Water-based resin emulsions and coatings

The aqueous resin emulsion with a structured inner and protective layer addresses the issues of poor adhesion and slow drying in water-based sealers, offering improved adhesion, quick drying, and enhanced water resistance.

JP7565123B1Active Publication Date: 2024-10-10SAIDEN CHEM IND
View PDF 24 Cites 0 Cited by

Patent Information

Application Number
JP2024031593
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2024-03-01
Publication Date
2024-10-10
Estimated Expiration
2044-03-01

AI Technical Summary

Technical Problem

Existing water-based repair sealers exhibit poor wetting and permeability to various substrates, slow drying, and inadequate adhesion to both base materials and top coats, with insufficient water resistance and storage stability.

Method used

An aqueous resin emulsion comprising resin particles with an inner layer and a protective layer, where the inner layer is formed from a copolymer containing polymerizable monomers and crosslinkable monomers, and the protective layer is formed from a copolymer containing carboxyl group-containing monomers, with a specific weight ratio and particle diameter ratio that ensures quick drying, strong adhesion, and improved water resistance.

Benefits of technology

The emulsion provides excellent adhesion to base materials and top coats, quick drying properties, and enhanced storage stability, while maintaining water resistance and substrate compatibility.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007565123000001_ABST
    Figure 0007565123000001_ABST
Patent Text Reader

Abstract

An object of the present invention is to provide an aqueous resin emulsion which is excellent in adhesion to substrates and topcoat paints, quick drying properties, water resistance, and storage stability. [Solution] An aqueous resin emulsion containing resin particles including an inner layer and a protective layer surrounding the inner layer, wherein the inner layer contains a copolymer (A) containing a polymerizable monomer (a1) and a crosslinkable monomer (a2) as constituent units, and the protective layer contains at least a copolymer (B) containing a polymerizable monomer (b1) and a carboxy group-containing polymerizable monomer (b2) as constituent units, and a chain transfer agent, wherein the copolymer (A) contains 0.1 to 15% by weight of the crosslinkable monomer (a2) based on 100% by weight of all monomers constituting the copolymer (A), and the copolymer (B) contains 5 to 20% by weight of the carboxy group-containing polymerizable monomer (b2) based on 100% by weight of all monomers constituting the copolymer (B).
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an aqueous resin emulsion and a coated article. [Background technology]

[0002] At construction sites, the demand for repair applications is increasing year by year. Currently, weak solvent soluble acrylic lacquer type NAD resin paint is widely used as a repair undercoat material (hereinafter referred to as sealer) that combines high adhesion to Western roof tiles, aged slate roofs, various ceramic roof materials, and old coatings, a fragile surface reinforcement effect, and adhesion to topcoat coatings. In recent years, due to environmental considerations, there has been a shift from solvent-based to water-based not only topcoat paints but also sealers, and many water-based repair sealers have been developed.

[0003] However, compared with solvent-based sealers, water-based repair sealers have poor wetting and penetration into various substrates and old coatings, and have low adhesion to substrates. In addition, water-based repair sealers dry slowly, so there are many problems such as poor film formation when dried at room temperature, and poor water resistance and adhesion to topcoats.

[0004] Therefore, Patent Documents 1 and 2 propose an aqueous emulsion in which a dense coating film is formed by polymerizing an aromatic vinyl monomer (eg, styrene, α-methylstyrene, etc.) and thereby water-based emulsions with improved water resistance and adhesion are formed.

[0005] Patent Documents 3 and 4 propose a water-soluble resin emulsion containing a water-soluble resin or a hydrophobic resin, which is made soluble in an aqueous dispersion medium by neutralizing a copolymer containing an acrylic acid or methacrylic acid ester and a carboxyl group-containing unsaturated monomer with an alkali, thereby improving the wettability and permeability to the substrate, and improving the substrate adhesion and reinforcing effect. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2001-181605 A [Patent Document 2] JP 2015-166428 A [Patent Document 3] Japanese Patent Application Publication No. 11-217559 [Patent Document 4] JP 2006-241427 A Summary of the Invention [Problem to be solved by the invention]

[0007] However, in Patent Documents 1 and 2, a large amount of aromatic vinyl monomer is used in the production process of the aqueous emulsion, so that the coating film made of the aqueous emulsion is hard and brittle. Therefore, the aqueous emulsions of Patent Documents 1 and 2 may not be able to obtain sufficient adhesion to the substrate and sufficient reinforcing effect for the substrate.

[0008] In addition, in Patent Documents 3 and 4, the amount of carboxy-containing unsaturated monomer is large, and the coating film dries slowly at low temperatures from room temperature to cold regions, and the water resistance and adhesion to the top coat paint are insufficient. In Patent Document 4, the water resistance of the coating film is improved by reducing the average particle size of the resin particles (50 nm or less), but the storage stability is insufficient.

[0009] Therefore, an object of the present invention is to provide an aqueous resin emulsion which is excellent in adhesion to substrates and topcoat paints, quick drying properties, water resistance, and storage stability. [Means for solving the problem]

[0010] In order to achieve the object of the present invention, the present invention has the following configuration: That is, an aqueous resin emulsion containing resin particles including an inner layer and a protective layer surrounding the inner layer, the inner layer contains a copolymer (A) containing a polymerizable monomer (a1) and a crosslinkable monomer (a2) as constituent units, the protective layer contains at least a copolymer (B) containing a polymerizable monomer (b1) and a carboxyl group-containing polymerizable monomer (b2) as constituent units, and a chain transfer agent, the polymerizable monomer (a1) and the polymerizable monomer (b1) being selected from the group consisting of a (meth)acrylic acid alkyl ester monomer, a hydroxyl group-containing unsaturated ... the copolymer (A) contains 0.1 to 15% by weight of the crosslinkable monomer (a2) based on 100% by weight of all monomers constituting the copolymer (A); the copolymer (B) contains 5 to 20% by weight of the carboxy group-containing polymerizable monomer (b2) based on 100% by weight of all monomers constituting the copolymer (B); the weight average molecular weight (Mw) of the copolymer (B) is 3,000 to 20,000; and the average particle diameter D of the copolymer (A) is 1.0 to 1.0 mm. A and the average particle diameter D of the resin particles B Ratio to (D A / D B ) is greater than 0 and less than or equal to 0.70, where the average particle size D A is measured by the laser diffraction / scattering method, and the average particle diameter D B is measured by dynamic light scattering. Effect of the Invention

[0011] According to the present invention, it is possible to provide an aqueous resin emulsion which is excellent in adhesion to a substrate and a topcoat paint, quick drying property, water resistance, and storage stability. [Brief description of the drawings]

[0012] [Figure 1] FIG. 2 is a diagram for explaining an outline of a resin particle. [Diagram 2] FIG. 1 is a diagram for explaining how a resin particle emulsion penetrates into a substrate when DA / DB=0. [Diagram 3]FIG. 1 is a diagram for explaining how a resin particle emulsion penetrates into a substrate when DA / DB=0.7. [Figure 4] FIG. 1 is a diagram for explaining how a resin particle emulsion penetrates into a substrate when DA / DB is greater than 0.7. [Diagram 5] FIG. 1 is a diagram for explaining a state in which a resin particle emulsion remains on a substrate when DA / DB=0. [Figure 6] FIG. 1 is a diagram for explaining a state in which a resin particle emulsion remains on a substrate when DA / DB=0.7. [Figure 7] FIG. 13 is a diagram for explaining the state in which a resin particle emulsion remains on a substrate when DA / DB is greater than 0.7. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The following embodiments are described in detail. Note that the following embodiments do not limit the scope of the invention, and not all of the combinations of features described in the embodiments are essential to the invention. Two or more of the features described in the embodiments may be combined in any combination.

[0014] In this specification, any numerical range specified using "to" is intended to include the numerical values ​​before and after "to" as the lower and upper limit values ​​of the range.

[0015] In this specification, the term "(meth)acrylic" means to include both the terms "acrylic" and "methacrylic". Similarly, the term "(meth)acrylate" means to include both the terms "acrylate" and "methacrylate". Examples of the (meth)acrylic monomer include (meth)acrylic acid esters and (meth)acrylic acid, and (meth)acrylic acid may be in the form of a salt. Of these, it is more preferable to use (meth)acrylic acid esters and (meth)acrylic acid, and it is even more preferable to use (meth)acrylic acid esters.

[0016] <Water-based resin emulsion> The aqueous resin emulsion contains resin particles including an inner layer and a protective layer surrounding the inner layer. Such an aqueous resin emulsion can also be called a protective colloid type emulsion. The inner layer is formed of copolymer (A). The protective layer is formed of copolymer (B). Here, FIG. 1 is a diagram for explaining the outline of the resin particle.

[0017] The resin particle 100 includes an inner layer 110 and a protective layer 120 surrounding the inner layer 110. Although FIG. 1 shows only one resin particle 100 for ease of explanation, a plurality of resin particles 100 are present in a dispersion medium (e.g., water). The inner layer 110 (copolymer (A)) is a high molecular weight polymer that is insoluble in the dispersion medium (water). The protective layer 120 (copolymer (B)) is a water-soluble resin neutralized with a basic compound. The protective layer 120 can function as a dispersion stabilizer. The average particle diameter 130 is the average particle diameter of the inner layer 110, and is the average particle diameter D described below. A The average particle diameter 140 is the average particle diameter of the resin particles 100 including the protective layer 120 surrounding the inner layer 110, and corresponds to the average particle diameter D B In this specification, the term "average particle diameter D B Please note that " does not represent the average particle size of protective layer 120 alone without surrounding inner layer 110.

