Manufacturing method of the positive electrode plate
By employing a two-step process with longer carbon nanotubes in the first paste layer to maintain conductive paths on the current collecting member, the method addresses the resistivity issue in positive electrode plates, improving current collection efficiency.
Patent Information
- Application Number
- JP2022069619
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-04-20
- Publication Date
- 2024-10-09
- Estimated Expiration
- 2042-04-20
AI Technical Summary
The issue with existing methods for manufacturing positive electrode plates is that carbon nanotubes, being lighter than active material particles, migrate to the surface during drying, reducing the number of conductive paths on the current collecting member side, thereby increasing electrical resistivity and decreasing current collecting properties.
A method involving the application of two positive electrode pastes with different carbon nanotube lengths, where the first paste contains longer carbon nanotubes, is used to form multiple layers, which are then dried and compressed, ensuring the nanotubes remain on the current collecting member side, maintaining conductive paths.
This approach reduces electrical resistivity in the thickness direction of the positive electrode plate by preventing the migration of carbon nanotubes away from the current collecting member, thereby enhancing the current collecting properties.
Smart Images

Figure 0007564838000001 
Figure 0007564838000002 
Figure 0007564838000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for manufacturing a positive electrode plate. [Background technology]
[0002] Patent Document 1 discloses a method for manufacturing a positive electrode plate having a positive electrode composite layer on the surface of a current collecting member. Specifically, the manufacturing method includes a positive electrode paste preparation step of preparing a positive electrode paste containing carbon nanotubes, positive electrode active material particles, and a solvent, a coating step of coating the positive electrode paste on the surface of the current collecting member to form a positive electrode paste layer on the surface of the current collecting member, and a drying step of drying the positive electrode paste layer to form the positive electrode composite layer. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2020-184490 A Summary of the Invention [Problem to be solved by the invention]
[0004] Incidentally, when a positive electrode paste containing carbon nanotubes, positive electrode active material particles, and a solvent is applied onto the surface of a current collector to form a positive electrode paste layer, and then the positive electrode paste layer is dried, some of the carbon nanotubes arranged on the current collector side in the positive electrode paste layer may move together with the solvent to the surface side (the side away from the current collector) of the positive electrode paste layer, resulting in fewer carbon nanotubes on the current collector side. Since the carbon nanotubes are lighter than the positive electrode active material particles, they move together with the solvent that is about to evaporate to the surface side of the positive electrode paste layer. For this reason, in the positive electrode mixture layer obtained by drying the positive electrode paste layer, the number of conductive paths on the current collector side may decrease, resulting in an increase in the electrical resistivity in the thickness direction of the positive electrode plate, and a decrease in the current collecting ability of the positive electrode plate.
[0005] The present invention has been made in view of the above-mentioned circumstances, and has an object to provide a method for manufacturing a positive electrode plate that is capable of manufacturing a positive electrode plate having a low electrical resistivity in the thickness direction. [Means for solving the problem]
[0006] (1) One aspect of the present invention relates to a method for manufacturing a positive electrode plate having a positive electrode composite layer on a surface of a current collecting member, the method including: a first positive electrode paste preparation step of preparing a first positive electrode paste containing first carbon nanotubes, positive electrode active material particles, and a solvent; a second positive electrode paste preparation step of preparing a second positive electrode paste containing second carbon nanotubes, the positive electrode active material particles, and the solvent; a first coating step of coating the first positive electrode paste on the surface of the current collecting member to form a first positive electrode paste layer on the surface of the current collecting member; a second coating step of coating the second positive electrode paste on a surface of the first positive electrode mixture layer obtained by drying the first positive electrode paste layer to form a second positive electrode paste layer, and a drying step of drying the first positive electrode paste layer together with the second positive electrode paste layer after the second coating step to form the positive electrode mixture layer, or a first drying step of drying the first positive electrode paste layer to form the first positive electrode mixture layer before the second coating step, and a second drying step of drying the second positive electrode paste layer coated on the surface of the first positive electrode mixture layer to form the positive electrode mixture layer; a pressing step of pressing and compressing the positive electrode mixture layer in a thickness direction; wherein an average length of the first carbon nanotubes is longer than an average length of the second carbon nanotubes.
