Nanodiamond manufacturing method and nanodiamond

The controlled detonation and purification method for nanodiamonds achieves a large specific surface area, addressing production limitations and improving mechanical and electrical properties for abrasive and insulating materials.

JP7565145B2Active Publication Date: 2024-10-10DAICEL CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2018230222
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2018-12-07
Publication Date
2024-10-10
Estimated Expiration
2038-12-07

AI Technical Summary

Technical Problem

Existing methods for producing nanodiamonds struggle to achieve a specific surface area of 100 m²/g or more, limiting their applications in abrasive, conductive, and insulating materials.

Method used

A nanodiamond production method involving a detonation process with a controlled container volume to explosive mass ratio of 10 or less, using a mixture of trinitrotoluene and cyclotrimethylene trinitramine, and subsequent purification steps to obtain nanodiamonds with a median diameter of 4.0 to 5.5 nm and a specific surface area of 320 to 500 m²/g.

Benefits of technology

The method produces nanodiamonds with a large specific surface area, enhancing their mechanical strength, electrical insulation, and thermal conductivity, suitable for abrasive, conductive, and insulating applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007565145000002
    Figure 0007565145000002
  • Figure 0007565145000001
    Figure 0007565145000001
Patent Text Reader

Abstract

To provide a production method of nanodiamond, with which nanodiamond with a large specific surface area can be obtained.SOLUTION: A production method of nanodiamond of this invention includes a nanodiamond generation step to detonate an explosive in a vessel under a condition in which a ratio of a capacity of the vessel to a mass of the explosive [(the capacity of the vessel (m)) / (the mass of the explosive (kg))] is 10 or less. The capacity of the vessel is preferably 0.05-10 m. The mass of the explosive is preferably 0.07-1 kg. A content of nanodiamond in a crude product of nanodiamond obtained by the nanodiamond generation step is preferably 5-55 mass%.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing nanodiamonds and nanodiamonds. More specifically, the present invention relates to a method for producing nanodiamonds and nanodiamonds obtained by the method. [Background technology]

[0002] Nano diamonds are ultrafine diamond particles with a very large specific surface area, and have high mechanical strength, electrical insulation, and excellent thermal conductivity. They also have deodorizing, antibacterial, and chemical resistance properties. For this reason, they are used as abrasives, electrical conductivity agents, insulating materials, deodorizers, antibacterial agents, etc.

[0003] Nanodiamonds are generally synthesized by the detonation method. Nanodiamonds obtained by the detonation method often form aggregates, and by subjecting the aggregates to a crushing process using a grinder such as a bead mill, so-called single-digit nanodiamonds with a median particle diameter (D50) of less than 10 nm can be obtained (see Patent Documents 1 and 2). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2005-001983 A [Patent Document 2] JP 2010-126669 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, in the detonation method, the specific surface area is 300 m 2 Although it has been relatively easy to produce nanodiamonds with a specific surface area of ​​about 320 m / g, 2 It has been difficult to produce nanodiamonds of about 1 / g or more.

[0006] Therefore, an object of the present invention is to provide a method for producing nanodiamonds that can produce nanodiamonds with a large specific surface area. [Means for solving the problem]

[0007] In order to achieve the above object, the inventors have conducted extensive research and have found that the ratio of the container volume to the explosive mass [container volume (m 3 It has been found that a nanodiamond having a large specific surface area can be obtained by a method for producing nanodiamonds, which includes a step of detonating the explosive in the container under conditions where the ratio of the explosive mass (kg) to the specific surface area (kg) of the explosive is within a specific range. The present invention has been completed based on these findings.

[0008] That is, the present invention is based on the ratio of the container volume to the explosive mass [container volume (m 3 The present invention provides a method for producing nanodiamonds, which includes a nanodiamond production step of detonating the explosive in the container under conditions where the ratio (mass of explosive (kg) / mass of explosive (kg)) is 10 or less.

[0009] The above container capacity is 0.05 to 10 m 3 It is preferable that:

[0010] The explosive mass is preferably 0.07 to 1 kg.

[0011] The nanodiamond content in the nanodiamond crude product obtained by the nanodiamond production step is preferably 5 to 55 mass %.

[0012] The particle size of the explosive is preferably 45 to 2360 μm.

