Microporous laminate film and laminate containing said film
The microporous laminated film, integrating polyolefin dry and wet films with a nonwoven fabric, addresses the limitations of existing protective clothing by providing enhanced virus barrier, breathability, and flexibility, ensuring effective protection against viruses and bodily fluids.
Patent Information
- Application Number
- JP2021016183
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-09-03
- Filing Date
- 2021-02-04
- Publication Date
- 2024-10-09
- Estimated Expiration
- 2041-02-04
AI Technical Summary
Existing disposable protective clothing lacks comprehensive virus barrier properties, breathability, and flexibility, failing to effectively prevent virus infection.
A microporous laminated film composed of a first polyolefin dry film with micro pores and a second polyolefin wet film, integrated with a nonwoven fabric, where the dry film supports the wet film, enhancing barrier properties and breathability.
The laminated film achieves superior blood and body fluid barrier properties, virus resistance, and water resistance, ensuring effective protection while maintaining flexibility and comfort.
Smart Images

Figure 0007564723000002 
Figure 0007564723000003 
Figure 0007564723000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a microporous laminate film and a laminate comprising the film, and further to a fabric comprising the laminate, and to protective clothing and medical wear comprising the fabric. [Background technology]
[0002] Patent Document 1 describes a protective suit for preventing infection used in medical settings that uses a composite sheet formed by laminating a nonwoven fabric in which the constituent fibers are partially heat-bonded together, the constituent fibers being core-sheath composite fibers having a core made of polyethylene terephthalate and a sheath made of polyethylene, and a nonporous moisture-permeable polyurethane film. The nonporous moisture-permeable polyurethane film is imparted with moisture permeability by introducing hydrophilic groups into the polyurethane resin structure.
[0003] On the other hand, Patent Document 2 describes a disposable protective suit using a composite sheet. This composite sheet is a laminate of a nonwoven fabric in which the constituent fibers are partially heat-bonded to each other, and a microporous polyethylene film, and the core-sheath composite fibers, the core of which is made of polyethylene terephthalate and the sheath of which is made of polyethylene. Examples of the microporous polyethylene film include a microporous film produced by dissolving an inorganic filler, an organic filler, or the like from a polyethylene film containing the filler with a solvent, and a microporous film obtained by forming a microporous structure by stretching a sheet made of a polyethylene resin containing a particulate inorganic filler or organic filler at least in one axial direction to generate voids between the particle surface and the resin (paragraph 0021 of Patent Document 2). The polyethylene film is microporous, and thus can have blood barrier properties, virus barrier properties, breathability, and flexibility.
[0004] Disposable protective clothing using a sheet containing a flash-spun nonwoven fabric in which ultrafine polyethylene mesh long fibers are randomly laminated is also known. Disposable protective clothing using these nonwoven fabrics is useful because it is light, flexible, and strong. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Utility Model Registration No. 3190510 [Patent Document 2] Utility Model Registration No. 3157107 Summary of the Invention [Problem to be solved by the invention]
[0006] However, known disposable protective clothing using nonwoven fabrics is still not perfect in terms of virus barrier properties, and may not be able to completely prevent virus infection. In other words, a structure that can be suitably applied to disposable protective clothing and the like by combining all of the following: blood and body fluid barrier properties, virus barrier properties, breathability, and flexibility has not yet been obtained.
[0007] Therefore, an object of the present invention is to provide a microporous laminate film that combines all of the following properties: barrier properties against blood and body fluids, barrier properties against viruses, breathability, and water resistance, and thus can be suitably used in disposable protective clothing, and a laminate containing this film. [Means for solving the problem]
[0008] To achieve this object, the microporous laminate film of the present invention is a laminated film of a first polyolefin-based dry film having micropores and a second polyolefin-based wet film having micropores, the dry film having a basis weight of 10 to 30 g / m. 2 The wet film weight is 3 to 12 g / m 2According to this, the wet film can exhibit a required barrier property, and the dry film can provide strength support for the wet film while maintaining required performance.
[0009] To achieve this, in the microporous laminate film of the present invention, it is preferable that the ratio of the basis weight of the dry film to the basis weight of the wet film is (basis weight of dry film) / (basis weight of wet film)=1 to 5 / 1.
[0010] In the microporous laminate film of the present invention, it is preferable that the dry film is a colored film, or that the dry film and the wet film are laminated and integrated by bonding with a colored adhesive.