[0007] The above-mentioned manufacturing method includes the following processes (a) or (b): (a) in a first coating step, a first positive electrode paste is applied onto a surface of a current collecting member to form a first positive electrode paste layer on the surface of the current collecting member, and then in a second coating step, a second positive electrode paste is applied onto the surface of the first positive electrode paste layer to form a second positive electrode paste layer. Then, in a drying step, the first positive electrode paste layer is dried together with the second positive electrode paste layer.
[0008] (b) In a first coating step, a first positive electrode paste is coated on a surface of a current collecting member to form a first positive electrode paste layer on the surface of the current collecting member, and then a first drying step is performed to dry the first positive electrode paste layer to form a first positive electrode mixture layer. Then, in a second coating step, a second positive electrode paste is coated on the surface of the first positive electrode mixture layer to form a second positive electrode paste layer, and then a second drying step is performed to dry the second positive electrode paste layer.
[0009] However, in the above-mentioned manufacturing method, the average length of the first carbon nanotubes contained in the first positive electrode paste is made longer than the average length of the second carbon nanotubes contained in the second positive electrode paste. As a result, when the first positive electrode paste layer is dried, the first carbon nanotubes arranged on the current collecting member side in the first positive electrode paste layer are less likely to move to the surface side (the side away from the current collecting member) together with the solvent, and the carbon nanotubes located on the current collecting member side (particularly those in contact with the current collecting member) are less likely to be reduced.
[0010] The reason is that when the first positive electrode paste layer is dried, the first carbon nanotubes in the first positive electrode paste layer attempt to move toward the surface side together with the solvent that is trying to evaporate, but because the first carbon nanotubes are long, they tend to get caught by the positive electrode active material particles, and being caught by the positive electrode active material particles makes it difficult for them to move toward the surface side. Therefore, according to the above-mentioned manufacturing method, it is possible to manufacture a positive electrode plate with a small electrical resistivity (Ω·cm) in the thickness direction.
[0011] (2) Furthermore, in the method for producing a positive electrode plate according to (1), the second coating step may include coating the second positive electrode paste on a surface of the first positive electrode paste layer to form the second positive electrode paste layer, and the drying step may include drying the first positive electrode paste layer together with the second positive electrode paste layer.
[0012] In the above-mentioned manufacturing method, in the second coating step, the second positive electrode paste is coated on the surface of the first positive electrode paste layer before drying, and then in the drying step, the second positive electrode paste layer is dried together with the first positive electrode paste layer. This makes it possible to further reduce the electrical resistivity in the thickness direction of the positive electrode plate compared to the case where "the first positive electrode paste layer is dried before coating the second positive electrode paste to form a first positive electrode mixture layer, and then the second positive electrode paste layer coated on the surface of the first positive electrode mixture layer is dried."
[0013] The reason is as follows. In the latter manufacturing method, when the second positive electrode paste layer is dried, some of the second carbon nanotubes located on the current collector side of the second positive electrode paste layer may migrate to the surface side together with the solvent, and the number of second carbon nanotubes on the current collector side in the second positive electrode paste layer may decrease. Note that, in the latter manufacturing method, when the second positive electrode paste layer is dried, the first positive electrode paste layer has already dried to become the first positive electrode mixture layer, so that the first carbon nanotubes in the first positive electrode mixture layer do not migrate into the second positive electrode paste layer.
