Rubber composition for undertread
A rubber composition for undertreads using isoprene and modified butadiene/styrene-butadiene rubbers with large particle size silica and carbon black achieves balanced handling stability, high-speed durability, and low heat generation, addressing the limitations of existing undertread compositions.
Patent Information
- Application Number
- JP2023057959
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-09
- Estimated Expiration
- 2043-03-31
AI Technical Summary
Existing rubber compositions for undertreads in tires face challenges in achieving a balance between handling stability, high-speed durability, and low heat generation, with methods like increasing the vulcanizing agent or reducing filler amounts compromising elongation at break and durability.
A rubber composition for undertreads comprising 40% to 90% isoprene rubber and 10% to 40% modified butadiene rubber or modified styrene-butadiene rubber, blended with silica having a CTAB adsorption specific surface area of 60 m²/g to 100 m²/g, and optionally carbon black, along with a silane coupling agent, to enhance low heat generation, handling stability, and durability.
The composition improves handling stability and high-speed durability while maintaining low heat generation, with balanced performance achieved through the specific blend of rubbers and fillers, enhancing tire performance under high-speed conditions.
Smart Images

Figure 0007564471000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an undertread rubber composition intended primarily for use in the undertread layer of a tire. [Background technology]
[0002] In pneumatic tires, there is a demand for improving fuel efficiency during driving in order to reduce the environmental load. For this reason, efforts have been made to suppress heat generation in rubber compositions constituting various parts of pneumatic tires. In recent years, in order to further improve fuel efficiency, for example, studies have been made on suppressing heat generation in rubber compositions constituting the undertread rubber layer of pneumatic tires (rubber compositions for undertread).
[0003] As an index of heat generation of a rubber composition, tan δ at 60°C (hereinafter referred to as "tan δ(60°C)") measured by dynamic viscoelasticity measurement is generally used, and the smaller the tan δ(60°C) of the rubber composition, the smaller the heat generation. Methods for decreasing the tan δ(60°C) of the rubber composition include, for example, increasing the amount of vulcanizing agent or decreasing the amount of filler such as carbon black (see, for example, Patent Document 1). However, these methods cannot sufficiently secure the breaking elongation required for the rubber composition for undertread, and there is a risk that the steering stability and high-speed durability of the tire are not necessarily sufficient. Therefore, further measures are required for improving the steering stability and high-speed durability while securing good low heat generation (tan δ(60°C)) in the rubber composition for undertread. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2013-177113 A Summary of the Invention [Problem to be solved by the invention]
[0005] An object of the present invention is to provide a rubber composition for undertread which improves steering stability and high-speed durability while ensuring good low heat build-up properties, thereby enabling these performance properties to be simultaneously achieved in a well-balanced manner to a high degree. [Means for solving the problem]
[0006] The rubber composition for undertread of the present invention, which achieves the above object, has a CTAB adsorption specific surface area of 60 m for 100 parts by mass of a rubber component containing 40% by mass to 90% by mass of isoprene-based rubber and 10% by mass to 40% by mass of modified butadiene rubber and / or modified styrene butadiene. 2 / g~100m 2 / g of silica 25 It is characterized in that it is blended in an amount of 10 to 60 parts by mass. Effect of the Invention
[0007] The rubber composition for undertread of the present invention, which is made up of the above-mentioned blending, can improve the driving stability and high-speed durability while ensuring good low heat generation properties. Specifically, by using an isoprene-based rubber and a modified butadiene rubber and / or a modified styrene butadiene rubber in the above-mentioned blending ratio as the rubber component, it is possible to improve the low heat generation properties and high-speed durability in a well-balanced manner. In addition, by adding large particle size silica (CTAB adsorption specific surface area of 60 m to this rubber component, 2 / g~100m 2 The combination of these two properties ensures good low heat generation while improving handling stability and high-speed durability, achieving a good balance between these performance characteristics.
[0008] In the present invention, the CTAB adsorption specific surface area is 40 m per 100 parts by mass of the rubber component. 2 / g~120m 2It is preferable that 20 to 70 parts by mass of carbon black having a particle size of 1 / g is blended. In addition to the large particle size silica described above, by blending an appropriate amount of carbon black having a specific particle size as a filler, the processability (rubber cohesion, adhesion to other materials, etc.) can be improved.
[0009] In the present invention, the glass transition temperature of the modified butadiene rubber is preferably −85° C. or lower. In addition, the cis-1,4 bond content of the modified butadiene rubber is preferably 95% or higher. By using a modified butadiene rubber that satisfies these specific conditions, the effect of improving the low heat buildup and high-speed durability described above can be enhanced, which is advantageous for improving the steering stability and high-speed durability while ensuring good low heat buildup.
[0010] In the present invention, a silane coupling agent can be blended, and in this case, the ratio of the blended amount of the silane coupling agent to the blended amount of silica is preferably 3.0% by mass to 10.0% by mass. This can improve the dispersion of silica, which is advantageous for improving low heat generation and high-speed durability.
