Leather-like sheet

The leather-like sheet design with ultrafine fibers, polyether polyurethane, and heat-resistant particles addresses frictional melting and bending resistance issues, ensuring durability and longevity in sports shoes.

JP7565300B2Active Publication Date: 2024-10-10KURARAY CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2021567143
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-12-25
Filing Date
2020-12-03
Publication Date
2024-10-10
Estimated Expiration
2040-12-03

AI Technical Summary

Technical Problem

Leather-like sheets used in sports shoes for gymnasiums face challenges with high frictional melting and bending resistance, leading to potential melting due to frictional heat and cracking from repeated bending during athletic movements.

Method used

A leather-like sheet design comprising a fiber base material with ultrafine fibers, an intermediate resin layer, and a surface resin layer containing polyether polyurethane and heat-resistant spherical fine particles, which provides high friction melting resistance and bending resistance.

Benefits of technology

The design achieves a leather-like sheet with a surface that resists frictional melting and bending, maintaining integrity through 300,000 cycles or more without cracking, with a balanced mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007565300000002
    Figure 0007565300000002
  • Figure 0007565300000001
    Figure 0007565300000001
Patent Text Reader

Abstract

This leather-like sheet comprises: a fiber base material; an intermediate resin layer layered on one surface of the fiber base material; and a surface resin layer layered on the intermediate resin layer. The surface resin layer contains a polyether polyurethane and spherical fine particles having heat resistance at 200°C, the content ratio of the spherical fine particles being 5 to 40% by mass. The spherical fine particles have a specific heat of 0.95 kJ / (kg·K) or more. Particle size D50 (median diameter), at the cumulative distribution of 50% by volume, is 2.5 to 10 μm. Particle size {D10, at the cumulative distribution of 10% by volume, satisfies D50 / D10≤3 which is a particle size dispersion degree.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a leather-like sheet. [Background technology]

[0002] Leather-like sheets such as artificial leather and synthetic leather have been used as interior materials for shoes, clothing, vehicles, and furniture. Some applications of such leather-like sheets involve contact with other objects. In such applications, the leather-like sheets are required to have a property of being resistant to wear due to friction with other objects.

[0003] For example, Patent Document 1 below discloses a leather-like sheet in which a resin skin layer mainly made of non-yellowing polycarbonate-based urethane resin is laminated on the surface of a natural leather substrate via an adhesive layer made of a resin mainly made of polycarbonate-based urethane resin, and the resin skin layer contains 3 to 50 parts by weight of spherical fine powder with an average particle size of 10 μm or less per 100 parts by weight of the resin mainly made of non-yellowing polycarbonate-based urethane resin. The spherical fine powder is disclosed to be melamine resin, phenol resin, or benzoguanamine resin.

[0004] For example, Patent Document 2 listed below discloses a ball cover material including a fiber base material and a surface resin layer that is disposed on one side of the fiber base material and contains a polymeric elastomer, inorganic particles, and protein powder. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 7-150479 [Patent Document 2] JP 2016-67666 A Summary of the Invention [Problem to be solved by the invention]

[0006] For example, shoes used for sports in gymnasiums are repeatedly rubbed against the floor during the game, and the rubbed parts may melt due to frictional heat. In addition, sports shoes used for sports in gymnasiums are repeatedly flexed due to the movements of the athletes. For this reason, there has been a demand for leather-like sheets with a surface that is highly resistant to frictional melting and is less likely to melt due to frictional heat, as well as highly flexing resistance, for sports shoes used for sports in gymnasiums.

[0007] An object of the present invention is to provide a leather-like sheet having a surface that combines high resistance to friction and melting with high resistance to bending. [Means for solving the problem]

[0008] One aspect of the present invention is a fiber substrate, comprising: an intermediate resin layer laminated on one surface of the fiber substrate; and a surface resin layer laminated on the intermediate resin layer. The fiber substrate is a fiber substrate having a thickness of 0.3 to 2.0 mm, which is obtained by impregnating a nonwoven fabric, woven fabric, knitted fabric, or a sheet combining these fabrics, containing ultrafine fibers having a fineness of 0.5 dtex or less, with a polymer elastomer so that the ultrafine fibers / polymer elastomer ratio is in the range of 50 / 50 to 95 / 5 (mass ratio), and the table The surface resin layer is , 10 to 60 μm thick, Polyurethane More than 60% by mass of Spherical particles with heat resistance up to 200℃ 5 ~40 mass %, contains Spherical particles have a specific heat of 0.95 kJ / (kg K) or more and a particle size D at a cumulative distribution of 50% by volume. 50 (Median diameter) is 2.5 to 10 μm, and the particle size D when the cumulative distribution is 10% by volume 10 is the particle size distribution D 50 / D 10 ≦3, meet In addition, when a bending test is performed using a flexometer at 20°C, the number of cycles at which cracks appear in the surface resin layer is 300,000 or more. According to such a leather-like sheet, a leather-like sheet having a surface that is both highly resistant to friction and melting and highly resistant to bending can be obtained.