[0014] In contrast, in the former manufacturing method, the second positive electrode paste layer is dried together with the first positive electrode paste layer. When these are dried, some of the second carbon nanotubes located on the current collector side of the second positive electrode paste layer may move to the surface side together with the solvent, and the second carbon nanotubes on the current collector side in the second positive electrode paste layer may decrease, but some of the first carbon nanotubes located on the surface side of the first positive electrode paste layer may move to the surface side together with the solvent and be arranged on the current collector side of the second positive electrode paste layer. Alternatively, some of the first carbon nanotubes may be arranged so as to straddle between the surface side of the first positive electrode paste layer and the current collector side of the second positive electrode paste layer. This allows the carbon nanotubes to be appropriately arranged on the current collector side of the second positive electrode paste layer, and the electrical resistivity in the thickness direction of the positive electrode plate can be further reduced. [Brief description of the drawings]
[0015] [Figure 1]3 is a flowchart showing the flow of a method for manufacturing a positive electrode plate according to the first embodiment. [Diagram 2] FIG. 4 is a diagram illustrating a first positive electrode paste preparation step according to Examples 1 and 2. [Diagram 3] FIG. 11 is a diagram illustrating a second positive electrode paste preparation step according to Examples 1 and 2. [Figure 4] FIG. 2 is a diagram illustrating a first coating step in Examples 1 and 2. [Diagram 5] FIG. 4 is a diagram illustrating a second coating step according to Example 1. [Figure 6] FIG. 2 is a diagram illustrating a drying step according to Example 1. [Figure 7] 1 is a schematic cross-sectional view of a positive electrode plate according to Example 1. [Figure 8] 10 is a flowchart showing the flow of a method for manufacturing a positive electrode plate according to Example 2. [Figure 9] FIG. 11 is a diagram illustrating the first drying in the drying step according to Example 2. [Figure 10] FIG. 11 is a diagram illustrating a second coating step according to Example 2. [Figure 11] FIG. 11 is a diagram illustrating the second drying in the drying step according to Example 2. [Figure 12] 1 is a schematic cross-sectional view of a positive electrode plate according to Example 2. [Figure 13] FIG. 1 is a diagram comparing electrical resistivities in the thickness direction of positive electrode plates. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] <Example 1> Next, a manufacturing method of the positive electrode plate according to Example 1 will be described. FIG. 1 is a flow chart showing the flow of the manufacturing method of the positive electrode plate 1 according to Example 1. First, in step S1 (first positive electrode paste preparation step), a first positive electrode paste 41 containing first carbon nanotubes 11, positive electrode active material particles 15, a binder (not shown), and a solvent 17 is prepared (see FIG. 2). The first positive electrode paste 41 contains only the first carbon nanotubes 11 as carbon nanotubes. In addition, in step S2 (second positive electrode paste preparation step), a second positive electrode paste 42 containing second carbon nanotubes 12, positive electrode active material particles 15, a binder (not shown), and a solvent 17 is prepared (see FIG. 3). The second positive electrode paste 42 contains only the second carbon nanotubes 12 as carbon nanotubes.
[0017] Also, the average length of the first carbon nanotubes 11 is longer than the average length of the second carbon nanotubes 12. Specifically, the average length of the first carbon nanotubes 11 is 1.3 μm, and the average length of the second carbon nanotubes 12 is 0.6 μm. More specifically, the length of the first carbon nanotubes 11 is within a range of 1.0 μm to 3.0 μm. On the other hand, the length of the second carbon nanotubes 12 is within a range of 0.3 μm to 0.8 μm.
[0018] Next, in step S3 (first coating step), the first positive electrode paste 41 is coated on the first surface 10b of the current collecting member 10 to form a first positive electrode paste layer 51 on the first surface 10b of the current collecting member 10 (see FIG. 4). In this embodiment 1, an aluminum foil having a first surface 10b and a second surface 10c is used as the current collecting member 10. Next, the process proceeds to step S4 (second coating step), where the second positive electrode paste 42 is coated on the surface 51b of the first positive electrode paste layer 51 to form a second positive electrode paste layer 52 (see FIG. 5). As a result, a drying target TD1 having the first positive electrode paste layer 51 on the first surface 10b of the current collecting member 10 and the second positive electrode paste layer 52 on the surface 51b of the first positive electrode paste layer 51 is prepared.
[0019] Thereafter, in step S5 (drying step), the first positive electrode paste layer 51 is dried together with the second positive electrode paste layer 52 to form the positive electrode composite layer 20. Specifically, as shown in Fig. 6, the first positive electrode paste layer 51 and the second positive electrode paste layer 52 of the drying target TD1 are dried by a drying furnace 80 including a plurality of hot air blowing units 81 located above and a plurality of transport rolls 85 located below. More specifically, while the drying target TD1 is transported in the transport direction DM by the transport rolls 85 with the second positive electrode paste layer 52 facing the hot air blowing unit 81 located above, the first positive electrode paste layer 51 and the second positive electrode paste layer 52 are dried by hot air HA blown out from the hot air blowing unit 81.