[0018] The weight ratio (B / A) of the copolymer (A) to the copolymer (B) is 25 / 75 to 75 / 25. When the weight ratio (B / A) is within the above-mentioned range, the D A / D B On the other hand, if the weight ratio (B / A) is not within the range of the above-mentioned predetermined ratio, D A / D B If the ratio is not equal to a predetermined ratio, only a part of the performance required for the aqueous resin emulsion will be achieved.

[0019] Average particle size D of copolymer (A) A and the average particle diameter of the resin particles D B Ratio to (D A / D B ) is greater than 0 and less than 0.70. Here, the average particle diameter D A is measured by the laser diffraction / scattering method, and the average particle diameter D B is measured by dynamic light scattering. The average particle diameter D of 100 resin particles in the aqueous resin emulsion is measured by the laser diffraction / scattering method. A and the average particle diameter D measured by dynamic light scattering. B D, which is the ratio of A / D B The thickness of the protective layer 120 can be determined by measuring A / D B If the thickness of the protective layer 120 satisfies the condition that the ratio is 0.70 or less, the particles of the inner layer 110 can be stably dispersed, and therefore the storage stability of the aqueous resin emulsion is excellent. A / D B The manner in which resin particles 100 having different ratios permeate into an inorganic porous substrate (one example being a calcium silicate board) will be described. Note that "calcium silicate board" is an abbreviated expression for calcium silicate board.

[0020] Figure 2(a) shows the D A / D B This shows the state before the resin particle emulsion is applied to the substrate when D = 0. A / D B When .gtoreq.0, the resin particles 100 have only the protective layer 120. The resin particles 100 are applied to the substrate 200. The substrate 200 is, for example, a calcium silicate board. FIG. 2(b) is a diagram showing the state after the resin particles 100 have penetrated into the substrate 200. Only the protective layer 120 exists in the substrate 200. This provides excellent reinforcement and adhesion to the substrate 200, but since there is no coating film on the substrate 200, adhesion to the topcoat paint and water resistance are poor.

[0021] Figure 3(a) shows the D A / D B This shows the state of the resin particle emulsion before it is applied to the substrate when D = 0.7. A / D BIn the case of .DELTA..times ...

[0022] Figure 4(a) shows the D A / D B This shows the state of the resin particle emulsion before it is applied to the substrate when D is greater than 0.7. A / D B = 0.7 or more, the resin particles 100 have both the inner layer 110 and the protective layer 120. The resin particles 100 are applied to the substrate 200. FIG. 4(b) is a diagram showing the state after the resin particles 100 have penetrated into the substrate 200. The inner layer 110 is present on the substrate 200, and the protective layer 120 is present inside the substrate 200. However, the average particle diameter D A Since the thickness of the protective layer 120 is increased, it is not possible to uniformly arrange the multiple protective layers 120 in the substrate 200, and gaps are generated between the protective layers 120. This reduces the reinforcement and adhesion of the substrate 200, but only improves the adhesion to the topcoat paint and water resistance.

[0023] <Protective layer> The protective layer contains at least a copolymer (B) containing, as structural units, a polymerizable monomer (b1) and a carboxy group-containing polymerizable monomer (b2), and a chain transfer agent.

[0024] (Copolymer (B)) The copolymer (B) contains 5 to 20% by weight of the carboxyl group-containing polymerizable monomer (b2) in 100% by weight of all monomers constituting the copolymer (B). Here, the acid amount (amount of the carboxyl group-containing polymerizable monomer) must be in the range of 5 to 20% by weight when all monomers constituting the copolymer (B) are taken as 100% by weight. For example, if the acid amount is less than 5% by weight, the copolymer (B) does not become a water-soluble resin. On the other hand, if the acid amount is more than 20% by weight, the drying of the coating film becomes slow and the adhesion to the substrate decreases.

[0025] (Polymerizable monomer (b1)) The copolymer (B) contains 80 to 95% by weight of the polymerizable monomer (b1) based on 100% by weight of all monomers constituting the copolymer (B).

[0026] The copolymer (B) can contain 0 to 15% by weight of a styrene-based monomer as a polymerizable monomer (b1) in 100% by weight of all monomers constituting the copolymer (B). Examples of styrene-based monomers include styrene, α-methylstyrene, chlorostyrene, methylstyrene, and t-butylstyrene. Here, when the copolymer (B) is produced using more than 15% by weight of a styrene-based monomer, the hydrophobicity of the copolymer (B) becomes strong, so that the water-soluble resin obtained by neutralizing the copolymer (B) becomes difficult to dissolve in water (that is, the dispersion stabilization function of the protective layer decreases). Therefore, when a styrene-based monomer is used as the polymerizable monomer (b1), it is preferable to use it in an amount of 15% by weight or less. That is, the copolymer (B) can contain 15% by weight or less of a styrene-based monomer as a polymerizable monomer (b1) in 100% by weight of all monomers constituting the copolymer (B).

[0027] The polymerizable monomer (b1) includes at least one of a (meth)acrylic acid alkyl ester monomer, a hydroxyl group-containing unsaturated monomer, an amide group-containing unsaturated monomer, and a piperidyl group-containing unsaturated monomer.

[0028] Examples of the (meth)acrylic acid alkyl ester monomer include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, sec-butyl (meth)acrylate, n-amyl (meth)acrylate, isoamyl (meth)acrylate, n-hexyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-nonyl (meth)acrylate, isononyl (meth)acrylate, n-decyl (meth)acrylate, iso Examples of the (meth)acrylic acid alkyl esters include linear or branched alkyl (meth) esters such as decyl (meth)acrylate, n-undecyl (meth)acrylate, n-dodecyl (meth)acrylate, n-tridecyl (meth)acrylate, n-tetradecyl (meth)acrylate, cetyl (meth)acrylate, stearyl (meth)acrylate, and behenyl (meth)acrylate; and alicyclic (meth)acrylic acid alkyl esters such as cyclohexyl (meth)acrylate, 4-tert-butylcyclohexyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentanyl (meth)acrylate, and dicyclopentenyl (meth)acrylate. One or more of these (meth)acrylic acid alkyl esters can be used. Among these, (meth)acrylic acid alkyl esters having linear or branched alkyl groups with 1 to 18 carbon atoms (more preferably 1 to 12) are preferred.

[0029] Examples of other (meth)acrylic acid ester monomers include polyalkylene glycol (meth)acrylates such as polyethylene glycol mono(meth)acrylate, polypropylene glycol mono(meth)acrylate, and methoxypolyethylene glycol mono(meth)acrylate; (meth)acrylic acid alkyl esters having halogen atoms such as 2-chloroethyl (meth)acrylate, trifluoroethyl (meth)acrylate, 2-(perfluorobutyl)ethyl (meth)acrylate, and perfluorooctylethyl (meth)acrylate; (meth)acrylic acid esters having amino groups such as 2-(dimethylamino)ethyl (meth)acrylate, 2-(diethylamino)ethyl (meth)acrylate, and 3-(dimethylamino)propyl (meth)acrylate; and (meth)acrylic acid esters having carboxy groups such as carboxyethyl (meth)acrylate and carboxypentyl (meth)acrylate. glycidyl (meth)acrylate, glycerin mono(meth)acrylate, 2-methylglycidyl (meth)acrylate, 3,4-epoxycyclohexylmethyl (meth)acrylate, and other (meth)acrylic acid esters and derivatives thereof having an epoxy group; 2-sulfoethyl (meth)acrylate, 3-sulfopropyl (meth)acrylate, and other (meth)acrylates having a sulfonic acid group; 2-(phosphonooxy)ethyl (meth)acrylate, and other (meth)acrylates having a phosphoric acid group; 2-isocyanatoethyl (meth)acrylate, and other (meth)acrylates having an isocyanate group; tetrahydrofurfuryl (meth)acrylate, and other (meth)acrylates having a heterocyclic ring; alkyl or aryl group-terminated polyalkylene glycol mono(meth)acrylate, and other (meth)acrylates having an alkyl or aryl group, and other (meth)acrylates. One or more of these may be used.

[0030] Examples of the hydroxyl group-containing unsaturated monomer include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, and (4-hydroxymethylcyclohexyl)methyl (meth)acrylate. One or more of these can be used.

[0031] Examples of the amide group-containing unsaturated monomer include unsaturated monomers having a cyano group, such as acrylonitrile and methacrylonitrile; acrylamide monomers such as (meth)acrylamide, N-methyl(meth)acrylamide, N-ethyl(meth)acrylamide, N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N-isopropyl(meth)acrylamide, N-methylol(meth)acrylamide, N-butoxymethyl(meth)acrylamide, N-[2-dimethylaminoethyl](meth)acrylamide, N-[3-dimethylaminopropyl](meth)acrylamide, diacetone acrylamide, 4-acryloylmorpholine, and 4-methacryloylmorpholine. These may be used alone or in combination.

[0032] Examples of the piperidyl group-containing unsaturated monomer include 1,2,2,6,6-pentamethyl-4-piperidyl methacrylate and 2,2,6,6-tetramethyl-4-piperidyl methacrylate, and one or more members selected from this group can be used.

