Positive electrode material and electrochemical and electronic devices containing same
A composite cathode material of metal fluorides and fluorinated graphite addresses the limitations of traditional cathode materials in solid-state lithium batteries, enhancing capacity and conductivity, suitable for 3C electronic products and electric vehicles.
Patent Information
- Application Number
- JP2023512754
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-08-27
- Publication Date
- 2024-10-10
- Estimated Expiration
- 2040-08-27
AI Technical Summary
Conventional lithium-ion batteries face challenges with low specific capacity and conductivity issues in solid-state lithium batteries due to the use of traditional lithium-containing cathode materials, and metal fluorides suffer from elution of transition metal ions causing capacity decay.
A composite cathode material is developed by combining metal fluorides with fluorinated graphite, enhancing specific capacity and conductivity through a process involving mixing, annealing, and sieving, which includes a method of preparing a composite material by mixing metal fluoride and fluorinated graphite, followed by annealing and crushing to improve the positive electrode material.
The composite material significantly improves specific capacity, rate performance, and cycle stability of lithium batteries, offering a wide range of raw materials, simple preparation, and low manufacturing costs, suitable for applications in 3C electronic products and electric vehicles.
Smart Images

Figure 00000014_0000 
Figure 00000014_0001
Abstract
Description
Technical Field
[0001] The present invention relates to the field of energy storage, and specifically, to a positive electrode material, an electrochemical device and an electronic device including the same, and particularly to an all-solid-state secondary lithium battery.
Background Art
[0002] With the popularization of consumer electronics products such as notebook computers, mobile phones, tablets, mobile power supplies and drones, the requirements for electrochemical devices in them are becoming increasingly strict. For example, for batteries, not only weight reduction is required, but also high capacity and long operating life are required. Lithium-ion batteries have become the mainstream in the market due to their excellent advantages such as high energy density, high safety, no memory effect, and long operating life.
Summary of the Invention
[0003] Embodiments of the present invention provide a positive electrode material so as to at least somewhat solve at least one problem existing in the related art. In addition, embodiments of the present invention provide a positive electrode, an electrochemical device and an electronic device using this positive electrode material.
[0004]
[0005] In one embodiment, the present invention provides a positive electrode material including a composite material, the composite material including a metal fluoride, when a molar ratio of fluorine element F to metal element M in the metal fluoride is y, and a molar ratio of fluorine element F to metal element M in the composite material is z, y and z satisfy y < z ≦ y + 2, and M includes at least one selected from the group consisting of Al, Cu, Co, Ni, Mn, Fe and Ag. (1) Mixing a metal fluoride and graphite fluoride and drying the mixture, and (2) Annealing at 200°C to 600°C for 10 hours to 72 hours, crushing, and sieving to obtain a composite material, and provides a method for preparing a composite material.
[0006]
[0006] Here, when the molar ratio of fluorine element F to metal element M in the metal fluoride is y, and the molar ratio of fluorine element F to metal element M in the composite material is z, y and z satisfy y < z ≦ y + 2, and the M contains at least one selected from the group consisting of Al, Cu, Co, Ni, Mn, Fe, and Ag.
[0007] In another embodiment, the present invention provides a positive electrode including the positive electrode material described in the embodiments of the present invention.
[0008] In another embodiment, the present invention provides an electrochemical device including the positive electrode described in the embodiments of the present invention.
[0009] In some embodiments, the electrochemical device is an all-solid-state secondary lithium battery. In some embodiments, the all-solid-state secondary lithium battery includes a positive electrode, a negative electrode, and a solid electrolyte. In some embodiments, the positive electrode includes the positive electrode material in the above embodiments.
[0010] In another embodiment, the present invention provides an electronic device including the electrochemical device described in the embodiments of the present invention.
[0011] The positive electrode material in the present invention has advantages such as a wide raw material supply source, a simple preparation process, easy operation, and low manufacturing cost. The lithium battery prepared with the positive electrode material in the present invention has improved specific capacity, rate performance, cycle performance, and charge-discharge performance of the positive electrode material.
[0012] Other aspects and advantages of the embodiments of the present invention will be described, shown, or explained through the implementation of the embodiments of the present invention, in part, in the following description.
Brief Description of the Drawings
[0013] In the following, in order to explain the embodiments of the present invention, the necessary drawings for explaining the embodiments of the present invention or the prior art will be described in a schematic manner. Obviously, the drawings described below are only a part of the embodiments of the present invention. Those skilled in the art can still obtain the drawings of other embodiments from the structures illustrated in these drawings without creative labor. [Figure 1] FIG. 1 shows a schematic diagram of the electrochemical reactions that occur after the first charge / discharge of the composite positive electrode active material of Example 9 of the present invention. [Diagram 2] FIG. 2 shows curves showing the change in capacity retention rate with the number of cycles for the all-solid-state secondary lithium batteries in Comparative Example 2, Comparative Example 4, and Example 4 of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] Examples of the present invention will be described in detail below. The examples of the present invention should not be construed as limiting the present invention.
