Image display device

By using optimized adhesive layers with controlled strain cross-sectional areas, the image display device addresses peeling and wrinkling issues in curved surfaces, ensuring durable bonding in image display devices.

JP7565162B2Active Publication Date: 2024-10-10NITTO DENKO CORP
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2020058620
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-03-27
Publication Date
2024-10-10
Estimated Expiration
2040-03-27

AI Technical Summary

Technical Problem

Existing image display devices with curved surfaces experience peeling and wrinkling issues at the bonding interface due to mechanical strain caused by differences in curvature between the optical film and the rigid cover window.

Method used

The image display device incorporates a rigid transparent plate with a curved portion facing inward, bonded to an optical film using a first adhesive layer, and the optical film is bonded to a flexible image display cell via a second adhesive layer, with specific strain cross-sectional areas and thicknesses for each layer to minimize peeling and wrinkling.

Benefits of technology

The solution effectively suppresses peeling and wrinkling in curved surface image display devices by optimizing the adhesive layers' strain cross-sectional areas, ensuring durable and reliable bonding.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000016_0000
    Figure 00000016_0000
  • Figure 00000016_0001
    Figure 00000016_0001
  • Figure 00000016_0002
    Figure 00000016_0002
Patent Text Reader

Abstract

To provide an image display device having a curved surface portion on a screen and capable of suppressing the occurrence of peeling between members or wrinkles to a flexible member.SOLUTION: An optical film 50 having a double-sided adhesive and used for forming an image display device in which at least a part of a screen has a curved surface shape includes a first adhesive layer 21 on a first main surface of an optical film 10 and a second adhesive layer 22 on a second main surface. The first adhesive layer is used for bonding to a transparent plate 80; the second adhesive layer is used for bonding to an image display cell 70; the distortion cross-sectional area S1 of the first adhesive layer is preferably 800 μm2 or less; and the distortion cross-sectional area S2 of the second adhesive layer is preferably 360 μm2 or less.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention ,song The present invention relates to an image display device that includes a rigid transparent plate having a surface portion. [Background technology]

[0002] In liquid crystal display devices and organic EL display devices, a polarizing plate is provided on the viewing side surface of the image display cell. A hard transparent plate (cover window) made of glass or resin may be provided on the surface of these image display devices to prevent damage to the image display panel due to impact from the outer surface, and this configuration is becoming mainstream for mobile and in-vehicle applications. By bonding the polarizing plate and the cover window via an adhesive layer, the refractive index difference at the interface is reduced, and the decrease in visibility caused by reflection and scattering can be suppressed, and impact resistance can be imparted.

[0003] In the configuration of an image display device having a polarizing plate on the viewing side surface of an image display cell and a cover window on the viewing side surface of the polarizing plate, it has been proposed to use a double-sided adhesive film having an adhesive layer on one side of the polarizing plate for bonding to the image display cell and an adhesive layer on the other side for bonding to the cover window (see, for example, Patent Document 1). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2014-115468 A Summary of the Invention [Problem to be solved by the invention]

[0005] In recent years, it has become possible to produce organic EL cells using flexible substrates such as resin films, and edge displays with curved edges (longer rectangular parts) of the screen have been put to practical use. In addition, four-sided edge displays in which all four edges of the screen are curved, and curved displays in which the entire screen is curved or spherical have also been proposed.

[0006] In such displays with a curved surface, a flexible optical film (such as a polarizing plate) and an image display cell are attached to a rigid cover window with a curved surface, so that the optical film and the image display cell take on a curved shape that follows the curved shape of the cover window, thereby maintaining the curved shape. In curved parts, the curvature of the inner side (the side closest to the center of curvature) is smaller than that of the outer side, so mechanical distortion occurs at the bonding interface. In particular, spherical displays and corners of the four edges have a three-dimensional curved shape, so distortion is Brushing This makes it easy for peeling and wrinkling to occur at the bonding interface.

[0007] In view of the above, an object of the present invention is to provide an optical film with a pressure-sensitive adhesive that is less likely to peel or wrinkle at the bonding interface even when applied to an image display device having a curved surface. [Means for solving the problem]

[0008] One embodiment of the present invention is an image display device in which at least a portion of the screen is curved. The image display device includes a rigid transparent plate, an optical film, and a flexible image display cell. The transparent plate has a curved portion with a second main surface facing inward, and a first main surface of the optical film is bonded to the second main surface of the transparent plate via a first adhesive layer. The second main surface of the optical film is bonded to the image display cell via a second adhesive layer.

[0009] Examples of the optical film include an optically isotropic film and an optically anisotropic film. Examples of the optically anisotropic film include a polarizer and a retardation plate. The optical film may be a circular polarizing plate formed by laminating a polarizer and a retardation plate. The image display cell may be an organic EL cell, and the image display device may be an organic EL display device having a circular polarizing plate as an optical film on the viewing side surface of the organic EL cell.

[0010] One embodiment of the present invention is a double-sided adhesive optical film used to form the above-mentioned image display device, which has a first adhesive layer on a first main surface of the optical film and a second adhesive layer on a second main surface of the optical film.

[0011] The first adhesive layer used to bond the optical film to the transparent plate has a cross-sectional strain area S 1 is 800μm 2 The second pressure-sensitive adhesive layer used for bonding the optical film and the image display cell preferably has a cross-sectional area S 2 is 360μm 2 The strain cross-sectional area S is an amount expressed by S = (1 / 2) × δT, where δ is the amount of strain in the shear direction when a shear load of 10 kPa is applied to the pressure-sensitive adhesive layer for 15 minutes, and T is the thickness of the pressure-sensitive adhesive layer.

[0012] Thickness T of the first adhesive layer 1 may be 25 to 100 μm, and the thickness T 2 The thickness T of the first pressure-sensitive adhesive layer may be 5 to 30 μm. 1 is the thickness T of the second adhesive layer 2 The strain cross-sectional area S of the first pressure-sensitive adhesive layer may be larger than 1 is the strain cross-sectional area S of the second adhesive layer 2 It may be larger than.