[0011] The rubber composition for undertread of the present invention can be suitably used for the undertread layer of a tire. Specifically, a tire using the rubber composition for undertread of the present invention includes a tread portion extending in the tire circumferential direction to form an annular shape, a pair of sidewall portions arranged on both sides of the tread portion, and a pair of bead portions arranged on the tire radial inner side of these sidewall portions, and has at least one carcass layer mounted between the pair of bead portions and a plurality of belt layers arranged on the outer circumferential side of the carcass layer in the tread portion, and the tread portion is preferably constructed by laminating a cap tread layer constituting the tire tread surface and an undertread layer arranged on its inner circumferential side, and in such a tire, it is preferable that the undertread layer is constructed of the rubber composition for undertread of the present invention. In this way, a tire having an undertread layer made of the rubber composition for undertread of the present invention can improve steering stability and high-speed durability while ensuring good low heat generation due to the excellent physical properties of the rubber composition for undertread of the present invention.
[0012] At this time, the tensile stress M100 of the undertread rubber constituting the undertread layer at 100% elongation at 23°C UT [Unit: MPa] and the tensile stress M100 of the coating rubber that covers the belt cord in the belt layer at 100% elongation at 23°C B [Unit: MPa] Ratio to M100 UT / M100 B It is preferable that M100 is 0.4 to 1.0. By optimizing the relationship of the tensile stress (M100) between the undertread layer (undertread rubber) using the rubber composition for undertread of the present invention and the belt layer (belt coat rubber) disposed on the inner circumferential side thereof, it is advantageous to improve low heat build-up property and high-speed durability.
[0013] In the present invention, the "CTAB adsorption specific surface area" is measured in accordance with ISO 5794. The "glass transition temperature" can be measured as the midpoint temperature of the transition region from a thermogram obtained by differential scanning calorimetry (DSC) under conditions of a heating rate of 20°C / min. The "cis-1,4 bond content" is the proportion of cis-1,4-bonds among the cis-1,4-bonds, trans-1,4-bonds, and 1,2-vinyl bonds, which are the bonding modes of butadiene, and is measured by infrared spectroscopy (Hampton method). The "tensile stress at 100% elongation at 23°C" is a value measured in accordance with JIS K6251 using a No. 3 dumbbell test piece at a tensile speed of 500 mm / min and a temperature of 23°C. [Brief description of the drawings]
[0014] [Figure 1] 1 is a meridian cross-sectional view showing an example of a pneumatic tire using the rubber composition for an undertread of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] The configuration of the present invention will be described in detail below with reference to the accompanying drawings.
[0016] As shown in FIG. 1, a pneumatic tire in which the rubber composition for undertread of the present invention is used includes a tread portion 1, a pair of sidewall portions 2 arranged on both sides of the tread portion 1, and a pair of bead portions 3 arranged on the tire radially inner side of the sidewall portions 2. In FIG. 1, the symbol CL indicates the tire equator. Although not depicted in FIG. 1 because it is a meridian cross section, the tread portion 1, the sidewall portions 2, and the bead portions 3 each extend in the tire circumferential direction to form an annular shape, thereby forming a toroidal basic structure of a pneumatic tire. The following description using FIG. 1 is basically based on the meridian cross section shown in the figure, but each tire component extends in the tire circumferential direction to form an annular shape.
[0017] A carcass layer 4 is installed between a pair of left and right bead portions 3. This carcass layer 4 includes a plurality of reinforcing cords extending in the tire radial direction, and is folded back from the inner side to the outer side in the tire width direction around a bead core 5 arranged in each bead portion 3. A bead filler 6 is arranged on the outer periphery of the bead core 5, and this bead filler 6 is wrapped by the main body and the folded back portion of the carcass layer 4. Meanwhile, a plurality of belt layers 7 (two layers in FIG. 1) are embedded on the outer periphery side of the carcass layer 4 in the tread portion 1. Each belt layer 7 is formed by covering a plurality of reinforcing cords (belt cords) with a belt coat rubber. The plurality of reinforcing cords are arranged inclined with respect to the tire circumferential direction in each layer, and are arranged so that the reinforcing cords cross each other between the layers. In these belt layers 7, the inclination angle of the reinforcing cords (belt cords) with respect to the tire circumferential direction is set to a range of, for example, 10° to 40°. Furthermore, a belt reinforcing layer 8 (two layers: a full cover 8a covering the entire width of the belt layer 7 and an edge cover 8b locally covering the end portion of the belt layer 7) may be provided on the outer circumferential side of the belt layer 7. The belt reinforcing layer 8 includes organic fiber cords oriented in the tire circumferential direction. In the belt reinforcing layer 8, the organic fiber cords are set at an angle of, for example, 0° to 5° with respect to the tire circumferential direction.