[0013] Preferably, the explosive is a mixture of trinitrotoluene and cyclotrimethylenetrinitramine.

[0014] In addition, the present invention provides a method for producing a sintered body having a median diameter of 4.0 to 5.5 nm and a specific surface area of ​​320 to 500 m. 2The present invention provides nanodiamonds having a nanoparticle size of 100 nm / g.

[0015] The nanodiamonds are preferably detonation nanodiamonds. Effect of the Invention

[0016] According to the method for producing nanodiamonds of the present invention, it is possible to obtain nanodiamonds with a large specific surface area. [Brief description of the drawings]

[0017] [Figure 1] FIG. 1 is a process diagram showing one embodiment of the nanodiamond manufacturing method of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] The method for producing nanodiamonds of the present invention includes a step of producing nanodiamonds by detonation (nanodiamond production step). In this specification, the method for producing nanodiamonds of the present invention may be simply referred to as the "production method of the present invention". The production method of the present invention may include other steps such as a purification step, an oxygen oxidation step, and a hydrogenation step in addition to the nanodiamond production step. Examples of the purification step include an acid treatment step, an oxidation treatment step, an alkaline peroxide treatment step, and a drying step.

[0019] Fig. 1 is a process diagram showing one embodiment of the manufacturing method of the present invention. The manufacturing method of the present invention shown in Fig. 1 includes at least a nanodiamond production step S1, an acid treatment step S2, an oxidation treatment step S3, an alkaline hydrogen peroxide treatment step S4, and a drying step S5.

[0020] (Nanodiamond production process) In the nanodiamond production process, nanodiamonds are produced by the detonation method. Specifically, first, a molded explosive with an electric detonator attached is placed inside a pressure-resistant container for detonation, and the container is sealed in a state in which a gas of a specific composition and the explosive used coexist in the container. In the nanodiamond production process, the electric detonator is then detonated to detonate the explosive in the container. Detonation refers to an explosion caused by a chemical reaction in which the flame surface of the reaction moves at a high speed exceeding the speed of sound. During detonation, nanodiamonds are produced by the action of the pressure and energy of the shock wave generated by the explosion, using carbon liberated by partial incomplete combustion of the explosive used as a raw material. Nanodiamonds are products obtained by the detonation method, and first, adjacent primary particles or crystallites are very firmly assembled due to the action of van der Waals forces and the Coulomb interaction between the crystal faces, resulting in an aggregate.

[0021] In the nanodiamond production process, the ratio of the container volume to the explosive mass [container volume (m 3 The explosive is detonated in the container under the condition that the ratio (kg / mass of explosive (kg)) is 10 or less. By making the ratio 10 or less, the heat dissipation after the detonation is slow, and the graphitization of the surface of the nanodiamond crude product produced progresses, and as a result, nanodiamonds having a small median diameter and a large specific surface area can be produced. The ratio is preferably 0.5 to 10, more preferably 1 to 7, and even more preferably 3.5 to 5.5. When the ratio is 0.5 or more, the particle size distribution of the primary particles is narrow, and nanodiamonds having a more uniform particle size can be obtained. In addition, the nanodiamond content in the nanodiamond crude product produced is high.

[0022] The above container capacity (volume) is 0.05 to 10 m 3 is preferable, and more preferably 0.07 to 0.2 m 3 The above container capacity is 0.05 m 3 When the capacity of the container is 10m or more, the productivity of nano-diamonds is excellent. 3If the temperature is less than 100° C., the heat release rate after detonation is slowed down, and the graphitization of the surface of the nanodiamond crude product is promoted, thereby making it possible to keep the particle size of the nanodiamond small.

[0023] The mass of the explosive is preferably 0.07 to 1 kg, more preferably 0.07 to 0.2 kg. When the mass of the explosive is 0.07 kg or more, the productivity of nanodiamonds is excellent.

[0024] As the explosive, a mixture of trinitrotoluene (TNT) and cyclotrimethylenetrinitramine, i.e., hexogen (RDX), can be used. The mass ratio of TNT to RDX (TNT / RDX) is set to, for example, a range of 40 / 60 to 60 / 40.