[0013] The first pressure-sensitive adhesive layer and the second pressure-sensitive adhesive layer may be acrylic pressure-sensitive adhesive layers. The pressure-sensitive adhesive constituting these pressure-sensitive adhesive layers preferably contains a polymer having a cross-linked structure. Effect of the Invention

[0014] When the strain cross-sectional area of ​​the pressure-sensitive adhesive layer bonding members together is within a predetermined range, peeling and wrinkling of flexible members in an image display device having curved portions can be suppressed. [Brief description of the drawings]

[0015] [Figure 1] FIG. 1 is a cross-sectional view of an optical film with double-sided pressure-sensitive adhesive according to an embodiment. [Diagram 2] 1 is a cross-sectional view of an image display device according to an embodiment. [Diagram 3] FIG. 2 is a cross-sectional view showing an example of a laminated structure of an organic EL cell. [Figure 4] FIG. 4 is an explanatory diagram of a strain cross-sectional area of ​​a pressure-sensitive adhesive layer. [Diagram 5] FIG. 2 is an explanatory diagram for measuring the amount of strain and the strain cross-sectional area using a rotational rheometer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] FIG. 1 is a cross-sectional view that typically shows an optical film with double-sided adhesive according to one embodiment of the present invention, and FIG. 2 is a cross-sectional view that typically shows an image display device according to one embodiment of the present invention.

[0017] The double-sided adhesive-backed optical film 50 includes an optical film 10, a first adhesive layer 21 provided on a first main surface of the optical film, and a second adhesive layer 22 provided on a second main surface of the optical film. In Fig. 1, a first release film 41 is releasably attached onto the first adhesive layer 21 of the double-sided adhesive-backed optical film 50, and a second release film 42 is releasably attached onto the second adhesive layer 22.

[0018] 2, a first main surface of the optical film 10 is bonded to a second main surface of the cover window 80 via a first pressure-sensitive adhesive layer 21, and a second main surface of the optical film 10 is bonded to an image display cell 70 via a second pressure-sensitive adhesive layer 22. The double-sided pressure-sensitive adhesive-coated optical film 50 and the image display cell 70 are housed in a housing (not shown).

[0019] At least a part of the screen of the image display device 100 has a curved shape with a convex viewer side (upper side of the figure). In Fig. 2, the screen is illustrated as having a spherical curved surface as a whole, but a part of the screen may be curved and the other part may be flat. For example, the screen may be rectangular in plan view, the central part of the screen may be flat, and the edges of the screen (sides of the rectangle) may have a curved shape that curves downward.

[0020] The screen of the image display device may have a three-dimensional curved shape. A three-dimensional curved surface refers to a shape in which the cross-sectional shape of all surfaces including the normal of the surface is a curved shape. For example, a spherical curved surface is a three-dimensional curved surface in which the cross-section of a surface including the normal (a radial straight line) is an arc. In addition, a display device (edge ​​display) in which the rectangular side portions are curved toward the bottom has a three-dimensional curved shape at the corner portion where these two sides intersect when two adjacent sides have curved shapes that are curved toward the bottom. For example, a four-sided edge display in which the entire periphery (all four sides) of a screen that is rectangular in plan view is curved has four corner portions with a three-dimensional curved shape. Note that the cross-section of the center of the rectangular side of the edge display is a curved line in the direction perpendicular to the side, but the cross-section of the direction parallel to the side is a straight line, so the center of the side is a "two-dimensional" curved shape.

[0021] [Image display cell] The image display cell may be an organic EL cell. To form an image display device having a curved surface, it is preferable to use a flexible image display cell. To form a flexible image display cell, a flexible substrate is used.

[0022] 3 shows an example of a layered structure of an image display cell, which is a top-emission organic EL cell. The top-emission organic EL cell includes a metal electrode 73, an organic light-emitting layer 75, and a transparent electrode 77 in this order on a substrate 71, and the transparent electrode 77 side (the upper side in the figure) is the light-emitting surface. A sealant 79 is laminated on the transparent electrode 77. Although not shown in the figure, the sealant 79 is preferably provided so as to cover the side surfaces of the electrodes 73, 77, and the organic light-emitting layer 75.

[0023] A flexible plastic substrate is preferably used as the substrate 71. In a top-emission organic EL cell, the substrate 71 does not need to be transparent, and a highly heat-resistant film such as a polyimide film may be used as the substrate 71. A flexible glass plate (glass film) may be used as the substrate 71.

[0024] The organic light-emitting layer 75 may include an electron transport layer, a hole transport layer, and the like, in addition to an organic layer that itself functions as a light-emitting layer. The transparent electrode 77 is a metal oxide layer or a metal thin film, and transmits light from the organic light-emitting layer 75. The metal electrode 73, the organic light-emitting layer 75, and the transparent electrode 77 are all thin films, and have a thickness that is sufficiently smaller than that of the substrate 71. Therefore, if the substrate 71 is flexible, the entire image display cell 70 is flexible. A back sheet (not shown) may be provided on the back side of the substrate 71 for the purpose of protecting and reinforcing the substrate.

[0025] The organic EL cell may be a bottom emission type in which a transparent electrode, an organic light emitting layer, and a metal electrode are laminated in this order on a substrate. In a bottom emission type organic EL cell, a transparent substrate is used, and the substrate is disposed on the viewing side (second adhesive layer 22 side). The image display cell is not limited to an organic EL cell, and may be a liquid crystal cell or an electrophoretic display cell (electronic paper), etc. A touch panel sensor (not shown) may be disposed on the viewing side surface of the image display cell 70.