[0018] A tread rubber layer 10 is disposed on the outer peripheral side of the carcass layer 4 in the tread portion 1, a side rubber layer 20 is disposed on the outer peripheral side (outside in the tire width direction) of the carcass layer 4 in the sidewall portion 2, and a rim cushion rubber layer 30 is disposed on the outer peripheral side (outside in the tire width direction) of the carcass layer 4 in the bead portion 3. The tread rubber layer 11 has a structure in which two types of rubber layers with different physical properties (a cap tread 11 that forms the tread surface of the tread portion 1 and an undertread 12 disposed on its inner peripheral side) are laminated in the tire radial direction.
[0019] The tire in which the rubber composition for undertread of the present invention is used is preferably a pneumatic tire (a tire filled with air, an inert gas such as nitrogen, or other gas) as described above, but may be a non-pneumatic tire. In the case of a non-pneumatic tire, the rubber composition for undertread of the present invention can be used in a rubber layer (a portion corresponding to the undertread layer 12 in a pneumatic tire) arranged on the inner periphery side of a portion that contacts the road surface (a portion corresponding to the cap tread layer 11 in a pneumatic tire). As long as the tread portion 1 (tread rubber layer 10) of the tire to which the present invention is applied is composed of the cap tread 11 and the undertread 12, the basic structure of the other portions is not limited to the above-mentioned structure.
[0020] In the rubber composition for undertread of the present invention, the rubber component is a diene rubber, and necessarily contains an isoprene rubber and a modified butadiene rubber and / or a modified styrene-butadiene rubber. The combined use of these rubbers is advantageous in improving low heat build-up while maintaining good elongation at break.
[0021] Examples of isoprene-based rubber include various natural rubbers, epoxidized natural rubbers, and various synthetic polyisoprene rubbers. Among these isoprene-based rubbers, natural rubbers are particularly suitable. The content of isoprene-based rubber is 40% by mass to 90% by mass, preferably 50% by mass to 90% by mass, and more preferably 60% by mass to 90% by mass, based on 100% by mass of the rubber component. By including such an amount of isoprene-based rubber (particularly natural rubber), it is possible to improve the elongation at break and low heat build-up properties in a well-balanced manner. If the amount of isoprene-based rubber is less than 40% by mass, the elongation at break decreases. If the amount of isoprene-based rubber is more than 90% by mass, the low heat build-up properties deteriorate.
[0022] In the rubber composition for undertread of the present invention, the rubber component contains the modified butadiene rubber and / or the modified styrene butadiene rubber described below together with the above-mentioned isoprene-based rubber. That is, the rubber composition for undertread of the present invention contains two kinds of rubber components, an isoprene-based rubber and a modified butadiene rubber, two kinds of rubber components, an isoprene-based rubber and a modified styrene butadiene rubber, or three kinds of rubber components, an isoprene-based rubber, a modified butadiene rubber, and a modified styrene butadiene rubber. In particular, it is preferable to use a combination of an isoprene-based rubber (natural rubber) and a modified butadiene rubber. In this case, the content (total) of the modified butadiene rubber and / or the modified styrene butadiene rubber is 10% by mass to 40% by mass, preferably 15% by mass to 35% by mass, and more preferably 20% by mass to 35% by mass, based on 100% by mass of the rubber component. By containing such an amount of the modified butadiene rubber and / or the modified styrene butadiene rubber, the hardness and the low heat generation property can be improved in a well-balanced manner. That is, by suppressing the heat generation of the rubber composition for undertread and maintaining high hardness, it is possible to suppress the rising of the belt during high-speed running in a tire, which is advantageous in improving durability against belt separation in particular. If the amount of modified butadiene rubber and / or modified styrene butadiene rubber is less than 10% by mass, the low heat generation property is deteriorated. If the amount of modified butadiene rubber and / or modified styrene butadiene rubber is more than 90% by mass, the elongation at break is reduced. When modified butadiene rubber and modified styrene butadiene rubber are contained, the individual contents are not particularly limited, but it is preferable that the modified butadiene rubber is contained in 100% by mass of the rubber component at 10% by mass to 35% by mass and the modified styrene butadiene rubber is contained in 100% by mass of the rubber component at 10% by mass to 35% by mass.
[0023] The modified butadiene rubber is a butadiene rubber modified at both or one of the molecular ends with a functional group having a heteroatom and reactive with the silanol group on the silica surface. Examples of the heteroatom include oxygen, nitrogen, silicon, and sulfur, and among these, nitrogen or silicon is preferred. Examples of such functional groups include at least one selected from polyorganosiloxane groups, hydroxyl group-containing polyorganosiloxane structures, alkoxysilyl groups, hydroxyl groups, aldehyde groups, carboxyl groups, amino groups, imino groups, epoxy groups, amide groups, thiol groups, and ether groups. Among these, polyorganosiloxane groups, hydroxyl group-containing polyorganosiloxane structures, alkoxysilyl groups, hydroxyl groups, and amino groups are preferred. In addition, a combination of a plurality of these functional groups (for example, two types of amino groups and alkoxysilyl groups) may be used. By using such modified butadiene rubber, the affinity with the large particle size silica described below is improved, which is advantageous for improving the breaking elongation and low heat generation in a well-balanced manner.
