in series Temperature: 40 °C Detection: Differential refractive index Solvent: Tetrahydrofuran Concentration: 2 mass% Calibration curve: Prepared using standard polystyrene (manufactured by VARIAN).

[0069] <Ratio of conjugated diene monomer units in the copolymer block> The ratio of the conjugated diene monomer units (butadiene) in the copolymer block was calculated using the "content of the copolymer block" determined by the above formula (B6) and the "content of the conjugated diene monomer units" in (A2) above, by the following formula (B7) (B7) (Ratio of conjugated diene monomer units in the copolymer block) = (Content of conjugated diene monomer units) / (Content of copolymer block) × 100 [%]

[0070] <Ratio of first vinyl aromatic block: S1 / (S1+S2)> The ratio of the first vinyl aromatic block (S1) and the ratio of the second vinyl aromatic block (S2), "S1 / (S1+S2)", when the total mass of the first vinyl aromatic block and the second vinyl aromatic block contained in the block copolymer is taken as 100 mass% were calculated using the "content of the first vinyl aromatic block" in the above formula (B4) and the "content of the second vinyl aromatic block" in the above formula (B5), respectively. Ratio of the first vinyl aromatic block = mass of the first vinyl aromatic block / (mass of the first vinyl aromatic block + mass of the second vinyl aromatic block) x 100 [mass %]

[0071] <Loss tangent value measurement> The loss tangent value (tan δ) of the block copolymer was measured by a dynamic viscoelasticity measurement method according to the following procedure. (1) Using pellets of the block copolymer, a molded product 4 mm thick and 10 mm wide was produced by injection molding. Test pieces of appropriate size were cut out from this molded product and stored in a room at 23°C and 50% RH for 48 hours for aging treatment. (2) Using a dynamic viscoelasticity measuring device RSAIII manufactured by TA Instruments, the storage modulus (E') and loss modulus (E") were measured in the temperature range of -120 to 120°C in accordance with ISO6721-1 at a heating rate of 4°C / min, a measurement frequency of 1 Hz, a strain of 0.02%, and a fixed three-point bending mode, and tan δ in the above temperature range was calculated using the following formula. tan δ=E" / E'

[0072] <Tensile elongation> In accordance with JIS K 7161, the pellets were used to injection-molde a dumbbell-shaped molded piece, and the nominal tensile strain at break was measured at a tensile speed of 50 mm / min using a Shimadzu Autograph AG-Xplus, which was used as the tensile elongation value.

[0073] <Fisheye level> The occurrence of gel foreign matter in the block copolymer was evaluated as the fisheye level. The fisheye level was evaluated by forming pellets of each block copolymer into an unstretched sheet of about 50 μm in thickness using a sheet extruder equipped with a T-die, and stretching the sheet to a length of 3.3 m. 2 The number of foreign objects of 0.2 mm or more present in the sheet was counted by an image recognition device and evaluated. A number of 300 or more foreign objects was judged as "bad", 50 to less than 300 foreign objects was judged as "passable", and less than 50 foreign objects was judged as "good". The evaluation results of each example and comparative example are shown in Table 1. Note that, for Comparative Example 2, although an unstretched sheet was produced, the molding process was difficult and there was a problem with moldability.

[0074] [Table 1]

[0075] [Preparation of heat-shrinkable film] The heat shrinkable film was produced by dry blending 50% by mass of pellets of block copolymers P1 to P8 with 50% by mass of the resin composition (DP) described in Example 4 of Japanese Patent No. 6000939, and melt-kneading the mixture at 200° C. using a single-screw extruder. As Comparative Example 9, a heat shrinkable film was also produced using only DP pellets.

[0076] A biaxial stretching device using a T-die method was used to prepare heat-shrinkable films for various measurements and evaluations. The pellets of the block copolymer composition were extruded into a sheet having a thickness of about 0.3 mm at a temperature of 210° C. using a sheet extruder equipped with a T-die, and stretched 1.1 times in the machine direction (MD) at 85° C. using a longitudinal stretching machine at a line speed of 10 m / min, and then stretched 4.5 times in the direction perpendicular to the machine direction (TD) at 95° C. using a transverse stretching machine to prepare heat-shrinkable films having an average thickness of about 50 μm, which were designated as Examples 5 to 8 and Comparative Examples 5 to 9. In Comparative Example 2, an attempt was made to mold the pellets of the block copolymer P6 into a film, but molding was not possible.