[0026] [Cover window] The cover window 80 arranged on the viewing side surface of the image display device is a rigid transparent plate, with a first main surface 81 arranged on the viewing side and a second main surface 82 arranged on the image display cell 70 side. Transparent resins such as acrylic resins and polycarbonate resins, and glass are used as materials for the transparent plate. The thickness of the cover window 80 is, for example, about 50 to 2000 μm. From the viewpoint of increasing durability against external impact, the thickness of the cover window 80 is preferably 200 μm or more, and more preferably 300 μm or more.

[0027] The cover window 80 may be integrated with a touch panel sensor. An anti-reflection layer, a hard coat layer, or the like may be provided on a first main surface 81 of the cover window 80. A light-shielding printed layer may be provided on a part of the surface of the cover window 80.

[0028] The cover window 80 has a curved portion in which the second main surface 82 is on the inside and the first main surface 81 side is convex in at least a part of the surface. The entire cover window 80 may have a curved shape. The curved shape may be three-dimensional. For example, when the entire screen is spherical, the entire cover window has a three-dimensional curved shape. In the cover window of a four-sided edge display, the center of the screen is flat, and at the peripheral portion of the screen, the center portions of the sides have a two-dimensional curved shape, and the corner portions have a three-dimensional curved shape.

[0029] The rigid cover window 80 having a curved portion and the flexible image display cell 70 are bonded together via the optical film 50 with adhesive and integrated, so that the image display cell 70 has a curved shape that conforms to the second main surface 82 (inner surface) of the cover window 80. Note that the first main surface 81 of the cover window 80 generally has a curved portion similar to the second main surface 82, but as long as the second main surface 82 has a curved portion, the first main surface may be a flat surface.

[0030] [Optical film with double-sided adhesive] 2, the cover window 80 and the image display cell 70 are laminated together via the double-sided adhesive optical film 50, and the first adhesive layer 21 arranged on the first main surface (viewing side surface) of the optical film 10 is bonded to the second main surface 82 of the cover window 80. The second adhesive layer 22 arranged on the second main surface of the optical film 10 is bonded to the light exit surface of the image display cell 70.

[0031] <Optical film> Examples of the optical film 10 include an optically isotropic film and an optically anisotropic film. The optically isotropic film is preferably a transparent film. The optically anisotropic film is preferably a retardation plate, a polarizer, or the like. The optical film may be a laminate of a plurality of films or an optically functional film having a coating layer on the film surface.

[0032] An example of a laminate of a plurality of optical films is a polarizing plate, which includes a polarizer and, if necessary, has a transparent film laminated on one or both sides as a polarizer protective film.

[0033] Examples of polarizers include hydrophilic polymer films such as polyvinyl alcohol films, partially formalized polyvinyl alcohol films, and partially saponified ethylene-vinyl acetate copolymer films, which are uniaxially stretched after adsorbing dichroic substances such as iodine or dichroic dyes, and polyene-based oriented films such as dehydrated polyvinyl alcohol and dehydrochlorinated polyvinyl chloride.

[0034] A thin polarizer having a thickness of 10 μm or less can also be used as the polarizer. Examples of the thin polarizer include polarizers described in JP-A-51-069644, JP-A-2000-338329, WO2010 / 100917, Japanese Patent No. 4691205, and Japanese Patent No. 4751481. The thin polarizer can be obtained by a manufacturing method including, for example, a step of stretching a polyvinyl alcohol-based resin layer and a resin substrate for stretching in a laminated state, and a step of dyeing with a dichroic material such as iodine.

[0035] As the polarizer protective film, a transparent resin film such as a cellulose-based resin, a cyclic polyolefin-based resin, an acrylic-based resin, a phenylmaleimide-based resin, a polycarbonate-based resin, etc. is preferably used. When a polarizer protective film is provided on both sides of the polarizer, the transparent films 13 and 15 may be films made of the same resin material or different resin materials.

[0036] Examples of optical functional films include retardation plates, viewing angle widening films, viewing angle limiting (peeping prevention) films, and brightness enhancing films. The optical film 10 may have an optical functional film on one or both surfaces of a polarizer. The optical film 10 may include a touch panel sensor as the optical functional film. In a polarizing plate with a touch panel sensor, a transparent film in contact with the polarizer may function as both a polarizer protective film and an optical functional film. The transparent film may also function as an electrode substrate film for a touch panel sensor.

[0037] The metal electrode 73 of the organic EL cell 70 is light reflective. Therefore, when external light enters the organic EL cell, the light is reflected by the metal electrode, and the reflected light is viewed from the outside as a mirror surface. By disposing a circular polarizing plate as the optical film 10 on the viewing side surface of the organic EL cell 70, the reflected light at the metal electrode is prevented from being re-emitted to the outside, and the visibility and design of the screen of the display device can be improved.

[0038] The circular polarizing plate includes a retardation film on the surface of the polarizer facing the organic EL cell 70. The transparent film disposed adjacent to the polarizer may be the retardation film. When the retardation film has a retardation of λ / 4 and the angle between the slow axis direction of the retardation film and the absorption axis direction of the polarizer is 45°, the laminate of the polarizer and the retardation film functions as a circular polarizing plate for suppressing re-emission of reflected light at the metal electrode. The retardation film constituting the circular polarizing plate may be a laminate of two or more films. For example, a polarizer, a λ / 2 plate, and a λ / 4 plate are laminated so that their optical axes form a predetermined angle, thereby obtaining a wideband circular polarizing plate that functions as a circular polarizing plate over a wide band of visible light. For example, a stretched resin film is used as the retardation film. The retardation film may be an oriented liquid crystal layer.

[0039] <Adhesive layer> The first pressure-sensitive adhesive layer 21 for bonding the optical film 10 to the cover window 80 and the second pressure-sensitive adhesive layer 22 for bonding the optical film 10 to the image display cell 70 are preferably made of an optically transparent pressure-sensitive adhesive. The first pressure-sensitive adhesive layer 21 and the second pressure-sensitive adhesive layer 22 may each be a laminate of a plurality of pressure-sensitive adhesive layers.