[0009] Examples of the spherical fine particles include melamine resin-silica composite particles, benzoguanamine resin particles, and polytetrafluoroethylene resin particles.

[0010] The surface resin layer has a thickness of 10 to 60 μm. Therefore, A leather-like sheet with a good balance of high friction melting resistance, high bending resistance, and mechanical properties is obtained. do.

[0011] In addition, when a bending test was performed using a flexometer in an environment of 20°C, the number of cycles required for cracks to appear in the surface resin layer was 300,000 or more. Therefore, A leather-like sheet with an excellent balance between high friction melting resistance and high bending resistance can be obtained. do.

[0012] In addition, the fiber base material is a nonwoven material containing ultrafine fibers with a fineness of 0.5 dtex or less. Included in sheets made of cloth, woven fabric, knitted fabric, or a combination of these The polymer elastomer is impregnated with the Therefore, A leather-like sheet with a good balance of high friction melting resistance, high bending resistance, and mechanical properties is obtained. do. Effect of the Invention

[0013] According to the present invention, a leather-like sheet is obtained having a surface that combines high resistance to friction melting and high resistance to bending. [Brief description of the drawings]

[0014] [Figure 1] FIG. 1 is a schematic cross-sectional view of a leather-like sheet 10 according to an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] An embodiment of the leather-like sheet of the present invention will now be described in detail with reference to the drawings, in which: Fig. 1 is a schematic cross-sectional view of a leather-like sheet 10 of this embodiment.

[0016] 1, the leather-like sheet 10 comprises a fiber base material 1, an intermediate resin layer 3 adhered to one surface of the fiber base material 1 via an adhesive layer 2, and a surface resin layer 4 laminated on the intermediate resin layer 3. The resin layer including the adhesive layer 2, the intermediate resin layer 3, and the surface resin layer 4 forms a grain-finished resin layer 5. The grain-finished resin layer 5 is a layer that gives the leather-like sheet 10 an appearance and feel similar to the grain surface of natural leather. The grain-finished resin layer 5 may further include other layers, such as a top coat layer, as necessary.

[0017] The surface resin layer 4 includes a polymer elastomer containing polyether polyurethane, and spherical fine particles 4a dispersed in the polymer elastomer, the spherical fine particles 4a having a heat resistance of 200° C. The spherical fine particles 4a have a specific heat of 0.95 kJ / (kg·K) or more and a particle diameter D at a cumulative distribution of 50% by volume. 50 (Median diameter) is 2.5 to 10 μm, and the particle size D when the cumulative distribution is 10% by volume 10 is the particle size distribution D 50 / D 10 The surface resin layer 4 contains a polymer elastomer containing polyether polyurethane and the above-mentioned spherical fine particles having a heat resistance of 200°C, thereby providing the leather-like sheet 10 with a surface that has both high resistance to friction and melting and high resistance to bending.

[0018] The fiber substrate is not particularly limited and is mainly made of nonwoven fabric, woven fabric, knitted fabric, or a combination of these materials that have been conventionally used in the manufacture of leather-like sheets, and further impregnated with a polymeric elastomer as necessary. Among these, a fiber substrate containing a nonwoven fabric, particularly a nonwoven fabric containing ultrafine fibers with a fineness of 0.5 dtex or less impregnated with a polymeric elastomer, is preferred because it is easy to obtain a dense leather-like sheet with high mechanical strength.

[0019] The fibers forming the fiber substrate preferably contain ultrafine fibers with a fineness of 0.5 dtex or less, and more preferably 0.0001 to 0.2 dtex, because it is easy to obtain a leather-like sheet with high homogeneity and low fiber density unevenness. The fineness is determined by taking a 3000x magnification image of a cross section parallel to the thickness direction of the raised artificial leather with a scanning electron microscope (SEM) and calculating the average value of 15 fiber diameters selected uniformly from the fiber using the density of the resin forming the fiber.

[0020] The type of resin forming the fiber is not particularly limited. Specific examples of resins forming the fiber include polyamide resins such as polyamide 6, polyamide 66, polyamide 610, aromatic polyamide, and polyamide elastomer; polyester resins such as polyethylene terephthalate (PET), polytrimethylene terephthalate, polybutylene terephthalate (PBT), and polyester elastomer; acrylic resins; olefin resins; synthetic fibers such as polyvinyl alcohol resins; and various natural and semi-synthetic fibers. These may be used alone or in combination of two or more. As a method for producing synthetic fibers, a method in which a resin is melted at a temperature above its melting point and extruded from an extruder to perform melt spinning, a dry solution spinning method in which a polymer solution is extruded through a fine hole and the solvent is evaporated, and a wet solution spinning method in which a polymer solution is spun into a non-solvent are used without particular limitation. In addition, a nonwoven fabric of ultrafine fibers can be obtained by, for example, entangling ultrafine fiber-generating fibers such as sea-island composite fibers to form a fiber entanglement body, and then subjecting the fiber to ultrafine fiber processing.