[0015] It should be noted that amounts, ratios, and other numerical values are presented herein in the form of ranges. As will be appreciated by those of skill in the art, such range forms are intended for convenience and brevity and include not only the numerical values expressly defined in the range, but also each and every value or subrange contained within said range, which is equivalent to expressly defining each value or subrange.
[0016] In specific embodiments and claims, a list of items connected by the terms "one selected from the group consisting of," "one selected from the group consisting of," "a type selected from the group consisting of," or other similar terms means any one of the listed items. For example, if items A and B are listed, the phrase "one selected from the group consisting of A and B" means A only or B only. In another specific example, if items A, B, and C are listed, the phrase "one selected from the group consisting of A, B, and C" means A only, B only, or C only. Item A may include a single element (element) or multiple elements. Item B may include a single element or multiple elements. Item C may include a single element or multiple elements.
[0017] In specific embodiments and claims, a list of items connected by the terms "at least one selected from the group consisting of," "at least one selected from the group consisting of," "at least one selected from the group consisting of," or other similar terms means any combination of the listed items. For example, if items A and B are listed, the phrase "at least one selected from the group consisting of A and B" means A only, B only, or A and B. In another specific example, if items A, B, and C are listed, the phrase "at least one selected from the group consisting of A, B, and C" means A only, B only, C only, A and B (excluding C), A and C (excluding B), B and C (excluding A), or all of A, B, and C. Item A may include a single element or multiple elements. Item B may include a single element or multiple elements. Item C may include a single element or multiple elements.
[0018] 1. Cathode material In some embodiments, the present invention provides a cathode material comprising a composite material, wherein the composite material contains a metal fluoride. When the molar ratio of fluorine element F to metal element M in the metal fluoride is y, and the molar ratio of fluorine element F to metal element M in the composite material is z, y and z satisfy y < z ≤ y + 2, and M contains at least one selected from the group consisting of Al, Cu, Co, Ni, Mn, Fe, and Ag.
[0019] In some embodiments, M contains Cu, Fe, or a combination thereof.
[0020] In some embodiments, y < z ≤ y + 1.5. In some embodiments, y < z ≤ y + 0.05, y < z ≤ y + 0.1, y < z ≤ y + 0.15, y < z ≤ y + 0.2, y < z ≤ y + 0.5, y < z ≤ y + 0.7, y < z ≤ y + 0.9, y < z ≤ y + 1, or y < z ≤ y + 1.2.
[0021] In some embodiments, the composite material further contains graphite fluoride with a structural formula of CF x and when the molar ratio of fluorine element F to carbon element C in the CF x is x, x satisfies 0 < x ≤ 1.
[0022] In some embodiments, 0 < x ≤ 0.9. In some embodiments, 0 < x ≤ 0.8. In some embodiments, 0 < x ≤ 0.7. In some embodiments, 0 < x ≤ 0.6. In some embodiments, 0 < x ≤ 0.5, 0 < x ≤ 0.4, 0 < x ≤ 0.3, or 0 < x ≤ 0.2.
[0023] In some embodiments, when the mass ratio of the graphite fluoride to the metal fluoride is w, w satisfies 0 < w ≤ 0.2. In some embodiments, 0 < w ≤ 0.15. In some embodiments, 0 < w ≤ 0.1. In some embodiments, 0 < w ≤ 0.05. In some embodiments, w may be 0.02, 0.03, 0.06, 0.07, etc.
[0024] In some embodiments, the metal fluoride includes at least one selected from the group consisting of CoF3, NiF3, MnF2, MnF3, FeF3, FeF2, AlF3, and CuF2. In some embodiments, the metal fluoride includes FeF3, CuF2, or a combination thereof.
[0025] In some embodiments, the positive electrode material contains lithium. In some embodiments, the positive electrode material does not contain lithium.
[0026] In some embodiments, the composite material included in the positive electrode material is MF y .w(CF x ), where the definitions of M, w, x, and y are as described above.
[0027] II. Preparation method of composite material Embodiments of the present invention include (1) mixing a metal fluoride and graphite fluoride and drying, and (2) annealing at 200°C to 600°C for 10 hours to 72 hours, crushing, and sieving to obtain a composite material. A preparation method of a composite material is provided.
[0028] Here, when the molar ratio of fluorine element F to metal element M in the metal fluoride is y, and the molar ratio of fluorine element F to metal element M in the composite material is z, y and z satisfy y < z ≤ y + 2, and M includes at least one selected from the group consisting of Al, Cu, Co, Ni, Mn, Fe, and Ag.
[0029] In some embodiments, the definitions of the metal fluoride and graphite fluoride are as described above.
[0030] In some embodiments, the mixing is performed by a ball mill, a V-mixer, a three-dimensional mixer, an airflow mixer, or a horizontal mixer, hi some embodiments, the mixing is high energy ball mill mixing.
[0031] In some embodiments, the ball mill is a wet ball mill or a dry ball mill. In some embodiments, the ball mill is a wet ball mill.