[0033] (Carboxy group-containing polymerizable monomer (b2)) Examples of the carboxyl group-containing polymerizable monomer (b2) include unsaturated carboxylic acids such as (meth)acrylic acid, itaconic acid, maleic acid, fumaric acid, crotonic acid, and citraconic acid; anhydrides of unsaturated carboxylic acids such as maleic anhydride and itaconic anhydride; and monoesters of unsaturated carboxylic acids such as monomethyl maleate, monobutyl maleate, monomethyl itaconic acid, and monobutyl itaconic acid. It is more preferable to use one or more of these unsaturated carboxylic acid monomers. Among these, (meth)acrylic acid is more preferable.

[0034] (Crosslinking monomer (b3)) The copolymer (B) may further contain a crosslinkable monomer (b3) as a constituent unit. The crosslinkable monomer (b3) is an optional component, and may be contained in an amount of, for example, 0 to 5% by weight based on 100% by weight of all monomers constituting the copolymer (B). The crosslinkable monomer (b3) includes at least one of a multifunctional monomer and a silane coupling agent.

[0035] As the polyfunctional monomer, a monomer having two or more polymerizable unsaturated bonds can be used. Examples of the polyfunctional monomer include 2-hydroxy-3-acryloyloxypropyl (meth)acrylate, ethylene glycol di(meth)acrylate, 1,3-butanediol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, and the like. Examples of the acrylates include bifunctional (meth)acrylates such as (meth)acrylate, tripropylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, polytetramethylene glycol di(meth)acrylate, and glycerin di(meth)acrylate; polyfunctional (meth)acrylates such as pentaerythritol tri(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tetraacrylate, and dipentaerythritol hexaacrylate; allyl (meth)acrylate; divinylbenzene; and diallyl phthalate. One or more of these can be used.

[0036] Examples of the crosslinkable monomer include silane coupling agents such as vinyltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, and 3-acryloxypropyltrimethoxysilane, and one or more of these can be used.

[0037] The crosslinkable monomer can be appropriately selected and used according to the type of reactive group. For example, when the reactive group is a carbonyl group, it is preferable to use a polyfunctional hydrazide compound or the like as a crosslinking agent. When the reactive group is a carboxy group, it is preferable to use a polyfunctional epoxy compound, a polyfunctional carbodiimide compound, a melamine-based crosslinking agent such as methylolmelamine, a polyfunctional oxazoline compound, a polyvalent metal, or the like as a crosslinking agent. When the reactive group is a phosphoric acid group or a phosphoric acid ester group, it is preferable to use a compound having many hydroxyl groups as a crosslinking agent. When the reactive group is a hydroxyl group, it is preferable to use a polyfunctional isocyanate compound, its blocked isocyanate, acid anhydride, or the like as a crosslinking agent. When the reactive group is a glycidyl group, it is preferable to use a polyfunctional carboxy group-containing compound, polyamine, acid anhydride, or the like as a crosslinking agent. When the reactive group is an isocyanate group or a blocked isocyanate group, it is preferable to use a polyol, polyamine, polycarboxylic acid compound, or the like as a crosslinking agent. One or more of these reactive groups can be used.

[0038] Examples of polymerizable monomers having a carbonyl group as a reactive group include acrolein, diacetone (meth)acrylamide, diacetone (meth)acrylate, and acetoacetoxyethyl (meth)acrylate, etc. One or more of these can be used.

[0039] Examples of polymerizable monomers having a carboxy group as a reactive group, i.e., carboxy group-containing polymerizable monomers, include unsaturated carboxylic acids such as (meth)acrylic acid, itaconic acid, maleic acid, fumaric acid, crotonic acid, and citraconic acid; and monoesters of unsaturated carboxylic acids such as maleic acid monomethyl ester, maleic acid monobutyl ester, itaconic acid monomethyl ester, and itaconic acid monobutyl ester. In addition, examples of the carboxy group-containing polymerizable monomers may include those that generate a carboxy group when dissolved in water, such as anhydrides of unsaturated carboxylic acids such as maleic anhydride and itaconic anhydride. One or more of these can be used.

[0040] Examples of polymerizable monomers having a phosphoric acid group or a phosphoric acid ester group as a reactive group include (meth)acrylates having a phosphoric acid group such as 2-(phosphonooxy)ethyl (meth)acrylate, etc. One or more of these can be used.

[0041] Examples of polymerizable monomers having a hydroxyl group as a reactive group include hydroxyl group-containing (meth)acrylic acid esters such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, glycerin mono(meth)acrylate, 4-hydroxyphenyl (meth)acrylate, and [4-(hydroxymethyl)cyclohexyl]methyl (meth)acrylate. One or more of these can be used.

[0042] Examples of polymerizable monomers having an isocyanate group or a blocked isocyanate group as a reactive group include (meth)acrylates having an isocyanate group such as 2-isocyanatoethyl (meth)acrylate and 2-(2-methacryloyloxyethyloxy)ethyl isocyanate, etc. One or more of these can be used.

[0043] Examples of polymerizable monomers having a glycidyl group as a reactive group include glycidyl (meth)acrylate, 2-methylglycidyl (meth)acrylate, and 3,4-epoxycyclohexylmethyl (meth)acrylate, etc. One or more of these can be used.

[0044] (Chain transfer agent) The copolymer (B) contains 0.1 to 15.0% by weight of a chain transfer agent relative to 100% by weight of all monomers constituting the copolymer (B). In addition, by incorporating the above-mentioned predetermined amount of chain transfer agent into the copolymer (B), the weight average molecular weight (Mw) of the copolymer (B) can be controlled to 3000 to 20000, thereby improving the impregnation into the substrate. The chain transfer agent is not particularly limited, and one or more of alkyl mercaptans such as hexyl mercaptan, lauryl mercaptan, octyl mercaptan, n-dodecyl mercaptan, and t-dodecyl mercaptan can be used.

[0045] (hydrophilic solvent) As the hydrophilic solvent, one or more of alcohols such as methyl alcohol, ethyl alcohol, n-propyl alcohol, isopropyl alcohol, n-butyl alcohol, isobutyl alcohol, sec-butyl alcohol, tert-butyl alcohol, and tert-amyl alcohol; polyhydric alcohols such as ethylene glycol, propylene glycol, diethylene glycol, dipropylene glycol, and glycerin; ketones such as acetone, methyl ethyl ketone, and diacetone alcohol; and ethers such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, propylene glycol monomethyl ether, and dipropylene glycol monomethyl ether can be used. In addition, by using a hydrophilic solvent during the polymerization reaction of the polymerizable monomer (b1), etc., the effect of adjusting the molecular weight of the copolymer (B) and penetrating into the molecular chain occurs, and thus the water-solubilization of the copolymer (B) can be assisted.

[0046] (Physical properties of copolymer (B)) The pH of the copolymer (B) is 7.0 to 10.5. Here, in order to make the copolymer (B) a water-soluble resin, the copolymer (B) is neutralized with a basic compound 30 minutes after the end of polymerization. By making the pH of the copolymer (B) in the range of 7.0 to 10.5, the particles of the copolymer (B) are made into a water-soluble resin. Here, if the copolymer (B) is not properly made into a water-soluble resin, the copolymer (A) cannot be encapsulated, and the adhesion with the topcoat paint cannot be exhibited.

[0047] The haze of the copolymer (B) is 0 to 25%. As a guide for making the copolymer (B) into a water-soluble resin, if the haze of the copolymer (B) after neutralization (with ion-exchanged water as the standard: 0) is within the range of 0 to 25%, the copolymer (B) functions as a protective layer.

[0048] The weight average molecular weight (Mw) of the copolymer (B) is 3000 to 20000. Here, by having the weight average molecular weight (Mw) of the copolymer (B) in the above numerical range, the impregnation of the copolymer (B) into the substrate can be improved. If the weight average molecular weight (Mw) of the copolymer (B) is less than 3000, the function of the protective layer is reduced, so that the aqueous resin particle emulsion of the final product cannot be formed. On the other hand, if the weight average molecular weight (Mw) of the copolymer (B) is greater than 20000, the copolymer (B) is less likely to dissolve in water, so that it is difficult to become a water-soluble resin, and the impregnation into the substrate is reduced. If the water-soluble resin in which the high molecular weight copolymer (B) is dissolved in water is impregnated into the substrate, the cohesive force of the copolymer (B) is high, which causes the substrate material to break. Thus, if the weight average molecular weight (Mw) of the copolymer (B) is greater than 20000, there is a problem that the adhesion to the substrate is reduced.

[0049] Average particle diameter D B The average particle size D is 50 to 300 nm. B If is less than 50 nm, D A / D B When the average particle diameter D is in the range of 0 to 0.70, the protective layer becomes smaller than the core (inner layer), and the particles in the inner layer cannot be dispersed. More specifically, in the above case, aggregation and sedimentation are observed in a storage stability test at 50°C. B If is greater than 300 nm, D A / D B When the particle size of the core (inner layer) is in the range of 0 to 0.70, the particle size of the core (inner layer) is a maximum of 210 nm or more, and the water resistance of the substrate into which the water-based sealer penetrates deteriorates. Since the protective layer penetrates into the substrate, there is no particular problem, but if the particle size of the core (inner layer) that becomes a membrane on the substrate is larger than 210 nm, the interparticle spots become too large, which adversely affects the water resistance.

[0050] (Method for producing copolymer (B)) The copolymer (B) is produced by emulsifying and dispersing any combination of the polymerizable monomer (b1) to the crosslinkable monomer (b3) in an aqueous dispersion medium. Examples of the method for emulsifying and dispersing include known emulsion polymerization.

