Negative electrode active material for non-aqueous electrolyte secondary battery and method for producing same

A silicon oxide composite with controlled magnesium silicate and carbon coating addresses the volume instability of silicon-based electrodes, enhancing the stability and efficiency of non-aqueous electrolyte secondary batteries.

JP7564710B2Active Publication Date: 2024-10-09DAEJOO ELECTRONICS MATERIALS CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020530303
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-12-05
Filing Date
2018-12-05
Publication Date
2024-10-09
Estimated Expiration
2038-12-05

AI Technical Summary

Technical Problem

Conventional negative electrode active materials for non-aqueous electrolyte secondary batteries face issues with high volumetric expansion and contraction during lithium intercalation, leading to reduced life characteristics and capacity retention rates, particularly with silicon-based materials like Si, Sn, and Sb.

Method used

A silicon oxide composite is developed with a specific ratio of magnesium silicate (MgSiO3) and silicon oxide (SiOx) phases, dispersed in a silicon dioxide matrix, coated with carbon to enhance conductivity and stability, using a gas-phase reaction to prevent excessive volume change and improve cycle characteristics.

Benefits of technology

The composite material achieves stable charge/discharge capacity, improved initial efficiency, and enhanced cycle life by minimizing volume changes and facilitating reversible lithium reactions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007564710000004
    Figure 0007564710000004
  • Figure 0007564710000005
    Figure 0007564710000005
  • Figure 0007564710000006
    Figure 0007564710000006
Patent Text Reader

Abstract

The present invention provides a negative electrode active material for a non-aqueous electrolyte lithium secondary battery, which has improved charge and discharge capacities, initial charge and discharge efficiencies, and capacity retention rates. [Solution] The present invention relates to a negative electrode active material for a non-aqueous electrolyte secondary battery and a manufacturing method thereof, and more particularly to a negative electrode active material for a non-aqueous electrolyte secondary battery, which is obtained by reacting silicon, silicon dioxide, and magnesium through a gas-phase reaction and coating the surface with carbon to impart conductivity. This results in a structure that is stable against volume changes due to lithium absorption and desorption, as well as conductivity, and significantly improves life and capacity characteristics, and a manufacturing method thereof. [Selection diagram] Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a negative electrode active material for a non-aqueous electrolyte secondary battery and a method for manufacturing the same. More specifically, silicon, silicon dioxide and magnesium are reacted by a gas phase reaction to produce a silicon oxide composite, and carbon is coated on the surface to improve conductivity. Of course, it shows a stable structure against volume changes due to lithium intercalation and deintercalation, and shows an effect of greatly improving the life characteristics and capacity efficiency characteristics. The present invention relates to a negative electrode active material for a non-aqueous electrolyte secondary battery and a method for manufacturing the same.

Background Art

[0002] Lithium secondary batteries, which have recently been in the spotlight as power sources for portable small electronic devices and electric vehicles, exhibit a high energy density with a discharge voltage more than twice that of existing batteries using an alkaline aqueous solution by using an organic electrolyte solution.

[0003] As the positive electrode active material of the lithium secondary battery, oxides composed of transition metals having a structure capable of lithium intercalation such as LiCoO 2 , LiMn 2 O 4 , LiNi 1-x Co x O 2 (0 < x < 1) etc. are mainly used. As the negative electrode active material, various forms of carbon-based materials including artificial graphite, natural graphite, and hard carbon capable of lithium insertion and desorption have been applied.

[0004] Graphite is mainly used as the negative electrode material of the lithium secondary battery, but the capacity per unit mass of graphite is as small as 372 mAh / g, making it difficult to increase the capacity of the lithium secondary battery.

[0005] Metallic materials such as Si, Sn, Al, and Sb are being considered as new materials that can replace carbon-based negative electrode active materials. It is known that such metallic materials charge / discharge by alloying / de-alloying reactions with Li, and exhibit higher capacity than graphite, which is a commercial negative electrode active material (Patent Document 1).

[0006] However, metals such as Si, Sn, Al, and Sb undergo large volume expansion and contraction during the alloying / dealloying process with Li, which causes problems such as reduced life characteristics due to pulverization, loss of conductive paths, etc. In particular, Si is known to be an optimal material for a high-capacity anode material in terms of discharge capacity (4200mAh / g) and discharge voltage (0.4V), but the large volume expansion of up to about 400% induced when Li ions are inserted into the material (charging) causes the active material to degrade, resulting in a rapid decline in life characteristics.

