Method of Etherification
By modifying zeolite catalysts with phosphorus to enhance etherification, the method achieves improved yields and rates of monoalkyl ethers, addressing efficiency limitations in existing production methods.
Patent Information
- Application Number
- JP2022516741
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-09-30
- Filing Date
- 2020-09-23
- Publication Date
- 2024-10-10
- Estimated Expiration
- 2040-09-23
AI Technical Summary
Existing methods for producing monoalkyl ethers are limited in yield and production rate, necessitating improved catalysts for enhanced efficiency.
Modifying a zeolite catalyst with phosphorus to create a phosphorus-modified zeolite catalyst, which is then contacted with olefins and alcohols to produce monoalkyl ethers.
The method results in higher yields and production rates of monoalkyl ethers, making it suitable for applications such as surfactant production with reduced production times and costs.
Smart Images

Figure 0007565345000001 
Figure 0007565345000002 
Figure 0007565345000003
Abstract
Description
[Technical field]
[0001] Embodiments of the present disclosure are directed to a process for etherification, and more specifically, embodiments are directed to a process for etherification that includes modifying a zeolite catalyst with phosphorus to provide a phosphorus-modified zeolite catalyst, and contacting the phosphorus-modified zeolite catalyst with an olefin and an alcohol to produce a mono-alkyl ether. [Background technology]
[0002] Monoalkyl ethers are useful in many applications, such as, for example, solvents, surfactants, and chemical intermediates. There is a continuing focus in the industry to develop new and improved materials and / or methods that can be utilized to produce monoalkyl ethers. Summary of the Invention
[0003] The present disclosure provides a method for etherification, the method including modifying a zeolite catalyst with phosphorus to provide a phosphorus-modified zeolite catalyst having a phosphorus to aluminum atomic ratio of 0.05:1 to 1.5:1 and a phosphorus loading of 0.05 to 6 weight percent based on the total weight of the phosphorus-modified zeolite catalyst, and contacting the phosphorus-modified zeolite catalyst with an olefin and an alcohol to produce a mono-alkyl ether.
[0004] The above summary of the present disclosure is not intended to describe each disclosed embodiment or every implementation of the present disclosure. More specifically, the present specification illustrates exemplary embodiments. In several places throughout the application, guidance is provided through lists of examples, which examples can be used in various combinations. In each instance, the recited list serves only as a representative group and should not be interpreted as an exclusive list. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0005] Disclosed herein is a method for etherification, comprising modifying a zeolite catalyst with phosphorus to provide a phosphorus-modified zeolite catalyst, and contacting the phosphorus-modified zeolite catalyst with an olefin and an alcohol to produce a mono-alkyl ether.
[0006] Advantageously, the etherification method disclosed herein can provide improved, i.e., higher, monoalkyl ether yields compared to etherification that does not utilize the phosphorus-modified zeolite catalyst further discussed herein. Improved monoalkyl ether yields may be desirable for many applications, such as providing chemical intermediates. As an example, monoalkyl ethers may be utilized as chemical intermediates in surfactant production by ethoxylation processes, making higher monoalkyl ether yields desirable.
[0007] In addition, the etherification methods disclosed herein can provide improved, i.e., higher, mono-alkyl ether production rates compared to etherification that does not utilize the phosphorus-modified zeolite catalysts discussed further herein. Improved mono-alkyl ether production rates may be desirable in many applications, for example, to provide a desired product at reduced production times and / or associated costs.
[0008] Zeolite catalysts are crystalline metallosilicates, e.g., aluminosilicates, composed of repeating tetrahedral units of, e.g., TO4, where T can be Si, Al, or P (or a combination of tetrahedral units). These units link together to form a framework with regular intracrystalline cavities and / or channels of molecular dimensions, e.g., micropores.
[0009] An embodiment of the present disclosure provides that the zeolite catalyst is a synthetic zeolite catalyst. Synthetic zeolite catalysts can be produced, for example, by known processes of crystallization of silica-alumina gel in the presence of alkali and template. Examples include zeolite beta catalyst (BEA), Linde type A (LTA), Linde type X and Y (Al-rich and Si-rich FAU), silicalite-1, ZSM-5 (MFI), Linde type B (zeolite P), Linde type F (EDI), Linde type L (LTL), Linde type W (MER), and SSZ-32 (MTT), which are described using IUPAC codes according to the nomenclature by the Structure Committee of the International Zeolite Association. The IUPAC codes describing the crystal structures depicted by the Structure Committee of the International Zeolite Association refer to the latest designations as of the priority date of this document, unless otherwise indicated.