[0011] The laminate of the present invention is characterized in that a nonwoven fabric is laminated on one or both sides of the microporous laminate film. 2 It is preferable that:
[0012] Here, it is preferable that the nonwoven fabric has core-sheath composite fibers having a core composed of polyethylene terephthalate and a sheath composed of polyethylene as its constituent fibers, and that the constituent fibers are partially thermally bonded to each other in a spot-like form.
[0013] According to the laminate of the present invention, the moisture permeability according to the A-1 method of JIS L1099 is 4500 g / m 2 -24 hours or more, water resistance of 900 mm or more according to JIS L1092 Method A, blood barrier property of Class 3 or more according to JIS T8060 or blood barrier property evaluation of "passed" according to ASTM F1670, and virus barrier property of Class 3 or more according to JIS T8061 or virus barrier property evaluation of "passed" according to ASTM F1671 are preferred. The fabric of the present invention is characterized by including the above laminate.Furthermore, the protective clothing and medical wear of the present invention are characterized by each including the above fabric. Effect of the Invention
[0014] The microporous laminate film of the present invention is a laminated integral product of a polyolefin-based dry film having a first micropore and a polyolefin-based wet film having a second micropore, and therefore the wet film can strongly exhibit the required barrier properties, and the dry film can provide strength support for the wet film while maintaining the required performance. [Brief description of the drawings]
[0015] [Figure 1] FIG. 1 is a diagram showing a first aspect of a colored laminate in an embodiment of the present invention. [Diagram 2] FIG. 2 shows a second embodiment of the same colored laminate. [Diagram 3] FIG. 2 is an enlarged view of the surface of a dry film of a microporous laminate film in an embodiment of the present invention. [Figure 4] FIG. 2 is an enlarged view of the surface of a wet film of a microporous laminate film in an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] The microporous laminate film of the present invention is obtained by laminating together a first polyolefin-based dry film having micropores and a second polyolefin-based wet film having micropores.
[0017] Among these, the polyolefin-based dry film contains fine particles in a polyolefin-based resin layer, and has voids between the surfaces of the fine particles and the polyolefin-based resin. The pore diameter of the voids in this dry film is about 0.1 to 15 μm, and the voids form first micropores. The voids can be formed by stretching a sheet made of a polyolefin-based resin containing fine particles at least in one axial direction to generate gaps between the surfaces of the fine particles and the resin, i.e., at the interface between the fine particles and the polyolefin-based resin. As a result of the stretching, the voids are formed, and the voids are connected to each other, thereby ensuring the required air permeability and water vapor permeability. At this time, the fine particles for forming the voids can be made small in particle size and have a narrow particle size distribution width, thereby obtaining the required protective performance such as blood barrier property and virus barrier property.
[0018] Any polyolefin can be used to form the resin layer of the dry film, and representative examples include polyethylene-based resins and polypropylene-based resins. Among them, polyethylene-based resins can be preferably used because they have good processability, flexibility, and lightness. The polyethylene-based resin may be a polymer of ethylene alone, or a copolymer in which ethylene is the main repeating unit and an α-olefin is copolymerized therewith. Examples of α-olefins include propylene, 1-butene, 1-pentene, 1-hexene, 1-octene, 1-decene, 1-dodecene, 4-methyl-1-pentene, and 3-methyl-1-pentene. The number average molecular weight of the polyolefin may also be arbitrary.
[0019] Examples of the fine particles include organic fine particles and inorganic fine particles. In particular, inorganic fine particles can be preferably used, and examples of such inorganic fine particles include calcium carbonate, barium carbonate, calcium sulfate, barium sulfate, titanium oxide, magnesium oxide, zinc oxide, alumina, talc, and silica. Among them, calcium carbonate can be preferably used because it is made from limestone, which is abundant in nature, is versatile, and is approved for use as a cosmetic raw material and a food additive, and is highly safe.
[0020] The fine particles preferably have an integrated distribution D10 of 0.2 μm or more and 0.5 μm or less, and an integrated distribution D100 of 10 μm or less, in terms of the amount of particles with a specific particle diameter or less. The integrated distribution D10 refers to the size (particle diameter) of the fine particles when all the fine particles are counted from the smallest particle diameter and the fine particles make up 10% of the total amount. The integrated distribution D100 refers to the size (particle diameter) of the fine particles when all the fine particles are counted from the smallest particle diameter and the fine particles make up 100% of the total amount, i.e., the maximum size (maximum particle diameter) of all the fine particles.