[0051] (aqueous dispersion medium) Examples of the aqueous dispersion medium include water, mixed solvents in which water is mixed with an alcohol (e.g., methanol, ethanol, etc.), and water-soluble solvents such as alcohols and glycol ethers. One or more solvents selected from this group can be used.

[0052] (emulsifier) When polymerizing the polymerizable monomer (b1) and the like, a surfactant can be used as an emulsifier. The emulsifier to be used is not particularly limited, but examples thereof include anionic surfactants, nonionic surfactants, cationic surfactants, and amphoteric surfactants, and one or more of these can be used. In the present invention, it is preferable to use an anionic surfactant and a nonionic surfactant, and it is more preferable to use an anionic surfactant.

[0053] (Polymerization initiator, polymerization accelerator) A polymerization initiator can be used when polymerizing the polymerizable monomer (b1) and the like. The polymerization initiator is not particularly limited, but examples thereof include persulfates, organic peroxides, and peroxides such as hydrogen peroxide, and azo compounds, and one or more of these can be used. In addition, a redox polymerization initiator used in combination with a peroxide, or one or more reducing agents can be used as a polymerization promoter.

[0054] Specific examples of persulfates include potassium persulfate, sodium persulfate, and ammonium persulfate.Specific examples of organic peroxides include diacyl peroxides such as benzoyl peroxide and dilauroyl peroxide, dialkyl peroxides such as t-butyl cumyl peroxide and dicumyl peroxide, peroxy esters such as t-butyl peroxy laurate and t-butyl peroxy benzoate, and hydroperoxides such as cumene hydroperoxide and t-butyl hydroperoxide.Specific examples of azo compounds include 2,2'-azobis(2-amidinopropane) dihydrochloride and 4,4'-azobis(4-cyanopentanoic acid).

[0055] The reducing agent as a polymerization promoter is not particularly limited, but examples thereof include ascorbic acid and its salts, erythorbic acid and its salts, tartaric acid and its salts, sulfurous acid and its salts, bisulfurous acid and its salts, thiosulfuric acid and its salts, and iron (II) salts.

[0056] (Basic compounds) Examples of basic compounds used when neutralizing the carboxyl group derived from the carboxyl group-containing polymerizable monomer (b2) include amines such as ammonia, methylamine, dimethylamine, trimethylamine, ethylamine, diethylamine, triethylamine, ethanolamine, diethanolamine, triethanolamine, and dimethylaminoethanol; aminoalcohols such as 1-amino-2-propanol, 2-amino-2-methyl-1-propanol, and N,N-dimethylaminoethanol; and alkali metal hydroxides such as potassium hydroxide and sodium hydroxide. One or more of these can be used.

[0057] (Other additives) A crosslinking agent may be used as necessary so long as the weight average molecular weight (Mw) of the copolymer (B) is within the range of 3000 to 20000. By using a crosslinking agent, the adhesion to the substrate and the water resistance of the aqueous resin emulsion can be improved.

[0058] <Inner layer> The inner layer contains a copolymer (A) containing a polymerizable monomer (a1) and a crosslinkable monomer (a2) as constituent units. By incorporating a crosslinking agent (crosslinkable monomer (a2)) into the copolymer (A), the copolymer (A) becomes hydrophobic, so that the coating film on the substrate can have water resistance and adhesion to the topcoat paint. In addition, the copolymer (A) is encapsulated in a highly hydrophilic protective layer (copolymer (B)).

[0059] (Copolymer (A)) The copolymer (A) contains 85 to 99.9% by weight of the polymerizable monomer (a1) and 0.1 to 15% by weight of the crosslinkable monomer (a2) based on 100% by weight of all monomers constituting the copolymer (A).

[0060] (Polymerizable monomer (a1)) The copolymer (A) can contain 0 to 15% by weight of a styrene-based monomer as a polymerizable monomer (a1) in 100% by weight of all monomers constituting the copolymer (A). Examples of styrene-based monomers include styrene, α-methylstyrene, chlorostyrene, methylstyrene, and t-butylstyrene. Here, when the copolymer (A) is produced using more than 15% by weight of a styrene-based monomer, the structural strength of the copolymer (A) increases, but the coating film becomes too hard, which may cause a decrease in adhesion to the substrate (substrate material breakage). Therefore, when a styrene-based monomer is used as the polymerizable monomer (a1), it is preferable to use it in an amount of 15% by weight or less. That is, the copolymer (A) can contain 15% by weight or less of a styrene-based monomer as a polymerizable monomer (a1) in 100% by weight of all monomers constituting the copolymer (A).

[0061] The polymerizable monomer (a1) includes at least one of a (meth)acrylic acid alkyl ester monomer, a hydroxyl group-containing unsaturated monomer, an amide group-containing unsaturated monomer, and a piperidyl group-containing unsaturated monomer.

[0062] Examples of the (meth)acrylic acid alkyl ester monomer include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, sec-butyl (meth)acrylate, n-amyl (meth)acrylate, isoamyl (meth)acrylate, n-hexyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-nonyl (meth)acrylate, isononyl (meth)acrylate, n-decyl (meth)acrylate, iso Examples of the (meth)acrylic acid alkyl esters include linear or branched alkyl (meth) esters such as decyl (meth)acrylate, n-undecyl (meth)acrylate, n-dodecyl (meth)acrylate, n-tridecyl (meth)acrylate, n-tetradecyl (meth)acrylate, cetyl (meth)acrylate, stearyl (meth)acrylate, and behenyl (meth)acrylate; and alicyclic (meth)acrylic acid alkyl esters such as cyclohexyl (meth)acrylate, 4-tert-butylcyclohexyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentanyl (meth)acrylate, and dicyclopentenyl (meth)acrylate. One or more of these (meth)acrylic acid alkyl esters can be used. Among these, (meth)acrylic acid alkyl esters having linear or branched alkyl groups with 1 to 18 carbon atoms (more preferably 1 to 12) are preferred.

[0063] Examples of other (meth)acrylic acid ester monomers include polyalkylene glycol (meth)acrylates such as polyethylene glycol mono(meth)acrylate, polypropylene glycol mono(meth)acrylate, and methoxypolyethylene glycol mono(meth)acrylate; (meth)acrylic acid alkyl esters having halogen atoms such as 2-chloroethyl (meth)acrylate, trifluoroethyl (meth)acrylate, 2-(perfluorobutyl)ethyl (meth)acrylate, and perfluorooctylethyl (meth)acrylate; (meth)acrylic acid esters having amino groups such as 2-(dimethylamino)ethyl (meth)acrylate, 2-(diethylamino)ethyl (meth)acrylate, and 3-(dimethylamino)propyl (meth)acrylate; and (meth)acrylic acid esters having carboxy groups such as carboxyethyl (meth)acrylate and carboxypentyl (meth)acrylate. glycidyl (meth)acrylate, glycerin mono(meth)acrylate, 2-methylglycidyl (meth)acrylate, 3,4-epoxycyclohexylmethyl (meth)acrylate, and other (meth)acrylic acid esters and derivatives thereof having an epoxy group; 2-sulfoethyl (meth)acrylate, 3-sulfopropyl (meth)acrylate, and other (meth)acrylates having a sulfonic acid group; 2-(phosphonooxy)ethyl (meth)acrylate, and other (meth)acrylates having a phosphoric acid group; 2-isocyanatoethyl (meth)acrylate, and other (meth)acrylates having an isocyanate group; tetrahydrofurfuryl (meth)acrylate, and other (meth)acrylates having a heterocyclic ring; alkyl or aryl group-terminated polyalkylene glycol mono(meth)acrylate, and other (meth)acrylates having an alkyl or aryl group, and other (meth)acrylates. One or more of these may be used.

[0064] Examples of the hydroxyl group-containing unsaturated monomer include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, and (4-hydroxymethylcyclohexyl)methyl (meth)acrylate. One or more of these can be used.

[0065] Examples of the amide group-containing unsaturated monomer include unsaturated monomers having a cyano group, such as acrylonitrile and methacrylonitrile; acrylamide monomers such as (meth)acrylamide, N-methyl(meth)acrylamide, N-ethyl(meth)acrylamide, N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N-isopropyl(meth)acrylamide, N-methylol(meth)acrylamide, N-butoxymethyl(meth)acrylamide, N-[2-dimethylaminoethyl](meth)acrylamide, N-[3-dimethylaminopropyl](meth)acrylamide, diacetone acrylamide, 4-acryloylmorpholine, and 4-methacryloylmorpholine. These may be used alone or in combination.

[0066] Examples of the piperidyl group-containing unsaturated monomer include 1,2,2,6,6-pentamethyl-4-piperidyl methacrylate and 2,2,6,6-tetramethyl-4-piperidyl methacrylate, and one or more members selected from this group can be used.

[0067] (Crosslinkable monomer (a2)) The crosslinkable monomer (a2) includes at least one of a polyfunctional monomer and a silane coupling agent.

[0068] As the polyfunctional monomer, a monomer having two or more polymerizable unsaturated bonds can be used. Examples of the polyfunctional monomer include 2-hydroxy-3-acryloyloxypropyl (meth)acrylate, ethylene glycol di(meth)acrylate, 1,3-butanediol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, and the like. Examples of the acrylates include bifunctional (meth)acrylates such as (meth)acrylate, tripropylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, polytetramethylene glycol di(meth)acrylate, and glycerin di(meth)acrylate; polyfunctional (meth)acrylates such as pentaerythritol tri(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tetraacrylate, and dipentaerythritol hexaacrylate; allyl (meth)acrylate; divinylbenzene; and diallyl phthalate. One or more of these can be used.