[0010] One or more embodiments provide a zeolite catalyst, a zeolite beta (BEA) catalyst. One or more embodiments provide that the zeolite catalyst contains many Bronsted acid sites, i.e., sites that donate protons.
[0011] The zeolite catalyst may have a SiO2 / Al2O3 molar ratio of 5:1 to 1500:1 as measured using neutron activation analysis. All individual values and subranges from 5:1 to 1500:1 are included, for example, the zeolite catalyst may have a SiO2 / Al2O3 molar ratio from a lower limit of 5:1, 10:1, 15:1, or 20:1 to an upper limit of 1500:1, 750:1, 300:1, or 100:1.
[0012] The zeolite catalyst may have an average pore diameter of 5 to 12 angstroms, including all individual values and subranges between 5 and 12 angstroms, for example, the zeolite catalyst may have an average pore diameter from a lower limit of 5 or 7 angstroms to an upper limit of 11 or 12 angstroms.
[0013] Zeolite catalyst is 130~1000m 2 / g.2 All individual values and subranges of / g are included, for example, zeolite catalysts may have lower limits of 130, 150, 175, 300, 400 or 500 m / g. 2 / g~upper limit 1000, 900 or 800m 2 / g. Surface area is measured according to ASTM D4365-19.
[0014] As mentioned above, the zeolite catalyst can be produced by a process utilizing a template, which may also be referred to as an organic template. The template may also be referred to as a templating agent and / or structure directing agent (SDA). For example, a template can be added to a reaction mixture for producing the zeolite catalyst to induce, e.g., direct, the molecular shape and / or pattern of the framework of the zeolite catalyst. Upon completion of the zeolite catalyst production process, the zeolite catalyst comprises a template, e.g., a template located in the micropores of the zeolite catalyst. The template is utilized in the formation of the zeolite catalyst. One or more embodiments provide that the template comprises ammonium ions. The template-containing zeolite catalyst can be produced by known processes. The template-containing zeolite catalyst can be commercially available. Examples of suitable commercially available metallosilicate catalysts include CP814E, CP814C, CP811C-300, CBV712, CBV720, CBV760, CBV2314, CBV10A from ZEOLYST INTERNATIONAL™ of Conshohocken, PA.
[0015] A variety of templates are known that can be utilized to prepare zeolite catalysts. Examples of templates include tetraethylammonium hydroxide, N,N,N-trimethyl-1-adamante-ammonium hydroxide, hexamethyleneimine, and dibenzylmethylammonium, among others.
[0016] An embodiment of the present disclosure provides for modifying a zeolite catalyst with phosphorus to provide a phosphorus-modified zeolite catalyst. The phosphorus modification, e.g., phosphatation, may include impregnation. The impregnation may be referred to as incipient wetness impregnation or wet impregnation. Modifying a zeolite catalyst with phosphorus may utilize known conditions, e.g., known phosphorus impregnation conditions, and may utilize known equipment and known components. For example, the zeolite catalyst may be contacted with an aqueous solution containing a phosphorus compound. Examples of phosphorus compounds include, but are not limited to, phosphoric acid, monoammonium phosphate, diammonium phosphate, sodium phosphate, disodium phosphate, and combinations thereof.
[0017] Modifying the zeolite catalyst with phosphorus can include contacting the zeolite catalyst with a solution containing a phosphorus compound. The solution can include water. Different applications can utilize different amounts of phosphorus compound and / or water.
[0018] The zeolite catalyst can be contacted with the aqueous solution containing the phosphorus compound at a temperature between 5° C. and 90° C. All individual values and subranges between 5° C. and 90° C. are included, for example, the zeolite catalyst can be contacted with the aqueous solution containing the phosphorus compound at a temperature from a lower limit of 5, 10, or 15° C. to an upper limit of 90, 85, or 80° C. Zeolite catalysts for different applications can be contacted with the aqueous solution containing the phosphorus compound for various periods of time.