[0007] Silicon oxide (SiO x ) has a capacity (approximately 1500mAh / g) that is several times higher than the capacity of carbon-based anodes (approximately 350mAh / g), which has a smaller capacity than silicon.It has a structure in which silicon nanocrystals are uniformly dispersed in a silicon dioxide matrix, and is attracting attention as a material with significantly improved volume expansion rate and lifespan (capacity retention rate) characteristics compared to other silicon-based materials.

[0008] However, in the case of silicon oxide, which has such excellent capacity and life characteristics, lithium reacts with silicon oxide during initial charging to produce lithium oxide (lithium oxide and lithium silicate, etc.), and the lithium oxide produced does not reversibly return to the positive electrode during discharge. On the other hand, silicon oxide (SiO x ) has a capacity (approximately 1500mAh / g) that is several times higher than the capacity of carbon-based anodes (approximately 350mAh / g), which has a smaller capacity than silicon.It has a structure in which silicon nanocrystals are uniformly dispersed in a silicon dioxide matrix, and is attracting attention as a material with significantly improved volume expansion rate and lifespan (capacity retention rate) characteristics compared to other silicon-based materials.

[0009] Conventionally, in order to improve the stability during the preparation of electrodes, SiO x A method of mixing and heating a silicon-silicon oxide composite with a magnesium compound has been proposed to improve the initial charge / discharge efficiency. x The powder was dissolved in magnesium hydrogen (MgH 2 ) or calcium hydride (CaH 2 A method for producing a magnesium- or calcium-containing silicon-silicon oxide composite by reacting SiO x Powder and MgH 2 or CaH 2 During the reaction, the amount of oxygen mixed in is reduced, but the size of the silicon crystals grows rapidly due to a localized exothermic reaction, and Mg or Ca is distributed unevenly, resulting in the formation of SiO x It was shown that the capacity retention rate decreased with increasing the temperature.

[0010] In order to solve the problems of the conventional technology, the present invention has conducted extensive research into a structure that is stable against volume changes due to lithium absorption and desorption as well as surface conductivity, and has found that the above problems can be solved by dispersing silicon microcrystals or particles in silicon dioxide through a gas phase reaction and coating at least a part of the surface with carbon to impart conductivity, thereby providing a stable, large-capacity charge / discharge capacity and greatly improving charge / discharge cycle characteristics and efficiency. [Prior art documents] [Patent documents]

[0011] [Patent Document 1] Korean Patent Publication No. 10-2014-0042146 (Publication date: 2014.04.07) [Patent Document 2] Japanese Patent Publication No. 2012-033317 (Publication date: 2012.02.16) Summary of the Invention [Problem to be solved by the invention]

[0012] In order to solve the problems of the conventional negative electrode active material for secondary batteries as described above, an object of the present invention is to provide a negative electrode active material for a non-aqueous electrolyte lithium secondary battery with improved charge and discharge capacity, initial charge and discharge efficiency, and capacity retention rate.

[0013] Another object of the present invention is to provide a manufacturing method for manufacturing a negative electrode active material for a non-aqueous electrolyte secondary battery containing a silicon oxide composite.

[0014] Another object of the present invention is to provide a negative electrode containing the negative electrode active material for a non-aqueous electrolyte secondary battery containing the silicon oxide composite, and a non-aqueous electrolyte lithium secondary battery.

Means for Solving the Problems

[0015] In order to solve the problems of the prior art as described above, the present invention provides a negative electrode active material containing a silicon oxide composite containing silicon, silicon oxide (SiO x , 0 < x ≦ 2), and magnesium silicate, wherein the magnesium silicate contains MgSiO 3 , and in X-ray diffraction analysis, the intensity I si(111) of the diffraction peak by Si(111) detected at 2θ = 27.5° to 29.5° and the intensity I 3 of the diffraction peak by MgSiO MgSiO3(610) detected at 2θ = 30° to 32° have a ratio of 0.1 < I MgSiO3(610) / I Si(111) < 0.5. A negative electrode active material for a non-aqueous electrolyte secondary battery is provided. In the negative electrode active material containing the silicon oxide composite according to the present invention, the preferable ratio of the I Si(111) and I MgSiO3(610) may be 0.15 < I MgSiO3(610) / I Si(111) < 0.3.