[0021] In this way, by using microparticles having an integrated distribution D10 of 0.2 μm or more and 0.5 μm or less and an integrated distribution D100 of 10 μm or less, the size (particle diameter) of the microparticles can be reduced and the width of the size distribution can be narrowed. As a result, the size of the voids formed around the microparticles can be reduced and made uniform, and the breathability and water vapor permeability caused by the presence of the voids can be made uniform, and the protective properties such as blood barrier property and virus barrier property based on the size of the voids can also be made uniform. If the integrated distribution D10 is less than 0.2 μm, the moisture permeability is easily impaired. If the integrated distribution D100 exceeds 10 μm, large-sized pores tend to appear, and the size of the micropores in the microporous film varies, making it difficult to form a dense and uniform microporous structure throughout the film. For this reason, it is more preferable that the cumulative distribution D10 is not less than 0.2 μm and not more than 0.4 μm, and it is even more preferable that the cumulative distribution D100 is not more than 6 μm.
[0022] The cumulative distribution D50 for the median value can also be taken into consideration, and the average particle size of the microparticles can be examined based on the cumulative distribution D50 for the median value. It is preferable that the cumulative distribution D50 is 1.0 μm or less in order to exhibit good water resistance, blood barrier property, and virus barrier property.
[0023] As calcium carbonate microparticles having such a particle size distribution, commercially available products can be used. For example, calcium carbonate microparticles with the product number "AFF-CB" from Fimatec Co., Ltd. can be preferably used. AFF-CB has a D10 of 0.31 μm, a D50 of 0.64 μm, and a D100 of 4.02 μm.
[0024] In the polyolefin-based dry film, the proportion of fine particles contained in the polyolefin-based resin layer is preferably 40% by mass or more and 60% by mass or less, because by containing the fine particles in this range, the required performance can be obtained when the microporous film is used to form protective clothing.
[0025] Next, the polyolefin-based wet film will be described. The polyolefin-based wet film has second micropores with a pore size of about 0.1 to 0.5 μm. For example, such a wet film is formed by melting and kneading a mixture of a polyolefin-based resin and a plasticizer, extruding the mixture to form a film, and then stretching the film. The plasticizer is extracted from the film formed, and the plasticizer is removed from the film, making the areas where the plasticizer was present into a large number of micropores. Since the polyolefin-based resin and the plasticizer are uniformly mixed by melt kneading, the second micropores are formed in this manner, and the pore size of the second micropores is about 0.1 to 0.5 μm, which is smaller than the pore size of the first micropores in the above-mentioned polyolefin-based dry film, and can be distributed more uniformly in the film. The microporous laminate film of the present invention contains a polyolefin-based wet film having micropores with a small pore size, and therefore can exhibit particularly excellent performance in terms of barrier properties against blood and body fluids and virus barrier properties. If the pore size of the second micropores is less than 0.1 μm, moisture permeability is impaired, whereas if the pore size exceeds 0.5 μm, the required blood barrier property and virus barrier property cannot be obtained.
[0026] The polyolefin for forming the resin layer of the wet film may be any of the polyolefins exemplified above for forming the resin layer of the dry film. Among them, the same polyolefin as that for forming the resin layer of the dry film may be preferably used.
[0027] As a plasticizer for forming the second micropores, an organic compound that can be uniformly melted and kneaded with a polyolefin resin is used, and examples thereof include aliphatic or cyclic hydrocarbons such as nonane, decane, decalin, paraffin oil, and paraffin wax, phthalate esters such as dibutyl phthalate and dioctyl phthalate, fatty acids having 10 to 20 carbon atoms such as palmitic acid, stearic acid, oleic acid, linoleic acid, and linolenic acid, fatty acid alcohols having 10 to 20 carbon atoms such as palmitic acid alcohol, stearic acid alcohol, and oleic acid alcohol, and mixtures thereof. Among these, paraffin oil is preferable because it is harmless to the human body, has a high boiling point, and has few volatile components.
[0028] The detailed manufacturing method of the polyolefin-based wet film is as follows. That is, the polyolefin-based resin and the organic compound serving as the plasticizer are melt-mixed, the mixture is extruded using a T-die, and the extrudate is stretched. Thereafter, the organic compound that was uniformly mixed in the polyolefin-based resin is removed by extracting the organic compound with a solvent, and the removed portion becomes microporous, thereby obtaining a polyolefin-based wet film. For example, methylene chloride may be used for extracting the plasticizer. In addition, since the methylene chloride used for extraction is attached to the film from which the plasticizer has been removed, it may be removed by drying.