[0019] The embodiment of the present disclosure provides that the phosphorus modified zeolite catalyst has an atomic ratio of phosphorus to aluminum of 0.05:1 to 1.5:1. All individual values and subranges from 0.05:1 to 1.5:1 are included, for example, the phosphorus modified zeolite catalyst may have an atomic ratio of phosphorus to aluminum with a lower limit of 0.05:1, 0.075:1, 0.10:1 or an upper limit of 1.5:1, 1.3:1, or 1.2:1. The atomic ratio of phosphorus to aluminum is determined by known processes. The atomic ratio of phosphorus to aluminum is calculated based on the components utilized to produce the phosphorus modified zeolite catalyst. For example, the atomic ratio of phosphorus to aluminum of the phosphorus modified zeolite catalyst is calculated using known amounts of phosphorus and aluminum of the zeolite catalyst, for example, based on the structure of the zeolite catalyst, and a known amount of phosphorus utilized to produce the phosphorus modified zeolite catalyst.
[0020] The embodiments of the present disclosure provide that the phosphorus modified zeolite catalyst has a phosphorus loading of 0.05 to 6 weight percent based on the total weight of the phosphorus modified zeolite catalyst, e.g., phosphorus provided via the phosphorus modification discussed herein. All individual values and subranges from 0.05 to 6 weight percent are included, e.g., the phosphorus modified zeolite catalyst may have a phosphorus loading of a lower limit of 0.05, 1.0, or 2.0 weight percent to an upper limit of 6, 5.5, or 4.5 weight percent based on the total weight of the phosphorus modified zeolite catalyst. The phosphorus loading may be determined by known processes. For example, the phosphorus loading, e.g., the nominal phosphorus loading, may be calculated based on the components utilized to produce the phosphorus modified zeolite catalyst.
[0021] One or more embodiments of the present disclosure provide that following modification with phosphorus, the phosphorus-modified zeolite catalyst can be calcined. The phosphorus-modified zeolite catalyst can be calcined at a temperature between 350° C. and 700° C. All individual values and subranges between 350° C. and 700° C. are included, for example, the phosphorus-modified zeolite catalyst can be calcined at a lower limit of 350° C., 400° C., or 450° C. to an upper limit of 700° C., 650° C., or 600° C.
[0022] The phosphorus-modified zeolite catalyst can be calcined in many known calcination environments, for example, the phosphorus-modified zeolite catalyst can be calcined in an air environment.
[0023] The phosphorus modified zeolite catalyst can be calcined, i.e., exposed to a temperature of 350° C. to 700° C. in a calcination environment for 1 hour to 24 hours. All individual values and subranges from 1 hour to 24 hours are included, for example, the phosphorus modified zeolite catalyst can be calcined from a lower limit of 1 hour, 3 hours, or 6 hours to an upper limit of 24 hours, 18 hours, or 12 hours.
[0024] One or more embodiments provide that the methods disclosed herein include reducing, e.g., removing, the template of the zeolite catalyst prior to the phosphorus modification discussed herein. An embodiment of the present disclosure provides that the template of the zeolite catalyst can be reduced by calcination.
[0025] To reduce the template, the zeolite catalyst can be calcined at a temperature between 525° C. and 750° C. All individual values and subranges between 525° C. and 750° C. are included, for example, the zeolite catalyst can be calcined at a lower limit of 525° C., 550° C., or 575° C. to an upper limit of 750° C., 700° C., or 650° C. to reduce the template.
[0026] To reduce the template, the zeolite catalyst can be calcined in a number of known calcination environments, for example, the zeolite catalyst can be calcined in an air environment.
[0027] To reduce the template, the zeolite catalyst can be calcined, i.e., exposed to a temperature of 525° C. to 750° C. in a calcination environment for 1 hour to 24 hours. All individual values and subranges from 1 hour to 24 hours are included, for example, the zeolite catalyst can be calcined from a lower limit of 1 hour, 3 hours, or 6 hours to an upper limit of 24 hours, 18 hours, or 12 hours.
[0028] The present disclosure relates to a method of etherification, which refers to a chemical process, e.g., a chemical reaction, that produces ethers. The method disclosed herein includes contacting a phosphorus-modified zeolite catalyst with an olefin and an alcohol to produce a mono-alkyl ether.
[0029] As used herein, "olefin" refers to a compound that is a hydrocarbon having one or more carbon-carbon double bonds. Embodiments of the present disclosure provide that the olefin comprises 6 to 30 carbon atoms. All individual values and subranges from 6 to 30 carbon atoms are included, for example, the olefin may comprise a lower limit of 6, 8, or 10 carbon atoms to an upper limit of 30, 20, or 14 carbon atoms.