[0025] The particle size of the explosive is preferably 45 to 2360 μm, more preferably 45 to 1700 μm, and even more preferably 75 to 90 μm. According to the manufacturing method of the present invention, even when an explosive having a particle size of 45 μm or more is used, nanodiamonds having a small particle size and a large specific surface area can be produced. The particle size of the explosive can be measured by the small angle X-ray scattering measurement sieve passing method (%).

[0026] The pressure during detonation is, for example, 18 to 35.4 GPa, preferably 24.4 to 29.3 GPa, and more preferably 24.4 to 25.5 GPa. If the pressure is 18 GPa or more, the graphitization of the surface of the generated nanodiamond crude product tends to be delayed, and the nanodiamond content tends to be high.

[0027] In the nanodiamond production process, the container and its interior are then left to cool at room temperature for about 24 hours to lower the temperature. After this cooling, the crude nanodiamond product (including the nanodiamond aggregates and soot produced as described above) adhering to the inner wall of the container is scraped off with a spatula, and the crude nanodiamond product is collected. By the above-mentioned detonation method, a crude nanodiamond particle product can be obtained. In addition, by performing the above-mentioned nanodiamond production process the required number of times, it is possible to obtain the desired amount of crude nanodiamond product.

[0028] The nanodiamond content in the nanodiamond crude product obtained by the nanodiamond production process is preferably 10 to 55 mass%, more preferably 13 to 50 mass%, and even more preferably 15 to 40 mass%. According to the production method of the present invention, it is possible to produce nanodiamonds with a small median diameter and a large specific surface area, and to obtain a nanodiamond crude product with a nanodiamond content of 10 mass% or more, which is excellent in production efficiency.

[0029] (Acid treatment process) In the acid treatment step, a strong acid is applied to the raw nanodiamond crude product in, for example, an aqueous solvent to remove metal oxides. The nanodiamond crude product obtained by the detonation method is likely to contain metal oxides, and these metal oxides are oxides of Fe, Co, Ni, etc., derived from the container used in the detonation method. For example, by applying a strong acid in an aqueous solvent, metal oxides can be dissolved and removed from the nanodiamond crude product (acid treatment). As the strong acid used in this acid treatment, mineral acids are preferable, and examples include hydrochloric acid, hydrofluoric acid, sulfuric acid, nitric acid, and aqua regia. One type of strong acid may be used, or two or more types may be used. The concentration of the strong acid used in the acid treatment is, for example, 1 to 50 mass%. The acid treatment temperature is, for example, 70 to 150°C. The acid treatment time is, for example, 0.1 to 24 hours. The acid treatment can be performed under reduced pressure, normal pressure, or pressure. After such acid treatment, the solid content (including nanodiamond aggregates) is washed with water, for example, by decantation. It is preferable to repeatedly wash the solid matter by decantation until the pH of the precipitation liquid reaches, for example, 2 to 3. When the content of metal oxide in the nanodiamond crude product obtained by the detonation method is small, the above-mentioned acid treatment may be omitted.

[0030] (Oxidation treatment process) The oxidation process is a process in which graphite is removed from the nanodiamond crude product using an oxidizing agent. The nanodiamond crude product obtained by the detonation method contains graphite, which is derived from the carbon liberated by partial incomplete combustion of the explosive used that did not form nanodiamond crystals. For example, after the above-mentioned acid treatment, graphite can be removed from the nanodiamond crude product by applying an oxidizing agent in an aqueous solvent. In addition, oxygen-containing groups such as carboxyl groups and hydroxyl groups can be introduced onto the nanodiamond surface by applying an oxidizing agent.

[0031] Examples of the oxidizing agent used in this oxidation treatment include chromic acid, chromic anhydride, dichromic acid, permanganic acid, perchloric acid, nitric acid, mixtures thereof, mixed acids of at least one acid selected from these with other acids (such as sulfuric acid), and salts thereof. Among these, the use of mixed acids (particularly mixed acids of sulfuric acid and nitric acid) is preferred because it is environmentally friendly and has an excellent effect of oxidizing and removing graphite.