[0029] The method for laminating a polyolefin-based dry film and a polyolefin-based wet film is as follows: The two films can be laminated by adopting a hot melt lamination method in which the films are thermally and pressure-bonded via a hot melt adhesive.
[0030] In the microporous laminate film of the present invention, in order to exhibit the required performance, the basis weight of the dry film is 10 to 30 g / m 2 The wet film weight is 3 to 12 g / m 2Furthermore, the ratio of the basis weight of the dry film to the basis weight of the wet film is preferably (basis weight of dry film) / (basis weight of wet film)=1 to 5 / 1.
[0031] From the same viewpoint, in the microporous laminate film of the present invention, the thickness of the dry film is preferably 15 to 30 μm, and the thickness of the wet film is preferably 4 to 15 μm. In particular, the total thickness of the microporous laminate film, which is the sum of the thickness of the dry film and the thickness of the wet film, is preferably 40 μm or less. By having a total thickness of 40 μm or less, when the protective clothing is made by laminating with a nonwoven fabric layer as described below, it can be made thin, therefore lightweight and flexible. If the thickness exceeds 40 μm, when laminating with a nonwoven fabric layer as described above, it becomes thick, and the comfort of the protective clothing, including flexibility, is reduced. The lower limit of the thickness is not particularly specified, but from the viewpoint of the required strength when the protective clothing is made using the microporous laminate film, it is preferable to set the lower limit at 20 μm.
[0032] The polyolefin resin composition constituting the dry film and the wet film of the microporous laminate film of the present invention may contain additives such as ultraviolet absorbers, light stabilizers, antifogging agents, antistatic agents, flame retardants, color inhibitors, antioxidants, fillers, and pigments depending on the application.
[0033] As the pigment, for example, a color pigment such as a white pigment or a blue pigment can be used. An example of the use of the pigment is, for example, adding the pigment to a dry film and disposing the dry film on the front side when obtaining a laminate described later. Another example of the use of the pigment is, for example, adding the pigment to the above-mentioned hot melt adhesive or other types of adhesives for laminating a polyolefin-based dry film and a polyolefin-based wet film.
[0034] An example of the manufacturing method of the microporous laminated film of the present invention will be described. First, an example of the manufacturing method of the dry film will be described. First, a polyolefin resin and fine particles such as calcium carbonate are mixed in a predetermined amount and melt-kneaded in a twin-screw kneading extruder to prepare compound pellets. After drying the compound pellets, the compound pellets are made into a film by inflation film formation or the like. As the inflation film formation method, a method in which the dried compound pellets are put into a single-screw kneading extruder, the molten polymer is pulled up into a tube shape from a round die, and simultaneously inflated into a balloon shape while being air-cooled to form a film, or a method in which the molten polymer is extruded downward into a cylindrical shape from a round die together with cooling water, folded once, pulled up, and then heated and inflated into a balloon shape to form a film, etc. can be preferably adopted. By using the inflation film formation method, a stretched film can be immediately obtained without performing a stretching process after the film formation. The polymer melting temperature in the twin-screw kneading extruder can be appropriately selected within the temperature range of 120 to 180° C., which is the melting temperature of the polyolefin resin. The polymer melting temperature of the compound pellets in the single-screw kneading extruder can be appropriately selected in consideration of the melting point and blending amount of the polyolefin resin, and the blending amount of fine particles such as calcium carbonate, but a temperature range of 120 to 180° C. is preferable.
[0035] Also, as a method for forming a film, a resin composition containing a predetermined amount of polyolefin resin and fine particles such as calcium carbonate is melted under a temperature condition of the melting point or higher and lower than the decomposition temperature of the polyolefin resin, extrusion molded using a T-die to obtain a non-porous unstretched sheet, and then uniaxially or biaxially stretched to develop micropores to obtain a microporous film. The uniaxial stretching method for stretching the non-porous unstretched sheet may be longitudinal uniaxial stretching or transverse uniaxial stretching. The biaxial stretching may be simultaneous biaxial stretching or sequential biaxial stretching. Sequential biaxial stretching allows the stretching conditions to be selected in each stretching step, making it easy to control the microporous structure.