[0032] In some embodiments, a ball milling dispersant is used in the ball milling process, hi some embodiments, the ball milling dispersant comprises anhydrous ethanol.
[0033] In some embodiments, in the ball milling step, the volume ratio of the ball milling material to the ball mill balls is 1:3 to 1:20. In some embodiments, the volume ratio of the ball milling material to the ball mill balls is 1:10.
[0034] In some embodiments, the rotation speed in the ball mill step is 300 r / min to 1200 r / min, In some embodiments, the rotation speed in the ball mill step is 800 r / min.
[0035] In some embodiments, the ball milling time is between 4 hours and 24 hours. In some embodiments, the ball milling time is 4 hours, 6 hours, 10 hours, 15 hours, 20 hours, 24 hours, or a range consisting of any two of the preceding values.
[0036] In some embodiments, the drying temperature is between 60° C. and 120° C. In some embodiments, the drying temperature is 60° C., 70° C., 80° C., 100° C., 120° C., or a range consisting of any two of these values.
[0037] In some embodiments, the annealing temperature is between 200° C. and 600° C. In some embodiments, the annealing temperature is 200° C., 250° C., 300° C., 350° C., 400° C., 500° C., 600° C., or a range consisting of any two of the foregoing values.
[0038] In some embodiments, the annealing time is between 10 hours and 72 hours, hi some embodiments, the annealing time is 10 hours, 15 hours, 20 hours, 25 hours, 30 hours, 35 hours, 40 hours, 50 hours, 60 hours, 65 hours, 72 hours, or a range consisting of any two of the preceding values.
[0039] In some embodiments, the annealing process is performed in an atmosphere sintering furnace, which may be a tube atmosphere sintering furnace, a box atmosphere sintering furnace, or other sintering furnaces with similar atmosphere protection capabilities.
[0040] In some embodiments, the atmosphere used in the atmospheric sintering furnace is an inert gas, hi some embodiments, the inert gas is high purity argon gas or high purity nitrogen gas.
[0041] In recent years, with the advent of the era of electric vehicles and 5G, the demand for lithium batteries with high energy density and high safety performance is also getting stronger. Lithium metal has a high specific capacity (3860mAh / g) and a low electrochemical potential (-3.040V against the standard hydrogen electrode), and is considered to be the most ideal high-energy density anode material. Therefore, solid-state lithium batteries with lithium metal as the anode are the focus of current research. Conventional lithium-ion batteries often adopt organic liquid electrolytes or gel electrolytes, and the organic liquids, which are flammable and explosive, pose a major safety hazard to the battery system.
[0042] The working principle of solid-state lithium batteries is basically the same as that of conventional lithium-ion batteries, and the structural change is to replace the conventional liquid organic electrolyte and separator with a solid electrolyte, which makes the battery safer. In addition, the structure of solid-state lithium batteries is simpler and mainly consists of a positive electrode, a solid electrolyte and a negative electrode. At present, the positive electrodes used in solid-state lithium batteries are often conventional lithium-containing positive electrode materials, such as LiCoO2, LiFePO4, etc. The specific capacity of these lithium-containing positive electrode materials is much lower than that of the negative electrode, and cannot meet the requirements of high energy density all-solid-state lithium batteries. Therefore, solid-state lithium batteries using lithium metal as the negative electrode need to be combined with a positive electrode material with a higher energy density. The energy density that can be provided by metal fluoride (e.g., FeF3, FeF2, and CuF2, etc.) positive electrode materials can reach 1000Wh / Kg to 1600Wh / Kg, which is much higher than the 600Wh / Kg to 800Wh / Kg of LiCoO2-based materials, and therefore has high applicability. In addition, lithium-free positive electrode materials such as metal fluorides often use inexpensive iron element, and therefore have the advantages of being abundant in resources, low cost, and environmentally friendly.
[0043] Currently, lithium-free positive electrode materials such as metal fluorides have the following significant drawbacks: (1) The electrical conductivity of metal fluorides is generally low. It has been reported that the electrical conductivity of FeF3 is 10 -17 S / cm, which is close to an insulator, and the discharge voltage is lower than the charge voltage during the charge and discharge process, that is, the so-called voltage hysteresis phenomenon occurs, and the rate performance and cycle stability of the material are poor; (2) transition metal ions are easily eluted from the positive electrode material during the charge and discharge process and enter the electrolyte to cause side reactions, accelerating the decay of capacity during the cycle process.