[0030] The olefin may be an alpha (α) olefin, an internally disubstituted olefin, or a cyclic structure (e.g., C3-C 12 The olefins may include alkenes such as cycloalkene. Alpha olefins contain unsaturated bonds at the alpha position of the olefin. Suitable alpha olefins may be selected from the group consisting of propylene, 1-butene, 1-hexene, 4-methyl-1-pentene, 1-heptene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene, 1-icosene, 1-docosene, and combinations thereof. Internal disubstituted olefins contain unsaturated bonds that are not at the terminal position of the olefin. The internal olefins may be selected from the group consisting of 2-butene, 2-pentene, 2-hexene, 3-hexene, 2-heptene, 3-heptene, 2-octene, 3-octene, 4-octene, 2-nonene, 3-nonene, 4-nonene, 2-decene, 3-decene, 4-decene, 5-decene, and combinations thereof. Other exemplary olefins may include butadiene and styrene.
[0031] Examples of suitable commercially available olefins include NEODENE™ 6-XHP, NEODENE™ 8, NEODENE™ 10, NEODENE™ 12, NEODENE™ 14, NEODENE™ 16, NEODENE™ 1214, NEODENE™ 1416, NEODENE™ 16148 from Shell (The Hague, Netherlands).
[0032] The embodiments of the present disclosure provide that the alcohol may contain a single hydroxyl group, or may contain two hydroxyl groups, i.e., glycol, or may contain three hydroxyl groups. The alcohol may contain 1 or more carbons, or 2 or more, or 3 or more, or 4 or more, or 5 or more, or 6 or more, or 7 or more, or 8 or more, or 9 or more carbons, but at the same time may contain 10 or less carbons, or 9 or less, or 8 or less, or 7 or less, or 6 or less, or 5 or less, or 4 or less, or 3 or less, or 2 or less carbons. The alcohol may be selected from the group consisting of methanol, ethanol, monoethylene glycol, diethylene glycol, propylene glycol, triethylene glycol, polyethylene glycol, monopropylene glycol, dipropylene glycol, tripropylene glycol, polypropylene glycol, 1,3-propanediol, 1,2-butanediol, 2,3-butanediol, 1,4-butanediol, 1,6-hexanediol, 1,4-cyclohexanemethanediol, glycerol, and combinations thereof. One or more embodiments provide that the alcohol is selected from the group consisting of monoethylene glycol, diethylene glycol, glycerol, and combinations thereof. One or more embodiments provide that the alcohol is a (poly)alkylene glycol, such as monoethylene glycol, diethylene glycol, propylene glycol, or triethylene glycol. Examples of (poly)alkylene glycols include monoethylene glycol, diethylene glycol, triethylene glycol, polyethylene glycol, monopropylene glycol, dipropylene glycol, tripropylene glycol, polypropylene glycol, 1,3-propanediol, 1,2-butanediol, 2,3-butanediol, 1,4-butanediol, 1,6-hexanediol, paraxylene glycol, glycerol, and 1,4-cyclohexanemethanediol. One or more embodiments provide that the (poly)alkylene glycol is monoethylene glycol.
[0033] Embodiments of the present disclosure provide for reacting the alcohol and olefin at a molar ratio of the alcohol to the olefin of, for example, 0.05:1 to 20:1, including all individual values and subranges from 0.05:1 to 20:1, for example, the alcohol and olefin can be reacted at a molar ratio of the alcohol to the olefin of from a lower limit of 0.05:1, 0.075:1, or 0.1:1 to an upper limit of 20:1, 18:1, or 15:1.
[0034] As previously mentioned, the method disclosed herein includes contacting a phosphorus-modified zeolite catalyst with an olefin and an alcohol to produce a monoalkyl ether. The olefin and alcohol can be contacted with the phosphorus-modified zeolite catalyst under known etherification conditions and can utilize known reactor equipment and known reaction components. For example, the olefin and alcohol can be contacted with the phosphorus-modified zeolite catalyst in a slurry reactor, a fixed bed reactor, or a fluidized bed reactor. The reactor can be operated in a batch mode or a continuous mode.
[0035] The phosphorus modified zeolite catalyst can be utilized in an amount, for example, such that the phosphorus modified zeolite catalyst is 1 wt. % to 50 wt. % based on the total weight of the olefins. All individual values and subranges between 1 wt. % and 50 wt. % are included, for example, (the phosphorus modified zeolite catalyst can be from a lower limit of 1 wt. %, 3 wt. %, or 5 wt. % to an upper limit of 50 wt. %, 40 wt. %, or 30 wt. % based on the total weight of the olefins.