[0036] In addition, when compound pellets are produced in a stage prior to the production of a microporous film, a crosslinking agent, a crosslinking assistant, an organic lubricant, etc. can be added as necessary. In addition, when a film is produced, additives can be added as necessary to an extent that does not affect the physical properties of the film.
[0037] As an example of a method for producing a wet film, as described above, a polyolefin resin and an organic compound that acts as a plasticizer are melt-mixed, the mixture is extruded using a T-die, the extrudate is stretched, and then the organic compound is extracted with a solvent, thereby removing the organic compound that was uniformly mixed in the polyolefin resin, and the removed areas become microporous, thereby obtaining a polyolefin wet film.
[0038] To explain the method of laminating a dry film and a wet film, as described above, the two can be laminated by adopting a dry lamination method in which the films are thermally pressed together via a hot melt adhesive, thereby obtaining the microporous laminate film of the present invention.
[0039] According to the present invention, the above-mentioned microporous laminate film is used to obtain a laminate for forming a fabric, or a protective suit and medical wear using the fabric. In particular, a laminate can be obtained in which a nonwoven fabric is laminated on both sides or one side of the microporous laminate film by bonding with an adhesive or heat bonding. Any suitable nonwoven fabric can be used, but a core-sheath composite fiber having a core made of polyethylene terephthalate and a sheath made of polyethylene, in which the constituent fibers are partially heat-bonded in a spot-like form, can be preferably used. As a result, the polyethylene terephthalate in the core maintains mechanical strength, and the polyethylene in the sheath makes it light and flexible, making it suitable for protective clothing, etc.
[0040] As the adhesive, a hot melt adhesive can be preferably used. Among hot melt adhesives, a polyurethane adhesive or a polyethylene adhesive is preferable from the viewpoint of adhesiveness.
[0041] The microporous laminate film and the nonwoven fabric can also be laminated together using an adhesive containing a particulate polyolefin resin as an adhesive component. The particulate polyolefin resin referred to here has the same composition as the polyolefin resin constituting the microporous laminate film, and therefore tends to selectively adhere to the nonporous regions of the microporous laminate film.
[0042] As the particulate polyolefin resin, one that is easily dispersible in water is used. This makes it possible to make a water-based adhesive. As such a polyolefin resin, one described in Japanese Patent No. 3699935 can be suitably used. This polyolefin resin is composed of a copolymer obtained by copolymerizing a monomer containing an unsaturated carboxylic acid or its anhydride (A) and an alkene (B) having 2 to 6 carbon atoms. Examples of the unsaturated carboxylic acid or its anhydride (A) include acrylic acid, methacrylic acid, maleic acid, maleic anhydride, itaconic acid, itaconic anhydride, fumaric acid, and crotonic acid. Examples of the alkene (B) having 2 to 6 carbon atoms include ethylene, propylene, isobutylene, 1-butene, 1-pentene, and 1-hexene. In addition to the unsaturated carboxylic acid or its anhydride (A) and the alkene having 2 to 6 carbon atoms (B), an acrylic acid ester such as methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, butyl acrylate, butyl methacrylate, dimethyl maleate, diethyl maleate, or dibutyl maleate may be copolymerized as a third component. Also, a copolymerization of a third component such as acrylic acid amide, methacrylic acid amide, methyl vinyl ether, ethyl vinyl ether, vinyl formate, vinyl acetate, vinyl propionate, vinyl piperidine, vinyl versatate, vinyl alcohol, or acrylonitrile may be used. The copolymerization ratio of the unsaturated carboxylic acid or its anhydride (A) and the alkene having 2 to 6 carbon atoms (B) is preferably about (A):(B)=0.5 to 20:99.5 to 80 by mass. In the copolymerization of the third component, the mass ratio of the third component is preferably 35 mass% or less of the total.
[0043] The polyolefin resin microparticles having the above composition disperse well in water as described in Japanese Patent No. 3699935, and the dispersion in water is treated as a microparticle dispersion. Therefore, when an adhesive is made by mixing an aqueous solution in which polyvinyl alcohol is dissolved and a microparticle dispersion in which microparticle-shaped polyolefin resin is dispersed in an aqueous solution, the two can be mixed uniformly, and the two adhesive components are mixed uniformly.