[0032] The mixing ratio of sulfuric acid and nitric acid in the mixed acid (the former / the latter; mass ratio) is preferably, for example, 60 / 40 to 95 / 5, because graphite can be efficiently oxidized and removed at a temperature of, for example, 130° C. or higher (particularly preferably 150° C. or higher. The upper limit is, for example, 200° C.) even under pressure near normal pressure (for example, 0.5 to 2 atm). The lower limit is preferably 65 / 35, more preferably 70 / 30. The upper limit is preferably 90 / 10, more preferably 85 / 15, and even more preferably 80 / 20. When the mixing ratio is 60 / 40 or higher, the content of sulfuric acid having a high boiling point is high, so that the reaction temperature is, for example, 120° C. or higher under pressure near normal pressure, and the graphite removal efficiency tends to be improved. When the mixing ratio is 95 / 5 or lower, the content of nitric acid, which greatly contributes to the oxidation of graphite, is high, so that the graphite removal efficiency tends to be improved.

[0033] The amount of the oxidizing agent (particularly the mixed acid) used is, for example, 10 to 50 parts by mass, preferably 15 to 40 parts by mass, and more preferably 20 to 40 parts by mass, per part by mass of the crude nanodiamond product. The amount of sulfuric acid used in the mixed acid is, for example, 5 to 48 parts by mass, preferably 10 to 35 parts by mass, and more preferably 15 to 30 parts by mass, per part by mass of the crude nanodiamond product. The amount of nitric acid used in the mixed acid is, for example, 2 to 20 parts by mass, preferably 4 to 10 parts by mass, and more preferably 5 to 8 parts by mass, per part by mass of the crude nanodiamond product.

[0034] In addition, when the mixed acid is used as the oxidizing agent, a catalyst may be used together with the mixed acid. By using a catalyst, the efficiency of removing graphite can be further improved. Examples of the catalyst include copper (II) carbonate. The amount of the catalyst used is, for example, about 0.01 to 10 parts by mass with respect to 100 parts by mass of the nanodiamond crude product.

[0035] The oxidation treatment temperature is, for example, 100 to 200° C. The oxidation treatment time is, for example, 1 to 24 hours. The oxidation treatment can be carried out under reduced pressure, normal pressure, or increased pressure.

[0036] (Alkaline hydrogen peroxide treatment process) Even after the above-mentioned acid treatment process, if the metal oxides that have not been completely removed remain in the nanodiamond, they will take the form of aggregates (secondary particles) in which the primary particles interact very strongly with each other and are assembled. In such a case, an alkali and hydrogen peroxide may be applied to the nanodiamond in an aqueous solvent. This can remove the metal oxides remaining in the nanodiamond, and can promote the separation of the primary particles from the aggregates. Examples of the alkali used in this treatment include sodium hydroxide, ammonia, and potassium hydroxide. In the alkaline peroxide treatment, the concentration of the alkali is, for example, 0.1 to 10 mass%, the concentration of the hydrogen peroxide is, for example, 1 to 15 mass%, the treatment temperature is, for example, 40 to 100°C, and the treatment time is, for example, 0.5 to 5 hours. The alkaline peroxide treatment can be performed under reduced pressure, normal pressure, or pressure.

[0037] (drying process) It is preferable to provide a drying step after the alkaline hydrogen peroxide treatment step. For example, the liquid is evaporated from the nanodiamond-containing solution obtained through the alkaline hydrogen peroxide treatment step using a spray dryer or evaporator, and the resulting residual solid is dried by heating in a drying oven. The heating and drying temperature is, for example, 40 to 150°C. Through this drying step, a nanodiamond aggregate (an aggregate of nanodiamond particles) is obtained as a powder.

[0038] (Oxygen oxidation process) The nanodiamond powder that has undergone the above purification process may be subjected to an oxygen oxidation process in which the nanodiamond powder is heated in an oxygen-containing gas atmosphere using a gas atmosphere furnace. In the oxygen oxidation process, specifically, the nanodiamond powder is placed in a gas atmosphere furnace, an oxygen-containing gas is supplied or passed through the furnace, and the temperature inside the furnace is raised to a temperature condition set as the heating temperature to perform the oxygen oxidation process. The temperature condition of this oxygen oxidation process is, for example, 250 to 500°C. In order to realize a negative zeta potential for the nanodiamond particles contained in the nanodiamond dispersion liquid to be produced, the temperature condition of this oxygen oxidation process is preferably relatively high, for example, 400 to 450°C. The oxygen-containing gas used in the oxygen oxidation process may be a mixed gas containing an inert gas in addition to oxygen. Examples of the inert gas include nitrogen, argon, carbon dioxide, and helium. The oxygen concentration of the mixed gas is, for example, 1 to 35% by volume.