[0069] Examples of the crosslinkable monomer (a2) include silane coupling agents such as vinyltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, and 3-acryloxypropyltrimethoxysilane, and one or more of these can be used.

[0070] The crosslinkable monomer (a2) can be appropriately selected and used according to the type of reactive group. For example, when the reactive group is a carbonyl group, it is preferable to use a polyfunctional hydrazide compound or the like as a crosslinking agent. When the reactive group is a carboxy group, it is preferable to use a polyfunctional epoxy compound, a polyfunctional carbodiimide compound, a melamine-based crosslinking agent such as methylolmelamine, a polyfunctional oxazoline compound, a polyvalent metal, or the like as a crosslinking agent. When the reactive group is a phosphoric acid group or a phosphoric acid ester group, it is preferable to use a compound having many hydroxyl groups as a crosslinking agent. When the reactive group is a hydroxyl group, it is preferable to use a polyfunctional isocyanate compound, its blocked isocyanate, acid anhydride, or the like as a crosslinking agent. When the reactive group is a glycidyl group, it is preferable to use a polyfunctional carboxy group-containing compound, polyamine, acid anhydride, or the like as a crosslinking agent. When the reactive group is an isocyanate group or a blocked isocyanate group, it is preferable to use a polyol, polyamine, polycarboxylic acid compound, or the like as a crosslinking agent. One or more of these reactive groups can be used.

[0071] Examples of polymerizable monomers having a carbonyl group as a reactive group include acrolein, diacetone (meth)acrylamide, diacetone (meth)acrylate, and acetoacetoxyethyl (meth)acrylate, etc. One or more of these can be used.

[0072] Examples of polymerizable monomers having a carboxy group as a reactive group, i.e., carboxy group-containing polymerizable monomers, include unsaturated carboxylic acids such as (meth)acrylic acid, itaconic acid, maleic acid, fumaric acid, crotonic acid, and citraconic acid; and monoesters of unsaturated carboxylic acids such as maleic acid monomethyl ester, maleic acid monobutyl ester, itaconic acid monomethyl ester, and itaconic acid monobutyl ester. In addition, examples of the carboxy group-containing polymerizable monomers may include those that generate a carboxy group when dissolved in water, such as anhydrides of unsaturated carboxylic acids such as maleic anhydride and itaconic anhydride. One or more of these can be used.

[0073] Examples of polymerizable monomers having a phosphoric acid group or a phosphoric acid ester group as a reactive group include (meth)acrylates having a phosphoric acid group such as 2-(phosphonooxy)ethyl (meth)acrylate, etc. One or more of these can be used.

[0074] Examples of polymerizable monomers having a hydroxyl group as a reactive group include hydroxyl group-containing (meth)acrylic acid esters such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, glycerin mono(meth)acrylate, 4-hydroxyphenyl (meth)acrylate, and [4-(hydroxymethyl)cyclohexyl]methyl (meth)acrylate. One or more of these can be used.

[0075] Examples of polymerizable monomers having an isocyanate group or a blocked isocyanate group as a reactive group include (meth)acrylates having an isocyanate group such as 2-isocyanatoethyl (meth)acrylate and 2-(2-methacryloyloxyethyloxy)ethyl isocyanate, etc. One or more of these can be used.

[0076] Examples of polymerizable monomers having a glycidyl group as a reactive group include glycidyl (meth)acrylate, 2-methylglycidyl (meth)acrylate, and 3,4-epoxycyclohexylmethyl (meth)acrylate, etc. One or more of these can be used.

[0077] (Method for producing copolymer (A)) The copolymer (A) is produced by emulsifying and dispersing the polymerizable monomer (a1) and the crosslinkable monomer (a2) in an aqueous dispersion medium. Examples of the method for emulsifying and dispersing include known emulsion polymerization.

[0078] (aqueous dispersion medium) Examples of the aqueous dispersion medium include water, mixed solvents in which water is mixed with an alcohol (e.g., methanol, ethanol, etc.), and water-soluble solvents such as alcohols and glycol ethers. One or more solvents selected from this group can be used.

[0079] (emulsifier) When polymerizing the polymerizable monomer (a1) and the like, a surfactant can be used as an emulsifier. The emulsifier to be used is not particularly limited, but examples thereof include anionic surfactants, nonionic surfactants, cationic surfactants, and amphoteric surfactants, and one or more of these can be used. In the present invention, it is preferable to use an anionic surfactant and a nonionic surfactant, and it is more preferable to use an anionic surfactant.

[0080] (Polymerization initiator, polymerization accelerator) When polymerizing the polymerizable monomer (a1), a polymerization initiator can be used. The polymerization initiator is not particularly limited, but examples thereof include persulfates, organic peroxides, and peroxides such as hydrogen peroxide, and azo compounds, and one or more of these can be used. In addition, a redox polymerization initiator used in combination with a peroxide, or one or more reducing agents can be used as a polymerization promoter.

[0081] Specific examples of persulfates include potassium persulfate, sodium persulfate, and ammonium persulfate.Specific examples of organic peroxides include diacyl peroxides such as benzoyl peroxide and dilauroyl peroxide, dialkyl peroxides such as t-butyl cumyl peroxide and dicumyl peroxide, peroxy esters such as t-butyl peroxy laurate and t-butyl peroxy benzoate, and hydroperoxides such as cumene hydroperoxide and t-butyl hydroperoxide.Specific examples of azo compounds include 2,2'-azobis(2-amidinopropane) dihydrochloride and 4,4'-azobis(4-cyanopentanoic acid).

[0082] The reducing agent as a polymerization promoter is not particularly limited, but examples thereof include ascorbic acid and its salts, erythorbic acid and its salts, tartaric acid and its salts, sulfurous acid and its salts, bisulfurous acid and its salts, thiosulfuric acid and its salts, and iron (II) salts.

[0083] <Applications of water-based resin emulsion> The aqueous resin emulsion has both a sealer application and a primer application. The aqueous resin emulsion can be used, for example, for both an aqueous sealer application (for inorganic building materials such as roof tiles, calcium silicate boards, aged slate roofs, various ceramic roof materials, and old coating films) and a primer application.

[0084] Conventional water-based sealers have only one of two uses: as a sealer (reinforcing impregnated substrates and adhering to substrates (anchor effect)) or as a primer (suppressing absorption of topcoat paint and improving adhesion to topcoats). In other words, users had to prepare water-based sealers for sealer use and water-based sealers for primer use, and engage in repair work while using these sealers appropriately. In this way, users felt that it was troublesome in terms of increasing the management and workload of the sealers. In addition, the substrate to which the water-based sealer is applied is generally an inorganic porous substrate, but the permeability of the sealer differs depending on the number of voids (large or small) in the inorganic porous substrate. In other words, when the type of inorganic porous substrate (for example, the size and number of voids) changes, there were cases where conventional water-based sealers could not exhibit sufficient sealing performance, or could not exhibit sealing performance at all.

[0085] On the other hand, the aqueous resin emulsion of the present invention is a sealer that can be used both as a sealer and as a primer, so that the burden on the user during management and operation of the sealer can be reduced. In addition, the aqueous resin emulsion of the present invention has the following characteristics so that it can exhibit sufficient sealing performance even if the type of inorganic porous substrate to which the aqueous sealer is applied is changed. That is, the aqueous resin emulsion can adequately seal and reinforce inorganic porous substrates having various voids by taking the form of a protective colloid type emulsion. The protective colloid type emulsion refers to a resin particle emulsion containing a water-soluble resin (first protective layer) obtained by neutralizing a high acid value emulsion and a water-insoluble high molecular weight polymer (second inner layer) formed therein.

[0086] The mechanism by which the aqueous resin emulsion of the present invention permeates into a calcium silicate board (a substrate into which an aqueous sealer can easily permeate) as an example of an inorganic porous substrate has been described with reference to Figs. 2 to 4, but a supplementary explanation will be given below.

[0087] First, the first layer of water-soluble resin is impregnated into the calcium silicate board, reinforcing it and increasing adhesion to the board. In this way, the water-soluble resin exerts a sealer effect. Next, the second layer of high molecular weight polymer that remains without impregnating the calcium silicate board exerts a primer effect, increasing adhesion to the top coat paint.

[0088] Meanwhile, the mechanism by which the aqueous resin emulsion of the present invention forms a coating film on a slate board (a substrate into which an aqueous sealer does not easily or does not penetrate) as an example of an inorganic porous substrate will be described with reference to Figs. 5 to 7.

[0089] First, Figure 5(a) shows the D A / D B This shows the state before the resin particle emulsion is applied to the substrate when D = 0. A / D B In the case where ρ=0, the resin particles 100 have only the protective layer 120. The resin particles 100 are applied to the substrate 300. The substrate 300 is, for example, a slate board. FIG. 5(b) is a diagram showing the state in which the resin particles 100 remain on the substrate 300. Since the resin particles 100 do not penetrate the substrate 300, only the protective layer 120 exists on the substrate 300. In the state of FIG. 5(b), the protective layer 120 (water-soluble resin) does not dry, and the protective layer 120, which has strong water retention, absorbs water. As a result, when the resin particle emulsion of FIG. 5 is applied to a substrate that is difficult to penetrate or does not penetrate, the film-forming property, adhesion to the topcoat paint, and water resistance are poor.