[0044] By laminating a nonwoven fabric on a microporous laminate film as described above to form a laminate, the microporous laminate film is reinforced by the nonwoven fabric, and the required strength can be obtained when the protective clothing is made. From the viewpoint of strength, a nonwoven fabric having a core-sheath composite fiber in which the core is composed of polyethylene terephthalate and the sheath is composed of polyethylene as described above is particularly suitable. In addition, since such a nonwoven fabric having a core-sheath structure has excellent heat sealability, when a protective clothing is obtained using a fabric composed of a laminate, it can be easily tailored by heat sealing, and since the fabrics can be joined together without gaps by heat sealing, the waterproofness, blood barrier property, and virus barrier property of the protective clothing at the joint between the fabrics can be reliably maintained. Of course, it is also possible to tailor protective clothing by sewing the fabrics together, or by using sewing and heat sealing in combination.
[0045] The laminate of the microporous laminate film and the nonwoven fabric is used for fabrics, protective clothing, medical gowns, etc., and has a moisture permeability of 4500 g / m2 according to the A-1 method of JIS L1099. 2It is preferable that the microporous laminate film has a water resistance of 900 mm or more according to JIS L1092 Method A, a blood barrier property of Class 3 or more according to JIS T8060 or an evaluation of blood barrier property of "pass" or better according to ASTM F1670, and a virus barrier property of Class 3 or more according to JIS T8061 or an evaluation of virus barrier property of "pass" according to ASTM F1671. In reality, the nonwoven fabric does not substantially contribute to these performances but mainly plays a role of reinforcing the microporous laminate film as described above, and therefore these various performances can be said to be the performances of the microporous laminate film of the present invention.
[0046] As described above, the nonwoven fabric can be laminated on one or both sides of the microporous laminate film, but when laminated on one side, if the nonwoven fabric is laminated on the surface of the wet film rather than on the surface of the dry film, the wet film is formed thinner than the dry film, so that the wet film can be effectively reinforced and protected by laminating the nonwoven fabric on the surface of the wet film. On the other hand, when laminated on one side, if the nonwoven fabric is laminated on the surface of the dry film rather than on the surface of the wet film, one side of the dry film is covered with the wet film and the other side is covered with the nonwoven fabric, so that the abrasion resistance is improved.
[0047] A laminate in which a nonwoven fabric is laminated on a microporous laminate film is colored, for example, blue. FIG. 1 shows a first embodiment of the colored laminate. Here, 1 is a nonwoven fabric, 2 is a white wet film in the microporous laminate film, and 3 is a dry film in the microporous laminate film. Here, the wet film 2 is sandwiched between the nonwoven fabric 1 and the dry film 3. That is, as described above, the nonwoven fabric 1 is laminated on the surface of the wet film 2. As a result, the wet film 2 is not exposed on the surface of the laminate, and is reinforced and protected. In addition, in the laminate shown in FIG. 1, a pigment is added to the dry film 3 arranged on the surface side of the laminate, and the dry film 3 is colored blue or the like. This allows the laminate to effectively develop color.
[0048] Fig. 2 shows a second embodiment of the colored laminate. Here, an adhesive layer 4 made of a hot melt adhesive or the like is depicted for bonding a white wet film 2 and a white dry film 3. The laminate in Fig. 2 has a structure in which the dry film 3 is sandwiched between a nonwoven fabric 1 and a wet film 2, i.e., the nonwoven fabric 1 is laminated on the surface of the dry film 3, and the surface side of the adhesive layer 4 to which a pigment is added is covered with a thin wet film 2. In Fig. 2, the adhesive layer 4 is colored by adding a pigment to the adhesive layer 4, and is further covered with a thin wet film 2, so that the laminate can be effectively colored in the same way. EXAMPLES
[0049] The physical properties in the following examples and comparative examples were measured by the following methods.
[0050] (1) Moisture permeability (g / m 2 24h) It was determined according to JIS L1099 A-1 method.
[0051] (2) Water resistance (mm) It was determined according to JIS L1092, Method A.
[0052] (3) Blood barrier properties (Class n) It was determined according to JIS T8060. According to JIS T8122, blood barrier properties are expressed as "Class n (n is an integer value ranging from 1 to 6)", and the larger the value of n, the better the blood barrier properties.
[0053] In addition, a blood barrier test was conducted according to ASTM F1670 to confirm whether or not the test passed.