[0021] The fiber substrate may include a polymeric elastomer impregnated therein. The type of polymeric elastomer impregnated in the fiber substrate is not particularly limited, but specific examples include polyurethane; acrylic elastomers such as acrylonitrile-butadiene copolymers and copolymers of acrylic acid esters or methacrylic acid esters; polyamide elastomers; and various polymeric elastomers such as silicone rubber. Among these, polyurethane is particularly preferred because it provides a good feel. The soft segment of polyurethane may include one of polyester units, polyether units, and polycarbonate units, or may be used in combination. These may be used alone or in combination of two or more.

[0022] Fiber-based Of materials, Impregnated polymer elasticity Body The content ratio is the mass ratio of the fiber forming the fiber substrate to the polymer elastomer (fiber / polymer elastomer). 、6 The range is 0 / 40~95 / 5. do.If the content of the polymeric elastomer is too high, the leather-like sheet obtained tends to have a hard, rubber-like feel.

[0023] Fiber substrate thickness teeth, 0.3~2.0m m, 0 It is preferable that it be .5 to 1.5 mm.

[0024] 1, a surface resin layer 4 is laminated on one side of a fiber substrate 1 of a leather-like sheet 10 via an adhesive layer 2 and an intermediate resin layer 3. The surface resin layer 4 is a layer that imparts a surface with both high resistance to friction and melting when the surface of the leather-like sheet is repeatedly rubbed and high bending resistance that makes it difficult for cracks to occur even when repeatedly bent. Such a surface resin layer 4 contains a polymeric elastomer containing polyether polyurethane, and spherical fine particles 4a having a heat resistance of 200°C that are dispersed in the polymeric elastomer.

[0025] The spherical particles have a heat resistance of 200°C, a specific heat of 0.95 kJ / (kg K) or more, and a particle diameter D at a cumulative distribution of 50% by volume. 50 (Median diameter) is 2.5 to 10 μm, and the particle size D when the cumulative distribution is 10% by volume 10 is the particle size distribution D 50 / D 10 The particles are spherical particles having a particle size distribution of ≦3.

[0026] As described below, the spherical fine particles having heat resistance at 200° C. are spherical fine particles that do not melt when heated for 10 minutes in a dryer set at 200° C. If the spherical fine particles do not have heat resistance at 200° C., the friction melting resistance decreases.

[0027] Moreover, the spherical particles satisfying a specific heat of 0.95 kJ / (kg·K) or more are those measured by DSC (differential scanning calorimetry) based on JIS K 7123: Method for measuring specific heat capacity of plastics, as described below. The specific heat of the spherical particles is 0.95 kJ / (kg·K) or more, and preferably 1.00 kJ / (kg·K) or more. If the specific heat of the spherical particles is less than 0.95 kJ / (kg·K), the resistance to frictional melting decreases. By having a specific heat of 0.95 kJ / (kg·K) or more, the rate at which the temperature of the surface resin layer containing the spherical particles rises due to frictional heat is suppressed.

[0028] Specific examples of spherical fine particles having a heat resistance of 200°C and a specific heat of 0.95 kJ / (kg·K) or more include melamine resin-silica composite particles, benzoguanamine resin particles, polytetrafluoroethylene (PTFE) resin particles, etc. These particles are preferably crosslinked spherical resin fine particles. Note that "spherical" does not necessarily mean that the particles are perfectly spherical, but at least means that the particles are not produced by crushing like flakes. Among these, melamine resin-silica composite particles are particularly preferred because the presence of silica on the particle surface makes the particles less likely to fuse together even at temperatures above 200°C.

[0029] And the particle diameter of spherical particles is D when the cumulative distribution is 50 volume percent. 50 (Median diameter) is 2.5 to 10 μm, and the particle size D when the cumulative distribution is 10% by volume 10 is the particle size distribution D 50 / D 10 The spherical fine particles have a heat resistance of 200°C and a specific heat of 0.95 kJ / (kg K) or more, and by having such a particle size and a sharply controlled particle size distribution, the friction melting resistance is improved.

[0030] Particle size D of spherical particles 50 (Median diameter) is 2.5 to 10 μm. Particle size D 50If the particle size D exceeds 10 μm, the surface of the surface resin layer becomes rough, and the abrasion resistance is likely to decrease, and coarse particles become visible, which is likely to cause a decrease in the appearance quality. In addition, when the surface resin layer is formed by coating, linear irregularities are likely to form on the surface. 50 If the particle size is less than 2.5 μm, the proportion of fine particles that do not contribute much to improving the resistance to frictional melting increases, making it difficult to obtain a sufficient effect.

[0031] In addition, the spherical particles have a particle size distribution D 50 / D 10 The particle size distribution of the spherical particles is controlled to have a sharp particle size distribution that satisfies D≦3. 50 / D 10 If >3, the particle size is D 10 The ratio of fine particles with a particle size of D or less is relatively high. 10 The following fine particles have a low contribution to improving resistance to frictional melting, so in order to obtain high resistance to frictional melting, it is necessary to increase the blending ratio of spherical fine particles, in which case bending resistance is likely to decrease.