[0024] The modified butadiene rubber that can be suitably used has a glass transition temperature Tg of preferably -85°C or lower, more preferably -110°C to -90°C. By having such a glass transition temperature, it is possible to improve the breaking strength and breaking elongation. If the glass transition temperature Tg of the modified butadiene rubber exceeds -85°C, the effect of improving the breaking elongation and low heat build-up cannot be expected to be sufficient.
[0025] The modified butadiene rubber preferably has a cis-1,4 bond content of 95% or more, more preferably 96% to 99%. A high cis-1,4 bond content is advantageous for improving the breaking strength and breaking elongation. If the cis-1,4 bond content is less than 95%, the breaking strength and breaking elongation decrease. The cis-1,4 bond content of the butadiene rubber can be increased or decreased by a normal method such as a catalyst.
[0026] The molecular weight distribution (Mw / Mn) calculated from the weight average molecular weight (Mw) and number average molecular weight (Mn) of the modified butadiene rubber is preferably 1.5 to 3.5, more preferably 2.0 to 3.3. In this way, by optimizing the molecular weight distribution of the modified butadiene rubber, the rubber properties become better, and the steering stability and high-speed durability of the tire when made into a tire can be effectively improved while maintaining the low heat generation property. If the molecular weight distribution (Mw / Mn) of the modified butadiene rubber is less than 1.5, the extrusion processability decreases. If the molecular weight distribution (Mw / Mn) of the modified butadiene rubber is more than 3.5, the low heat generation property decreases. The "weight average molecular weight Mw" and "number average molecular weight Mn" are measured by gel permeation chromatography (GPC) in terms of standard polystyrene.
[0027] The modified butadiene rubber is preferably a butadiene rubber (Nd-BR) synthesized with a neodymium catalyst modified with the above-mentioned functional group. Although the desired effect can be obtained by using butadiene rubber polymerized with other catalysts (e.g., nickel, cobalt, titanium, etc.), Nd-BR is preferably used from the viewpoint of achieving both low heat generation, breaking strength, and breaking elongation. Note that butadiene rubber polymerized with a neodymium catalyst (Nd-BR) is a known material, and is butadiene rubber polymerized with a neodymium catalyst such as simple neodymium, a compound of neodymium and other metals, or an organic neodymium compound. These butadiene rubbers synthesized with neodymium catalysts have the characteristics of a high molecular weight and a sharp molecular weight distribution. As the Nd-BR, a commercially available product can be used.
[0028] The modified styrene butadiene rubber is a styrene butadiene rubber in which both or one of the molecular ends are modified with a functional group having a heteroatom and reactive with the silanol group on the silica surface. Examples of the heteroatom include oxygen, nitrogen, silicon, and sulfur, and among these, nitrogen or silicon is preferred. Examples of such functional groups include at least one selected from a polyorganosiloxane group, a hydroxyl group-containing polyorganosiloxane structure, an alkoxysilyl group, a hydroxyl group, an aldehyde group, a carboxyl group, an amino group, an imino group, an epoxy group, an amide group, a thiol group, and an ether group. Among these, a polyorganosiloxane group, a hydroxyl group-containing polyorganosiloxane structure, an alkoxysilyl group, a hydroxyl group, and an amino group are preferred. In addition, a combination of a plurality of these functional groups (for example, two types of amino groups and alkoxysilyl groups) may be used. By using such a modified butadiene rubber, the affinity with the large particle size silica described below is improved, which is advantageous for improving the breaking elongation and low heat generation in a well-balanced manner.
[0029] The modified styrene butadiene rubber preferably has a glass transition temperature Tg of -75°C to -45°C, more preferably -75°C to -55°C. The modified styrene butadiene rubber has such a glass transition temperature, which can improve the low heat generation property. If the glass transition temperature Tg of the modified styrene butadiene rubber is less than -75°C, the effect of improving the breaking strength cannot be expected sufficiently. If the glass transition temperature Tg of the modified styrene butadiene rubber is more than -45°C, the effect of further improving the low heat generation property cannot be expected sufficiently.
[0030] The styrene content of the modified styrene butadiene rubber used in the present invention is preferably 5% by mass to 25% by mass, more preferably 5% by mass to 20% by mass. The vinyl content of the modified styrene butadiene rubber is preferably 15% by mass to 50% by mass, more preferably 20% by mass to 45% by mass. In this way, the reaction rate of silica and silane is improved by the moderate range of the styrene content and vinyl content, and the low heat generation property can be improved. If the styrene content of the modified styrene butadiene rubber is less than 5% by mass, the effect of improving the breaking strength cannot be expected sufficiently. If the styrene content of the modified styrene butadiene rubber is more than 25% by mass, the effect of improving the low heat generation property cannot be expected sufficiently. If the vinyl content of the modified styrene butadiene rubber is less than 15% by mass, the effect of improving the low heat generation property cannot be expected sufficiently. If the vinyl content of the modified styrene butadiene rubber is more than 50% by mass, the effect of improving the breaking elongation cannot be expected sufficiently. The styrene content and vinyl content of the modified styrene butadiene rubber are measured by infrared spectroscopy (Hampton method). The styrene content and vinyl content in the styrene-butadiene rubber can be appropriately adjusted by a usual method such as using a catalyst.