[0054] (4) Virus barrier properties (Class n) It was determined according to JIS T8061. According to JIS T8122, the virus barrier property is expressed as "Class n (n is an integer value ranging from 1 to 6)", and the larger the value of n, the better the virus barrier property.
[0055] In addition, a virus barrier test was conducted according to ASTM F1671 to confirm whether it passed or failed.
[0056] (5) Weight Determined according to JIS L1913.
[0057] (6) Thickness Determined according to JIS Z1702.
[0058] Example 1 [Film preparation] The first compound raw material was produced by feeding 42 parts of linear low-density polyethylene, 8 parts of low-density polyethylene, and 52 parts of calcium carbonate (manufactured by Fimatec) with an integrated distribution D10 of 0.3 μm, D50 of 0.6 μm, and D100 of 4 μm into a twin-screw kneading extruder, melt-kneading the mixture, and extruding it at an extrusion temperature of 160°C.
[0059] Next, this first compound raw material was melt-extruded at a set temperature of 160°C using a single-screw extruder, and the sheet-like material extruded from the die was stretched in the longitudinal direction (machine direction) at a stretch ratio of 3 times and wound up by a winder at a speed of 200 m / min. As a result, the basis weight was 18 g / m 2 A dry film having a thickness of 20 μm was prepared.
[0060] In addition, 42 parts by mass of linear low density polyethylene, 8 parts by mass of low density polyethylene, and 50 parts by mass of liquid paraffin as a plasticizer, i.e., a solvent, were charged into a twin-screw kneading extruder and melt-kneaded, and extruded from a T-die at an extrusion temperature of 230°C. The extruded film was then stretched in the longitudinal direction (machine direction) at a stretching ratio of 2.5 times, after which methylene chloride was used to remove the liquid paraffin, and the methylene chloride adhering to the film was removed by drying, resulting in a film with a basis weight of 6 g / m. 2 A wet film with a thickness of 7 μm was prepared.
[0061] Then, the dry film and the wet film obtained as described above were used to apply a hot melt adhesive (2 g / m 2) and then heat-pressed together using the dry lamination method to laminate the two, resulting in a basis weight of 26g / m 2 A microporous laminate film of 1000 nm was obtained.
[0062] Fig. 3 is an enlarged view of the surface of the dry film in the obtained microporous laminate film. In Fig. 3, the granular parts with high brightness, i.e., the whitish granular parts, are calcium carbonate, and the parts with low brightness, i.e., the dark parts, are micropores. Fig. 4 is an enlarged view of the surface of the wet film in the same microporous laminate film, and the magnification is the same as Fig. 3. In Fig. 4, the dark parts with low brightness are micropores as in Fig. 3, but it can be seen that the pore size of these micropores is smaller than that of the micropores in Fig. 3, and that micropores with a uniform pore size are formed overall.
[0063] [Preparation of nonwoven fabric] Polyethylene terephthalate and polyethylene were prepared. They were fed into a core-sheath type composite spinning hole so that the polyethylene terephthalate was arranged in the core and the polyethylene was arranged in the sheath, and the mass ratio of the two was 50 / 50, and melt spinning was performed at a spinning temperature of 295°C and a spinning speed of 3000 m / min. After melt spinning, the fiber was taken up and thinned by an aspirator, and the yarn discharged from the aspirator was opened, and the opened yarn, that is, the core-sheath composite fiber (fineness: 3.5 dtex), was accumulated on a moving collection surface to obtain a nonwoven web. The nonwoven web was partially subjected to a heat-pressure bonding treatment to partially heat-pressure bond the constituent fibers of the nonwoven web in a spot-like form, thereby obtaining a nonwoven web having a basis weight of 20 g / m 2 Thus, a nonwoven fabric having the following properties was obtained.
[0064] [Laminate manufacturing] Hot melt adhesive was applied to one side of the obtained nonwoven fabric at a rate of 4 g / m 2 The microporous wet film was attached to the adhesive-coated surface so that the adhesive was in contact with the microporous laminate film, thereby obtaining a laminate of the microporous laminate film and the nonwoven fabric.
[0065] The performance of the obtained laminate is shown in Table 1.
[0066] [Table 1]
[0067] Example 2 A hot melt adhesive was melt-coated on the surface of the microporous laminate film in the laminate of Example 1 under the same conditions as in Example 1, and another nonwoven fabric having the same specifications as the nonwoven fabric in Example 1 was attached to the surface coated with the adhesive. This produced a laminate of a first nonwoven fabric, a microporous laminate film, and a second nonwoven fabric.