[0039] (Hydrogenation process) In order to realize a positive zeta potential for the nanodiamond particles contained in the nanodiamond dispersion liquid to be produced, it is preferable to carry out a hydrogenation process after the oxygen oxidation process. In the hydrogenation process, the nanodiamond powder that has been subjected to the oxygen oxidation process is heated in a gas atmosphere containing hydrogen using a gas atmosphere furnace. Specifically, a hydrogen-containing gas is supplied or passed through a gas atmosphere furnace in which the nanodiamond powder is disposed, and the temperature inside the furnace is raised to a temperature condition set as the heating temperature to carry out the hydrogenation process. The temperature condition of this hydrogenation process is, for example, 400 to 800 ° C. The hydrogen-containing gas used in the hydrogenation process may be a mixed gas containing an inert gas in addition to hydrogen. Examples of the inert gas include nitrogen, argon, carbon dioxide, and helium. The hydrogen concentration of the mixed gas is, for example, 1 to 50 volume %. In order to realize a negative zeta potential for the nanodiamond particles contained in the nanodiamond dispersion liquid to be produced, the crushing process described below may be carried out without carrying out such a hydrogenation process.

[0040] According to the manufacturing method of the present invention, for example, a cellulose having a median diameter of primary particles of 4.0 to 5.5 nm and a specific surface area of ​​320 to 500 m 2 In this specification, the median diameter of the primary particles is 4.0 to 5.5 nm, and the specific surface area is 320 to 500 m 2 / g may be referred to as the "nanodiamond of the present invention."

[0041] The nanodiamond of the present invention has a median diameter (D50) of the primary particles of 4.0 to 5.5 nm, preferably 4.2 to 5.2 nm, and more preferably 4.4 to 5 nm. The median diameter of the primary particles of the nanodiamond can be measured by small angle X-ray scattering measurement method or dynamic light scattering method.

[0042] The nanodiamond of the present invention has a specific surface area of ​​320 to 500 m 2 / g, preferably 340 to 450 m 2 / g, more preferably 350 to 430m 2 / g. The specific surface area of ​​nanodiamond can be measured by the BET method. For example, the redispersion liquid of nanodiamond can be measured using a product called "BELSORP-max" (manufactured by Nippon BEL Co., Ltd.).

[0043] Even after being refined through the above-mentioned purification step, oxygen oxidation step, or hydrogenation step, etc., the detonation nanodiamond tends to take the form of an aggregate (secondary particle) in which the primary particles are aggregated through very strong interactions between them. In order to separate many primary particles from this aggregate, a crushing step may be performed after the above-mentioned purification step, oxygen oxidation step, or hydrogenation step. Specifically, first, the nanodiamond that has been subjected to the oxygen oxidation step or the subsequent hydrogenation step is suspended in pure water to prepare a slurry containing the nanodiamond. In preparing the slurry, a centrifugation process may be performed to remove relatively large aggregates from the nanodiamond suspension, or the nanodiamond suspension may be subjected to ultrasonic treatment. The slurry is then subjected to a wet crushing process. The crushing process may be performed using, for example, a high shear mixer, a high shear mixer, a homomixer, a ball mill, a bead mill, a high pressure homogenizer, an ultrasonic homogenizer, a colloid mill, etc. The crushing process may be performed by combining these. From the viewpoint of efficiency, it is preferable to use a bead mill.