[0031] The rubber component constituting the rubber composition for undertread of the present invention includes at least the above-mentioned isoprene-based rubber (particularly natural rubber), modified butadiene rubber, and modified styrene butadiene rubber, but may optionally contain other diene-based rubbers. As the other diene-based rubbers, rubbers that can be generally used in rubber compositions for tires can be used. For example, unmodified butadiene rubber, unmodified styrene butadiene rubber, etc. can be exemplified. In addition, when natural rubber is adopted as the isoprene-based rubber, isoprene rubber can also be used in combination as the other diene-based rubber. These other diene-based rubbers can be used alone or as an arbitrary blend.
[0032] In the present invention, silica is necessarily blended as a filler with the above-mentioned rubber component. As the silica used in the present invention, for example, silica usually used in rubber compositions for tires, such as wet process silica, dry process silica, or surface-treated silica, can be used. However, the CTAB adsorption specific surface area of silica is 60 m 2 / g~100m 2 / g, preferably 70m 2 / g~90m 2 / g, more preferably 75m 2 / g~85m 2 / g. By using silica with such a large particle size, it is possible to improve low heat generation and wear resistance. 2 If the CTAB adsorption specific surface area of silica is less than 100 m 2 If the silica satisfies the above-mentioned conditions, it may be appropriately selected from commercially available products and used, or silica obtained by a conventional manufacturing method may be used.
[0033] The amount of silica to be blended is 3 to 60 parts by mass, preferably 5 to 50 parts by mass, and more preferably 10 to 50 parts by mass, per 100 parts by mass of the rubber component. By blending an appropriate amount of silica in this manner, it is possible to improve the low heat build-up properties, steering stability, and high-speed durability of a tire in a well-balanced manner. If the amount of silica blended is less than 3 parts by mass, the elongation at break decreases. If the amount of silica blended exceeds 60 parts by mass, the low heat build-up properties deteriorate.
[0034] In the present invention, in addition to the above-mentioned silica, carbon black can also be blended as a filler. The carbon black used in the present invention is preferably a carbon black having a CTAB adsorption specific surface area of 40 m among the carbon blacks usually used in rubber compositions for tires. 2 / g~120m 2 / g, more preferably 70m 2 / g~100m 2 / g. Using such carbon black is advantageous in improving the balance of low heat generation, driving stability, and high-speed durability when made into a tire. The CTAB adsorption specific surface area of carbon black is 40 m 2 If the CTAB adsorption specific surface area of carbon black is less than 120 m 2 If it exceeds 1 / g, the low heat build-up property deteriorates.
[0035] When carbon black is used in addition to silica as described above, the total amount of silica and carbon black is preferably 40 to 95 parts by mass, more preferably 45 to 90 parts by mass, per 100 parts by mass of the rubber component. By mixing an appropriate amount of silica and carbon black in this way, it is advantageous to improve low heat build-up, steering stability, and high-speed durability in a well-balanced manner when the tire is made. If the total amount of silica and carbon black is less than 40 parts by mass, the breaking strength decreases and the high-speed durability deteriorates. If the total amount of silica and carbon black is more than 95 parts by mass, fuel efficiency deteriorates and the breaking elongation decreases.
[0036] Furthermore, when silica and carbon black are used in combination, the ratio Ms / Mc of the amount of silica to the amount of carbon black, Mc, is preferably 0.05 to 0.7, more preferably 0.1 to 0.6. In this way, by blending silica and carbon black in a suitable balance, and particularly by keeping the amount of silica in the filler low, it is possible to suppress the deterioration of tan δ(60°C) caused by blending large particle size silica, and to improve the elongation at break and low heat build-up in a well-balanced manner. If the ratio Ms / Mc of the amount of silica to the amount of carbon black exceeds 0.7, the processability (rubber cohesion, adhesion to other components, etc.) will deteriorate.
[0037] The rubber composition of the present invention may contain fillers other than silica and carbon black, such as clay, talc, calcium carbonate, mica, aluminum hydroxide, and other materials that are generally used in rubber compositions for tires.
[0038] In the rubber composition for undertread of the present invention, a silane coupling agent may be added when compounding the silica. By compounding the silane coupling agent, the dispersibility of the silica in the rubber component (diene rubber) can be improved. Examples of the silane coupling agent include bis-(3-triethoxysilylpropyl) tetrasulfide, bis(3-triethoxysilylpropyl) disulfide, 3-trimethoxysilylpropyl benzothiazole tetrasulfide, γ-mercaptopropyl triethoxysilane, and 3-octanoylthiopropyl triethoxysilane. Among these, those having a tetrasulfide bond in the molecule can be preferably used. The compounding amount of the silane coupling agent is preferably 3.0 mass% to 10.0 mass%, more preferably 4.0 mass% to 9.0 mass%, based on the compounding amount of the silica. If the compounding amount of the silane coupling agent is less than 3.0 mass% of the compounding amount of the silica, the compounding amount is so small that the effect of compounding the silane coupling agent cannot be expected sufficiently. If the amount of the silane coupling agent exceeds 10 mass % of the amount of silica, the silane coupling agents will condense with each other, making it difficult to obtain the desired hardness and strength in the rubber composition.