[0036] The olefin and alcohol can be contacted with the phosphorus-modified zeolite catalyst at a reaction temperature between 80° C. and 200° C. All individual values and subranges between 80° C. and 200° C. are included, for example, the olefin and alcohol can be contacted with the phosphorus-modified zeolite catalyst at a lower limit of 80° C., 90° C., or 100° C. to an upper limit of 200° C., 175° C., or 150° C.
[0037] The reaction pressure may vary depending on the application, for example, the reaction pressure may be reduced, atmospheric, or elevated.
[0038] By contacting the phosphorus-modified zeolite catalyst with an olefin and an alcohol, a monoalkyl ether is produced. A variety of monoalkyl ethers can be produced for different applications, for example, by varying which olefin is utilized and / or by varying which alcohol is utilized. Advantageously, the etherification method disclosed herein can provide improved, i.e., higher, monoalkyl ether yields compared to etherification that does not utilize the phosphorus-modified zeolite catalyst described herein.
[0039] In addition, the etherification methods disclosed herein can provide improved, i.e., higher, mono-alkyl ether production rates compared to etherification that does not utilize the phosphorus-modified zeolite catalysts described herein. EXAMPLES
[0040] In the present examples, various terms and names for materials are used, including, for example:
[0041] Zeolite beta catalyst (CP814E, CAS number 1318-02-1, SiO2 / Al2O3 molar ratio of 25:1, average pore size 6.7 Å, surface area 680 m 2 / g, all organic templates removed by commercial supplier prior to receipt, obtained from Zeolyst International);
[0042] Zeolite beta catalyst (CP806EL, CAS number 1318-02-1, SiO2 / Al2O3 molar ratio of 25:1, average pore size in Angstroms, surface area of 177 m 2 / g, containing the resulting organic template, obtained from Zeolyst International).
[0043] Example 1 was carried out as follows: Zeolite beta catalyst (CP806EL) was calcined in an air environment at 550° C. for 12 hours to remove the template from the zeolite beta catalyst. The calcined template-removed zeolite beta catalyst was then modified with phosphorus as follows: Zeolite beta catalyst (50 grams) and an aqueous phosphoric acid solution (2.2 grams phosphoric acid, 120 grams deionized water) were added to a container at room temperature for approximately 10 minutes with constant stirring to obtain a phosphorus-modified zeolite catalyst. The phosphorus-modified zeolite catalyst was dried in a box oven at 80° C. for 1 hour and then calcined in an air environment at 550° C. for 8 hours. The phosphorus-modified zeolite catalyst was calculated to have a nominal phosphorus content of 1.4 weight percent based on the total weight of the phosphorus-modified zeolite catalyst, and a phosphorus / aluminum atomic ratio of 0.38:1.
[0044] Etherification was carried out as follows: phosphorus modified zeolite catalyst (0.75 grams) was added to a vial reactor (40 mL) equipped with a rare earth magnetic stir bar (part number: VP 772FN-13-13-150, V&P Scientific, Inc.), 1-dodecene (6.2 grams) and monoethylene glycol (6.7 grams) were added to the vial reactor, and the contents of the vial reactor were heated to 135° C. and stirred for 3 hours for etherification. The contents of the vial reactor were then analyzed by gas chromatography. Gas chromatography samples were prepared by adding the contents of the vial reactor (100 μL) to 10 mL of an internal standard solution (1 mL of hexadecane dissolved in 1 L of ethyl acetate) and then analyzed offline using an Agilent GC (7890). For analysis, dioxane, 1-dodecene (1-C 12 ) and its isomers (C 12 ), 2-dodecanol, diethylene glycol, monoalkyl ethers and their isomers, and dialkyl ethers and their isomers were included for product quantification to provide weight percentages of species of interest.
[0045] The rate of monoalkyl ether production (grams / hour / gram of zeolite Beta catalyst) was determined as follows: [C 12 Net change in conversion x 1-C 12 g loading × ME selectivity / 168.32 × 230.39 / g catalyst / reaction time in h].
[0046] The dodecene-derived species were the monoether, diether, and 2-dodecanol.
[0047] Total amount of dodecene derived species = moles monoether + 2 × moles diether + 2-dodecanol.