[0068] The performance of the obtained laminate is shown in Table 1.
[0069] Example 3 The production conditions were changed compared to Example 1 to obtain a microporous laminate film different from that of Example 1. In detail, the extrusion amount and the like were changed compared to Example 1 to obtain a microporous laminate film having a basis weight of 20 g / m as a dry film. 2 The wet film had a basis weight of 4 g / m 2 A microporous laminate film having a thickness of 4.4 μm was obtained. Except for using these, a microporous laminate film was obtained under the same conditions as in Example 1. Furthermore, this microporous laminate film and a nonwoven fabric obtained under the same conditions as in Example 1 were attached under the same conditions as in Example 1 to obtain a laminate of the microporous laminate film and the nonwoven fabric.
[0070] The performance of the obtained laminate is shown in Table 1.
[0071] Example 4 A laminate was obtained in the same manner as in Example 1, except that a blue pigment was added to produce a blue dry film.
[0072] Example 5 In Example 1, a laminate was obtained in the same manner as in Example 1, except that in obtaining the microporous laminate film, a blue pigment was contained in the hot melt adhesive used to laminate the dry film and the wet film, and in obtaining a laminate of a nonwoven fabric and a microporous laminate film, the microporous dry film was attached so as to be in contact with the nonwoven fabric via the adhesive.
[0073] Comparative Example 1 Instead of the microporous laminate film of Example 1, a dry microporous polyethylene film (manufactured by Mitsubishi Chemical Corporation, product name: CAU6020B, basis weight 20 g / m 2 ) was used. Otherwise, the same procedure as in Example 1 was carried out to obtain a laminate of a microporous polyethylene film and a nonwoven fabric.
[0074] The performance of the obtained laminate is shown in Table 1.
[0075] As shown in Table 1, the laminates of Examples 1, 2 and 3 were films excellent in all of moisture permeability, water resistance, blood barrier property and virus barrier property.
[0076] In contrast, the film of Comparative Example 1 had excellent moisture permeability, but was inferior to the laminates of Examples 1, 2 and 3 in water resistance, blood barrier property and virus barrier property.
Claims
1. A first polyolefin-based dry film having micropores and a second polyolefin-based wet film having micropores are laminated together, and the weight of the dry film is 10 to 30 g / m 2 and the weight of the wet film is 3 to 12 g / m 2 A microporous laminate film characterized by:
2. 2. The microporous laminate film according to claim 1, wherein the ratio of the basis weight of the dry film to the basis weight of the wet film is (basis weight of the dry film) / (basis weight of the wet film)=1 to 5 / 1.
3. 3. The microporous laminate film according to claim 1, wherein the dry film is a colored film.
4. 3. The microporous laminate film according to claim 1, wherein the dry film and the wet film are laminated and integrated with each other by bonding with a colored adhesive.
5. A laminate comprising the microporous laminate film according to any one of claims 1 to 4 and a nonwoven fabric laminated on one or both sides thereof.
6. Weight per unit area: 40 to 80 g / m 2 6. The laminate according to claim 5,
7. The nonwoven fabric is a laminate according to claim 5 or 6, characterized in that the constituent fibers are core-sheath composite fibers having a core made of polyethylene terephthalate and a sheath made of polyethylene, and the constituent fibers are partially thermally bonded to each other in a spot-like form.
8. Moisture permeability according to JIS L1099 A-1 method is 4500g / m 2The laminate according to any one of claims 5 to 7, characterized in that it has a water resistance of 900 mm or more according to JIS L1092 Method A, a blood barrier property of Class 3 or more according to JIS T8060 or an evaluation of blood barrier property of "pass" according to ASTM F1670, and a virus barrier property of Class 3 or more according to JIS T8061 or an evaluation of virus barrier property of "pass" according to ASTM F1671.
9. A fabric comprising the laminate according to any one of claims 5 to 8.
10. 10. Protective clothing comprising the fabric of claim 9.
11. A medical wear comprising the fabric according to claim 9.
Citation Information
Patent Citations
Semiochemicals and audio signals to monitor and kill koiga
JP2004538286A
Disposable protective clothing
JP3157107U
Composite sheet
JP3190510U
Waterproof moisture-permeable fabric and infection protective clothing
WO2016175250A1
Material for personal protective equipment
WO2021216390A1