[0039] Other compounding agents than those mentioned above can be added to the rubber composition for undertread of the present invention. Examples of other compounding agents include various compounding agents generally used in rubber compositions for tires, such as vulcanizing or crosslinking agents, vulcanization accelerators, antiaging agents, and liquid polymers. The compounding amounts of these compounding agents can be conventional general compounding amounts as long as they do not go against the object of the present invention. In addition, as the kneading machine, a normal rubber kneading machine, such as a Banbury mixer, a kneader, or a roll, can be used.
[0040] The rubber composition for undertread of the present invention can be suitably used in the undertread layer of a tire as described above, and a tire having an undertread layer made of the rubber composition for undertread of the present invention can improve the driving stability and high-speed durability while ensuring good low heat generation due to the excellent physical properties of the rubber composition for undertread of the present invention. When the rubber composition for undertread of the present invention is used in a tire, the tensile stress M100 at 100% elongation at 23°C of the undertread rubber constituting the undertread layer (i.e., the vulcanizate of the rubber composition for undertread of the present invention) is 0.01 to 0.01 mm. UT [Unit: MPa] and the tensile stress M100 at 100% elongation at 23°C of the coating rubber covering the belt cord in the belt layer 7 B [Unit: MPa] Ratio to M100 UT / M100 B is preferably 0.4 to 1.0, and more preferably 0.5 to 0.9. By optimizing the relationship of the tensile stress (M100) between the undertread layer using the rubber composition for undertread of the present invention and the belt layer 7 (coat rubber) arranged on the inner peripheral side thereof, it is advantageous to improve the driving stability and high-speed durability while ensuring low heat buildup. The ratio M100 UT / M100 B If the ratio is less than 0.4, the effects of improving low heat generation, steering stability, and high-speed durability are limited. UT / M100 B If it exceeds 1.0, the effects of improving low heat generation, driving stability, and high-speed durability will be limited.
[0041] The present invention will be further described below with reference to examples, but the scope of the present invention is not limited to these examples. EXAMPLES
[0042] The tire size is 245 / 45R18, and has the basic structure shown in FIG. 1. The compounding of the rubber composition for the undertread and the tensile stress (M100) at 100% elongation at 23°C of the undertread rubber and the belt coat rubber areUT , M100 B ) and its ratio M100 UT / M100 B Tires (test tires) of Standard Example 1, Comparative Examples 1 to 7, and Examples 1 to 10, each of which had the values shown in Tables 1 and 2, were manufactured.
[0043] Regarding the compounding of the rubber composition for undertread, the compounding common to all the examples is summarized in Table 3. The type of belt coat rubber used in each example is also listed in Tables 1 and 2. The type of belt coat rubber is listed with the number of coat rubber A to B listed in Table 4, and the compounding of these coat rubbers A to B is as shown in Table 4.
[0044] The tensile stress (M100 UT , M100 B ) is the value (unit: MPa) measured using undertread rubber and coat rubber, using a No. 3 dumbbell test piece prepared in accordance with JIS K6251, at a tensile speed of 500 mm / min and a temperature of 23°C.
[0045] Using each test tire, evaluations of steering stability, low rolling resistance, and high-speed durability were carried out by the methods described below.
[0046] Steering stability Each test tire was mounted on a wheel with a rim size of 18x7J, the air pressure was set to 240kPa, and the tire was mounted on a test vehicle with an engine displacement of 2000cc. The test driver performed a sensory evaluation of the handling stability on a test course consisting of a paved road surface. The evaluation results were evaluated on a 5-point scale, with the result of Standard Example 1 being 3 points (standard). The higher the score, the better the handling stability.
[0047] Low rolling resistance Each test tire was mounted on a wheel with a rim size of 18x7J, and the rolling resistance was measured using an indoor drum test machine (drum diameter: 1707.6mm) in accordance with ISO28580 under conditions of air pressure of 210kPa, load of 4.82kN, and speed of 80km / h. The evaluation results were expressed as an index using the reciprocal of the measured value, with standard example 1 being 100. The higher the index value, the lower the rolling resistance and the better the low rolling resistance.