[0040] The adhesive layers 21 and 22 are preferably transparent and have low visible light absorption. The total light transmittance of the adhesive layers 21 and 22 is preferably 85% or more, more preferably 90% or more. The haze of the adhesive layers 21 and 22 is preferably 2% or less, more preferably 1% or less. The total light transmittance and haze are measured using a haze meter in accordance with JIS K7136.

[0041] The adhesive constituting the adhesive layers 21 and 22 can be appropriately selected and used from adhesives having base polymers such as acrylic polymers, silicone polymers, polyesters, polyurethanes, polyamides, polyvinyl ethers, vinyl acetate / vinyl chloride copolymers, modified polyolefins, epoxy-based, fluorine-based, and rubber-based polymers as the adhesive constituting the adhesive layer 21. In particular, acrylic adhesives are preferably used because they have excellent optical transparency, exhibit adhesive properties such as appropriate wettability, cohesiveness, and adhesiveness, and are also excellent in weather resistance and heat resistance.

[0042] The acrylic adhesive preferably contains 50% by weight or more of the acrylic base polymer relative to the total solid content of the adhesive composition, more preferably 70% by weight or more, and even more preferably 80% by weight or more. The acrylic base polymer preferably has a main skeleton of a monomer unit of (meth)acrylic acid alkyl ester. In this specification, "(meth)acrylic" means acrylic and / or methacrylic.

[0043] As the (meth)acrylic acid alkyl ester, a (meth)acrylic acid alkyl ester having an alkyl group with 1 to 20 carbon atoms is preferably used. The (meth)acrylic acid alkyl ester may have a branched alkyl group. The content of the (meth)acrylic acid alkyl ester is preferably 40% by weight or more, more preferably 50% by weight or more, and even more preferably 60% by weight or more, based on the total amount of the monomer components constituting the base polymer. The acrylic base polymer may be a copolymer of a plurality of (meth)acrylic acid alkyl esters. The arrangement of the constituent monomer units may be random or block.

[0044] The acrylic base polymer may contain an acrylic monomer having a crosslinkable functional group as a copolymerization component. When the base polymer has a crosslinkable functional group, the gel fraction of the adhesive can be easily increased by thermal crosslinking or photocuring of the base polymer. Examples of the acrylic monomer having a crosslinkable functional group include a hydroxyl group-containing monomer and a carboxyl group-containing monomer.

[0045] Examples of hydroxy group-containing monomers include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate, and (4-hydroxymethyl)cyclohexylmethyl (meth)acrylate.

[0046] The acrylic base polymer may contain a nitrogen-containing monomer as a monomer component. Examples of the nitrogen-containing monomer include vinyl monomers such as N-vinylpyrrolidone, methylvinylpyrrolidone, vinylpyridine, vinylpiperidone, vinylpyrimidine, vinylpiperazine, vinylpyrazine, vinylpyrrole, vinylimidazole, vinyloxazole, vinylmorpholine, (meth)acryloylmorpholine, N-vinylcarboxylic acid amides, and N-vinylcaprolactam, and cyanoacrylate monomers such as acrylonitrile and methacrylonitrile. Among them, N-vinylpyrrolidone and (meth)acryloylmorpholine are preferably used.

[0047] The monomer components forming the acrylic polymer may contain a polyfunctional polymerizable compound (polyfunctional monomer). Examples of the polyfunctional polymerizable compound include a compound having two or more ethylenically unsaturated groups in one molecule, and a compound having one C=C bond and a polymerizable functional group such as epoxy, aziridine, oxazoline, hydrazine, or methylol. Among them, a compound having two or more ethylenically unsaturated groups in one molecule, such as a polyfunctional (meth)acrylate, is preferred. Specific examples of the polyfunctional polymerizable compound include polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, polytetramethylene glycol di(meth)acrylate, bisphenol A ethylene oxide modified di(meth)acrylate, bisphenol A propylene oxide modified di(meth)acrylate, alkanediol di(meth)acrylate, tricyclodecane dimethanol di(meth)acrylate, ethoxylated isocyanuric acid triacrylate, pentaerythritol tri(meth)acrylate, and pentaerythritol di(meth)acrylate. acrylate, trimethylolpropane tri(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, ethoxylated pentaerythritol tetra(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol poly(meth)acrylate, dipentaerythritol hexa(meth)acrylate, neopentyl glycol di(meth)acrylate, glycerin di(meth)acrylate, urethane (meth)acrylate, epoxy (meth)acrylate, butadiene (meth)acrylate, isoprene (meth)acrylate, etc. The polyfunctional polymerizable compound may be an oligomer.

[0048] The base polymer can be prepared by a known polymerization method such as solution polymerization, UV polymerization, bulk polymerization, emulsion polymerization, etc. In preparing the base polymer, a polymerization initiator such as a photopolymerization initiator or a thermal polymerization initiator may be used depending on the type of polymerization reaction. A chain transfer agent may be used to adjust the molecular weight of the base polymer.

[0049] From the viewpoint of providing the pressure-sensitive adhesive with appropriate adhesive retention and flexibility, the weight-average molecular weight of the base polymer is preferably from 200,000 to 1,000,000, and more preferably from 250,000 to 800,000. The molecular weight of the base polymer refers to the molecular weight of the polymer before the introduction of a crosslinked structure.

[0050] When a polyfunctional monomer is used in addition to a monofunctional monomer as a monomer component forming a base polymer, the monofunctional monomer may be polymerized first to form a prepolymer composition with a low degree of polymerization (prepolymerization), and the polyfunctional monomer may be added to the syrup of the prepolymer composition to polymerize the prepolymer and the polyfunctional monomer (postpolymerization). In this way, by performing prepolymerization of the prepolymer, a crosslinked structure by the polyfunctional monomer can be uniformly introduced into the base polymer. In addition, a mixture (adhesive composition) of a prepolymer composition and an unpolymerized monomer component may be applied onto a substrate, and then postpolymerization may be performed on the substrate to form a pressure-sensitive adhesive layer. Since the prepolymer composition has low viscosity and excellent coatability, the method of performing postpolymerization on a substrate after applying a pressure-sensitive adhesive composition, which is a mixture of a prepolymer composition and an unpolymerized monomer, can increase the productivity of the pressure-sensitive adhesive layer and make the thickness of the pressure-sensitive adhesive layer uniform.