[0032] The surface resin layer contains a polymeric elastomer containing a polyether polyurethane.

[0033] The polyether polyurethane can be obtained by reacting urethane raw materials including a high molecular weight polyol including a polyether polyol, an organic polyisocyanate, and a chain extender.

[0034] Specific examples of polyether polyols include polyethylene glycol, polypropylene glycol, polytetramethylene glycol, and poly(methyltetramethylene glycol).

[0035] Specific examples of organic polyisocyanates include 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, 4,4'-diphenylmethane diisocyanate, and xylylene diisocyanate. To et al.Examples of suitable diisocyanates include aromatic diisocyanates such as resistant to yellowing, non-yellowing diisocyanates including hexamethylene diisocyanate, isophorone diisocyanate, norbornene diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, and other aliphatic or alicyclic diisocyanates.

[0036] Specific examples of chain extenders include diamines such as hydrazine, ethylenediamine, propylenediamine, hexamethylenediamine, nonamethylenediamine, xylylenediamine, isophoronediamine, piperazine and its derivatives, adipic acid dihydrazide, and isophthalic acid dihydrazide; triamines such as diethylenetriamine; tetramines such as triethylenetetramine; diols such as ethylene glycol, propylene glycol, 1,4-butanediol, 1,6-hexanediol, 1,4-bis(β-hydroxyethoxy)benzene, and 1,4-cyclohexanediol; triols such as trimethylolpropane; and pentaerythritol. Tetraols amino alcohols such as aminoethyl alcohol and aminopropyl alcohol;

[0037] The proportion of polyether polyurethane contained in the polymeric elastomer contained in the surface resin layer is preferably 60% by mass or more, further 80% by mass or more, and particularly 90 to 100% by mass, in terms of easy maintenance of high flex resistance. Examples of polymeric elastomers other than polyether polyurethane contained in the polymeric elastomer include polyurethanes other than polyether polyurethane such as polyester polyurethane and polycarbonate polyurethane, acrylic elastomers such as acrylonitrile-butadiene copolymers and copolymers of acrylic acid esters or methacrylic acid esters, polyamide elastomers, silicone rubber, and other polymeric elastomers. The proportion of polyether polyurethane contained in the surface resin layer is 60% by mass or more.

[0038] The content of the spherical particles in the surface resin layer is 5 to 40% by mass. If the content of the spherical particles in the surface resin layer is less than 5% by mass, the friction melting resistance is not sufficiently improved. If the content of the spherical particles in the surface resin layer is more than 40% by mass, the bending resistance is likely to decrease.

[0039] The surface resin layer may contain various additives such as antioxidants, ultraviolet absorbers, pigments, dyes, surfactants, antistatic agents, flame retardants, anti-adhesive agents, fillers, crosslinking agents, etc., as necessary, as long as the effects of the present invention are not impaired.

[0040] The thickness of the surface resin layer is 10 to 60 μ m, 1 A thickness of 5 to 45 μm is preferred since it is easy to obtain a leather-like sheet having a surface that combines high resistance to friction and melting, high resistance to bending, and a supple feel similar to natural leather.

[0041] 1, a surface resin layer 4 is laminated to a fiber substrate 1 via an adhesive layer 2 and an intermediate resin layer 3. The leather-like sheet of this embodiment can be produced, for example, by a method in which a surface resin layer is formed on a release paper, an intermediate resin layer is further formed on the surface of the surface resin layer, an adhesive layer is further formed on the surface of the intermediate resin layer, the adhesive layer formed on the release paper is pressure-bonded to the surface of the fiber substrate, and then the release paper is peeled off.

[0042] The intermediate resin layer is a layer mainly made of a polymeric elastomer, and contains various additives such as antioxidants, ultraviolet absorbers, pigments, dyes, surfactants, antistatic agents, flame retardants, anti-tack agents, fillers, crosslinking agents, etc., as necessary. The type of polymeric elastomer forming the intermediate resin layer is not particularly limited, and examples thereof include polyurethane; acrylic elastomers such as acrylonitrile-butadiene copolymers and copolymers of acrylic acid esters or methacrylic acid esters; polyamide elastomers; and various polymeric elastomers such as silicone rubber. Among these, polyurethane is preferred because it provides a good feel, and polyether polyurethane is particularly preferred because it is easy to increase flex resistance.

[0043] The thickness of the intermediate resin layer is not particularly limited, but is preferably 10 to 60 μm, more preferably 15 to 45 μm, since this makes it easier to obtain a leather-like sheet having an excellent balance between mechanical properties and texture.