[0044] In order to solve the above problems, the present invention provides a lithium battery positive electrode material. The initial state of the positive electrode material is a composite material of metal fluoride and graphite fluoride. The composite material of metal fluoride and graphite fluoride in the present invention has the following advantages as a positive electrode material compared with metal fluoride positive electrode materials: (1) The specific capacity of the positive electrode material can be significantly improved by adding graphite fluoride. (2) As shown in FIG. 1, during the first discharge process, the graphite fluoride on the surface of the positive electrode material undergoes a chemical reaction with the lithium ions released from the negative electrode, and generates nanocarbon in situ, thereby increasing the conductivity of the positive electrode, which is favorable for stabilizing the discharge voltage and improving the discharge efficiency. (3) As shown in FIG. 1, after the first discharge reaction is completed, in addition to generating nanocarbon in situ, the graphite fluoride also generates LiF, and these products can be used as lithium sources to compensate for the loss of lithium during multiple cycles of the positive electrode material, thereby improving the long-term cycle stability performance.
[0045] In addition, the present invention has the following advantageous effects. 1) The composite positive electrode material of metal fluoride and graphite fluoride in the present invention has higher specific capacity and improved rate and cycle performance. 2) The lithium battery positive electrode material provided by the present invention has a wide source of raw materials, a simple preparation process, easy operation, and low production cost. 3) The all-solid-state secondary lithium battery prepared with the positive electrode material of the present invention has good charge and discharge performance and is expected to be applied in the fields of 3C electronic products and electric vehicle batteries.
[0046] 3. Electrochemical equipment Embodiments of the present invention provide electrochemical devices, which include any device that undergoes an electrochemical reaction.
[0047] In some embodiments, an electrochemical device of the present invention includes a negative electrode having a negative electrode active material capable of absorbing and releasing metal ions, a positive electrode according to any embodiment of the present invention, an electrolyte, and a separator disposed between the positive electrode and the negative electrode.
[0048] In some embodiments, the electrochemical device of the present invention includes, but is not limited to, a secondary battery.
[0049] In some embodiments, the electrochemical device is a lithium secondary battery.
[0050] In some embodiments, the lithium secondary battery includes, but is not limited to, a lithium metal secondary battery, a lithium ion secondary battery, a lithium polymer secondary battery or a lithium ion polymer secondary battery, and an all-solid-state secondary lithium battery.
[0051] 1, negative electrode The materials, configurations and methods of manufacture of the negative electrodes used in the electrochemical devices of the present invention may include any of those disclosed in the prior art. In some embodiments, the negative electrodes are those described in U.S. Patent Application No. US9812739B, the entire contents of which are incorporated herein by reference.
[0052] In some embodiments, the negative electrode includes a current collector and a layer of negative electrode active material disposed on the current collector. In some embodiments, the layer of negative electrode active material includes a negative electrode active material. In some embodiments, the negative electrode active material includes lithium metal, structured lithium metal, natural graphite, synthetic graphite, mesocarbon microbeads (MCMB), hard carbon, soft carbon, silicon, silicon-carbon composites, silicon-oxygen materials, Li-Sn alloys, Li-Sn-O alloys, Sn, SnO, SnO2, lithiated TiO2-Li4Ti5O in a spinel structure, or the like. 12 , Li-Al alloys, or any combination thereof.
[0053] In some embodiments, the negative electrode active material layer includes a binder, which may include, but is not limited to, polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene oxide-containing polymers, polyvinylpyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene butadiene rubber, acrylated styrene butadiene rubber, epoxy resin, or nylon.
[0054] In some embodiments, the negative electrode active material layer includes a conductive material, which may include, but is not limited to, natural graphite, artificial graphite, carbon black, acetylene black, ketjen black, carbon fiber, metal powder, metal fiber, copper, nickel, aluminum, silver, or a polyphenylene derivative.
[0055] In some embodiments, the current collector includes, but is not limited to, copper foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, or a polymer substrate coated with a conductive metal.
[0056] In some embodiments, the negative electrode can be obtained by mixing an active material, a conductive material, and a binder in a solvent to prepare an active material composition, and coating the active material composition on a current collector.
[0057] In some examples, the solvent may include, but is not limited to, deionized water, N-methylpyrrolidone.
[0058] In some embodiments, the negative electrode of the all-solid-state secondary lithium battery is a metallic lithium foil.
[0059] 2, positive electrode
[0023] In some embodiments, the positive electrode in an all-solid-state secondary lithium battery comprises a positive electrode material as described in any of the embodiments of the present invention and a conductive agent.
[0060] In some embodiments, the positive electrode comprises a current collector and a positive electrode active material layer disposed on the current collector, the positive electrode active material layer comprising a positive electrode material described in any embodiment of the present invention.
[0061] In some embodiments, the positive electrode active material layer further includes a binder and / or a conductive agent. The binder improves the bonding between the positive electrode active material particles and also improves the bonding between the positive electrode active material and the current collector.
[0062] In some embodiments, the binder comprises at least one selected from the group consisting of polyvinyl alcohol, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene oxide-containing polymers, polyvinylpyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene butadiene rubber, acrylated styrene butadiene rubber, epoxy resin, nylon, and the like.
[0063] In some embodiments, the conductive agent comprises at least one selected from the group consisting of conductive carbon black, carbon fiber, acetylene black, ketjen black, graphene, and carbon nanotubes.
[0064] In some embodiments, the current collector may include, but is not limited to, aluminum.