[0051] The prepolymer composition can be prepared, for example, by partially polymerizing (preliminarily polymerizing) a composition (referred to as a "prepolymer-forming composition") obtained by mixing a monomer component constituting an acrylic base polymer with a polymerization initiator. The monomer in the prepolymer-forming composition is preferably a monofunctional monomer such as a (meth)acrylic acid alkyl ester or a polar group-containing monomer among the monomer components constituting the acrylic polymer. The prepolymer-forming composition may contain a polyfunctional monomer. For example, a part of the polyfunctional monomer component that is the raw material of the base polymer may be contained in the prepolymer-forming composition, and the remaining part of the polyfunctional monomer component may be added after polymerization of the prepolymer to be subjected to post-polymerization.

[0052] The prepolymer forming composition may contain a chain transfer agent or the like as necessary in addition to the monomer and the polymerization initiator. The polymerization method of the prepolymer is not particularly limited, but from the viewpoint of adjusting the reaction time to set the molecular weight (polymerization rate) of the prepolymer in a desired range, polymerization by irradiation with active light such as UV light is preferred. The polymerization initiator and chain transfer agent used in the preliminary polymerization are not particularly limited.

[0053] The polymerization rate of the prepolymer is not particularly limited, but is preferably 3 to 50% by weight, more preferably 5 to 40% by weight, from the viewpoint of obtaining a viscosity suitable for application onto a substrate. The polymerization rate of the prepolymer can be adjusted to a desired range by adjusting the type and amount of the photopolymerization initiator used, the irradiation intensity and irradiation time of the actinic ray such as UV light, etc.

[0054] The prepolymer composition is mixed with the remaining monomer components constituting the acrylic base polymer (post-polymerization monomer), and, if necessary, a polymerization initiator, a chain transfer agent, a silane coupling agent, a crosslinking agent, etc. to form a pressure-sensitive adhesive composition. The post-polymerization monomer preferably contains a polyfunctional monomer. As the post-polymerization monomer, a monofunctional monomer may be added in addition to the polyfunctional monomer.

[0055] The base polymer of the pressure-sensitive adhesive preferably has a cross-linked structure. When the base polymer has a cross-linked structure, the creep rate C of the pressure-sensitive adhesive decreases, and therefore the strain cross-sectional area described below tends to decrease.

[0056] For example, as described above, a base polymer having a crosslinked structure can be obtained by using a polyfunctional polymerizable compound as a monomer component forming the base polymer. After polymerizing the base polymer, a crosslinked structure can also be formed by adding a crosslinking agent. As the crosslinking agent, a commonly used one such as an isocyanate-based crosslinking agent, an epoxy-based crosslinking agent, an oxazoline-based crosslinking agent, an aziridine-based crosslinking agent, a carbodiimide-based crosslinking agent, or a metal chelate-based crosslinking agent can be used. The content of the crosslinking agent is usually in the range of 0.01 to 5 parts by weight, preferably 0.05 to 3 parts by weight, and more preferably 0.07 to 2.5 parts by weight, relative to 100 parts by weight of the base polymer. The base polymer may contain both a crosslinked structure due to a polyfunctional polymerizable compound and a crosslinked structure due to a crosslinking agent such as polyisocyanate.

[0057] The adhesive may contain an ultraviolet absorbing agent. Examples of ultraviolet absorbing agents include benzotriazole-based ultraviolet absorbing agents, benzophenone-based ultraviolet absorbing agents, triazine-based ultraviolet absorbing agents, salicylate-based ultraviolet absorbing agents, and cyanoacrylate-based ultraviolet absorbing agents. Triazine-based ultraviolet absorbing agents and benzotriazole-based ultraviolet absorbing agents are preferred because they have high ultraviolet absorbing properties and excellent compatibility with acrylic polymers, and are easy to obtain highly transparent acrylic adhesive sheets. Among them, triazine-based ultraviolet absorbing agents containing a hydroxyl group and benzotriazole-based ultraviolet absorbing agents having one benzotriazole skeleton in one molecule are preferred.

[0058] In addition to the above-listed components, the adhesive may contain additives such as a silane coupling agent, a tackifier, a plasticizer, a softener, an anti-degradation agent, a filler, a colorant, an antioxidant, a surfactant, and an antistatic agent.

[0059] The adhesive composition is applied in layers onto the substrate, and the solvent is dried and the base polymer is crosslinked and cured as necessary to form an adhesive layer. The thickness of the adhesive layers 21, 22 is not particularly limited, and is generally about 5 to 500 μm. When a decorative printed layer is provided on the second main surface of the cover window 80, the thickness of the first adhesive layer 21 is preferably 25 μm or more, and more preferably 30 μm or more, in order to provide step absorbency for printed steps. The thickness of the first adhesive layer 21 may be 35 μm or more, 40 μm or more, or 45 μm or more.

[0060] In the curved portion of the cover window 80, the curvature of the image display cell 70 located inside the curved surface is the largest (the radius of curvature is the smallest), and the distortion is large. Therefore, peeling and wrinkling are likely to occur in the portion where the distortion of the flexible image display cell 70 is large. In particular, when the cover window 80 has a three-dimensional curved surface shape, distortion occurs in all directions, and it is difficult to release the distortion, so peeling and wrinkling are likely to occur.