[0048] The total amount of dodecenes, which is 1-dodecene and all non-1-dodecenes, other C 12 Includes isomers.
[0049] Dodecyl monoether (ME) selectivity (%) was calculated by dividing [total amount of ME] by [C 12 The percentage was determined as [total amount of species of origin] × 100%.
[0050] Dodecyl diether (DE) selectivity (%) is calculated as 2 × [total amount of DE / [C 12 The percentage was determined as [total amount of species of origin] × 100%.
[0051] The olefin conversion rate (%) was calculated by [C 12 Total amount of seeds from origin] / [C 12 The total amount of dodecene derived from each species was determined as [total amount of species derived from each species + total amount of dodecene] × 100%.
[0052] The dodecyl monoether (ME) yield (%) was calculated by 12 It was determined as conversion x dodecyl monoether selectivity.
[0053] The results are reported in Table 1.
[0054] Example 2 was carried out identically to Example 1, except that the aqueous phosphoric acid solution contained 4.0 grams of phosphoric acid and 120 grams of deionized water.
[0055] Example 3 was carried out similarly to Example 1, except that the aqueous phosphoric acid solution contained 6.5 grams of phosphoric acid and 120 grams of deionized water.
[0056] Comparative Example A was carried out identically to Example 1, utilizing 23 grams of zeolite beta catalyst in which the template had been removed by calcination, and changing the aqueous phosphoric acid solution to contain 6.8 grams of phosphoric acid and 4.9 grams of deionized water.
[0057] Comparative Example B was carried out in the same manner as Example 1, except that the zeolite beta catalyst was not modified with phosphorus, i.e., no aqueous phosphoric acid solution was utilized. [Table 1]
[0058] The data in Table 1 show that each of Examples 1-3 had improved, ie, higher, monoalkyl ether yields compared to each of Comparative Examples A and B.
[0059] The data in Table 1 show that each of Examples 1-3 had an improved, ie, higher, monoalkyl ether production rate compared to each of Comparative Examples A and B.
[0060] Example 4 was carried out as follows. Zeolite beta catalyst (CP814E) was calcined in an air environment at 550°C for 12 hours to convert the catalyst from NH4 form to H form, and then the catalyst was modified with phosphorus as follows. Zeolite beta catalyst (7 grams) and aqueous phosphoric acid solution (0.3 grams phosphoric acid, 14 grams deionized water) were added to a container and stirred at room temperature for approximately 10 minutes to obtain a phosphorus-modified zeolite catalyst. The phosphorus-modified zeolite catalyst was dried in a box oven at 80°C for 1 hour and then calcined in an air environment at 550°C for 5 hours. The phosphorus-modified zeolite catalyst was calculated to have a nominal phosphorus content of 1.4 weight percent based on the total weight of the phosphorus-modified zeolite catalyst, and a phosphorus / aluminum atomic ratio of 0.38:1. The etherification was carried out as previously discussed, with the contents of the vial reactor heated to 125°C instead of 135°C for etherification, and the etherification was modified to be 3 hours, and the etherification results were determined as previously discussed.
[0061] Example 5 was carried out as in Example 4, except that the aqueous phosphoric acid solution contained 0.58 grams of phosphoric acid and 14 grams of deionized water.
[0062] Comparative Example C was carried out as in Example 4, utilizing 9 grams Zeolite Beta catalyst (H-form) and changing the aqueous phosphoric acid solution to contain 2.35 grams phosphoric acid and 18 grams deionized water.
[0063] Comparative Example D was carried out as in Example 4, except that the zeolite beta catalyst was not modified with phosphorus, i.e., no aqueous phosphoric acid solution was utilized.
[0064] The results are reported in Table 2. [Table 2]
[0065] The data in Table 2 show that Examples 4 and 5 each had improved, ie, higher, monoalkyl ether yields compared to Comparative Examples C and D, respectively.
[0066] The data in Table 2 show that Examples 3 and 4 each had an improved, ie, higher, monoalkyl ether production rate compared to Comparative Examples C and D, respectively.
[0067] Example 6 was carried out as in Example 4 with the following modifications: 5 grams of Zeolite Beta catalyst (H type) was utilized, the aqueous phosphoric acid solution contained 0.07 grams of phosphoric acid and 10 grams of deionized water, the contents of the vial reactor were heated to 150° C. instead of 135° C. for etherification, and the reaction was for 1 hour.