[0016] The silicon oxide composite according to the present invention is MgSiO 3The silicon oxide composite according to the present invention is characterized in that it contains a magnesium silicate phase of the type at a certain portion or more. 3 The silicon particles can be homogeneously dispersed in a matrix containing MgSiO 3 Since it does not easily react with Li ions, when it is used as an electrode, it can improve the cycle characteristics and the initial charge and discharge efficiency by reducing the amount of expansion of the electrode when Li ions are absorbed.

[0017] The silicon oxide composite according to the present invention is MgSiO3(610) / I Si(111) By satisfying the range of 0.1 to 0.5, deterioration of battery characteristics due to the presence of magnesium silicate can be suppressed, and stable production, absorption and desorption of Li compounds can be facilitated. Also, the initial efficiency can be further improved.

[0018] The silicon oxide composite according to the present invention is MgSiO3(610) / I Si(111) When exceeds 0.5, MgSiO 3 Since an excessive amount of crystals of the type I is formed, the initial charge and discharge capacity becomes small, which is undesirable. MgSiO3(610) / I si(111) When is less than 0.1, MgSiO 3 The amount of magnesium silicate phase of SiO type is small, which reduces the effect of improving cycle characteristics during charge and discharge tests. The reason for the small initial charge and discharge capacity is that the SiO x The Si atoms, which are alloyed with the original Li atoms, react with the added Mg atoms, and the MgSiO 3 This may be due to excessive mold formation.

[0019] The silicon oxide composite according to the present invention is characterized in that, in X-ray diffraction analysis, a diffraction peak due to Si(111) is shown at 2θ=27.5° to 29.5°, and the size of the silicon crystallite calculated from the full width at half maximum (FWHM) of the diffraction peak is 2 nm to 100 nm.

[0020] In the silicon oxide composite of the present invention, the fine crystal grain size of silicon particles calculated by the Scherer's formula based on the spread of the diffraction line assigned to Si(111) centered around 2θ=27.5° to 29.5° in X-ray diffraction (Cu-Kα) using a copper counter electrode is preferably 2 to 100 nm, more preferably 2 to 50 nm, and even more preferably 2 to 30 nm.

[0021] In the negative electrode active material for a non-aqueous electrolyte secondary battery according to the present invention, the silicon oxide composite contains magnesium in a ratio of 2 to 30 parts by weight per 100 parts by weight of the total.

[0022] In the negative electrode active material for a non-aqueous electrolyte secondary battery according to the present invention, the magnesium silicate is 2 SiO 4 Magnesium silicate is an oxide having a more negative Gibbs free energy than silicon oxide thermodynamically, and may be preferable because it is amorphous and stably ions lithium and suppresses the occurrence of an initial irreversible reaction.

[0023] In the negative electrode active material for a non-aqueous electrolyte secondary battery according to the present invention, the magnesium silicate is represented by the general formula Mg x SiO y (0.5≦x≦2, 2.5≦y≦4). In the negative electrode active material for a non-aqueous electrolyte secondary battery according to the present invention, the magnesium silicate is MgSiO 3 It is preferable that the main component is MgSiO 3 When analyzing the X-ray diffraction pattern of enstatite crystals, peaks attributable to silicon crystals were observed within the diffraction angle range of 28°<2θ<29°, and peaks attributable to MgSiO 3 It is preferable that the peaks attributable to crystals are shown. 2 SiO 4 It is preferred that the crystals contain forsterite.

[0024] In the negative electrode active material for a non-aqueous electrolyte secondary battery according to the present invention, the silicon oxide complex is characterized in that the ratio of silicon atoms to oxygen atoms (Si / O) is 0.5 to 2.

[0025] In the negative electrode active material for a non-aqueous electrolyte secondary battery according to the present invention, the silicon oxide composite further comprises a coating layer containing carbon on a surface thereof. In the negative electrode active material for a non-aqueous electrolyte secondary battery according to the present invention, the coating layer is 2 to 20 parts by weight per total 100 parts by weight of the silicon oxide composite. In the negative electrode active material for a non-aqueous electrolyte secondary battery according to the present invention, if the coating amount of the carbon coating layer is 2 parts by weight or less, a sufficient conductivity improvement effect cannot be obtained, and if the coating amount is 20 parts by weight or more, the effect of improving conductivity due to an increase in the coating amount is not observed.

[0026] In the negative electrode active material for a non-aqueous electrolyte secondary battery according to the present invention, the average thickness of the carbon coating may be 1 nm to 2 μm, preferably 5 nm to 1 μm, and more preferably 10 nm to 0.8 μm. In the negative electrode active material for a non-aqueous electrolyte secondary battery according to the present invention, if the average thickness of the carbon coating is less than 1 nm, the conductivity cannot be improved, and if the average thickness exceeds 2 μm, the effect of improving the conductivity by adding the carbon material cannot be obtained.