[0020] At this time, the solvent 17 contained in the first positive electrode paste layer 51 and the second positive electrode paste layer 52 moves to the surface 52b of the second positive electrode paste layer 52 and evaporates. As a result, the first positive electrode paste layer 51 becomes the first positive electrode mixture layer 21, and the second positive electrode paste layer 52 becomes the second positive electrode mixture layer 22, and a positive electrode mixture layer 20 consisting of the first positive electrode mixture layer 21 and the second positive electrode mixture layer 22 is formed on the first surface 10b of the current collecting member 10.
[0021] Thereafter, a positive electrode composite layer 20 consisting of a first positive electrode composite layer 21 and a second positive electrode composite layer 22 is also formed on the second surface 10c of the current collecting member 10. Specifically, in step S6 (first coating step), the first positive electrode paste 41 is coated on the second surface 10c of the current collecting member 10 to form a first positive electrode paste layer 51 on the second surface 10c of the current collecting member 10. Next, the process proceeds to step S7 (second coating step), where the second positive electrode paste 42 is coated on the surface 51b of the first positive electrode paste layer 51 to form a second positive electrode paste layer 52.
[0022] Thereafter, in step S8 (drying step), the first positive electrode paste layer 51 is dried together with the second positive electrode paste layer 52 by a drying furnace 80 to form a positive electrode mixture layer 20. At this time, the solvent 17 contained in the first positive electrode paste layer 51 and the second positive electrode paste layer 52 moves to the surface 52b of the second positive electrode paste layer 52 and evaporates. As a result, the first positive electrode paste layer 51 becomes the first positive electrode mixture layer 21, and the second positive electrode paste layer 52 becomes the second positive electrode mixture layer 22, and a positive electrode mixture layer 20 consisting of the first positive electrode mixture layer 21 and the second positive electrode mixture layer 22 is also formed on the second surface 10c of the current collecting member 10 (see FIG. 7). As a result, a positive electrode plate 1 (positive electrode plate 1 before pressing) having a positive electrode mixture layer 20 on both sides (the first surface 10b and the second surface 10c) of the current collecting member 10 is obtained. Thereafter, in step S9 (pressing step), positive electrode plate 1 is pressed in thickness direction DT to compress positive electrode mixture layer 20 in thickness direction DT, thereby completing positive electrode plate 1 (see FIG. 7).
[0023] In the past, when a positive electrode paste containing carbon nanotubes, positive electrode active material particles, and a solvent was applied onto the surface of a current collector to form a positive electrode paste layer, and the positive electrode paste layer was dried, some of the carbon nanotubes arranged on the current collector side in the positive electrode paste layer moved together with the solvent to the surface side (the side away from the current collector) of the positive electrode paste layer, resulting in a decrease in the amount of carbon nanotubes on the current collector side. Since the carbon nanotubes are lighter than the positive electrode active material particles, they move together with the solvent that is about to evaporate to the surface side of the positive electrode paste layer. For this reason, in the positive electrode mixture layer obtained by drying the positive electrode paste layer, the number of conductive paths on the current collector side decreased, which increased the electrical resistivity in the thickness direction of the positive electrode plate, and the current collecting ability of the positive electrode plate decreased.
[0024] In contrast, in this Example 1, the average length of the first carbon nanotubes 11 contained in the first positive electrode paste 41 is made longer than the average length of the second carbon nanotubes 12 contained in the second positive electrode paste 42. As a result, when the first positive electrode paste layer 51 is dried in steps S5 and S8 (drying steps), the first carbon nanotubes 11 arranged on the current collecting member 10 side in the first positive electrode paste layer 51 are less likely to move together with the solvent 17 toward the surface 51b side (the side away from the current collecting member 10, upward in FIG. 6), and therefore the first carbon nanotubes 11 located on the current collecting member 10 side (particularly, in contact with the current collecting member 10) are less likely to be reduced.
[0025] The reason is that when the first positive electrode paste layer 51 is dried, the first carbon nanotubes 11 in the first positive electrode paste layer 51 attempt to move toward the surfaces 51b, 52b together with the solvent 17 which is evaporating. However, since the first carbon nanotubes 11 are long, they are more likely to get caught on the positive electrode active material particles 15, and being caught on the positive electrode active material particles 15 makes it difficult for them to move toward the surfaces 51b, 52b.