[0090] Figure 6(a) shows the D A / D B This shows the state of the resin particle emulsion before it is applied to the substrate when D = 0.7. A / D B When .gtoreq.0.7, the resin particle 100 has both the inner layer 110 and the protective layer 120. The resin particle 100 is applied to the substrate 300. FIG.

[0091] The first protective layer 120 (water-soluble resin) hardly penetrates into the substrate 300 (slate board), and remains on the substrate 300 (slate board) together with the second inner layer 110 (high molecular weight polymer). However, since the water-soluble resin has high water retention and does not take a particulate form, it acts as an aid in particle fusion of the second layer copolymer (A), i.e., the high molecular weight polymer. As a result, as shown in Figure 6(c), a uniform film with no gaps between the particles of the inner layer 110 (high molecular weight polymer) is formed, resulting in excellent water resistance, adhesion to the top coat paint, and aesthetic appearance of the coated product (slate board).

[0092] Figure 7(a) shows the D A / D B This shows the state of the resin particle emulsion before it is applied to the substrate when D is greater than 0.7. A / D B = 0.7 or more, the resin particles 100 have both the inner layer 110 and the protective layer 120. The resin particles 100 are applied to the substrate 300. FIG. 7(b) is a diagram showing the state in which the resin particles 100 remain on the substrate 300. Here, the resin particles 100 in FIG. 7(b) have the inner layer 110 with a larger average particle diameter 130 and the protective layer 120 with a smaller thickness and less than a predetermined amount compared to the resin particles 100 in FIG. 6. Therefore, the protective layer 120 (water-soluble resin) cannot promote particle fusion of the inner layer 110, and it is difficult to form a uniform film without gaps between the inner layers 110 on the substrate 300. As a result, when the resin particle emulsion in FIG. 7 is applied to a substrate that is difficult or not permeable, the film-forming property, adhesion to the topcoat paint, and water resistance are poor.

[0093] In this way, the aqueous resin emulsion of the present invention can fully exert the effect of being used as a sealer and / or a primer for various inorganic porous substrates having different permeabilities. Therefore, the aqueous resin emulsion of the present invention has the excellent effect of being able to play two roles as a sealer and a primer.

[0094] <Painted items> The coated article comprises a substrate and a coating film formed of an aqueous resin emulsion provided on at least one surface of the substrate. The aqueous resin emulsion is the aqueous resin emulsion described above.

[0095] The gel fraction of the coating film is 50 to 100%. Here, the level of water resistance can be determined by preparing a coating film of the aqueous resin emulsion (a film formed by drying the aqueous resin emulsion) and measuring the gel fraction of the coating film. If the gel fraction of the coating film is less than 50%, the coating film has poor water resistance and the coating film will have blisters and peeling, resulting in reduced adhesion to the substrate.

[0096] (base material) The substrate includes an inorganic porous substrate. Examples of the substrate include substrates into which the aqueous resin emulsion easily penetrates, such as calcium silicate boards, wood-chip cement boards, pulp cement boards, siding boards, and deteriorated old coatings (such as deteriorated roof tiles and deteriorated Colonial (registered trademark)), and substrates into which the aqueous resin emulsion does not easily penetrate, such as slate boards (flexible boards), roof tiles, and galvanized iron.

[0097] <Method for producing aqueous resin emulsion> The method for producing the aqueous resin emulsion includes at least the following three steps: a step of polymerizing 80 to 95% by weight of a polymerizable monomer (b1) and 5 to 20% by weight of a carboxyl group-containing polymerizable monomer (b2) in an aqueous medium in the presence of a surfactant, a polymerization initiator, and a chain transfer agent to produce a copolymer (B), a step of neutralizing the copolymer (B) with a basic compound, and a step of polymerizing 85 to 99.9% by weight of a polymerizable monomer (a1) and 0.1 to 15% by weight of a crosslinkable monomer (a2) in an aqueous solution of the neutralized copolymer (B) to produce a copolymer (A). The polymerizable monomer (a1) and the polymerizable monomer (b1) include at least one of a (meth)acrylic acid alkyl ester monomer, a hydroxyl group-containing unsaturated monomer, an amide group-containing unsaturated monomer, and a piperidyl group-containing unsaturated monomer. The weight average molecular weight (Mw) of the copolymer (B) is 3000 to 20000. The average particle size D of the copolymer (A) A and the average particle diameter of the resin particles DB Ratio to (D A / D B ) is greater than 0 and less than 0.70. Here, the average particle diameter D A is measured by the laser diffraction / scattering method, and the average particle diameter D B The specific configuration and characteristics of the aqueous resin emulsion are described above, and therefore will not be described in detail.

[0098] The manufacturing method of the aqueous resin emulsion will be described below. Table 1 shows the raw material composition and physical property values ​​of Examples 1 to 7. Table 2 shows the raw material composition and physical property values ​​of Examples 8 to 14. Table 3 shows the raw material composition and physical property values ​​of Examples 15 to 17 and Comparative Examples 1 to 4. Table 4 shows the raw material composition and physical property values ​​of Comparative Examples 5 to 11.

[0099] [Table 1]

[0100] [Table 2]

[0101] [Table 3]

[0102] [Table 4]

[0103] (Example 1: Method for producing copolymer (B)) 21.8 parts of ion-exchanged water, 2.0 parts of sodium polyoxyethylene alkyl ether sulfate (manufactured by Kao Corporation, product name: Latemul E-118B) as an emulsifier, 6.5 parts of cyclohexyl methacrylate and 15 parts of methyl methacrylate as polymerizable monomers (b1), 3.5 parts of methacrylic acid (100%) as a carboxyl group-containing polymerizable monomer (b2), 1.5 parts of ISO-propyl alcohol as a hydrophilic solvent, and 1.5 parts of n-dodecyl mercaptan as a chain transfer agent were weighed and stirred. In this way, an emulsified mixture (1) in which the monomers constituting the copolymer (B) were mixed was prepared.

[0104] A 2L three-neck round-bottom flask equipped with a stirrer, reflux condenser, thermometer, dropping device, and nitrogen gas inlet tube was charged with 52.5 parts of ion-exchanged water and 0.3 parts of sodium polyoxyethylene alkyl ether sulfate (manufactured by Kao Corporation, product name: LATEMURU E-118B), and the air in the flask was replaced with nitrogen gas, and the internal temperature of the flask was heated to 80°C while stirring. Next, 4.0 parts of a 5% aqueous solution of ammonium persulfate (manufactured by Mitsubishi Gas Chemical Co., Ltd., product name: ammonium persulfate) was added to the flask, and immediately, the previously prepared emulsion mixture (1) and 1.0 part of a 5% aqueous solution of ammonium persulfate were dropped over 1.0 hour. After 30 minutes, 4.4 parts of triethanolamine were added, and the mixture was left at 80°C for 30 minutes to obtain a copolymer (B).

[0105] (Example 1: Production method of copolymer (A)) 41.7 parts of ion-exchanged water, 2.5 parts of polyoxyethylene-1-(allyloxymethyl) alkyl ether ammonium sulfate (manufactured by Daiichi Kogyo Seiyaku Co., Ltd., product name: Aqualon KH-10) as an emulsifier, 34.5 parts of 2-ethylhexyl acrylate, 19 parts of cyclohexyl methacrylate, and 21 parts of methyl methacrylate as polymerizable monomers (a1), and 0.5 parts of trimethylolpropane trimethacrylate as crosslinkable monomers (a2) were weighed and stirred. In this way, an emulsified mixture (2) containing the monomers constituting the copolymer (A) was prepared.

[0106] (Example 1: Manufacturing method of aqueous resin emulsion) Then, 60 minutes after the dropwise addition of the emulsified mixture (1) was completed, the prepared emulsified mixture (2) and 3.0 parts of 5% ammonium persulfate were dropped into the flask over 3.0 hours. Then, while maintaining the internal temperature of the flask at 80°C, the reaction was continued for another 3.0 hours, after which the internal temperature was cooled to room temperature, and the pH was adjusted to about 8.5 with ammonia (25%) and water, and the solid content was adjusted to 35.0%, and then the mixture was filtered to remove aggregates. As a result, an aqueous resin emulsion of Example 1 was obtained, which contains resin particles in which a protective layer (copolymer (B)) surrounds an inner layer (copolymer (A)). The physical property analysis results of the aqueous resin emulsion were viscosity: 10 mPa·s / 25°C, solid content: 35.0%, pH: 8.5, and average particle diameter D by dynamic light scattering method. B Here, the method for analyzing the physical properties of the copolymer (A / B) and the aqueous resin emulsion will be described.

[0107] (Measurement of weight average molecular weight (Mw) of copolymer (B)) The weight average molecular weight (Mw) of the copolymer (B) was measured by GPC (gel permeation chromatography) under the following measurement conditions. Measurement conditions Analytical equipment: Tosoh HLC-8120GPC Column: Shodex KF-G (guard column) + KF-806M x 2 Column temperature: 40℃ ·Flow rate: 1.0ml / min ·Injection volume: 100μl Mobile phase: Tetrahydrofuran (THF) Detector: Refractometer (RI) Standard sample: polystyrene

[0108] (Measurement of Haze of Copolymer (B)) The haze of the copolymer (B) was measured by the following measurement and calculation methods. Haze meter: Nippon Denshoku Industries Co., Ltd., NDH4000 type Haze (diffuse transmittance / total light transmittance x 100%)

[0109] (Average particle size D of copolymer (A) measured by laser diffraction / scattering method) A Measurement of Average particle size D of resin particles in water-based resin emulsion measured by laser diffraction / scattering method A Specifically, the particle size distribution measuring device using the laser diffraction / scattering method (Shimadzu Corporation, product name "Laser Diffraction Nanoparticle Size Distribution Measuring Device SALD-7100") was used to measure the particle size (D50) at a cumulative 50% in the volume-based particle size distribution when the refractive index was 1.35-0.05i, which was defined as the average particle size D A was measured as.