[0044] The adhesive layer is also a layer mainly made of a polymeric elastomer, and contains various additives such as antioxidants, ultraviolet absorbers, pigments, dyes, surfactants, antistatic agents, flame retardants, anti-tack agents, fillers, and crosslinking agents as necessary. The type of polymeric elastomer forming the adhesive layer is not particularly limited, and any adhesive mainly made of a polymeric elastomer having high adhesive strength with a fiber substrate, including various polymeric elastomers similar to those described above, is used without any particular limitation. As the polymeric elastomer mainly forming the adhesive layer, polyurethane is preferred because it provides a good feel, and in particular polyether polyurethane is preferred because it is easy to increase bending resistance.

[0045] The thickness of the adhesive layer is not particularly limited, but is preferably 20 to 100 μm, more preferably 30 to 90 μm, since this makes it easier to obtain a leather-like sheet having an excellent balance between mechanical properties and texture.

[0046] The leather-like sheet of the present embodiment described above has both high resistance to friction and melting and high resistance to bending. In particular, when a bending test is performed using a flexometer in an environment of 20°C, the number of cycles at which cracks occur in the surface resin layer is 300,000 or less. Above, Furthermore, a leather-like sheet having a durability of 500,000 cycles or more can be obtained. EXAMPLES

[0047] The present invention will now be described in more detail with reference to examples, but the scope of the present invention is not limited to the following examples. First, the evaluation methods used in the examples will be summarized below.

[0048] (1) Heat resistance of spherical particles at 200℃ The powder of the spherical fine particles used in each example was weighed out in an aluminum foil container in an amount of 2-3 g and heated in an electric dryer at 200°C for 10 minutes. If the spherical fine particles remained in powder form after cooling, or if they were lightly stuck together but could be broken up and returned to powder by applying light pressure with a medicine spoon or the like, they were judged as A (with heat resistance at 200°C). If they were melted and formed a film, or if the particles were completely fused together and could not be returned to powder even by applying light pressure, they were judged as B (without heat resistance at 200°C).

[0049] (2) Measurement of particle size and particle size distribution of spherical particles The cumulative particle size distribution of the spherical microparticles used in each example was measured by a dry method using a laser diffraction scattering measuring device LA-950V2 (Horiba, Ltd.). From the measured cumulative particle size distribution, the particle size at 50% by volume of the cumulative distribution was defined as D 50 , the particle size at 10% cumulative distribution is D 10 and the particle size distribution D 50 / D 10 asked for.

[0050] (3) Specific heat of spherical particles The specific heat (kJ / (kg·K)) of the spherical fine particles used in each example was measured using a differential scanning calorimeter DSC8500 (Perkin Elmer) based on JIS K 7123: Specific heat capacity measurement method for plastics.

[0051] (4) Resistance to friction and melting A strip-shaped test piece (3 x 6 cm) was cut out from the leather-like sheet obtained in each Example. Then, a cherry blossom roller (diameter 73 mm, width 26 mm) rotating at 1800 rpm was brought into contact with the surface of the strip-shaped test piece on which the surface resin layer was formed, with a load of 2.0 lb (907 g). Then, the time until the surface resin layer melted and the fiber substrate was exposed was measured at 1 second intervals (rounded off), up to a maximum of 10 seconds.

[0052] (5) Flexibility The leather-like sheets obtained in each example were subjected to a bending resistance test using a flexometer conforming to JIS K6545 under an environment of relative humidity 65±5% and temperature 20±2°C. Specifically, the presence or absence of cracks on the surface of the leather-like sheet on which the surface resin layer was formed was confirmed every 100,000 cycles of bending using a flexometer. The cracks were confirmed visually using a 30x magnifying glass. Then, when cracks were confirmed at 100,000 cycles, it was determined that "less than 100,000 cycles", when cracks were confirmed at 200,000 cycles, it was determined that "100,000 cycles", and similarly, every "100,000 cycles". Note that the number of samples in each cycle was N=3. Then, when cracks occurred in any of the samples, it was determined that cracks occurred.

[0053] [Example 1] Using a water-soluble thermoplastic polyvinyl alcohol as the sea component and PET modified with 6 mol% isophthalic acid as the island component, the number of islands per fiber was 25, and a sea component / island component ratio was 25 / 75 (mass ratio), a melt conjugate spinning die was used, and filaments of islands-in-sea type conjugate fiber were extruded from the die at 260° C. Then, the ejector pressure was adjusted so that the spinning speed was 4000 m / min, and islands-in-sea type conjugate fiber with an average fineness of 2.5 dtex was collected on a net and had a basis weight of 30 g / m 2 Thus, a web of long fibers was obtained.

[0054] The web was then cross-wrapped to pile up 12 layers, which were then sprayed with a needle breakage prevention oil. Then, the web was cut with a 6-barb needle to achieve 2000 punches / cm. 2 An entangled web was obtained by needle punching at a punch density of 0.1 mm.

[0055] The entangled web was then heat-shrunk by steam. Specifically, first, 30% by mass of moisture based on the mass of the sea component was added to the entangled web, and then the web was heat-treated for 80 seconds in a heated steam atmosphere at a relative humidity of 90% and a temperature of 110° C. The area shrinkage rate at this time was 45%.