[0026] In this Example 1, the viscosity of the first positive electrode paste 41 is set higher than the viscosity of the second positive electrode paste 42. As a result, when the first positive electrode paste layer 51 is dried in steps S5 and S8 (drying steps), the first carbon nanotubes 11 arranged on the current collecting member 10 side in the first positive electrode paste layer 51 are even less likely to move toward the surface 51b side (the side away from the current collecting member 10, upward in FIG. 6).
[0027] Therefore, according to the manufacturing method of this Example 1, it is possible to prevent the number of conductive paths on the current collecting member 10 side from decreasing in the first positive electrode mixture layer 21 obtained by drying the first positive electrode paste layer 51. This makes it possible to prevent the electrical resistivity of the positive electrode plate 1 in the thickness direction DT from increasing, and to prevent a decrease in the current collecting ability of the positive electrode plate 1. Therefore, according to the manufacturing method of this Example 1, it is possible to manufacture a positive electrode plate 1 having a small electrical resistivity (Ω·cm) in the thickness direction DT.
[0028] <Example 2> The manufacturing method of Example 2 is different from the manufacturing method of Example 1 in that after first positive electrode paste layer 151 is dried to form first positive electrode composite layer 121, second positive electrode paste 42 is applied onto surface 121b of first positive electrode composite layer 121, but otherwise is similar. The manufacturing method of the positive electrode plate of Example 2 will be described below. Fig. 8 is a flowchart showing the flow of the manufacturing method of positive electrode plate 101 of Example 2.
[0029] First, in step T1 (first positive electrode paste preparation step), a first positive electrode paste 41 equivalent to that in Example 1 is prepared (see FIG. 2). In addition, in step T2 (second positive electrode paste preparation step), a second positive electrode paste 42 equivalent to that in Example 1 is prepared (see FIG. 3). Next, in step T3 (first coating step), the first positive electrode paste 41 is coated on the first surface 10b of the current collecting member 10 to form a first positive electrode paste layer 151 on the first surface 10b of the current collecting member 10 (see FIG. 4). Next, the process proceeds to step T4 (first drying), where the first positive electrode paste layer 151 is dried using a drying furnace 80 to form a first positive electrode composite layer 121 (see FIG. 9).
[0030] Thereafter, in step T5 (second coating step), the second positive electrode paste 42 is coated on the surface 121b of the first positive electrode mixture layer 121 to form the second positive electrode paste layer 152 (see FIG. 10). Next, the process proceeds to step T6 (second drying), where the second positive electrode paste layer 152 is dried using a drying furnace 80 to form the second positive electrode mixture layer 122. As a result, the positive electrode mixture layer 120 consisting of the first positive electrode mixture layer 121 and the second positive electrode mixture layer 122 is formed on the first surface 10b of the current collecting member 10 (see FIG. 11).
[0031] Thereafter, a positive electrode mixture layer consisting of the first positive electrode mixture layer 121 and the second positive electrode mixture layer 122 is also formed on the second surface 10c of the current collecting member 10. 120 is formed. Specifically, in step T7 (first coating step), first positive electrode paste 41 is coated on second surface 10c of current collecting member 10 to form first positive electrode paste layer 151. Next, the process proceeds to step T8 (first drying), where first positive electrode paste layer 151 is dried to form first positive electrode composite layer 121. Thereafter, in step T9 (second coating step), second positive electrode paste 42 is coated on surface 121b of first positive electrode composite layer 121 to form second positive electrode paste layer 152.
[0032] Next, proceeding to step TA (second drying), the second positive electrode paste layer 152 is dried to form the second positive electrode composite layer 122. As a result, the positive electrode composite layer 120 consisting of the first positive electrode composite layer 121 and the second positive electrode composite layer 122 is also formed on the second surface 10c of the current collecting member 10 (see FIG. 12). As a result, the positive electrode plate 101 (the positive electrode plate 101 before pressing) having the positive electrode composite layer 120 on both sides (the first surface 10b and the second surface 10c) of the current collecting member 10 is obtained. Thereafter, in step TB (pressing step), the positive electrode plate 101 is pressed in the thickness direction DT to compress the positive electrode composite layer 120 in the thickness direction DT, thereby completing the positive electrode plate 101 (see FIG. 12). Note that step T4 (first drying), step T6 (second drying), step T8 (first drying), and step TA (second drying) in this embodiment 2 correspond to the drying step.