[0061] In the present invention, the first pressure-sensitive adhesive layer 21 and the second pressure-sensitive adhesive layer 22 of the double-sided pressure-sensitive adhesive optical film have a predetermined creep characteristic, so that peeling between layers and the occurrence of wrinkles in a display device having a curved surface portion can be suppressed. 1 is 800μm 2 The following is preferable, and the strain cross-sectional area S s is 360μm 2 The following is preferable. The strain cross-sectional area S is an amount expressed by S = (1 / 2) × δT, where δ is the amount of strain in the shear direction when a shear load (stress) of 10 kPa is applied to the adhesive layer for 15 minutes, and T is the thickness of the adhesive layer.

[0062] Fig. 4 is an explanatory diagram of the concept of strain cross-sectional area of ​​a pressure-sensitive adhesive layer, and shows a schematic cross section of a state in which a shear load is applied in the direction of the arrow with one surface of an end of the pressure-sensitive adhesive layer 2 attached to an adherend 1. The cross section of the pressure-sensitive adhesive layer 2 before the shear load is applied is rectangular (dashed line in Fig. 4), whereas when a certain shear load is applied with the bottom surface of the pressure-sensitive adhesive layer 2 fixed to the adherend 1, the upper surface deforms the most and the cross section of the pressure-sensitive adhesive layer deforms into a parallelogram (solid line in Fig. 4).

[0063] If the amount of strain on the top surface is δ and the thickness of the adhesive layer is T, the amount of deformation in the cross section of the adhesive layer is expressed as the area of ​​a triangle S = (1 / 2) × δT. This cross-sectional area S is the strain cross-sectional area. The creep rate C is the ratio of the amount of strain δ to the thickness T, and is expressed as C = δ / T, so the strain cross-sectional area is S = (1 / 2)CT 2 can be rewritten as:

[0064] The amount of strain δ of the adhesive layer can be measured using a rotational rheometer. As shown in Figure 5, when a constant torsional force is applied to parallel plates of diameter D, the upper plate rotates by θ°. The amount of rotation of the outer periphery of the parallel plates at this time, i.e., the length of the arc πD(θ / 360), is the amount of strain δ, and the creep rate C, which is the ratio of thickness T to the amount of strain δ, is C=πDθ / 360T.

[0065] The creep rate C does not change even if the thickness of the adhesive layer changes. For example, when two identical adhesive layers are laminated and the same stress (twice the shear load) is applied as when there is only one adhesive layer, the thickness of the adhesive layer is 2T and the amount of strain is 2δ, so the creep rate C is 2δ / 2T=δ / T, which is the same as when there is only one adhesive layer. In other words, it can be said that the creep rate is a value specific to the adhesive material.

[0066] As mentioned above, the strained cross-sectional area S is a function of the creep rate C and the square of the thickness T. 2Therefore, when the material of the adhesive layer is the same, the greater the thickness, the greater the strain cross-sectional area. In order to reduce the strain cross-sectional area S of the adhesive layer and suppress the occurrence of peeling and wrinkles, it is preferable that the thickness T of the adhesive layer is small. In particular, the second adhesive layer 22 used to bond the optical film 10 and the image display cell 70 bonds flexible members together, and therefore, if the strain caused by the curved surface is large, it is likely to cause peeling and wrinkles. Therefore, the thickness T of the second adhesive layer 22 2 is preferably 30 μm or less, more preferably 25 μm or less, even more preferably 20 μm or less, and particularly preferably 15 μm or less. 2 is 250μm 2 Less than 150μm is preferable 2 Less than 100μm is more preferable. 2 More preferred are: S 2 is 70μm 2 Below, 50μm 2 Below, 40μm 2 Less than or equal to 30μm 2 It may be the following.

[0067] From the viewpoint of suppressing wrinkles and peeling at the curved surface portion, the strain cross-sectional area S 2 It is preferable that S is as small as possible. 2 The smaller the strain cross-sectional area S of the second adhesive layer 22, the more the occurrence of peeling and wrinkles can be suppressed even when the layer is used to bond a curved surface with a large curvature (small radius of curvature). On the other hand, if the strain cross-sectional area S of the second adhesive layer 22 is excessively small, peeling may occur due to insufficient adhesive strength. Therefore, 2 is 1μm 2 More than 2μm is preferable. 2 The above is more preferable.

[0068] Creep rate C of the second adhesive layer 2is preferably 80% or less, more preferably 50% or less, and even more preferably 40% or less. As described above, the smaller the thickness T of the adhesive layer and the smaller the creep rate C, the smaller the strain cross-sectional area S. The higher the molecular weight of the base polymer and the higher the degree of cross-linking, the smaller the creep rate of the adhesive tends to be. Therefore, by increasing the amount of cross-linking agent or polyfunctional monomer, an adhesive with a small creep rate can be obtained. In addition, the higher the glass transition temperature of the base polymer, the greater the interaction between molecular chains, such as entanglement of molecular chains, and therefore the smaller the creep rate at room temperature tends to be.

[0069] In the curved surface portion of the image display device, the first pressure-sensitive adhesive layer 21 has a smaller curvature (larger radius of curvature) than the second pressure-sensitive adhesive layer 22. In addition, since the first pressure-sensitive adhesive layer 21 bonds the optical film 10 to the cover window 80, which is a rigid member, the pressure-sensitive adhesive layer does not deform at the interface on the cover window 80 side, and is less likely to cause wrinkles than the second pressure-sensitive adhesive layer 22. Therefore, the strain cross-sectional area S 1 is the strain cross-sectional area S of the second adhesive layer 22 2 The thickness T of the first pressure-sensitive adhesive layer 21 may be larger than 1 is the thickness T of the second adhesive layer 22 2 It may be larger than.

[0070] As described above, the thickness T of the second adhesive layer 22 2 Reduce the strain cross-sectional area S 2 By reducing the thickness T 1 The cross-sectional area S 1 By using an adhesive layer with a large thickness, it is possible to provide impact resistance against impact from the viewing side surface and step absorption for printing steps such as a decorative printing layer provided on the second main surface 82 of the cover window 80.