[0065] The positive electrode can be prepared by a preparation method known in the art. For example, the positive electrode can be obtained by mixing an active material, a conductive material, and a binder in a solvent to prepare an active material composition, and then coating the active material composition on a current collector. In some embodiments, the solvent can include, but is not limited to, N-methylpyrrolidone.
[0066] 3, Electrolyte The electrolyte used in the embodiments of the present invention may be any electrolyte known in the art.
[0067] In some embodiments, the electrolyte solution includes an organic solvent, a lithium salt, and an additive. The organic solvent included in the electrolyte solution of the present invention may be any organic solvent known in the prior art to be used as a solvent for electrolyte solutions. The electrolyte used in the electrolyte solution of the present invention is not limited and may be any electrolyte known in the prior art. The additive included in the electrolyte solution of the present invention may be any additive known in the prior art to be used as an additive for electrolyte solutions.
[0068] In some embodiments, the organic solvent includes, but is not limited to, ethylene carbonate (EC), propylene carbonate (PC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), propylene carbonate, or ethyl propionate.
[0069] In some embodiments, the lithium salt comprises at least one selected from the group consisting of organic lithium salts and inorganic lithium salts.
[0070] In some embodiments, the lithium salt includes, but is not limited to, lithium hexafluorophosphate (LiPF), lithium tetrafluoroborate (LiBF), lithium difluorophosphate (LiPOF), lithium bis(trifluoromethanesulfonyl)imide LiN(CFSO) (LiTFSI), lithium bis(fluorosulfonyl)imide Li(N(SOF)) (LiFSI), lithium bisoxalatoborate LiB(C0) (LiBOB), or lithium difluorooxalatoborate LiBF(C0) (LiDFOB).
[0071] In some embodiments, the concentration of the lithium salt in the electrolyte is 0.5 mol / L to 3 mol / L, 0.5 mol / L to 2 mol / L, or 0.8 mol / L to 1.5 mol / L.
[0072] In some embodiments, the solid electrolyte used in the all-solid-state secondary lithium battery is Li3YCl6, Li3YBr6, Li3OCl, LiPON, Li 0.5 La 0.5 TiO3, Li 1+x Al x Ti 2-x (PO4)3, Li7La3Zr2O 12 , Li 10 GeP2S 12 (LGPS), Li 9.54 S 1.74 P 1.44 S 11.7 Cl 0.3 , Li 3.25 Ge 0.25 P 0.75 S4, Li 11 AlP2S 12 , and Li7P3S 11 The compound includes at least one selected from the group consisting of:
[0073] 4. Separator In some embodiments, a separator is provided between the positive and negative electrodes to prevent short circuit. The material and shape of the separator in the present invention are not particularly limited and may be any technology disclosed in the prior art. In some embodiments, the separator includes a polymer or inorganic material made of a material stable against the electrolyte in the present invention.
[0074] For example, the separator may include a substrate layer and a surface treatment layer. The substrate layer is a nonwoven fabric, film, or composite film having a porous structure, and the material of the substrate layer is at least one selected from the group consisting of polyethylene, polypropylene, polyethylene terephthalate, and polyimide. Specifically, a polypropylene porous film, a polyethylene porous film, a polypropylene nonwoven fabric, a polyethylene nonwoven fabric, or a polypropylene-polyethylene-polypropylene porous composite film can be adopted.
[0075] A surface treatment layer is provided on at least one surface of the base material layer, and the surface treatment layer may be a polymer layer or an inorganic layer, or may be a layer formed by mixing a polymer and an inorganic material.
[0076] The inorganic layer includes inorganic particles and a binder, and the inorganic particles are one or more selected from the group consisting of aluminum oxide, silicon oxide, magnesium oxide, titanium oxide, hafnium dioxide, tin oxide, cerium dioxide, nickel oxide, zinc oxide, calcium oxide, zirconium oxide, yttrium oxide, silicon carbide, boehmite, aluminum hydroxide, magnesium hydroxide, calcium hydroxide, and barium sulfate. The binder is one or more selected from the group consisting of polyvinylidene fluoride, vinylidene fluoride-hexafluoropropylene copolymer, polyamide, polyacrylonitrile, polyacrylic acid ester, polyacrylic acid, polyacrylic acid salt, polyvinylpyrrolidone, polyvinyl ether, polymethyl methacrylate, polytetrafluoroethylene, and polyhexafluoropropylene.
[0077] The polymer layer includes a polymer, and the polymer material is at least one selected from the group consisting of polyamide, polyacrylonitrile, acrylic ester polymer, polyacrylic acid, polyacrylate, polyvinylpyrrolidone, polyvinyl ether, polyvinylidene fluoride, and poly(vinylidene fluoride-hexafluoropropylene).
[0078] 4.Electronic equipment The electronic device of the present invention may be any device that uses the electrochemical device described in the embodiments of the present invention.