[0027] In the negative electrode active material for a nonaqueous electrolyte secondary battery according to the present invention, the carbon-containing coating layer includes at least one selected from the group consisting of amorphous carbon, carbon nanofibers, carbon nanotubes, graphite, graphene, graphene oxide, and reduced graphene oxide.

[0028] In the negative electrode active material for a non-aqueous electrolyte secondary battery according to the present invention, the carbon-coated silicon composite may have an average particle size of 0.5 μm to 20 μm. The average particle size is determined by measuring the particle size distribution by a laser diffraction method using a weight average D 50(i.e., the particle size or median diameter when the cumulative weight is 50%). In the negative electrode active material for a nonaqueous electrolyte secondary battery according to the present invention, if the average particle size of the carbon-coated silicon composite is too small, the volume density becomes small and the charge / discharge capacity per unit volume decreases, whereas if the average particle size is too large, it is difficult to prepare an electrode film, and there is a risk of peeling off from the current collector.

[0029] In the negative electrode active material for a non-aqueous electrolyte secondary battery according to the present invention, the specific surface area of ​​the carbon-coated silicon composite is 1 to 40 m 2 In the negative electrode active material for a non-aqueous electrolyte secondary battery according to the present invention, the specific surface area of ​​the carbon-coated silicon composite is preferably 1 m 2 / g~20m 2 In the negative electrode active material for a non-aqueous electrolyte secondary battery according to the present invention, it is more preferable that the specific surface area of ​​the composite oxide is 1 m 2 If it is less than 40m / g, the charge / discharge characteristics are deteriorated, which is undesirable. 2 If it exceeds this value, the contact area with the electrolyte increases, promoting the decomposition reaction of the electrolyte and causing side reactions, which is undesirable.

[0030] The present invention also provides a negative electrode comprising a negative electrode active material comprising the silicon oxide composite according to the present invention.

[0031] The negative electrode according to the present invention is characterized in that it contains at least one selected from the group consisting of graphite, conductive carbon black, soft carbon, hard carbon, carbon nanofibers, carbon nanotubes, graphene, reduced graphene oxide, and graphene nanoflakes in a ratio of 30 wt% to 95 wt% based on the total weight of the negative electrode active material. That is, the negative electrode according to the present invention may further contain, in addition to the silicon oxide composite, a negative electrode material used in conventional negative electrodes, specifically, at least one selected from the group consisting of graphite, conductive carbon black, soft carbon, hard carbon, carbon nanofibers, carbon nanotubes, graphene, reduced graphene oxide, and graphene nanoflakes. The material contained in the negative electrode other than the silicon oxide composite according to the present invention is preferably contained in a ratio of 30 wt% to 95 wt% based on the total weight of the negative electrode active material.

[0032] The present invention also provides a non-aqueous electrolyte lithium secondary battery comprising the negative electrode active material for a non-aqueous electrolyte secondary battery according to the present invention.

[0033] The present invention also provides a method for preparing a negative electrode active material for a non-aqueous electrolyte secondary battery according to the present invention, comprising: a first step of feeding a mixture of silicon particles having an average particle size of 0.1 μm to 20 μm and silicon dioxide particles having an average particle size of 10 nm to 300 nm and magnesium having an average particle size of 1 mm to 100 mm into a reactor; a second step of adjusting the pressure of the reactor to 0.000001 torr to 1 torr; a third step of heating the mixture and the magnesium at 600° C. to 1600° C. to prepare a silicon oxide composite; a fourth step of cooling the silicon oxide composite and depositing it on a metal plate; and a fifth step of pulverizing and classifying the silicon oxide composite cooled and deposited on the metal plate to an average particle size of 0.5 μm to 15 μm.

[0034] The method for producing a negative electrode active material for a non-aqueous electrolyte secondary battery according to the present invention comprises the steps of: 2 The raw powder mixture and magnesium were heated together to form a Si / SiO 2The silicon composite is synthesized by a uniform gas-phase reaction between the raw material powder mixture and magnesium particles, which prevents the rapid growth of silicon due to an exothermic reaction caused by localized excessive mixing of magnesium, as occurs in conventional solid-phase reactions, and as a result, the capacity retention rate of the silicon oxide composite can be improved.