[0044] The bead mill, which is a grinding device or dispersing machine, is equipped with, for example, a cylindrical mill container, a rotor pin, a centrifugal separation mechanism, a raw material tank, and a pump. The rotor pin has a common axis with the mill container and is configured to be able to rotate at high speed inside the mill container. The centrifugal separation mechanism is arranged at the upper part of the mill container. In bead milling using a bead mill in the crushing process, the mill container is filled with beads and the rotor pin is stirring the beads, and the above-mentioned slurry (including nanodiamond aggregates) is introduced as a raw material from the raw material tank to the lower part of the mill container by the action of the pump. The slurry reaches the upper part of the mill container through the beads being stirred at high speed in the mill container. In this process, the nanodiamond aggregates contained in the slurry are subjected to the action of crushing or dispersing by contact with the beads that are moving vigorously. This advances the crushing of the nanodiamond aggregates (secondary particles) into primary particles. The slurry and beads that reach the centrifugal separation mechanism at the top of the mill vessel are centrifuged by the centrifugal separation mechanism using the difference in specific gravity, the beads remain in the mill vessel, and the slurry is discharged outside the mill vessel via a hollow line slidably connected to the centrifugal separation mechanism. The discharged slurry is returned to the raw material tank, and then is again charged into the mill vessel by the action of the pump (circulation operation). In such bead milling, the crushing media used are, for example, zirconia beads, and the diameter of the beads is, for example, 15 to 500 μm. The amount of beads (apparent volume) filled in the mill vessel is, for example, 50 to 80% of the volume of the mill vessel. The circumferential speed of the rotor pin is, for example, 8 to 12 m / min. The amount of the circulated slurry is, for example, 200 to 600 ml, and the flow rate of the slurry is, for example, 5 to 15 L / hour. The processing time (circulation operation time) is, for example, 30 to 300 minutes. In the crushing step, a batch-type bead mill may be used instead of the above-mentioned continuous bead mill.

[0045] By undergoing such a crushing process, a nanodiamond dispersion liquid containing primary particles of nanodiamond dispersed as colloidal particles can be obtained.

[0046] The slurry that has been subjected to the crushing process may be classified to remove coarse particles. For example, a classification device may be used to remove coarse particles from the slurry by a classification operation using centrifugation. This results in a black, transparent nanodiamond dispersion in which the primary particles of nanodiamond are dispersed as colloidal particles.

[0047] The nanodiamond that has undergone the crushing process, or the nanodiamond that has undergone the crushing process and classification operation, may be subjected to a drying process. In the drying process, specifically, the dispersion liquid containing the nanodiamond is subjected to a drying process to obtain a dry powder of the nanodiamond. Examples of the drying process include spray drying using a spray drying device and evaporation to dryness using an evaporator.

[0048] The nanodiamond dispersion contains nanodiamond particles and a dispersion medium. The nanodiamond particles contained in the nanodiamond dispersion are primary nanodiamond particles or secondary nanodiamond particles derived from nanodiamonds obtained by the manufacturing method of the present invention, and are dispersed as colloidal particles in the dispersion medium while being separated from each other. The median diameter of the nanodiamond particles is, for example, 60 nm or less, preferably 30 nm or less, more preferably 28 nm or less, even more preferably 25 nm or less, even more preferably 22 nm or less, and particularly preferably 20 nm or less. The median diameter of the primary nanodiamond particles constituting the nanodiamond particles is, for example, 5.5 nm or less, preferably 5.2 nm or less, and more preferably 5 nm or less. For example, when using a nanodiamond dispersion as a material for adding or supplying nanodiamonds to a transparent resin or the like when forming a nanodiamond-containing transparent member, the smaller the median diameter of the nanodiamond particles, the more favorable it tends to be in terms of achieving high transparency in the transparent member. On the other hand, the lower limit of the median diameter of the nanodiamond particles is, for example, 1 nm. The median diameter in the dispersion can be measured by dynamic light scattering.

[0049] The specific surface area of ​​the nanodiamond particles in the nanodiamond dispersion is preferably 320 to 500 m 2 / g, more preferably 340 to 450m 2 / g, more preferably 350 to 430 m 2 / g. The specific surface area of ​​nanodiamond can be measured by the BET method. For example, the redispersion liquid of nanodiamond can be measured using a product called "BELSORP-max" (manufactured by BEL Japan Co., Ltd.).

[0050] The dispersion medium contained in the nanodiamond dispersion liquid is a medium for properly dispersing nanodiamond particles in the nanodiamond dispersion liquid. As the dispersion medium, a solvent in which nanodiamond can be dissolved is preferable, for example, water, methanol, ethanol, ethylene glycol, dimethyl sulfoxide, N-methylpyrrolidone, etc. may be mentioned. Only one type of dispersion medium may be used, or two or more types may be used. From the viewpoint of dispersibility of nanodiamond particles, the dispersion medium is preferably water or an aqueous dispersion medium containing water at 50 mass% or more.