[0071] On the other hand, the strain cross-sectional area S 1If the strain cross-sectional area S of the first pressure-sensitive adhesive layer 21 is excessively large, this may cause peeling or wrinkling of the optical film 10 and the image display cell 70. 1 is 800μm 2 The following is preferred: S 1 is 600μm 2 Less than 500μm is more preferable. 2 More preferably, the strain cross-sectional area S 1 In order to set the thickness T of the first pressure-sensitive adhesive layer in the above range, 1 is preferably 100 μm or less, more preferably 90 μm or less, and even more preferably 80 μm or less. 1 may be 70 μm or less, 60 μm or less, or 50 μm or less.

[0072] From the viewpoint of providing the first pressure-sensitive adhesive layer 21 with appropriate impact resistance and flexibility, the storage modulus G' of the first pressure-sensitive adhesive layer 21 at 25°C is preferably 0.35 MPa or less, more preferably 0.30 MPa or less, and even more preferably 0.25 MPa or less. On the other hand, when the pressure-sensitive adhesive layer 21 is excessively soft, the creep rate C 1 becomes larger, and the strain cross-sectional area S 1 The storage modulus of the first pressure-sensitive adhesive layer 21 at 25° C. is preferably 0.05 MPa or more, and more preferably 0.10 MPa or more. From the same viewpoint, the storage modulus of the second pressure-sensitive adhesive layer 22 at 25° C. is preferably 0.05 MPa or more, and more preferably 0.10 MPa or more.

[0073] <Release film> As shown in Fig. 1, the double-sided adhesive-attached optical film preferably has release films 41, 42 temporarily attached to the surfaces of the adhesive layers 21, 22 until it is used to form an image display cell. The release films 41, 42 preferably have a release layer on the surface of the film substrate. Examples of materials for the release layer include silicone-based release agents, fluorine-based release agents, long-chain alkyl-based release agents, and fatty acid amide-based release agents. Silicone release agents are preferred because they can achieve both adhesion to acrylic adhesives and releasability.

[0074] The film substrate of the release film is preferably a resin film having transparency. Examples of the resin material include polyester-based resins such as polyethylene terephthalate and polyethylene naphthalate, acetate-based resins, polyethersulfone-based resins, polycarbonate-based resins, polyamide-based resins, polyimide-based resins, polyolefin-based resins, (meth)acrylic-based resins, polyvinyl chloride-based resins, polyvinylidene chloride-based resins, polystyrene-based resins, polyvinyl alcohol-based resins, polyarylate-based resins, and polyphenylene sulfide-based resins. Among these, polyester-based resins such as polyethylene terephthalate (PET) are particularly preferred. The thickness of the release film is preferably 10 to 200 μm, and more preferably 25 to 80 μm. The thickness of the first release film 41 and the thickness of the second release film 42 may be the same or different.

[0075] [Formation of image display device] The image display device 100 is formed by bonding the cover window 80 to the first adhesive layer 21 and bonding the image display cell 70 to the second adhesive layer 22. The order of bonding is not particularly limited, and the bonding of the cover window 80 may be performed first, the bonding of the image display cell 70 may be performed first, or both may be performed simultaneously.

[0076] After the cover window 80 and the image display cell 70 are bonded to the adhesive layers 21 and 22, treatments such as heating, pressurization, and decompression may be performed to remove air bubbles at the bonding interface and in the vicinity of the printing step. Autoclave treatment may be performed to suppress delay bubbles, etc.

[0077] As described above, since the first adhesive layer 21 and the second adhesive layer 22 have predetermined properties, peeling between layers and the occurrence of wrinkles in the optical film 10 and the image display cell 70 can be suppressed even in an image display device in which the cover window 80 has a curved portion. EXAMPLES

[0078] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples.

[0079] [Preparation of adhesive sheets and creep measurements] <Adhesive A~N> Monomers (total 100 parts by weight) were charged in a reaction vessel in the weight ratio shown in Table 1, 0.1 parts by weight of photopolymerization initiator (BASF's "Irgacure 184") was added, and ultraviolet light was irradiated under a nitrogen atmosphere to obtain a prepolymer composition with a polymerization rate of about 10%. To 100 parts by weight of this prepolymer composition, 0.2 parts by weight of photopolymerization initiator (BASF's "Irgacure 651"), 1,6-hexanediol diacrylate (HDDA) in the amount shown in Table 1 as a multifunctional monomer, and 0.3 parts by weight of a silane coupling agent (Shin-Etsu Chemical's "KBM-403") were added and mixed uniformly to prepare a pressure-sensitive adhesive composition.

[0080] The above-mentioned pressure-sensitive adhesive composition was applied to the release-treated surface of a release film (a polyester film with one side treated with silicone for release) to a thickness of 50 μm to form a coating layer, and the release-treated surface of another release film was laminated onto this coating layer. After that, the irradiation intensity on the irradiated surface directly under the lamp was 5 mW / cm 2 The black light was adjusted so that the cumulative light output was 3000mJ / cm 2 Polymerization was allowed to proceed by UV irradiation until the polymer reached a state where a pressure-sensitive adhesive sheet had release films temporarily attached to both sides.

[0081] <Adhesive O, P> Monomers (total 100 parts by weight) in the weight ratio shown in Table 1, 233 parts by weight of ethyl acetate, and 0.2 parts by weight of azobisisobutyronitrile (AIBN) as a thermal polymerization initiator were charged into a reaction vessel, and the mixture was stirred for 1 hour under a nitrogen atmosphere at 23°C, followed by nitrogen substitution. After that, the mixture was reacted at 65°C for 5 hours, and then at 70°C for 2 hours to prepare a solution of an acrylic polymer with a weight average molecular weight of about 450,000. 0.27 parts by weight of trimethylolpropane xylylene diisocyanate (Mitsui Chemicals' "Takenate D110N") was added to this solution as an isocyanate crosslinking agent to prepare a pressure-sensitive adhesive composition.