[0035] The negative electrode active material for a non-aqueous electrolyte secondary battery according to the present invention reacts in the vapor phase in this way, and therefore, Si, SiO 2 Because the silicon and magnesium phases are bonded at the atomic level, the volume change during absorption and release of Li-ions is small, and cracks are less likely to occur in the electrode active material due to repeated charging and discharging. Therefore, even with a large number of cycles, the capacity is less likely to decrease. Unlike existing materials, there is no sudden decrease in capacity over a small number of cycles, and the cycle characteristics are excellent. Because each phase of this silicon composite is bonded at the atomic level, Li-ions are easily released during discharge, and the charging and discharging of Li-ions are well balanced, resulting in high charge and discharge efficiency.

[0036] The method for preparing a negative electrode active material for a non-aqueous electrolyte secondary battery according to the present invention further comprises a sixth step of supplying the silicon oxide composite of the fifth step and a carbon source and reacting them at 600° C. to 1200° C. to form a coating layer containing carbon disposed on a surface of the silicon oxide composite.

[0037] In the method for producing a negative electrode active material for a non-aqueous electrolyte secondary battery according to the present invention, the silicon used as the raw material has an average particle size of 2 μm to 20 μm, and the silicon dioxide has an average particle size of 10 nm to 300 nm.

[0038] In the method for producing a negative electrode active material for a non-aqueous electrolyte secondary battery according to the present invention, the carbon source is at least one selected from the group consisting of methane, propane, butane, acetylene, benzene, and toluene.

[0039] The method for producing a negative electrode active material for a non-aqueous electrolyte secondary battery according to the present invention is characterized in that the silicon oxide composite and a carbon source are charged, and at least one selected from the group consisting of nitrogen, helium, argon, carbon dioxide gas, hydrogen and water vapor is further charged. Effect of the Invention

[0040] The negative electrode active material for a non-aqueous electrolyte secondary battery according to the present invention is prepared by reacting silicon, silicon dioxide and magnesium through a gas phase reaction, and coating the surface with carbon to impart electrical conductivity, thereby exhibiting a structure that is stable against volume changes due to the absorption and release of lithium, as well as electrical conductivity of a lithium secondary battery including the negative electrode active material for a non-aqueous electrolyte secondary battery according to the present invention, and improving life characteristics, charge and discharge capacity, initial charge and discharge efficiency, and capacity retention rate. Thus, a stable and high-performance non-aqueous electrolyte lithium secondary battery can be provided including the negative electrode active material according to the present invention. [Brief description of the drawings]

[0041] [Figure 1] 1 shows the results of XRD measurement of carbon-coated silicon oxide composites prepared in an example and a comparative example of the present invention. [Diagram 2] 1 shows the results of XRD measurement of carbon-coated silicon oxide composites prepared in an example and a comparative example of the present invention. [Diagram 3] 1 shows the results of XRD measurement of carbon-coated silicon oxide composites prepared in an example and a comparative example of the present invention. [Figure 4] 1 shows the results of XRD measurement of carbon-coated silicon oxide composites prepared in an example and a comparative example of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0042] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the following examples.

[0043] <Example 1> Preparation of magnesium-containing silicon oxide composite

[0044] Silicon powder and silicon dioxide (SiO 2 15 kg of powder obtained by uniformly mixing silicon, silicon dioxide (SiO) powders in a 1:1 molar ratio and 1.5 kg of magnesium were heat-treated at 1,400°C in a reduced pressure atmosphere of 0.0001 to 1 torr to obtain the silicon, silicon dioxide (SiO 2 ) mixed powder, silicon oxide vapor and magnesium vapor are generated simultaneously to react in the gas phase, then cooled at 700℃ to precipitate, and then crushed in a jet mill to obtain powder with an average particle size (D 50 A magnesium-containing silicon oxide composite powder having a particle size of 6.3 μm was recovered.

[0045] The magnesium-containing silicon oxide composite powder that was recovered to form the carbon-containing coating layer was heated in a tubular electric furnace at 1,000°C for 2 hours in a mixture of argon (Ar) and methane (CH 4 ) was subjected to CVD treatment under a mixed gas of magnesium and silicon oxide, and a carbon coating layer having a carbon content of 5 wt% was formed to prepare a silicon oxide composite (sample 1) containing 6.2 wt% magnesium.