[0051] The nanodiamond dispersion liquid having the above-mentioned structure can be used as a nanodiamond supply material when preparing a composite material containing nanodiamond. And, the manufacturing method of the present invention can produce nanodiamond particles that can be used for preparing such a nanodiamond dispersion liquid, for example.

[0052] The manufacturing method of the present invention includes a step of producing nanodiamonds by a detonation method, and in the nanodiamond production step, the ratio of the container volume to the explosive mass [container volume (m 3The explosive is detonated in the container under the condition that the ratio (kg) / mass of explosive (kg) is 10 or less. The detonation in the manufacturing method of the present invention is characterized by the fact that the ratio, i.e., the container volume relative to the explosive mass, is small, and by carrying out the detonation under such conditions, the heat release after the detonation is slowed down, and the graphitization of the surface of the nanodiamond crude product produced proceeds, resulting in a smaller diameter of the nanodiamond portion, i.e., the diameter of the nanodiamond particles after the purification process, and a larger specific surface area. EXAMPLES

[0053] The present invention will be described in more detail below based on examples, but the present invention is not limited to these examples.

[0054] Example 1 Nanodiamonds and nanodiamond dispersions were produced through the following steps. (Nanodiamond production process) In the nanodiamond production process, the explosives were first fitted with electric detonators and placed inside a pressure-resistant detonation vessel, which was then sealed. The vessel was made of iron and had a volume of 0.2 m. 3 The explosive used was a mixture of 0.2 kg of TNT and RDX. The mass ratio of TNT to RDX in the explosive (TNT / RDX) was 60 / 40. Next, an electric detonator was detonated to detonate the explosive in the container. The container and its interior were then allowed to cool for 24 hours at room temperature. After cooling, the nanodiamond crude product (containing the aggregates of nanodiamond particles and soot produced by the detonation method) adhering to the inner wall of the container was scraped off with a spatula, and the nanodiamond crude product was collected.

[0055] (Acid treatment process) Next, the crude nanodiamond product obtained by performing the nanodiamond production process multiple times was subjected to acid treatment. Specifically, 200 g of the crude nanodiamond product was added with 6 L of 10 mass % hydrochloric acid to obtain a slurry, which was then heated for 1 hour under reflux at normal pressure. The heating temperature in this acid treatment was 85 to 100°C. Next, after cooling, the solid matter (including nanodiamond aggregates and soot) was washed with water by decantation. The solid matter was repeatedly washed with water by decantation until the pH of the precipitation liquid reached 2 from the low pH side.

[0056] (Oxidation treatment process) Next, an oxidation treatment was performed. Specifically, 6 L of 98% by mass sulfuric acid aqueous solution and 1 L of 69% by mass nitric acid aqueous solution were added to the precipitate liquid (containing nanodiamond aggregates) obtained by decantation after the acid treatment to form a slurry, and then the slurry was subjected to a heat treatment for 48 hours under reflux at normal pressure. The heating temperature in this oxidation treatment was 140 to 160°C. Next, after cooling, the solid matter (including nanodiamond aggregates) was washed with water by decantation. The supernatant liquid at the beginning of the washing was colored, and the solid matter was repeatedly washed with water by decantation until the supernatant liquid became visually transparent.

[0057] (drying process) Next, the precipitate (containing nanodiamond aggregates) obtained by decantation after the oxidation process was dried to obtain a dry powder. The drying process was carried out by evaporation to dryness using an evaporator. In this way, the nanodiamond powder of Example 1 was obtained.

[0058] (Crushing process) Next, a crushing process was performed. Specifically, 0.3 g of the nanodiamond powder that had undergone the drying process and 29.7 ml of pure water were added to a 50 ml sample bottle and mixed to obtain a slurry. Next, the pH of the slurry was adjusted to 11 using a 3 mol / L aqueous sodium hydroxide solution. As a result, 30 ml of a slurry containing 1 mass% solids and having a pH of 11 was prepared. Next, an ultrasonic irradiator (product name "ultrasonic cleaner AS-3", manufactured by AS ONE Co., Ltd.) was used to irradiate the slurry for 1 hour. After this, bead milling was performed using a bead milling device (product name "parallel four-cylinder sand grinder LSG-4U-2L type", manufactured by IMEX Co., Ltd.). Specifically, 30 ml of the slurry after ultrasonic irradiation and zirconia beads with a diameter of 30 μm were put into a 100 ml mill container, a vessel (manufactured by IMEX Co., Ltd.), sealed in the container, and the device was driven to perform bead milling. In this bead milling, the amount of zirconia beads charged is, for example, 33% of the volume of the mill container, the rotation speed of the mill container is 2570 rpm, and the milling time is 1 hour.