[0056] Next, the heat-shrunk web was impregnated with a dispersion of an anionic self-emulsifying aqueous polyurethane (100% modulus 3.0 MPa). The concentration of the aqueous polyurethane dispersion was 10 / 90 (weight ratio of aqueous polyurethane / island component). The aqueous polyurethane dispersion was gelled in a water vapor atmosphere to prevent migration, and then dried at 120°C for 10 minutes.

[0057] The web impregnated with the aqueous polyurethane was then immersed in hot water at 95°C for 10 minutes to remove the sea component and form ultrafine fibers. The web was then dried at 120°C for 10 minutes to obtain a 2.1 mm thick fiber substrate containing a nonwoven fabric of 0.1 dtex ultrafine fibers. The 2.1 mm thick fiber substrate was then sliced ​​along a plane approximately parallel to its surface to obtain a 1.0 mm thick fiber substrate containing a nonwoven fabric of 0.1 dtex ultrafine fibers and a basis weight of 525 g / m. 2 Thus, a fiber substrate of 100 g was obtained.

[0058] Then, on the pore-patterned release paper, a coating liquid for forming a surface resin layer was applied in a wet amount of 130 g / m, which was a mixture of 100 parts by mass of polyether polyurethane (PEt-based PU, Resamine ME-8116 manufactured by Dainichi Seika Chemical Industry Co., Ltd., solid content 30 mass%), 8.5 parts by mass of melamine resin-silica composite particles (Optbeads 6500M manufactured by Nissan Chemical Industries, Ltd.), 30 parts by mass of DMF, 10 parts by mass of MEK, and 30 parts by mass of black pigment dispersion (DUT-4794 manufactured by Dainichi Seika Chemical Industry Co., Ltd., pigment content 12 mass%). 2 The mixture was applied using a roll coater at a rate of 1000 ml at 1000 rpm and dried. In this manner, a surface resin layer was formed. The surface resin layer thus formed contained 20% by mass of melamine resin-silica composite particles.

[0059] Next, a coating liquid for forming an intermediate resin layer, which was a mixture of 100 parts by mass of polyether polyurethane (Rezamin ME-8116 manufactured by Dainichi Seika Chemicals Mfg. Co., Ltd., solid content 30% by mass), 30 parts by mass of DMF, 10 parts by mass of methyl ethyl ketone, and 30 parts by mass of black pigment dispersion (DUT-4794 manufactured by Dainichi Seika Chemicals Mfg. Co., Ltd., pigment content 12% by mass), was applied to the surface of the surface resin layer at a wet coating amount of 105 g / m. 2The mixture was applied with a roll coater at a rate of 1000 μg / cm2 and then dried to form an intermediate resin layer.

[0060] Then, a coating liquid for forming an adhesive layer, which was mixed with 100 parts by mass of polyether polyurethane (Rezamin UD-8310NTT manufactured by Dainichi Seika Chemicals Mfg. Co., Ltd., solid content 60% by mass), 10 parts by mass of an isocyanate crosslinking agent (NE crosslinking agent manufactured by Dainichi Seika Chemicals Mfg. Co., Ltd.), 2 parts by mass of a crosslinking accelerator (UD-103 manufactured by Dainichi Seika Chemicals Mfg. Co., Ltd.), 30 parts by mass of DMF, and 20 parts by mass of MEK, was applied to the surface of the intermediate resin layer at a wet coating amount of 150 g / m. 2 After applying the adhesive using a roll coater at 100°C, it was dried at 80°C for 2 minutes, and in the semi-dried state, it was attached to the surface of the fiber substrate and further dried at 130°C for 5 minutes. After that, in order to promote the crosslinking reaction of the adhesive layer, it was heated in a dryer at an atmospheric temperature of 60°C for 48 hours. The release paper was then peeled off to expose the surface resin layer.

[0061] In this way, a leather-like sheet with a thickness of about 1 mm was obtained. The cross section of the obtained leather-like sheet was observed with a scanning electron microscope (300x), and the film thickness was measured at 30 randomly selected points, and the average value was calculated. The thickness of the surface resin layer was 30 μm, the thickness of the intermediate resin layer was 30 μm, and the thickness of the adhesive layer was 60 μm.

[0062] The properties of the resulting leather-like sheet were evaluated by the methods described above. The evaluation results are shown in Table 1.

[0063] [Table 1]

[0064] [Example 2] A leather-like sheet was produced and evaluated in the same manner as in Example 1, except that benzoguanamine resin particles (Eposter M05, manufactured by Nippon Shokubai Co., Ltd.) were used in place of the melamine resin-silica composite particles (Optobeads 6500M, manufactured by Nissan Chemical Industries, Ltd.) in the surface resin layer. The results are shown in Table 1.

[0065] [Example 3] A leather-like sheet was produced and evaluated in the same manner as in Example 1, except that the surface resin layer contained 5% by mass of melamine resin-silica composite particles instead of 20% by mass of melamine resin-silica composite particles in Example 1. The results are shown in Table 1.