[0110] (Average particle size of resin particles measured by dynamic light scattering method D B Measurement of Average particle size D of resin particles in water-based resin emulsion measured by dynamic light scattering method B Specifically, the average particle diameter D (nm) was measured by cumulant analysis using a particle size distribution measuring device (manufactured by Otsuka Electronics, product name "Concentrated Particle Size Analyzer FPER-1000") that utilizes dynamic light scattering and a concentrated probe. B The average particle diameter D A and D. B Using the measured values ​​of each, the ratio of them, D A / D B was calculated.

[0111] (manufacturing stability) The agglomerates formed during the production of the aqueous resin emulsion were evaluated according to the following criteria. ◯: Almost no formation of aggregates was observed. △: A small amount of aggregates was formed. ×: A large amount of aggregates was formed.

[0112] (Storage stability) The aqueous resin emulsion was placed in a glass vial and allowed to stand at 50° C. After one week of standing, the state of the contents was visually evaluated based on the presence or absence of sediment. ○: No sediment is observed. ×: Sediment is observed.

[0113] (Gel fraction) The aqueous resin emulsion was dried at 130°C for 30 minutes to form a resin film, and the resin film was peeled off to obtain a measurement sample. Then, 0.5 g of the measurement sample was weighed out, immersed in 100 ml of tetrahydrofuran at 23°C, and left at 23°C for 1 day. Then, the above tetrahydrofuran solution was filtered through a 200-mesh wire net, and the insoluble matter remaining on the wire net was dried at 130°C for 1 hour, returned to 23°C, and then its weight was measured. Then, the gel fraction (%) was calculated using the following formula. Gel fraction (%) = insoluble matter / weight before immersion × 100

[0114] (Examples 2 to 17: Method for producing aqueous resin emulsion) The aqueous resin emulsions of Examples 2 to 17 were produced in the same manner as in Example 1, except that the polymerizable monomer (a1), polymerizable monomer (b1), crosslinkable monomer (a2, b3), carboxyl group-containing polymerizable monomer (b2), hydrophilic solvent, and chain transfer agent in Example 1 were changed to the amounts shown in Table 1. However, since multi-stage emulsion polymerization was used, the amounts of the polymerization initiator and surfactant were divided and used according to the monomer ratio. The solid content and pH of the aqueous resin emulsions of Examples 2 to 17 were adjusted to be almost the same as those of Example 1.

[0115] (Comparative Examples 1 to 11: Methods for Producing Aqueous Resin Emulsions) The aqueous resin emulsions of Comparative Examples 1 to 11 were produced in the same manner as in Example 1, except that the polymerizable monomer (a1), polymerizable monomer (b1), crosslinkable monomer (a2, b3), carboxyl group-containing monomer (b2), hydrophilic solvent, and chain transfer agent in Example 1 were changed to the amounts shown in Table 1. However, since multistage emulsion polymerization was used, the amounts of the polymerization initiator and surfactant were each divided and used according to the monomer ratio.

[0116] <Manufacturing method of test sample 1> Using the aqueous resin emulsions prepared in Examples 1 to 17 and Comparative Examples 1 to 11, a film-forming agent (butyl glycol), a wetting agent (manufactured by Nissin Chemical Industry Co., Ltd., product name: Olfin E1010), a defoaming agent (manufactured by ADEKA Corporation, product name: Adekanol UH-420), and a solid content of 28% was adjusted with water to produce a test sample 1. The test sample 1 was diluted with water by 10% before the test, and the evaluation tests "drying property test, water resistance test, adhesion test (initial and after immersion in water)" described later were performed. Note that gelation occurred during polymerization of the aqueous resin emulsion in Comparative Example 7, so all subsequent evaluation tests could not be performed.

[0117] (Drying test) Test sample 1 was attached to the surface of a slate board (TP Giken Co., Ltd., product name: flexible board) with a thickness of 200 g / m 2 After applying the coating with a brush so as to give the coating, the coating was dried for 1 hour in an atmosphere of 23°C x 50% humidity, and the drying property of the coating was evaluated by touching with a finger. (Evaluation Criteria) ○: Dry and fingertips do not get dirty. ×: Semi-dry, or not dry and sticks to fingertips and stains.

[0118] (Water resistance test) Test sample 1 was attached to the surface of a slate board (TP Giken Co., Ltd., product name: flexible board) with a thickness of 200 g / m 2 After painting with a brush so that the color was as shown in the figure, the sample was dried for 1 hour in an atmosphere of 23°C x 50% humidity, immersed in water at 23°C for 1 day, and then removed. The degree of whitening was evaluated visually. (Evaluation Criteria) ◯: Almost no whitening is observed. ×: bleached.

[0119] (Initial adhesion test: cross-cut method) [Preparation of test samples 2, 3, 4, and 5] The aqueous resin emulsions prepared in Examples 1 to 17 and Comparative Examples 1 to 11 were used to paint various inorganic substrates or various old coating films, and then topcoat paint was applied to prepare test samples 2 to 5. The adhesion of the formed coating films was evaluated by the cross-cut method using test samples 2 to 5.

[0120] (Preparation of test sample 2 for evaluating the adhesion of the coating film on an inorganic substrate at 23°C) Test sample 2 was prepared to evaluate the adhesion of the coating film of the aqueous resin emulsion to various inorganic substrates and topcoat paints at 23°C. Using the aqueous resin emulsions prepared above in the Examples and Comparative Examples, 200 g / m2 was applied to the surface of a slate board and a calcium silicate board. 2 After painting with a brush so that the surface was painted as shown above, the surface was dried for 36 hours in an atmosphere of 23°C and 50% humidity. After drying, a one-component water-based silicone resin (SK Chemical Co., Ltd., product name: Water-based Yane Fresh Silicone) was applied as a topcoat at 300 g / m 2 After painting with a brush so that the number of coats was two, the coating was dried for three days in an atmosphere of 23°C x 50% humidity to form a coating film, and test sample 2 was obtained.

[0121] (Preparation of test sample 3 for evaluating the adhesion of the coating film on an inorganic substrate at 10°C) In addition, assuming a cold region, test sample 3 was prepared under more severe drying conditions with the plate temperature lowered to 10°C (the inorganic substrate was left in an incubator set at 10°C for 3 hours, and a surface thermometer was used to confirm that the temperature had reached 10°C). Except for the inorganic substrate plate temperature being set to 10°C, the same preparation conditions were used as for test sample 2, and the aqueous resin emulsion and topcoat paint were applied in that order to form a coating. This resulted in test sample 3.

[0122] (Preparation of test sample 4 to evaluate the adhesion of the paint film on the old paint film at 23°C) Test sample 4 was prepared to evaluate the adhesion of the water-based resin emulsion coating to the old coating at 23°C. A slate board (TP Giken Co., Ltd., product name: Flexible Board) was coated with 200 g / m2 of two-liquid weak solvent sealer (SK Kaken Co., Ltd., product name: Mild Sealer EPO). 2After painting with a brush so that the surface was as shown, the surface was dried for 3 days in an atmosphere of 23°C x 50% humidity to prepare the base. Next, each of the paints (1) and (2) was applied in the following coating amounts and dried for 3 days in an atmosphere of 23°C x 50% humidity. (1) A one-component water-based fluororesin (SK Chemical Co., Ltd., product name: Water-based Yane Fresh Fusso) was applied at a coating weight of 300 g / m 2 The paint was applied with a brush so that the surface was painted twice. (2) A two-component weak solvent resin (SK Chemicals, product name: Cooltite Si) was applied with a brush so that the coating amount was 300 g / m2 (2 coats).

[0123] After drying, the old paint film was formed on the slate board using a Super Xenon Weather Meter (manufactured by Suga Test Instruments) for 1,000 cycles (based on JIS K 5600-7-7 Cycle A: Cycle 1 irradiation for 102 minutes (irradiance: 60 W / m2, black panel temperature: 63°C, humidity: 50%), cycle 2 irradiation + pure water shower for 18 minutes (irradiance: 60 W / m2, room temperature: 38°C, humidity: 95%, a total of 120 minutes is one cycle).

[0124] Next, using each slate board on which an old coating film made of the above-mentioned various paints was formed, the aqueous resin emulsions prepared in the Examples and Comparative Examples were applied at 200 g / m2 on the old coating film. 2 The paint was applied so that the surface was coated with 300g / m2 of one-component water-based silicone resin (SK Chemical Co., Ltd., product name: Water-based Yane Fresh Silicone) as a topcoat paint. 2 After painting with a brush so that the number of coats was two, the coating was dried for three days in an atmosphere of 23°C and 50% humidity to form a coating, and test sample 4 was obtained.

[0125] (Preparation of test sample 5 to evaluate the adhesion of the coating film on the old coating film at 10°C) In addition, assuming a cold region, and under more severe drying conditions, the temperature of each old coating film was lowered to 10°C (each old coating film was left in an incubator set at 10°C for 3 hours, and a surface thermometer was used to confirm that the temperature had reached 10°C), and the samples were then coated. Except for the fact that the temperature of each old coating film was set to 10°C, the water-based resin emulsion and topcoat were applied in that order under the same preparation conditions as for test sample 4 to form a coating film. This resulted in test sample 5.