[0077] The heat-shrinkable films thus produced were analyzed and evaluated as follows. <Measurement of heat shrinkage rate> The heat shrinkage of the film was measured by the following method. (1) A test piece having an MD width of 100 mm and a TD width of 100 mm was cut out from a heat-shrinkable film. (2) The test piece was completely immersed in warm water at 80°C or 100°C for 10 seconds, then taken out and thoroughly wiped to remove the water, and the length L (mm) of TD was measured. (3) The thermal shrinkage rate was calculated using the following formula. Heat shrinkage rate (%) = {(100-L) / 100} x 100

[0078] <Measurement of tensile elongation> The tensile elongation of the film was measured by the following method. (1) A rectangular sample piece having an MD width of 200 mm and a TD width of 10 mm was cut out from a heat-shrinkable film. (2) Using a Tensilon universal material testing machine manufactured by Orientec Co., Ltd., the cut-out sample pieces were tensioned in the MD at a measurement temperature of 23°C and a tensile speed of 200 mm / min to measure the tensile elongation.

[0079] <Measurement of natural shrinkage rate> The natural shrinkage rate of the heat shrinkable film was measured by the following method. (1) A sample piece having an MD width of 100 mm and a TD width of 350 mm was cut out from a heat-shrinkable film. (2) A mark was drawn in the center of the test piece so that the TD mark interval was 300 mm, and the test piece was stored in an environmental tester at 40°C. After storage for 7 days, the mark interval N (mm) was measured. (3) The natural shrinkage rate was measured using the following formula. Natural shrinkage rate (%) = {(300-N) / 300} x 100

[0080] <Measurement of impact strength> The impact strength of the heat shrinkable film was measured using an impact tester (manufactured by Tester Sangyo Co., Ltd.) with an R25 tip in accordance with ASTM D3420.

[0081] <Fisheye level> The fisheye level of the heat shrinkable film was measured by cutting out 22 pieces of film, each 50 cm long in the MD direction and 30 cm long in the TD direction, from the stretched film, and visually counting the number of fisheyes with a major axis of 0.2 mm or more using a magnifying glass with a scale. 2 A sample with 300 or more fish eyes per unit was judged as "bad," between 50 and 300 as "passable," and less than 50 as "good."

[0082] [Table 2]

Claims

1. A block copolymer having a first vinyl aromatic block (S1), a second vinyl aromatic block (S2), and a copolymer block (B / S), The first vinyl aromatic block (S1) is Consisting essentially of vinyl aromatic monomer units, The second vinyl aromatic block (S2) is Consisting essentially of vinyl aromatic monomer units, a weight average molecular weight equal to or less than that of the first vinyl aromatic block; The copolymer block (B / S) is Consisting essentially of vinyl aromatic monomer units and conjugated diene monomer units, The content of the conjugated diene monomer unit in the copolymer block is 55% by mass or more and 82% by mass or less, a ratio of the first vinyl aromatic block is 50% by mass or more and 85% by mass or less, when the total mass of the first vinyl aromatic block and the second vinyl aromatic block is 100% by mass, the content of the copolymer block in the block copolymer is 40% by mass or more and 60% by mass or less, When the total mass of the vinyl aromatic monomer units and the conjugated diene monomer units in the block copolymer is taken as 100 mass%, the ratio of the vinyl aromatic monomer units in the block copolymer is 64 mass% or more and 75 mass% or less, The first vinyl aromatic block (S1) has a weight average molecular weight of 30,000 or more and 100,000 or less, In accordance with ISO 6721-1, when dynamic viscoelasticity is measured under conditions of a heating rate of 4°C / min, a frequency of 1 Hz, and a strain of 0.02%, the loss tangent value (tan δ) has at least one peak in the range of -70°C to -35°C. Block copolymers (excluding block copolymers in which the half-value width of the molecular weight distribution curve of the vinyl aromatic block is 3.1 to 4.5).

2. The block copolymer according to claim 1 , wherein the copolymer block (B / S) is a random copolymer block of vinyl aromatic monomer units and conjugated diene monomer units.

3. 3. The block copolymer according to claim 1 or 2, which is linear and has a polymer block arrangement of (S1)-(B / S)-(S2) or (S2)-(B / S)-(S1).

4. A composition comprising the block copolymer according to any one of claims 1 to 3, and further comprising a polymer different from the block copolymer.

5. The composition according to claim 4 , wherein the content of the block copolymer is 15% by mass or more and 85% by mass or less.

6. A heat shrinkable film comprising a layer formed from the composition according to claim 4 or 5.

7. A sheet comprising a layer formed from the composition according to claim 4 or 5.

8. A molded product obtained by molding the sheet according to claim 7.

Citation Information

Patent Citations

  • Block copolymer, block copolymer composition and heat shrinkable film therefrom

    JP1999158241A

  • Styrenic resin composition, and sheet as well as embossed carrier tape comprised of the same

    JP2010174166A

  • Heat-shrinkable film

    JP2010235666A

  • Modified block copolymer and composition of the same

    JP2011094073A