[0079] In some embodiments, the electronic device includes, but is not limited to, a notebook computer, a pen-based computer, a mobile computer, an e-book player, a mobile phone, a mobile facsimile, a mobile copier, a mobile printer, a stereo headset, a video recorder, an LCD television, a portable cleaner, a portable CD player, a mini optical disk, a walkie-talkie, an electronic notepad, a calculator, a memory card, a mobile recorder, a radio, a backup power supply, a motor, an automobile, a motorcycle, an electrically assisted bicycle, a bicycle, a lighting device, a toy, a game machine, a clock, an electric tool, a flash lamp, a camera, a large household battery, or a lithium ion capacitor.
[0080] Hereinafter, the preparation of lithium battery is described with reference to specific examples, taking lithium battery as an example. Those skilled in the art should understand that the preparation method described in the present invention is merely exemplary, and any other suitable preparation method is also within the scope of the present invention.
[0081] [Example] As described below, performance evaluation was carried out on examples and comparative examples of the all-solid-state secondary lithium battery of the present invention.
[0082] 1.Measurement method 1. Powder X-ray diffraction (XRD) measurement XRD measurements were performed on the positive electrode active material powders prepared in the comparative examples and examples. The reference standard for the measurement was JIS K 0131-1996 X-ray diffraction analysis general rules. Measurement operating conditions: CuKα radiation (λ=1.5418Å), operating current 250mA, continuous scanning, operating voltage 40kV, scanning range 2θ10-70°, step size 0.1°, scanning speed 0.2 seconds / step.
[0083] The principle of XRD measurement was as follows. When monochromatic X-rays are incident on a crystal, the crystal is composed of a unit cell in which atoms are regularly arranged, so the distance between these regularly arranged atoms is on the same order of magnitude as the wavelength of the incident X-rays. Therefore, X-rays scattered by different atoms interfere with each other, and strong X-ray diffraction occurs in some special directions. The phases present in the material are determined by comparing the lattice spacing and diffraction intensity measured for the material with the diffraction data of standard phases.
[0084] 2. Scanning electron microscope (SEM) measurement The positive electrode active material powders prepared in the comparative examples and examples were subjected to SEM measurement. The reference standard for SEM measurement is JY / T010-1996 General Rules for Analytical Scanning Electron Microscope Methods. The measurement principle of the scanning electron microscope is as follows. The basis for the manufacture of a scanning electron microscope is the interaction between electrons and materials, and a high-energy electron beam that becomes very thin by focusing is used to scan a sample and excite various physical information. Through reception, magnification and display imaging of this information, the structural morphology of the surface of the measurement sample is obtained.
[0085] 3, Charge / discharge measurement The equipment used to measure the capacity per gram of the all-solid-state secondary lithium batteries prepared in the comparative examples and examples was a LAND measuring device (model CT2001A). The measurement environment temperature was room temperature (25°C). The measurement method was constant current discharge to the discharge cut-off voltage according to the set rate, and then constant current charging to the charge cut-off voltage at a certain rate. In the present invention, other than as specified, the charge and discharge measurement rates were all 0.1C, the theoretical specific capacity of FeF3 as reference was 712mAh / g, and the theoretical specific capacity of CuF2 as reference was 893mAh / g.
[0086] 2. Preparation of all-solid-state secondary lithium battery The positive electrode active material prepared in the examples and comparative examples was mixed uniformly with Ketjen Black, a conductive agent. The resulting powder was mixed with Li7P3S, a solid electrolyte. 11The sheet was placed in a stainless steel cold press mold together with the cathode and cold press molded at a pressure of 300 MPa to obtain a two-layer sheet of the cathode and solid electrolyte. 11 and the mass ratio of the conductive agent Ketjen black was 60:30:10. A lithium metal foil sheet was placed on the other side of the solid electrolyte in the bilayer sheet, and placed in a cold press mold together, and a pressure of 200 MPa was further applied to ensure complete contact between the lithium metal and the solid electrolyte film, to obtain an all-solid-state secondary lithium battery.
[0087] 3. Preparation of positive electrode active material Comparative Example 1 10g of FeF3 was weighed and added to a 50ml agate ball mill jar, then 40 φ5mm agate balls and 5 φ10mm agate balls were added and ball milled for 12 hours at a rotation speed of 500r / min. After ball milling, the material adhered to the wall of the ball mill jar and ball milling was insufficient.
[0088] Comparative Example 2 10g of FeF3 was weighed and added to a 50ml agate ball mill jar, then 40 φ5mm agate balls and 5 φ10mm agate balls were added, 20ml of anhydrous ethanol was added, and the ball mill was run at a rotation speed of 800r / min for 12 hours. The resulting material was removed, transferred to a vacuum oven, and dried at 80℃. The dried material was sieved through a 400 mesh sieve to obtain the positive electrode active material FeF3.