[0126] (Evaluation of initial adhesion by cross-cut method) Using the test samples 2 to 5 prepared above, the adhesion to inorganic substrates, old coating films, and topcoats was evaluated by cross-cutting 5 mm wide in accordance with JIS K5600-5-6 (cross-cut adhesion method), and the results were visually evaluated using the following 6-level scale of classifications 0 to 5. Classifications 0 and 1 indicate pass, and classifications 2 to 5 indicate fail. (Evaluation Criteria) Classification 0 (pass): No peeling on any grid Class 1 (pass): Small peeling of the coating at the intersection of the cuts, peeling of the cross-cut area is less than 5% Category 2 (Fail): The coating has delaminated along the edges of the cuts and / or at the intersections, with more than 5% to 15% delamination in the cross-cut areas. Category 3 (Fail): The coating has peeled off significantly all over the surface along the edges of the cuts, and peeling in the cross-cut areas is greater than 15% but not greater than 35%. Category 4 (Fail): The coating has peeled off significantly all along the edges of the cuts, and the peeling in the cross-cut area is more than 35% but not more than 65%. Class 5 (fail): Peeling of Class 4 or higher

[0127] (Adhesion test after immersion in water) A set of test samples 2 to 5 identical to the test samples 2 to 5 used in the initial adhesion test was prepared, and test samples 2 to 5 were used to evaluate adhesion after submersion in water. Test samples 2 to 5 were immersed in water for 7 days in an atmosphere of 23°C x 50%, removed, and then dried for 30 minutes. Then, using the dried test samples 2 to 5, adhesion after submersion was evaluated in the same manner as in the initial adhesion test. The following evaluation criteria are the same as those for the initial adhesion test. (Evaluation Criteria) Classification 0 (pass): No peeling on any grid Class 1 (pass): Small peeling of the coating at the intersection of the cuts, peeling of the cross-cut area is less than 5% Category 2 (Fail): The coating has delaminated along the edges of the cuts and / or at the intersections, with more than 5% to 15% delamination in the cross-cut areas. Category 3 (Fail): The coating has peeled off significantly all over the surface along the edges of the cuts, and peeling in the cross-cut areas is greater than 15% but not greater than 35%. Category 4 (Fail): The coating has peeled off significantly all along the edges of the cuts, and the peeling in the cross-cut area is more than 35% but not more than 65%. Class 5 (fail): Peeling of Class 4 or higher

[0128] (Test Results) Table 5 shows the test results of Examples 1 to 14. Table 6 shows the test results of Examples 15 to 17 and Comparative Examples 1 to 11.

[0129] [Table 5]

[0130] [Table 6]

[0131] (Test results of Examples 1 to 17) According to Tables 5 and 6, Examples 1 to 17 have excellent properties in all of drying property, water resistance, initial adhesion, and adhesion after immersion in water.

[0132] (Test results for Comparative Examples 1 to 11) On the other hand, a large amount of aggregates was generated during polymerization in Comparative Examples 2, 3, 8, and 9. The reasons why aggregates were generated in Comparative Examples 2, 3, 8, and 9 will be explained below. In addition, the reason why a water-soluble resin emulsion could not be produced in Comparative Example 7 will also be explained.

[0133] In Comparative Example 2, in the production process of copolymer (B), the amount of basic compound added 30 minutes after polymerization of polymerizable monomer (b1) etc. was small, and neutralization and dissolution were not possible, resulting in a decrease in the function of the protective layer, which is thought to have reduced the stability of the aqueous resin emulsion.

[0134] In Comparative Example 3, the amount of acid (the amount of the carboxy-containing polymerizable monomer (b2)) was small, which is believed to have deteriorated the function of the protective layer and reduced the stability of the aqueous resin emulsion.

[0135] In Comparative Example 8, the amount of chain transfer agent in the mixed solution of the polymerizable monomer (b1) etc. was large, and the weight average molecular weight (Mw) of the copolymer (B) was low, which is considered to have deteriorated the function of the protective layer and reduced the stability of the aqueous resin emulsion.

[0136] In Comparative Example 9, the blending ratio of copolymer (B) (20 parts) was low, which is believed to have deteriorated the function of the protective layer and reduced the stability of the aqueous resin emulsion.

[0137] In Comparative Example 7, since no chain transfer agent was added to the mixed solution of the polymerizable monomer (b1) etc., the weight average molecular weight (Mw) of the copolymer (B) was high, and the copolymer (B) was not dissolved in water, so that the viscosity of the polymerization solution of the copolymer (B) became very high, the particle size became too large, and it was not possible to prepare an aqueous resin emulsion.

[0138] As described above, the aqueous resin emulsion of the present invention has remarkable effects such as excellent adhesion to substrates and topcoat paints, quick drying properties, water resistance, and storage stability.

[0139] Furthermore, the present invention can provide an aqueous resin emulsion that is environmentally friendly and highly safe for the human body, making it possible to contribute to Goal 12 of the Sustainable Development Goals (SDGs) led by the United Nations, "Responsible Consumption and Production."

[0140] The invention is not limited to the above-described embodiment, and various modifications and variations are possible within the scope of the gist of the invention. [Explanation of symbols]

[0141] 100 resin particles 110 Inner layer 120 protective layer 130 Average particle size 140 Average particle size 200 Base material 300 Base material

Claims

1. An aqueous resin emulsion containing resin particles including an inner layer and a protective layer surrounding the inner layer, The inner layer contains a copolymer (A) containing a polymerizable monomer (a1) and a crosslinkable monomer (a2) as structural units, the protective layer contains at least a copolymer (B) containing, as structural units, a polymerizable monomer (b1) and a carboxy group-containing polymerizable monomer (b2), and a chain transfer agent; the polymerizable monomer (a1) and the polymerizable monomer (b1) each contain at least one of a (meth)acrylic acid alkyl ester monomer, a hydroxyl group-containing unsaturated monomer, an amide group-containing unsaturated monomer, and a piperidyl group-containing unsaturated monomer; The copolymer (A) contains the crosslinkable monomer (a2) in an amount of 0.1 to 15% by weight based on 100% by weight of all monomers constituting the copolymer (A), The copolymer (B) contains the carboxy group-containing polymerizable monomer (b2) in an amount of 5 to 20% by weight based on 100% by weight of all monomers constituting the copolymer (B), The weight average molecular weight (Mw) of the copolymer (B) is 3,000 to 20,000; The average particle diameter D of the copolymer (A) A and the average particle diameter D of the resin particles B Ratio to (D A / D B ) is greater than 0 and less than or equal to 0.70; Here, the average particle diameter D A is measured by a laser diffraction / scattering method, and the average particle diameter D B is measured by dynamic light scattering, Water-based resin emulsion.

2. The copolymer (B) further contains a crosslinkable monomer (b3) as a constituent unit, The crosslinkable monomer (b3) and the crosslinkable monomer (a2) each contain at least one of a polyfunctional monomer and a silane coupling agent; The aqueous resin emulsion according to claim 1.

3. The copolymer (B) contains the chain transfer agent in an amount of 0.1 to 15.0% by weight based on 100% by weight of all monomers constituting the copolymer (B). The aqueous resin emulsion according to claim 1.

4. The copolymer (A) contains the polymerizable monomer (a1) in an amount of 85 to 99.9% by weight based on 100% by weight of all monomers constituting the copolymer (A), The copolymer (B) contains the polymerizable monomer (b1) in an amount of 80 to 95% by weight based on 100% by weight of all monomers constituting the copolymer (B). The aqueous resin emulsion according to claim 3.

5. The pH of the copolymer (B) is 7.0 to 10.

5. The aqueous resin emulsion according to claim 1.

6. The haze of the copolymer (B) is 0 to 25%. The aqueous resin emulsion according to claim 1.

7. The weight ratio (B / A) of the copolymer (A) to the copolymer (B) is 25 / 75 to 75 / 25; The aqueous resin emulsion according to claim 1.

8. The average particle diameter D B is 50 to 300 nm; The aqueous resin emulsion according to claim 1.

9. It has both sealer and primer applications. The aqueous resin emulsion according to claim 1.

10. The copolymer (A) contains a styrene-based monomer as the polymerizable monomer (a1) in an amount of 15% by weight or less based on 100% by weight of all monomers constituting the copolymer (A), and / or The copolymer (B) contains a styrene-based monomer as the polymerizable monomer (b1) in an amount of 15% by weight or less based on 100% by weight of all monomers constituting the copolymer (B). The aqueous resin emulsion according to any one of claims 1 to 9.

11. A substrate; A coating film formed from the aqueous resin emulsion according to claim 1, which is provided on at least one surface of the substrate. Painted items.

12. The gel fraction of the coating film is 50 to 100%. The coated article according to claim 11.

13. The substrate comprises an inorganic porous substrate; The coated article according to claim 11.

Citation Information

Patent Citations

  • Acrylic emulsion for curing fibers, preparation method of acrylic emulsion, nylon polyester wadding, preparation method of nylon polyester wadding and grinding wheel

    CN114316301A

  • Water-based primer and method for finishing outer wall of construction

    JP1995278463A

  • Aqueous sealer and reinforcement using the same

    JP1999217559A

  • Aqueous sealer for inorganic material and method for producing sealer-coated inorganic material

    JP2001181605A

  • Aqueous emulsion and water-based coating composition comprising the same

    JP2004307544A