[0082] The above-mentioned adhesive composition was applied to the release-treated surface of a release film so that the thickness after drying would be 50 μm, and the adhesive was heated at 130° C. for 3 minutes to remove the solvent.The release-treated surface of another release film was then superimposed on the adhesive layer to obtain an adhesive sheet with release films temporarily attached to both sides.

[0083] <Measurement of creep amount and storage modulus> The release film was peeled off and the pressure-sensitive adhesive layer was laminated to a thickness of about 1.5 mm to prepare a measurement sample. Creep measurement and dynamic viscoelasticity measurement were performed under the following conditions using a rotational rheometer (Rheometric Scientific's "Advanced Rheometric Expansion System (ARES)") equipped with a parallel plate of 8.0 mmφ. The creep rate C was calculated from the strain amount δ in the creep measurement, and the storage modulus at 25°C was read from the results of the dynamic viscoelasticity measurement. (Creep measurement) Stress: 10kPa Measurement temperature: 25℃ (Dynamic viscoelasticity measurement) Measurement frequency: 1Hz Heating rate: 5℃ / min

[0084] Table 1 shows the compositions of adhesives A to P, as well as the measurement results of the creep rate and storage modulus of adhesive sheets with a thickness of 50 μm.

[0085] [Table 1]

[0086] [Preparation of polarizing plate with double-sided adhesive] Using a roll laminator, adhesive sheet 1 was laminated on one side (on the hard coat layer) of a polarizing plate having a thickness of about 75 μm, and adhesive sheet 2 was laminated on the other side to obtain a long polarizing plate with double-sided adhesive (samples 1 to 42). The polarizing plate used was one in which a triacetyl cellulose film (32 μm) provided with a hard coat layer was laminated on one side of a polarizer made of a stretched polyvinyl alcohol film having a thickness of 12 μm impregnated with iodine, and a triacetyl cellulose film (31 μm) provided with a coating retardation layer was laminated on the other side of the polarizer.

[0087] The adhesive sheets 1 and 2 used were those shown in Table 2. The adhesive types A to P shown in Table 2 were the same as those used in the adhesive sheets A to P in the adhesive sheet production examples described above, and the thicknesses were changed as shown in Table 2. The strain cross-sectional area S of the adhesive sheet was calculated based on the following formula from the adhesive sheet thickness T and the creep amount C measured using adhesive sheets A to P with a thickness of 50 μm. S = (1 / 2) × CT 2

[0088] <Lamination evaluation> The release film was peeled off from the adhesive sheet 2 of samples 1 to 42, and a 25 μm thick polyimide film ("Kapton EN100" manufactured by Toray DuPont) was laminated by roll-to-roll. This sample was cut into a 40 mm x 40 mm square, the release film was peeled off from the adhesive sheet 1, and the adhesive sheet 1 was laminated to the center of the inner surface of a spherical glass having a thickness of 2 mm, a diameter of 65 mm, and an inner surface curvature radius of 100 mm. The lamination was performed using a vacuum laminator under the conditions of a vacuum pressure of 100 Pa, a pressure of 0.2 MPa, and a pressure time of 10 seconds at room temperature. After that, the sample was treated in an autoclave at 50°C and 0.5 MPa for 15 minutes.

[0089] The sample after autoclaving was placed in a heating oven at 85° C. for 240 hours, and then the sample was taken out and the state of bonding was visually inspected and evaluated according to the following criteria. 〇: The bonding state of each layer was maintained △: Wrinkles less than 5mm wide were found ×: Wrinkles or peeling of 5 mm or more were confirmed

[0090] Table 2 shows the adhesive sheets (type of adhesive, thickness and strain cross-sectional area of ​​adhesive sheet) used in Samples 1 to 42, as well as the results of the bonding evaluation.

[0091] [Table 2]

[0092] As shown in Table 2, the small thickness of Adhesive Sheet 1 and Adhesive Sheet 2 reduces the strain cross-sectional area, and peeling and wrinkling can be suppressed when the sheets are attached to a curved rigid member. [Explanation of symbols]

[0093] 10 Optical film (circular polarizing plate) 21, 22 Adhesive layer 41,42 Release film 50 Optical film with double-sided adhesive 70 Image display cell (organic EL cell) 71 Flexible substrate 80 Transparent plate (cover window) 100 Image display device

Claims

1. An image display device in which at least a part of a screen has a three-dimensional curved shape, a rigid transparent plate having a first main surface and a second main surface, the second main surface being on the inside, and having a three-dimensional curved portion; an optical film having a first major surface and a second major surface; A flexible image display cell; A first pressure-sensitive adhesive layer that bonds the first main surface of the optical film and the second main surface of the transparent plate; and a second pressure-sensitive adhesive layer that bonds a second main surface of the optical film to the image display cell; The first pressure-sensitive adhesive layer has a strain cross-sectional area S 1 is 800 μm 2 is as follows: The second pressure-sensitive adhesive layer has a strain cross-sectional area S 2 is 360 μm 2 Below is the Image display device: Here, the strain cross-sectional area S is an amount expressed by S = (1 / 2) × δT, where δ is the amount of strain in the shear direction when a shear load of 10 kPa is applied to the pressure-sensitive adhesive layer for 15 minutes, and T is the thickness of the pressure-sensitive adhesive layer. A three-dimensional curved surface shape is a shape in which the cross-sectional shape of every plane including the normal line of the plane is a curve.

2. The image display device according to claim 1 , wherein the optical film comprises a polarizer.

3. The image display device according to claim 2 , wherein the optical film includes a circular polarizing plate, and the image display cell is an organic EL cell.

Citation Information

Patent Citations

  • Optical film having adhesive agent on both sides, and manufacturing method of image display unit using the same

    JP2014115468A

  • Optical laminate

    JP2018025764A

  • Optical laminate

    JP2018025765A

  • Optical film with adhesive on both sides and image display device

    JP2018200387A

  • Polarizing plate with front plate

    JP2020046649A