[0066] [Example 4] A leather-like sheet was produced and evaluated in the same manner as in Example 1, except that the surface resin layer contained 40% by mass of melamine resin-silica composite particles instead of 20% by mass of melamine resin-silica composite particles in Example 1. The results are shown in Table 1.

[0067] [Example 5] A leather-like sheet was produced and evaluated in the same manner as in Example 1, except that PTFE particles (Polysciences, Microdispers-3000) were blended into the surface resin layer instead of the melamine resin-silica composite particles (Nissan Chemical Industries, Ltd., Optobeads 6500M) in Example 1. The results are shown in Table 1.

[0068] [Example 6] A leather-like sheet was produced and evaluated in the same manner as in Example 1, except that the thickness of the surface resin layer was changed to 60 μm instead of 30 μm in Example 1. The results are shown in Table 1.

[0069] [Example 7] A leather-like sheet was produced and evaluated in the same manner as in Example 1, except that the thickness of the surface resin layer was changed to 80 μm instead of 30 μm in Example 1. The results are shown in Table 1.

[0070] [Comparative Example 1] A leather-like sheet was produced and evaluated in the same manner as in Example 1, except that the melamine resin-silica composite particles (Optobeads 6500M, manufactured by Nissan Chemical Industries, Ltd.) were not blended into the surface resin layer. The results are shown in Table 1.

[0071] [Comparative Example 2] A leather-like sheet was produced and evaluated in the same manner as in Example 1, except that melamine resin particles (PERGOPAK M4, manufactured by Huber Engineered Materials) were blended into the surface resin layer instead of the melamine resin-silica composite particles (Optobeads 6500M, manufactured by Nissan Chemical Industries, Ltd.) in Example 1. The results are shown in Table 1.

[0072] [Comparative Example 3] A leather-like sheet was produced and evaluated in the same manner as in Example 1, except that the surface resin layer contained 3% by mass of melamine resin-silica composite particles instead of 20% by mass of melamine resin-silica composite particles in Example 1. The results are shown in Table 1.

[0073] [Comparative Example 4] A leather-like sheet was produced and evaluated in the same manner as in Example 1, except that the surface resin layer contained 50% by mass of melamine resin-silica composite particles instead of 20% by mass of melamine resin-silica composite particles in Example 1. The results are shown in Table 1.

[0074] [Comparative Example 5] A leather-like sheet was produced and evaluated in the same manner as in Example 1, except that polymethyl methacrylate (PMMA) resin particles (Tuftic AR650SX, manufactured by Nippon Exlan Kogyo Co., Ltd.) were used in place of the melamine resin-silica composite particles (Optbeads 6500M, manufactured by Nissan Chemical Industries, Ltd.) in the surface resin layer. The results are shown in Table 1.

[0075] [Comparative Example 6] A leather-like sheet was produced and evaluated in the same manner as in Example 1, except that aluminum flakes (TS-408PM, Toyo Aluminum Co., Ltd.) were used in place of the melamine resin-silica composite particles (Optobeads 6500M, Nissan Chemical Industries, Ltd.) in the surface resin layer. The results are shown in Table 1.

[0076] [Comparative Example 7] A leather-like sheet was produced and evaluated in the same manner as in Example 1, except that 100 parts by mass of polycarbonate-based polyurethane (PC-based PU, Resamin ME-8210NS manufactured by Dainichiseika Color & Chemicals Mfg. Co., Ltd., solids content 30% by mass) was blended in the surface resin layer instead of 100 parts by mass of polyether-based polyurethane (Resamin ME-8116 manufactured by Dainichiseika Color & Chemicals Mfg. Co., Ltd., solids content 30% by mass). The results are shown in Table 1.

[0077] [Comparative Example 8] In Example 1, instead of 100 parts by mass of polyether polyurethane (Rezamin ME-8116 manufactured by Dainichiseika Chemicals Mfg. Co., Ltd., solid content 30% by mass), 100 parts by mass of polycarbonate polyurethane (Rezamin ME-8210NS manufactured by Dainichiseika Chemicals Mfg. Co., Ltd., solid content 30% by mass) was blended as the polymer elastomer blended in the surface resin layer, and instead of containing 20% ​​by mass of melamine resin-silica composite particles (Optbeads 6500M manufactured by Nissan Chemical Industries, Ltd.), 33% by mass of benzoguanamine resin particles (Eposter MS manufactured by Nippon Shokubai Co., Ltd.) was contained. A leather-like sheet was manufactured and evaluated in the same manner as in Example 1. The results are shown in Table 1.

[0078] [Comparative Example 9] In Example 1, instead of 100 parts by mass of polyether polyurethane (Rezamin ME-8116 manufactured by Dainichiseika Chemicals Co., Ltd., solid content 30% by mass), 100 parts by mass of polycarbonate polyurethane (Rezamin ME-8210NS manufactured by Dainichiseika Chemicals Co., Ltd., solid content 30% by mass) was blended as the polymer elastomer blended in the surface resin layer, and instead of containing 20% ​​by mass of melamine resin-silica composite particles (Optbeads 6500M manufactured by Nissan Chemical Industries, Ltd.), 50% by mass of melamine resin particles (Eposter S12 manufactured by Nippon Shokubai Co., Ltd.) was contained. A leather-like sheet was manufactured and evaluated in the same manner as in Example 1. The results are shown in Table 1.