[0089] Comparative Example 3 10g of CuF2 was weighed and added to a 50ml agate ball mill jar, then 40 φ5mm agate balls and 5 φ10mm agate balls were added, 20ml of anhydrous ethanol was added, and ball milled at a rotation speed of 500r / min for 12 hours. After the ball milling was completed, the obtained material was uniformly dispersed in the ethanol, and there was no wall adhesion or deposition phenomenon. The obtained material was taken out and transferred to a vacuum oven and dried at 80℃, and the dried material was sieved through a 400 mesh sieve to obtain CuF2, which is a positive electrode active material.
[0090] Comparative Example 4 10g of FeF3 and 0.5g of conductive carbon powder were weighed and added to a 50ml agate ball mill jar, then 40 φ5mm agate balls and 5 φ10mm agate balls were added, 20ml of anhydrous ethanol was added, and ball milled at a rotation speed of 500r / min for 12 hours. After the ball milling was completed, the materials were removed and transferred to a vacuum oven and dried at 80℃, and the dried materials were sieved through a 400 mesh sieve to obtain carbon-coated FeF3 as a positive electrode active material.
[0091] Example 1 Weigh out 10g of FeF3 and add it to a 50ml agate ball mill jar, then add 40 φ5mm agate balls and 5 φ10mm agate balls, add 20ml of anhydrous ethanol, and ball mill at a rotation speed of 500r / min for 12 hours. After the ball milling was completed, the materials were uniformly dispersed in the ethanol, and there was no phenomenon of wall adhesion or precipitation.
[0092] Examples 2 to 13 Metal fluoride MF y and CF, which is graphite fluoride. x The mixture was added to a 50 ml agate ball mill jar, 40 φ5 mm agate balls and 5 φ10 mm agate balls were added, 20 ml of anhydrous ethanol was added, and the mixture was ball milled at a rotation speed of 500 r / min for 12 hours. After the ball milling was completed, the material was removed, transferred to a vacuum oven, dried at 80°C, and sieved through a 300 or 400 mesh sieve to obtain a uniform mixture of graphite fluoride and metal fluoride. The obtained mixture material was transferred to a tubular furnace, and heated to 300-500°C at a heating rate of 3°C / min under the protection of a high-purity argon gas flow of 0.3 L / min, and annealed by maintaining the temperature for 24 hours. After the annealing was completed, the material was cooled to room temperature together with the tubular furnace, and then the material was crushed and sieved to obtain MF, a composite material of metal fluoride and graphite fluoride, as the positive electrode active material in the present invention. y .w(CF x) was obtained. Here, y is the molar ratio of fluorine element F to metal element M in the metal fluoride, z is the molar ratio of fluorine element F to metal element M in the composite material, x is the molar ratio of fluorine element F to carbon element C in the CFx, and w is the mass ratio of the fluorinated graphite to the metal fluoride. In addition, in Example 7, annealing treatment was not performed after drying. Table 1 shows the types and amounts of raw materials used in Examples 2 to 13, and process parameters.
[0093] [Table 1] Here, "-" indicates that the step was not performed.
[0094] Table 2 shows the measurement results of relevant performance of some examples and comparative examples.
[0095] [Table 2]
[0096] Table 3 shows the measurement results at different charge / discharge rates for some examples and comparative examples.
[0097] [Table 3] Here, "x" indicates that the battery had no charge / discharge capacity after 20 charge / discharge cycles.
[0098] As can be seen from the measurement results of Comparative Example 1 and Example 1, when no dispersant was added during ball milling, the material showed serious adhesion to the wall of the jar, and the milling was insufficient. On the other hand, when anhydrous ethanol was added as a dispersant to perform wet milling, the large particles cracked during the ball milling process due to the milling and impact action of the ball milling media, and the dispersant ethanol entered the gaps of the cracks formed and prevented them from closing, which is effective in rapidly expanding the cracks and greatly improving the efficiency of the ball mill.
[0099] As can be seen from the measurement results of Comparative Example 2, Comparative Example 4, and Examples 2 to 6, the charge / discharge capacity per gram of FeF3 can be significantly improved by incorporating CFx into FeF3, and the effect of improving the charge / discharge capacity per gram satisfies the relationship of fluoride graphite composite treatment>conductive carbon coating treatment>untreated. From the above results, it can be seen that the incorporation of F element is one of the factors that improve the performance of FeF3 material.
[0100] As can be seen from the measurement results of Comparative Example 2 and Examples 7 to 10, the annealing temperature has a significant effect on the capacity per gram of the composite positive electrode active material of graphite fluoride and iron trifluoride. Without annealing, the initial discharge capacity and the initial charge capacity of the material were 377.5mAh / g and 232.9mAh / g, respectively. As the annealing temperature increased from 150°C to 350°C, the initial discharge capacity and the initial charge capacity of the material were both significantly improved, to 554.8mAh / g and 458.7mAh / g, respectively. This is because the CFx and FeF3 crystal lattices are more likely to undergo a diffusion reaction as the temperature increases.