[0033] In this Example 2, similarly to Example 1, the average length of the first carbon nanotubes 11 contained in the first positive electrode paste 41 is set to be longer than the average length of the second carbon nanotubes 12 contained in the second positive electrode paste 42. As a result, when the first positive electrode paste layer 151 is dried in steps T4 and T8 (first drying), the first carbon nanotubes 11 arranged on the current collecting member 10 side in the first positive electrode paste layer 151 are less likely to move together with the solvent 17 toward the surface 151b side (the side away from the current collecting member 10, upward in FIG. 9), and therefore the first carbon nanotubes 11 located on the current collecting member 10 side (particularly, in contact with the current collecting member 10) are less likely to be reduced.
[0034] Also in this Example 2, the viscosity of the first positive electrode paste 41 is set higher than the viscosity of the second positive electrode paste 42. As a result, when the first positive electrode paste layer 151 is dried in steps T4 and T8 (first drying), the first carbon nanotubes 11 arranged on the current collecting member 10 side in the first positive electrode paste layer 151 become even less likely to move toward the surface 151b side (the side away from the current collecting member 10).
[0035] Therefore, according to the manufacturing method of this Example 2, it is possible to prevent the number of conductive paths on the current collecting member 10 side from decreasing in the first positive electrode composite layer 121 obtained by drying the first positive electrode paste layer 151. This makes it possible to prevent the electrical resistivity of the positive electrode plate 101 in the thickness direction DT from increasing, and to prevent a decrease in the current collecting ability of the positive electrode plate 101. Therefore, according to the manufacturing method of this Example 2, it is possible to manufacture a positive electrode plate 101 having a small electrical resistivity (Ω·cm) in the thickness direction DT.
[0036] <Comparison of electrical resistivity in the thickness direction of the positive electrode plate> Next, the electrical resistivity (Ω·cm) in the thickness direction DT of the positive electrode plates 1, 101 of Examples 1 and 2 was measured. In this measurement, the electrical resistivity in the thickness direction DT of the positive electrode plates 1, 101 was measured by a known method while a load of 3.5 kN was applied to the positive electrode plates 1, 101 in the thickness direction DT. These results are shown in comparison in FIG. 13. In addition, as Comparative Example 1, a positive electrode plate having only the second positive electrode mixture layer 122 on the first surface 10b and the second surface 10c of the current collecting member 10 was produced. That is, in Comparative Example 1, only the second positive electrode paste 42 containing the second carbon nanotubes 12 having a short average length was applied to the first surface 10b and the second surface 10c of the current collecting member 10 to produce a positive electrode plate.
[0037] In addition, as Comparative Example 2, a positive electrode plate having a second positive electrode composite layer 122 on the first surface 10b and the second surface 10c of the current collecting member 10 and a first positive electrode composite layer 121 on the second positive electrode composite layer 122 was produced. In this Comparative Example 2, contrary to Example 2, a second positive electrode paste 42 containing a second carbon nanotube 12 having a short average length was applied to the first surface 10b and the second surface 10c of the current collecting member 10, and this was dried to form the second positive electrode composite layer 122, and then the first positive electrode paste 41 was applied to the surface of the second positive electrode composite layer 122 and this was dried to form the first positive electrode composite layer 121. The electrical resistivity in the thickness direction of the positive electrode plates of Comparative Examples 1 and 2 was also measured in the same manner as the positive electrode plates 1 and 101 of Examples 1 and 2. These results are also shown in comparison in FIG. 13.
[0038] As shown in Fig. 13, the electrical resistivity in the thickness direction of the positive electrode plate in Examples 1 and 2 was smaller than that in Comparative Examples 1 and 2. The reason is that, unlike Comparative Examples 1 and 2, the first positive electrode paste 41 containing only the first carbon nanotubes 11 having an average length longer than that of the second carbon nanotubes 12 is applied to the first surface 10b and the second surface 10c of the current collecting member 10 in Examples 1 and 2. As a result, when the first positive electrode paste layer 51, 151 made of the first positive electrode paste 41 is dried, the first carbon nanotubes 11 arranged on the current collecting member 10 side in the first positive electrode paste layer 51, 151 are less likely to move to the surface 51b, 151b side together with the solvent 17, and the first carbon nanotubes 11 located on the current collecting member 10 side (particularly, in contact with the current collecting member 10) are less likely to decrease.