[0079] [Comparative Example 10] A leather-like sheet was produced and evaluated in the same manner as in Example 1, except that melamine resin-silica composite particles (Optobeads 10500M, manufactured by Nissan Chemical Industries, Ltd.) were blended into the surface resin layer instead of the melamine resin-silica composite particles (Optobeads 6500M, manufactured by Nissan Chemical Industries, Ltd.) in Example 1. The results are shown in Table 1.

[0080] Referring to Table 1, the composition contains polyether polyurethane and spherical particles having a heat resistance of 200°C, the content of the spherical particles is 5 to 40 mass%, the specific heat of the spherical particles is 0.95 kJ / (kg K) or more, and the particle diameter D at a cumulative distribution of 50 volume% is 50 (Median diameter) is 2.5 to 10 μm, and the particle size D when the cumulative distribution is 10% by volume 10 is the particle size distribution D 50 / D 10 The leather-like sheets obtained in Examples 1 to 7, each having a surface resin layer satisfying the condition of ≦3, had a friction melting resistance of 5 seconds or more and a bending resistance of 300,000 times or more. On the other hand, the leather-like sheet of Comparative Example 1, which had a surface resin layer that did not contain spherical fine particles, had a friction melting resistance of less than 1 second. In addition, the particle size distribution D 50 / D 10 The leather-like sheet of Comparative Example 2, which had a surface resin layer containing spherical fine particles not satisfying ≦3, had a friction melting resistance of 2 seconds. The leather-like sheet of Comparative Example 3, which had a surface resin layer containing 3 mass% of spherical fine particles, had a friction melting resistance of 1 second. The leather-like sheet of Comparative Example 4, which had a surface resin layer containing 50 mass% of spherical fine particles, had a flex resistance of less than 100,000 times. The leather-like sheet of Comparative Example 5, which had a surface resin layer containing PMMA particles, which are spherical fine particles that do not have heat resistance at 200°C, had a friction melting resistance of less than 1 second. The leather-like sheet of Comparative Example 6, which had a surface resin layer containing aluminum flakes with a specific heat of less than 0.95 kJ / (kg·K), had a friction melting resistance of less than 1 second. The leather-like sheets of Comparative Examples 7 to 9, which had surface resin layers containing polycarbonate-based polyurethane, all had a flex resistance of less than 100,000 times. 50The leather-like sheet of Comparative Example 10, in which the particle size was more than 10 μm, had a bending resistance of 100,000 times. Furthermore, when the coating was applied using a roll coater, the particles formed streaky irregularities on the surface of the coating. [Explanation of symbols]

[0081] 1. Fiber base material 2 Adhesive layer 3. Intermediate resin layer 4 Surface resin layer 5. Grain-finish resin layer 4a Spherical fine particles 10. Leather-like sheet

Claims

1. The present invention comprises a fiber base material, an intermediate resin layer laminated on one surface of the fiber base material, and a surface resin layer laminated on the intermediate resin layer, The fiber substrate is a fiber substrate having a thickness of 0.3 to 2.0 mm, which is obtained by impregnating a nonwoven fabric, a woven fabric, a knitted fabric, or a sheet combining these fabrics, each containing ultrafine fibers having a fineness of 0.5 dtex or less, with a polymeric elastomer so that the ratio of the ultrafine fibers to the polymeric elastomer is in the range of 50 / 50 to 95 / 5 (mass ratio); the surface resin layer has a thickness of 10 to 60 μm and contains 60% by mass or more of polyether-based polyurethane and 5 to 40% by mass of spherical fine particles having a heat resistance of 200° C.; The spherical fine particles have a specific heat of 0.95 kJ / (kg·K) or more and a particle diameter D at a cumulative distribution of 50% by volume. 50 (Median diameter) is 2.5 to 10 μm, and the particle diameter D when the cumulative distribution is 10% by volume 10 is the particle size distribution D 50 / D 10 ≦3, The leather-like sheet has a bending test performed with a flexometer in an environment of 20° C., and the number of cycles at which cracks appear in the surface resin layer is 300,000 or more.

2. 2. The leather-like sheet according to claim 1, wherein the spherical fine particles comprise at least one kind selected from the group consisting of melamine resin-silica composite particles, benzoguanamine resin particles, and polytetrafluoroethylene resin particles.

Citation Information

Patent Citations

  • Superfine fiber artificial leather

    CN103132344A

  • Fragrant synthetic leather

    JP1990182980A

  • Sublimation-dyeable synthetic leather

    JP1994192967A

  • Leathery sheet and its production

    JP1995150479A

  • Ball skin material and hard baseball

    JP2016067666A