[0048] Belt separator durability Each test tire was mounted on a wheel with a rim size of 18×7J, and stored for 7 days under conditions of 70°C with an internal pressure of 350 kPa and oxygen sealed in. The test tire thus pretreated was inflated to an air pressure of 230 kPa, mounted on an indoor drum tester (drum diameter: 1707.6 mm), and a running test was performed in which the tire was run for 12 hours and 30 km at a speed of 100 km / h under a load of 88% of the JATMA maximum load capacity. After running, the tire was cut open and the separation length in the width direction at the end of the belt width direction was measured. The evaluation results were expressed as an index using the reciprocal of the measured value, with the value of standard example 1 being 100. The larger the index value, the smaller the separation length and the better the durability against belt edge separation.
[0049] [Table 1]
[0050] [Table 2]
[0051] [Table 3]
[0052] The types of raw materials used in Tables 1 to 3 are shown below. NR: Natural rubber, TSR20 BR1: Nipol 1220 manufactured by Zeon Corporation (unmodified butadiene rubber synthesized using a cobalt catalyst, glass transition temperature Tg = -105°C, cis-1,4 bond content: 98 mol%) BR2: Nipol 1250H manufactured by Zeon Corporation (modified butadiene rubber synthesized using a lithium catalyst, modified group: N-methylpyrrolidone, glass transition temperature Tg = -93°C, cis-1,4 bond content: 35 mol%) BR3: ENEOS BR511 manufactured by JSR Corporation (modified butadiene rubber synthesized using a neodymium catalyst, glass transition temperature Tg = -78°C, cis-1,4 bond content: 25 mol%) BR4: ENEOS BR54 manufactured by JSR Corporation (modified butadiene rubber synthesized using a neodymium catalyst, glass transition temperature Tg = -107°C, modifying group: hydrocarbyloxysilane compound, cis-1,4 bond content: 96 mol%) SBR: JSR ENEOS HPR940 CB1: Carbon black (grade: ISAF), manufactured by Tokai Carbon Co., Ltd., SEAT 6 (CTAB adsorption specific surface area: 109 m 2 / g) CB2: Carbon black (grade: HAF), manufactured by Tokai Carbon Co., Ltd., SEAT 3 (CTAB adsorption specific surface area: 82 m 2 / g) CB3: Carbon black (grade: FEF), manufactured by Tokai Carbon Co., Ltd., SEAT F (CTAB adsorption specific surface area: 47 m 2 / g) ·Silica 1: Evonik ULTRASIL VN3GR (CTAB adsorption specific surface area: 175m 2 / g) Silica 2: Solvay ZEOSIL 115GR (CTAB adsorption specific surface area: 115 m 2 / g) Silica 3: Solvay Zeosil 1185GR (CTAB adsorption specific surface area: 80 m 2 / g) Silane coupling agent: Si69 manufactured by Evonik Industries AG Tackifier: Hitachi Chemical's Hitanol 1502Z Zinc oxide: Three types of zinc oxide manufactured by Seido Chemical Industry Co., Ltd. · Anti-aging agent: PILFLEX 13 by NOCIL LIMITED Stearic acid: Stearic acid 50S manufactured by Nisshin Rika Co., Ltd. Sulfur: Shikoku Chemical Industry Co., Ltd., Myucron OT-20 Vulcanization accelerator: Sancerer NS-G manufactured by Sanshin Chemical Industry Co., Ltd.
[0053] [Table 4]
[0054] The types of raw materials used in Table 4 are shown below. NR: Natural rubber, natural rubber, RSS#3 CB: Carbon black (grade: HAF), Tokai Carbon Co., Ltd., Seast 300 Tackifier: Hitachi Chemical's Hitanol 1502Z Zinc oxide: Three types of zinc oxide manufactured by Seido Chemical Industry Co., Ltd. · Anti-aging agent: PILFLEX 13 by NOCIL LIMITED Cobalt stearate: Cobalt stearate manufactured by Airec Sulfur: Shikoku Chemical Industry Co., Ltd., Myucron OT-20 Vulcanization accelerator: Sancerer NS-G manufactured by Sanshin Chemical Industry Co., Ltd.
[0055] As is clear from Tables 1 and 2, Examples 1 to 10 improved the steering stability, low rolling resistance, and belt separator durability compared to Standard Example 1, and these performances were well balanced. On the other hand, in Comparative Example 1, the CTAB specific surface area of silica was large, so the steering stability and belt separator durability were deteriorated. In Comparative Example 2, the CTAB specific surface area of silica was large, so the steering stability and belt separator durability were deteriorated. In Comparative Example 3, unmodified butadiene rubber was used, so the belt separator durability was deteriorated. In Comparative Example 4, the blending amount of silica was small, so the belt separator durability was deteriorated. In Comparative Example 5, the blending amount of silica was large, so the steering stability and belt separator durability were deteriorated. In Comparative Example 6, the blending amount of isoprene-based rubber (natural rubber) was large and the blending amount of unmodified butadiene rubber was small, so the belt separator durability was deteriorated. In Comparative Example 7, the blending amount of isoprene-based rubber (natural rubber) was small and the blending amount of unmodified butadiene rubber was large, so the steering stability and belt separator durability were deteriorated.