[0039] More specifically, when the first positive electrode paste layer 51, 151 is dried, the first carbon nanotubes 11 in the first positive electrode paste layer 51, 151 tend to move toward the surface 51b, 151b side together with the solvent 17 that is about to evaporate, but the first carbon nanotubes 11 are more likely to be caught by the positive electrode active material particles 15 due to their long length, and are less likely to move toward the surface 51b, 151b side due to their being caught by the positive electrode active material particles 15. This is believed to have suppressed the decrease in the carbon nanotubes on the current collector 10 side. Therefore, it is believed that the conductive path on the current collector 10 side is well formed in the positive electrode mixture layer 20, 120, and the electrical resistivity in the thickness direction of the positive electrode plate 1, 101 can be reduced.
[0040] On the other hand, in Comparative Examples 1 and 2, the second positive electrode paste 42 containing only the second carbon nanotubes 12 having an average length shorter than that of the first carbon nanotubes 11 as carbon nanotubes is applied to the first surface 10b and the second surface 10c of the current collecting member 10. For this reason, when the second positive electrode paste layer made of the second positive electrode paste 42 is dried, the second carbon nanotubes 12 arranged on the current collecting member 10 side in the second positive electrode paste layer tend to move toward the surface side together with the solvent 17, and the second carbon nanotubes 12 located on the current collecting member 10 side (particularly, in contact with the current collecting member 10) tend to decrease. For this reason, the conductive paths on the current collecting member 10 side in the positive electrode mixture layer are reduced, and the electrical resistivity in the thickness direction of the positive electrode plate is increased.
[0041] Furthermore, when the results of Example 1 and Example 2 are compared, the electrical resistivity in the thickness direction DT is smaller in Example 1 than in Example 2 (see FIG. 13). The reason for this is considered as follows. In Example 1, in the second coating step (step S4), the second positive electrode paste 42 is coated on the surface 51b of the first positive electrode paste layer 51 before drying, and then, in the drying step (step S5), the second positive electrode paste layer 52 is dried together with the first positive electrode paste layer 51. On the other hand, in Example 2, the first positive electrode paste layer 151 is dried to form the first positive electrode mixture layer 121 before the second positive electrode paste 42 is coated, and then, the second positive electrode paste layer 152 coated on the surface 121b of the first positive electrode mixture layer 121 is dried.
[0042] Specifically, in Examples 1 and 2, when the second positive electrode paste layer 52, 152 is dried, some of the second carbon nanotubes 12 located on the current collecting member 10 side of the second positive electrode paste layer 52, 152 migrate toward the surfaces 52b, 152b together with the solvent 17, and the number of second carbon nanotubes 12 on the current collecting member 10 side in the second positive electrode paste layer 52, 152 decreases.
[0043] However, in Example 1, since the second positive electrode paste layer 52 is dried together with the first positive electrode paste layer 51, when they are dried, a part of the first carbon nanotubes 11 located on the surface 51b side of the first positive electrode paste layer 51 moves to the surface 52b side together with the solvent 17 and is arranged on the current collecting member 10 side of the second positive electrode paste layer 52. In addition, a part of the first carbon nanotubes 11 is arranged so as to straddle between the surface 51b side of the first positive electrode paste layer 51 and the current collecting member 10 side of the second positive electrode paste layer 52. In this way, the first carbon nanotubes 11 are arranged on the current collecting member 10 side in the second positive electrode paste layer 52 so as to compensate for at least a part of the reduction in the second carbon nanotubes 12. As a result, in Example 1, the carbon nanotubes are appropriately arranged even on the current collecting member 10 side of the second positive electrode paste layer 52, and the electrical resistivity in the thickness direction DT of the positive electrode plate 1 is reduced.