[0068] Example 7 was carried out as in Example 4 with the following modifications: 7.5 grams of Zeolite Beta catalyst (H type) was utilized, the aqueous phosphoric acid solution contained 0.03 grams of phosphoric acid and 15 grams of deionized water, the contents of the vial reactor were heated to 150° C. instead of 135° C. for etherification, and the reaction was for 1 hour.
[0069] Comparative Example E was carried out as in Example 4, with the following modifications: 5 grams of Zeolite Beta catalyst (H type), the aqueous phosphoric acid solution contained 1.0 grams of phosphoric acid and 10 grams of deionized water, the contents of the vial reactor were heated to 150° C. instead of 135° C. for etherification, and the reaction was for 1 hour.
[0070] Comparative Example F was carried out as in Example 4, except that the zeolite beta catalyst was not modified with phosphorus, i.e., no aqueous phosphoric acid solution was utilized, the contents of the vial reactor were heated to 150° C. instead of 135° C. for etherification, and the reaction was for 1 hour.
[0071] The results are reported in Table 3. [Table 3]
[0072] The data in Table 3 show that Examples 6 and 7 each had improved, ie, higher, monoalkyl ether yields compared to Comparative Examples E and F, respectively.
[0073] The data in Table 3 show that Examples 6 and 7 each had an improved, ie, higher, monoalkyl ether production rate compared to Comparative Examples E and F, respectively. (Aspect) (Aspect 1) 1. A process for etherification, said process comprising: modifying a zeolite catalyst with phosphorus to provide a phosphorus-modified zeolite catalyst having an atomic ratio of phosphorus to aluminum of 0.05:1 to 1.5:1 and a phosphorus loading of 0.05 to 6 weight percent, wherein the weight percent is based on a total weight of the phosphorus-modified zeolite catalyst; and contacting the phosphorus modified zeolite catalyst with an olefin and an alcohol to produce a monoalkyl ether. (Aspect 2) 2. The method of embodiment 1, wherein the zeolite catalyst is a zeolite beta catalyst. (Aspect 3) A method according to any one of aspects 1 to 3, comprising reducing the template of the zeolite catalyst before the modification. (Aspect 4) The method of claim 3, wherein reducing the zeolite catalyst comprises calcining the zeolite catalyst. (Aspect 5) The process of any one of aspects 1 to 4, wherein the olefin comprises 6 to 30 carbon atoms. (Aspect 6) The olefin is 12 A method according to any one of aspects 1 to 5, wherein the —C olefin is (Aspect 7) Aspect 7. The method of any one of aspects 1-6, wherein the alcohol is selected from the group consisting of monoethylene glycol, diethylene glycol, glycerol, and combinations thereof.
Claims
1. 1. A process for etherification, said process comprising: modifying a zeolite catalyst with phosphorus to provide a phosphorus-modified zeolite catalyst having an atomic ratio of phosphorus to aluminum of 0.05:1 to 1.5:1 and a phosphorus loading of 0.05 to 6 weight percent, wherein weight percent is based on a total weight of the phosphorus-modified zeolite catalyst; contacting the phosphorus-modified zeolite catalyst with an olefin and an alcohol to produce a monoalkyl ether; The process according to claim 1, wherein said zeolite catalyst is a zeolite beta catalyst and said alcohol is a (poly)alkylene glycol.
2. 2. The method of claim 1, comprising reducing the template of the zeolite catalyst prior to said modification.
3. 3. The method of claim 2, wherein reducing the template of the zeolite catalyst comprises calcining the zeolite catalyst.
4. 4. The process of claim 1, wherein the olefin contains from 6 to 30 carbon atoms.
5. The olefin is 12 -C 14 The method according to any one of claims 1 to 4, wherein the copolymer is an olefin.
6. The method of any one of claims 1 to 5, wherein the alcohol is selected from the group consisting of monoethylene glycol, diethylene glycol, glycerol, and combinations thereof.
Citation Information
Patent Citations
Ringanjushokubai oyobi sonoseizoho
JP1976057688A
Production of (POLY)alkylene glycol mono(higher alkyl) ether
JP1998168016A
Catalyst for manufacturing alkylene glycol monoalkyl ether and its method of use
JP2000300994A
Preparation of glycerol tert-butyl ethers
US20090240086A1
Process for preparing pure methyl tert.-butyl ether
US4219678A