[0056] The present disclosure includes the following inventions. Invention [1] A rubber component having a CTAB adsorption specific surface area of 60 m for 100 parts by mass of a rubber component containing 40% by mass to 90% by mass of isoprene-based rubber and 10% by mass to 40% by mass of modified butadiene rubber and / or modified styrene butadiene. 2 / g~100m 2 3 to 60 parts by mass of silica having a molecular weight of 100 / g are compounded in the rubber composition for undertread. Invention [2] The CTAB adsorption specific surface area is 40 m per 100 parts by mass of the rubber component. 2 / g~120m 2 The rubber composition for undertread according to the invention [1], characterized in that 20 parts by mass to 70 parts by mass of carbon black having a molecular weight of 1 / g are blended. Invention [3] The rubber composition for undertread according to invention [1] or [2], characterized in that the glass transition temperature of the modified butadiene rubber is -85°C or lower. Invention [4] The rubber composition for undertread according to any one of inventions [1] to [3], wherein the modified butadiene rubber has a cis-1,4 bond content of 95% or more. Invention [5] The rubber composition for undertread according to any one of inventions [1] to [4], characterized in that a silane coupling agent is blended therein, and the ratio of the blending amount of the silane coupling agent to the blending amount of the silica is 3.0% by mass to 10.0% by mass. Invention [6] A tire comprising a tread portion extending in a circumferential direction of the tire to form an annular shape, a pair of sidewall portions arranged on both sides of the tread portion, and a pair of bead portions arranged on the radially inner side of the sidewall portions, and the tire has at least one carcass layer mounted between the pair of bead portions and a plurality of belt layers arranged on the outer peripheral side of the carcass layer in the tread portion, the tread portion being constructed by laminating a cap tread layer constituting the tire tread surface and an undertread layer arranged on its inner peripheral side, wherein the undertread layer is constructed from the rubber composition for an undertread according to any one of inventions [1] to [5]. Invention [7] The tensile stress M100 of the undertread rubber constituting the undertread layer at 100% elongation at 23°C UT [Unit: MPa] and the tensile stress M100 at 100% elongation at 23°C of the coating rubber covering the belt cord in the belt layer B [Unit: MPa] Ratio to M100 UT / M100 B The tire according to the invention [6], wherein the ratio of the axial length of the tire to the radial length of the tire is 0.4 to 1.0. [Explanation of symbols]
[0057] 1 Tread section 2 Sidewall 3 Bead section 4 Carcass layer 5 Bead Core 6 Bead Filler 7 Belt layer 8 Belt cover layer 10 Tread rubber layer 11 Cap tread layer 12 Undertread layer 20 Side rubber layer 30 Rim cushion rubber layer CL Tire Equator
Claims
1. A rubber component having a CTAB adsorption specific surface area of 60 m for 100 parts by mass of a rubber component containing 40% by mass to 90% by mass of isoprene-based rubber and 10% by mass to 40% by mass of modified butadiene rubber and / or modified styrene butadiene. 2 / g to 100m 2 / g of silica is blended in an amount of 25 to 60 parts by mass.
2. A CTAB adsorption specific surface area of 40 m per 100 parts by mass of the rubber component. 2 / g ~ 120m 2 2. The rubber composition for undertread according to claim 1, characterized in that 20 to 70 parts by mass of carbon black having a viscosity of 1 / g is blended.
3. The rubber composition for undertread according to claim 1 or 2, characterized in that the glass transition temperature of the modified butadiene rubber is −85° C. or lower.
4. 3. The rubber composition for undertread according to claim 1, wherein the modified butadiene rubber has a cis-1,4 bond content of 95% or more.
5. 3. The rubber composition for undertread according to claim 1, further comprising a silane coupling agent, the ratio of the amount of the silane coupling agent to the amount of the silica being 3.0% by mass to 10.0% by mass.
6. 3. A tire comprising a tread portion extending in a circumferential direction of the tire to form an annular shape, a pair of sidewall portions arranged on both sides of the tread portion, and a pair of bead portions arranged on the radially inner side of the sidewall portions, the tire having at least one carcass layer mounted between the pair of bead portions, and a plurality of belt layers arranged on the outer peripheral side of the carcass layer in the tread portion, the tread portion being constructed by laminating a cap tread layer constituting a tire tread surface and an undertread layer arranged on its inner peripheral side, the undertread layer being constructed from the rubber composition for undertreads according to claim 1 or 2.
7. The tensile stress M100 of the undertread rubber constituting the undertread layer at 23° C. when elongated to 100% UT [Unit: MPa] and the tensile stress M100 at 100% elongation at 23°C of the coating rubber covering the belt cord in the belt layer B Ratio to M100 [unit: MPa] UT / M100 B 7. The tire according to claim 6, wherein the tread width is 0.4 to 1.0.
Citation Information
Patent Citations
Rubber composition for tire, and pneumatic tire
JP2012219224A
Pneumatic tire
JP2013177113A
JP2013‐177113A
Rubber composition for tire
JP2019026757A
Rubber composition for tread, and tire
JP2019151738A