[0046] The magnesium-containing silicon oxide composite (sample 1) had a BET specific surface area of ​​6.2 m 2 / g, specific gravity 2.3g / cm 3 , average particle size (D 50 ) was 6.3 μm, and the size of the silicon crystallites measured by X-ray diffraction analysis (CuKα) was confirmed to be 8 nm.

[0047] <Example 2> Preparation of magnesium-containing silicon oxide composite

[0048] A silicon oxide composite containing 9 wt% magnesium was prepared in the same manner as in Example 1, except for cooling at 800°C and precipitating, and a silicon oxide composite powder having a carbon coating layer with a carbon content of 5 wt% was prepared.

[0049] The magnesium-containing silicon oxide composite (sample 2) had a BET specific surface area of ​​6.3 m 2 / g, specific gravity 2.3g / cm 3 , average particle size (D 50 ) was 6.2 μm, and the size of the silicon crystallites measured by X-ray diffraction analysis (CuKα) was confirmed to be 8 nm.

[0050] <Example 3> Preparation of magnesium-containing silicon oxide composite

[0051] A silicon oxide composite containing 11.7 wt% magnesium was prepared in the same manner as in Example 1, except for cooling at 900°C to precipitate, and a silicon oxide composite powder (sample 3) having a carbon coating layer with a carbon content of 10 wt% was prepared.

[0052] The magnesium-containing silicon oxide composite (sample 3) had a BET specific surface area of ​​5.8 m 2 / g, specific gravity 2.4g / cm 3 , average particle size (D 50 ) was 6.7 μm, and the size of the silicon crystallites measured by X-ray diffraction analysis (CuKα) was confirmed to be 11 nm.

[0053] <Example 4> Preparation of magnesium-containing silicon oxide composite

[0054] A silicon oxide composite containing 4.6 wt% magnesium was prepared in the same manner as in Example 1, except for cooling at 1000°C to precipitate, and a silicon oxide composite powder (sample 4) having a carbon coating layer with a carbon content of 7 wt% was prepared.

[0055] The magnesium-containing silicon oxide composite (sample 4) had a BET specific surface area of ​​7.3 m 2 / g, specific gravity 2.3g / cm 3 , average particle size (D 50) was 6.2 μm, and the size of the silicon crystallites measured by X-ray diffraction analysis (CuKα) was confirmed to be 7 nm.

[0056] <Example 5> Preparation of magnesium-containing silicon oxide composite

[0057] A silicon oxide composite containing 16.6 wt% magnesium was prepared in the same manner as in Example 1, except for cooling at 1100°C to precipitate, and a silicon oxide composite powder (sample 5) having a carbon coating layer with a carbon content of 4 wt% was prepared.

[0058] The magnesium-containing silicon oxide composite (sample 5) had a BET specific surface area of ​​6.8 m 2 / g, specific gravity 2.4g / cm 3 , average particle size (D 50 ) was 7.1 μm, and the size of the silicon crystallites measured by X-ray diffraction analysis (CuKα) was confirmed to be 14 nm.

[0059] <Example 6> Preparation of magnesium-containing silicon oxide composite

[0060] A silicon oxide composite containing 3 wt% magnesium was prepared in the same manner as in Example 1, except for cooling at 800°C to precipitate, and a silicon oxide composite powder (sample 6) having a carbon coating layer with a carbon content of 5 wt% was prepared.

[0061] The magnesium-containing silicon oxide composite (sample 6) had a BET specific surface area of ​​6.3 m 2 / g, specific gravity 2.3g / cm 3 , average particle size (D 50 ) was 5.9 μm, and the size of the silicon crystallites measured by X-ray diffraction analysis (CuKα) was confirmed to be 6 nm.

[0062] <Comparative Example 1> Preparation of magnesium-free silicon oxide composite

[0063] A silicon oxide composite (sample 7) having a carbon coating layer with a carbon content of 5 wt % was prepared in the same manner as in Example 1, except that the heat treatment was performed without adding magnesium.

[0064] The silicon oxide composite (sample 7) had a BET specific surface area of ​​6.5 m 2 / g, specific gravity 2.0g / cm 3 , average particle size (D 50 ) was 6.0 μm, and the size of the silicon crystallites measured by X-ray diffraction analysis (CuKα) was confirmed to be 5 nm.

[0065] <Comparative Example 2> Preparation of magnesium-containing silicon oxide composite

[0066] A silicon oxide composite containing 1 wt% magnesium and having a carbon coating layer with a carbon content of 5 wt% was prepared in the same manner as in Example 1, except that the precipitation was performed by natural cooling.