[0044] On the other hand, in Example 2, when the second positive electrode paste layer 152 is dried, the first positive electrode paste layer 151 has already dried to become the first positive electrode mixture layer 121, so that the first carbon nanotubes 11 in the first positive electrode mixture layer 121 do not move into the second positive electrode paste layer 152. For this reason, when the second positive electrode paste layer 152 is dried, the carbon nanotubes on the current collecting member 10 side in the second positive electrode paste layer 152 are reduced by an amount that corresponds to the movement of the second carbon nanotubes 12 located on the current collecting member 10 side of the second positive electrode paste layer 152 toward the surface 152b.
[0045] As described above, it can be said that the manufacturing method of Example 1 can further reduce the electrical resistivity in the thickness direction of the positive electrode plate compared to the manufacturing method of Example 2. Therefore, it can be said that the manufacturing method of the positive electrode plate in which "in the second coating step, the second positive electrode paste is coated on the surface of the first positive electrode paste layer to form the second positive electrode paste layer, and in the drying step, the first positive electrode paste layer is dried together with the second positive electrode paste layer" is more preferable.
[0046] Although the present invention has been described above based on the embodiments (Examples 1 and 2), it goes without saying that the present invention is not limited to the above-mentioned embodiments and can be appropriately modified and applied without departing from the spirit of the present invention. [Explanation of symbols]
[0047] 1,101 Positive plate 10 Current collecting member 11 The first carbon nanotube 12 Secondary carbon nanotube 15 Positive electrode active material particles 17 Solvents 20,120 Positive electrode composite layer 21,121 First positive electrode mixture layer 22,122 Second positive electrode mixture layer 41 First positive electrode paste 42 2nd positive electrode paste 51,151 First positive electrode paste layer 52,152 Second positive electrode paste layer 80 Drying oven
Claims
1. A method for producing a positive electrode plate having a positive electrode mixture layer on a surface of a current collecting member, comprising the steps of: a first positive electrode paste preparation step of preparing a first positive electrode paste including first carbon nanotubes, positive electrode active material particles, and a solvent; a second positive electrode paste preparation step of preparing a second positive electrode paste containing second carbon nanotubes, the positive electrode active material particles, and the solvent; a first coating step of coating the first positive electrode paste on the surface of the current collecting member to form a first positive electrode paste layer on the surface of the current collecting member; a second coating step of coating the second positive electrode paste on a surface of the first positive electrode paste layer to form a second positive electrode paste layer; a drying step of drying the first positive electrode paste layer together with the second positive electrode paste layer to form the positive electrode mixture layer after the second coating step; a pressing step of pressing the positive electrode mixture layer in a thickness direction to compress it, The average length of the first carbon nanotubes is greater than the average length of the second carbon nanotubes. A method for manufacturing a positive electrode plate.
2. A method for producing a positive electrode plate having a positive electrode mixture layer on a surface of a current collecting member, comprising the steps of: a first positive electrode paste preparation step of preparing a first positive electrode paste including first carbon nanotubes, positive electrode active material particles, and a solvent; a second positive electrode paste preparation step of preparing a second positive electrode paste containing second carbon nanotubes, the positive electrode active material particles, and the solvent; a first coating step of coating the first positive electrode paste on the surface of the current collecting member to form a first positive electrode paste layer on the surface of the current collecting member; a first drying step of drying the first positive electrode paste layer to form a first positive electrode mixture layer; a second coating step of coating the second positive electrode paste on a surface of the first positive electrode mixture layer to form a second positive electrode paste layer; a second drying step of performing a second drying step of drying the second positive electrode paste layer to form the positive electrode mixture layer; a pressing step of pressing the positive electrode mixture layer in a thickness direction to compress it, The average length of the first carbon nanotubes is greater than the average length of the second carbon nanotubes. A method for manufacturing a positive electrode plate.
Citation Information
Patent Citations
Battery pole piece with multi-layer structure and preparation method of battery pole piece
CN113725399A
Positive electrode for lithium secondary battery, its manufacturing method, and lithium secondary battery
JP2008198596A
Positive electrode paste for lithium ion secondary battery, positive electrode manufacturing method, and positive electrode
JP2020184490A
Positive electrode for lithium ion secondary battery, lithium ion secondary battery, and manufacturing method of positive electrode for lithium ion secondary battery
JP2022055890A
Secondary battery electrode manufacturing method and secondary battery manufacturing method
WO2018186017A1