[0101] As can be seen from the measurement results of Comparative Example 3 and Examples 11 to 13, the electrochemical performance of the copper fluoride material can be improved by composite treatment of copper fluoride and graphite fluoride. In addition, the charge / discharge capacity of the composite positive electrode material is further related to x, which is the molar ratio of fluorine to carbon in the graphite fluoride material. The higher the molar ratio of fluorine to carbon, the more favorable it is for improving the capacity per gram of discharge of the material.
[0102] As can be seen from the measurement results of Comparative Example 3 and Example 13, after the incorporation of CFx into copper fluoride, the rate performance and cycle performance of the all-solid-state secondary lithium battery prepared with the positive electrode active material of the present invention are significantly improved. Under similar conditions, the charge and discharge at a high rate of 0.5C in Example 13 significantly reduced the decrease in discharge capacity and charge capacity compared to the charge and discharge at 0.05C. This indicates that the incorporation of graphite fluoride significantly improves the charge and discharge rate performance of the material. After 20 stable charge and discharge cycles, the solid-state lithium battery prepared with the positive electrode material of the present invention was charged and discharged at different rates, and the capacity retention rates were all 85% or more. In contrast, in the comparative example, the capacity was greatly attenuated, and the charge and discharge capacity was almost gone after 20 cycles, especially at high rates of 0.2C and 0.5C. In the embodiment, after the metal fluoride material and the graphite fluoride material are combined, during the first discharge, the graphite fluoride on the surface of the positive electrode material undergoes a conversion reaction with lithium to generate nanocarbon in situ, which is favorable for increasing the conductivity of the positive electrode and improving the conversion reaction kinetics. During the first discharge, the graphite fluoride not only generates nanocarbon in situ, but also generates lithium fluoride, which can be used as a lithium source to compensate for the lithium loss during multiple cycles of the positive electrode material, thereby improving the long-term cycle stability of the material.
[0103] 2 shows curves showing the change in capacity retention rate with the number of cycles for the all-solid-state secondary lithium batteries in Comparative Example 2, Comparative Example 4, and Example 4 of the present invention. As can be seen from FIG. 2, by incorporating CFx into FeF3, the capacity retention rate of the all-solid-state secondary lithium battery can be significantly improved.
[0104] Throughout the specification, references to "some embodiments," "partial embodiments," "one embodiment," "another embodiment," "an example," "embodiment," or "partial embodiment" mean that at least one embodiment or example of the invention includes the particular feature, structure, material, or characteristic described in that embodiment or example. Thus, the appearances of, for example, "in some embodiments," "in an embodiment," "in one embodiment," "in another example," "in one example," "in a particular example," or "giving an example" in various places throughout the specification do not necessarily refer to the same embodiment or example of the invention. Furthermore, particular features, structures, materials, or characteristics herein may be combined in any suitable manner in one or more embodiments or examples.
[0105] Although illustrative embodiments have been disclosed and described, those skilled in the art should understand that the above-described embodiments cannot be construed as limiting the present invention, and that changes, substitutions, and alterations to the embodiments are possible without departing from the technical spirit, principle, and scope of the present invention.
Claims
1. A cathode material comprising a composite material, the composite material comprises a metal fluoride; When a molar ratio of the fluorine element F to the metal element M in the metal fluoride is y and a molar ratio of the fluorine element F to the metal element M in the composite material is z, y and z satisfy y<z≦y+2; The M includes at least one selected from the group consisting of Al, Cu, Co, Ni, Mn, Fe, and Ag, The composite material further includes graphite fluoride having a structural formula of CF x , in which a molar ratio of elemental fluorine F to elemental carbon C in the CF x is x, where x satisfies 0<x≦1; A positive electrode material, wherein when a mass ratio of the graphite fluoride to the metal fluoride is w, w satisfies 0<w≦0.
2.
2. The metal fluoride is CoF 3 , NiF 3 , MnF 2 , MnF 3 , FeF 3 , FeF 2 , AlF 3 and CuF 2 The positive electrode material according to claim 1 , comprising at least one selected from the group consisting of:
3. (1) mixing a metal fluoride and graphite fluoride and drying the mixture; and (2) Annealing at 200°C to 600°C for 10 hours to 72 hours, crushing and sieving to obtain a composite material, When a molar ratio of the fluorine element F to the metal element M in the metal fluoride is y and a molar ratio of the fluorine element F to the metal element M in the composite material is z, y and z satisfy y<z≦y+2; The method for preparing a composite material for a positive electrode material, wherein M contains at least one selected from the group consisting of Al, Cu, Co, Ni, Mn, Fe, and Ag.
4. A positive electrode comprising the positive electrode material of claim 1 or 2.
5. An electrochemical device comprising the positive electrode of claim 4.
6. 6. The electrochemical device of claim 5 which is an all-solid-state secondary lithium battery.
7. An electronic device comprising an electrochemical device according to claim 5 or 6.
Citation Information
Patent Citations
Lithium battery
JP1991089462A
A rechargeable battery with solid electrolyte
JP1992502533A
Fluoride positive electrode manufacturing method
JP2008243646A
Nonaqueous electrolyte secondary battery
JP2013073792A