[0067] For the magnesium-containing silicon oxide composite (sample 8), the BET specific surface area was 5 m 2 / g, specific gravity 2.2g / cm 3 , average particle size (D 50 ) was 6.5 μm, and the size of the silicon crystallites measured by X-ray diffraction analysis (CuKα) was confirmed to be 8 nm.

[0068] <Experimental Example 1>

[0069] The average particle size, specific surface area, and magnesium content of the silicon oxide composites (samples 1 to 8) prepared in Examples 1 to 6 and Comparative Examples 1 and 2 were analyzed, and the results are shown in Table 1 below.

[0070] [Table 1]

[0071] <Experimental Example> XRD Analysis

[0072] XRD measurements were carried out on the silicon composites containing magnesium (Samples 1 to 8) produced in Example 1, Example 2, and Example 6, and the results are shown in Table 2 and Figures 1 to 3 below.

[0073] The measurements were carried out using XRD from Malvern panalytical (equipment name: X’Pert3), and the measurements were carried out at 45 kV and 40 mV from 10 degrees to 60 degrees for 30 minutes.

[0074] The starting point and the ending point of the Si(111) peak were connected by a line through X-ray diffraction analysis (CuKα), and the height from the center value to the maximum peak point was determined as Intensity Si(111), and MgSiO 3 (610) peak was also set as Intensity MgSiO 3 (610) in the same way as Si(111). Also, the size of the Si crystal was calculated using the following Scherrer’s equation.

[0075] <Scherrer’s equation (the equation of Scherrer)>

[0076] D = 0.9 * λ / (β * cosθ)

[0077] D: particle diameter size

[0078] β: FWHM (full width at half maximum)

[0079] λ: wave length of X-Ray (0.1541 nm)

[0080] In Table 2 below, the intensity I of the diffraction peak by Si(111) detected at 2θ = 27.5° to 29.5° during X-ray diffraction analysis si(111) and the intensity I of the diffraction peak by MgSiO 3 detected at 2θ = 30° to 32° MgSiO3 The ratio I of MgSiO3(610) / ISi(111) In the case of Examples 1 to 6 of the present invention, the ratio is greater than 0.1 and less than 0.5, whereas in the case of the comparative example, the ratio is MgSiO 3 It can be confirmed that no peak is detected or is less than 0.1.

[0081] [Table 2]

[0082] <Manufacturing example> Battery manufacturing

[0083] A negative electrode for a lithium secondary battery and a battery (coin cell) containing the silicon oxide composite powder prepared according to the above examples and comparative examples as an electrode active material were fabricated.

[0084] The active material, SUPER-P as a conductive material, and polyacrylic acid were mixed with water in a weight ratio of 80:10:10 to prepare a negative electrode slurry.

[0085] The composition was applied to a copper foil having a thickness of 18 μm and dried to prepare an electrode having a thickness of 70 μm. The copper foil to which the electrode was applied was punched into a circle having a diameter of 14 mm to prepare a negative electrode for a coin cell, and a metallic lithium foil having a thickness of 0.3 mm was used as the counter electrode.

[0086] A 0.1 mm thick porous polyethylene sheet was used as the separator, and 1M LiPF was added to a solution of ethylene carbonate (EC) and diethylene carbonate (DEC) mixed in a volume ratio of 1:1 as the electrolyte. 6 was dissolved and used as an electrolyte, and the above-mentioned components were applied to prepare a coin cell (battery) having a thickness of 2 mm and a diameter of 32 mm.

[0087] <Experimental Example>

[0088] The coin cell manufactured in the above manufacturing example was charged at a constant current of 0.1 C until the voltage reached 0.005 V, and discharged at a constant current of 0.1 C until the voltage reached 2.0 V. The charge capacity (mAh / g), discharge capacity (mAh / g), and initial charge / discharge efficiency (%) were determined, and the results are shown in Table 3 below.

[0089] In addition, the coin cells prepared for each sample in the above manufacturing example were charged and discharged once, and then from the second charge and discharge, they were charged at a constant current of 0.5 C until the voltage reached 0.005 V, and discharged at a constant current of 0.5 C until the voltage reached 2.0 V. The cycle characteristics (capacity retention rate for 50 cycles) were determined, and the results are shown in Table 3 below.