[0059] Next, the slurry or suspension that had undergone the above-mentioned crushing process was centrifuged using a centrifuge. The centrifugal force in this centrifugation process was 20,000×g, and the centrifugation time was 10 minutes. Next, 10 ml of the supernatant of the nanodiamond-containing solution that had undergone the centrifugal process was collected. In this way, the nanodiamond dispersion of Example 1 in which nanodiamonds are dispersed in pure water was obtained.

[0060] Examples 2 and 3, and Comparative Example 1 In the nanodiamond production process, a container with the volume and an explosive with the mass shown in Table 1 were used, and the same procedure as in Example 1 was repeated to obtain a crude nanodiamond product, nanodiamond powder, and nanodiamond dispersion.

[0061] The nanodiamond crude products, nanodiamond powders, and nanodiamond dispersions obtained in the Examples and Comparative Examples were evaluated as follows. The results are shown in Table 1.

[0062] (1) Median diameter of primary particles For the nanodiamond powder obtained after the drying process, small angle X-ray scattering measurements were performed using an X-ray diffraction device (trade name "SmartLab", manufactured by Rigaku Corporation), and the primary particle diameter of the nanodiamond was estimated in the scattering angle range of 1° to 3° using particle size distribution analysis software (trade name "NANO-Solver", manufactured by Rigaku Corporation). In this estimation, the primary nanodiamond particles were assumed to be spherical and had a particle density of 3.51 g / cm. 3 It was assumed that.

[0063] (2) Specific surface area The nanodiamond dispersion was measured using an automatic specific surface area / pore distribution measuring device (product name "BELSORP-max", manufactured by BEL Japan Co., Ltd.).

[0064] (3) Nanodiamond content The nanodiamond crude product was calculated according to the following formula. Nanodiamond content [mass%] = dry powder mass after drying process / nanodiamond crude product mass after nanodiamond production process × 100

[0065] [Table 1] [Explanation of symbols]

[0066] S1 Nanodiamond production process S2 Acid treatment process S3 Oxidation treatment process S4 Alkaline peroxide treatment process S5 Drying process

Claims

1. Container capacity is 0.05 to 0.2 m 3 and the ratio of the container volume to the explosive mass [container volume (m 3 The explosive is detonated in the container under the condition that the ratio of the explosive mass (kg) to the explosive mass (kg) is 1 to 10. A method for producing nanodiamonds, including a nanodiamond production process.

2. 2. The method of claim 1, wherein the explosive mass is 0.07 to 1 kg. method.

3. The nanodiamonds in the crude product of nanodiamonds obtained in the nanodiamond production process The nanodiamond manufacturing method according to claim 1 or 2, wherein the yamond content is 5 to 55 mass %. Construction method.

4. The explosive according to any one of claims 1 to 3, wherein the particle size of the explosive is 45 to 2360 μm. How nanodiamonds are produced.

5. The explosive is a mixture of trinitrotoluene and cyclotrimethylenetrinitramine. A method for producing nanodiamonds according to any one of claims 1 to 4.

6. The nanodiamond has a primary particle median diameter of 4.0 to 5.5 nm and a specific surface area of ​​360 to 430 m 2 The method for producing nanodiamonds according to any one of claims 1 to 5, wherein the nanodiamond content is 1 / g.

Citation Information

Patent Citations

  • Nano-diamond explosion synthesis tank and nano-diamond explosion synthesis device

    CN1785493A

  • Super-dispersion state nano-carbon and method for manufacturing the same

    JP2005001983A

  • Method for producing diamond microparticle dispersion, and diamond microparticle dispersion

    JP2010126669A

  • Method for producing diamond fine particle having excellent water dispersibility, and diamond fine particle-water dispersion

    JP2015113278A

  • Water-repellent coating film, article having water-repellent coating film and dispersion

    JP2016044092A