[0090] Intensity I of the diffraction peak due to Si(111) detected at 2θ=27.5° to 29.5° according to an embodiment of the present invention si(111) and MgSiO detected at 2θ = 30° to 32° 3 Intensity of the diffraction peak due to I MgSiO3 The ratio is 0.1 MgSiO3(610) / I Si(111) When the ratio is <0.5, it can be confirmed that the initial efficiency and the capacity retention rate at 50 cycles are significantly improved.

[0091] [Table 3] ​

Claims

1. Silicon, silicon oxide (SiO x , 0<x≦2), and a silicon oxide complex containing magnesium silicate, The magnesium silicate is MgSiO 3 Including, In the X-ray diffraction analysis, the intensity I of the diffraction peak due to Si (111) detected at 2θ = 27.5 ° to 29.5 ° si(111) and MgSiO detected at 2θ = 30° to 32° 3 Intensity of the diffraction peak due to I MgSiO3(610) The ratio of is 0.1<I MgSiO3(610) / I Si(111) < 0.3, The silicon oxide composite has a ratio of silicon atoms to oxygen atoms (Si / O) of 0.5 to 2; The silicon oxide composite contains magnesium in an amount of 2 wt % to 30 wt % based on the total weight of the silicon oxide composite; The silicon oxide composite further comprises a coating layer containing carbon on a surface thereof, The coating layer is 2 to 20 parts by weight per 100 parts by weight of the silicon oxide composite. Negative electrode active material for non-aqueous electrolyte secondary batteries.

2. In the X-ray diffraction analysis, the silicon oxide composite has a diffraction peak due to Si(111) at 2θ=27.5° to 29.5°; 2. The negative electrode active material for a non-aqueous electrolyte secondary battery according to claim 1, wherein the size of the silicon crystallites calculated from the full width at half maximum (FWHM) of the diffraction peak is 2 nm to 100 nm.

3. The magnesium silicate is Mg 2 SiO 4 The negative electrode active material for a non-aqueous electrolyte secondary battery according to claim 1 , further comprising:

4. The negative electrode active material for a non-aqueous electrolyte secondary battery as described in claim 1, wherein the carbon-containing coating layer includes at least one selected from the group consisting of amorphous carbon, carbon nanofibers, carbon nanotubes, graphite, graphene, graphene oxide, and reduced graphene oxide.

5. A negative electrode comprising the negative electrode active material for a non-aqueous electrolyte secondary battery according to claim 1.

6. A non-aqueous electrolyte lithium secondary battery comprising a negative electrode according to claim 5.

7. A method for producing a silicon-based composite material comprising: a first step of introducing a mixture of silicon particles and silicon dioxide particles and magnesium into a reactor; a second step of adjusting the pressure of the reactor to 0.000001 torr to 1 torr; a third step of heating the mixture and the magnesium in a vapor phase to produce a silicon oxide composite; a fourth step of cooling the silicon oxide composite at 700°C to 1100°C and depositing the cooled silicon oxide composite on a metal plate; 2. The method of claim 1, further comprising: a fifth step of pulverizing and classifying the silicon oxide composite deposited on the cooling and metal plate to an average particle size of 0.5 to 15 μm.

8. A method for producing a negative electrode active material for a non-aqueous electrolyte secondary battery as described in claim 7, further comprising a sixth step of adding the silicon oxide complex of the fifth step and a carbon source and heat treating the silicon oxide complex at 600°C to 1200°C to form a carbon-containing coating layer on a surface of the silicon oxide complex.

9. The method for producing a negative electrode active material for a non-aqueous electrolyte secondary battery described in claim 8, wherein the carbon source is at least one selected from the group consisting of methane, propane, butane, acetylene, benzene, and toluene.

10. The method for producing a negative electrode active material for a non-aqueous electrolyte secondary battery as described in claim 8, wherein in the sixth step, in addition to the carbon source, at least one selected from the group consisting of nitrogen, helium, argon, carbon dioxide, hydrogen and water vapor is further added.

Citation Information

Patent Citations

  • Cathode material for nonaqueous electrolytic secondary battery and method of manufacturing the same, and lithium ion secondary battery

    JP2012033317A

  • Anode material for non-aqueous electrolyte secondary battery, preparation method therefor, and non-aqueous electrolyte secondary battery including same

    WO2016204366A1

  • Compound and preparation method thereof as well as negative electrode prepared by adopting compound and lithium ion battery

    CN106356508A

  • Negative active material for lithium secondary battery, method of manufacturing the same, and lithium secondary battery comprising the negative active material

    JP2005243640A

  • Negative electrode material for secondary battery, and its manufacturing method

    JP2010170943A