Ion-permeable membrane and method for producing same

The ion permeable membrane, composed of ion conductor particles and a fiber base material with a water-soluble polymer compound, addresses brittleness issues in conventional membranes, ensuring high-speed, efficient lithium recovery with minimal mechanical failure and crossover.

JP7565521B2Active Publication Date: 2024-10-11PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2021073998
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-04-26
Publication Date
2024-10-11
Estimated Expiration
2041-04-26

AI Technical Summary

Technical Problem

Conventional permselective membranes for lithium recovery are brittle and lack sufficient mechanical strength when processing large amounts of solution at high speed, leading to cracking and inefficiencies in ion permeation.

Method used

An ion permeable membrane comprising ion conductor particles embedded within a fiber base material, reinforced with a water-soluble polymer compound, which forms a connected ion conduction path and enhances mechanical strength and ion permeability.

Benefits of technology

The membrane exhibits sufficient mechanical strength and ion permeability, enabling high-speed processing of large volumes without cracking or ion loss, with improved ion recovery rates and reduced crossover phenomena.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007565521000001
    Figure 0007565521000001
  • Figure 0007565521000002
    Figure 0007565521000002
  • Figure 0007565521000003
    Figure 0007565521000003
Patent Text Reader

Abstract

To provide an ion-permeable membrane showing sufficient mechanical strength and ion permeability and a manufacturing method thereof.SOLUTION: An ion-permeable membrane comprises an ionic conductor particle, a fiber substrate, and a fiber containing a water-soluble polymer compound. The ionic conductor particle has a part embedded inside the fiber substrate and a part exposed from the fiber substrate. In a thickness direction of the ion-permeable membrane, the exposed part links one surface of the ion-permeable membrane to a surface opposite the one surface. The water-soluble polymer compound has waterproofness.SELECTED DRAWING: Figure 1B
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an ion-permeable membrane and a method for producing the same. [Background technology]

[0002] Rare metals are essential for many high-tech devices such as mobile phones, smartphones, home appliances, and automobile parts, but because it is difficult to secure a stable supply of rare metals, attention is being focused on rare metal recovery technology. In addition, technology that reuses wastewater that was previously disposed of industrially without disposing of it by adding a treatment process is also gaining importance. Ion exchange resins and / or adsorbents are the mainstream of rare metal recovery technology and wastewater reuse technology, but in recent years, the use of separation technology using various functional membranes as an environmentally friendly recovery and reuse process for building a recycling-oriented society is being considered effective.

[0003] In recent years, the industrial importance of lithium (Li) as a raw material for lithium-ion batteries has been increasing. In particular, Li-ion batteries have come to be adopted for electric vehicles (EVs), and large amounts of Li are being required as a raw material. Li can be extracted from ores or salt lakes in dry regions with high water evaporation rates, but it is also known that seawater contains a very large amount of Li, and the total amount of Li contained in all seawater on Earth is known to be far greater than the total amount of Li buried on land. As with other rare metals, there are also studies underway to recover Li from Li-ion batteries that have been discarded from industrial waste in order to ensure a stable supply of resources.

[0004] However, seawater contains only about 0.2 mg of Li per liter. In addition, industrially discarded Li-ion batteries also contain a large amount of compounds such as nickel (Ni) and cobalt (Co) in addition to Li. Therefore, Li is a metal material that is difficult to efficiently recover from seawater and Li-ion batteries.

[0005] In light of this background, Patent Document 1 attempts to efficiently recover only Li from a source solution containing Li ions by using a selectively permeable membrane that selectively allows Li to pass through. Patent Document 1 discloses a selectively permeable membrane that selectively allows Li ions to pass through, which is a sintered body of an inorganic compound that contains Li, and which is formed by bonding and integrating sintered bodies each having a size of about 5 cm square in the in-plane direction to form a substantially large-area selectively permeable membrane. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] WO2015 / 020121 Summary of the Invention [Problem to be solved by the invention]

[0007] However, in the conventional technology disclosed in Patent Document 1, the sintered body is very fragile, and when a large amount of raw liquid is treated at high speed, it is cracked under high pressure. It was also found that the mechanical strength is insufficient and the ion permeability is also insufficient.

[0008] The present invention is intended to solve the above problems, and has an object to provide an ion-permeable membrane that exhibits sufficient mechanical strength and ion-permeability, and a method for producing the same. [Means for solving the problem]

[0009] A first aspect of the present invention is an ion-permeable membrane comprising ion conductor particles, a fiber substrate, and a filler containing a water-soluble polymer compound, the ion conductor particles have a portion embedded in the fiber substrate and a portion exposed from the fiber substrate, the exposed portion is connected from one surface of the ion-permeable membrane to a surface opposite to the one surface in a thickness direction of the ion-permeable membrane, The water-soluble polymer compound is a water-resistant, ion-permeable membrane.

[0010] A second aspect of the present invention is the ion-permeable membrane according to the first aspect, wherein the ion conductor particles are an inorganic compound containing lithium (Li).

[0011] A third aspect of the present invention is the ion-permeable membrane according to the first or second aspect, wherein the fiber substrate is hydrophobic.

[0012] A fourth aspect of the present invention is a fiber substrate comprising a fluoropolymer, The ion-permeable membrane according to any one of Aspects 1 to 3, wherein the fluoropolymer contains, as a monomer unit, at least one selected from the group consisting of a vinylidene fluoride unit, a tetrafluoroethylene unit, and a chlorotrifluoroethylene unit.

[0013] A fifth aspect of the present invention is Co-spinning the ion conductor particles and a fiber substrate material to obtain a spun membrane; immersing the spun membrane in a solution of a water-soluble polymer compound and drying it; The method for producing the ion-permeable membrane according to any one of aspects 1 to 4, further comprising subjecting the water-soluble polymer compound to a water-resistant treatment. Effect of the Invention

[0014] According to the embodiments of the present invention, it is possible to provide an ion-permeable membrane exhibiting sufficient mechanical strength and ion-permeability, and a method for producing the same. [Brief description of the drawings]

[0015] [Figure 1A] FIG. 1A is a schematic diagram of an ion-permeable membrane according to an embodiment of the present invention. [Figure 1B] FIG. 1B is an enlarged view of a portion A1 enclosed by a dashed line in FIG. 1A. [Figure 1C] FIG. 1C is a cross-sectional view taken along line IC-IC shown in FIG. 1B. [Figure 1D] FIG. 1D is an enlarged view of a portion B1 enclosed by a dashed line in FIG. 1A. [Figure 2A] FIG. 2A is a schematic diagram of a spun membrane 5 in the process of producing an ion-permeable membrane 1 according to an embodiment of the present invention. [Figure 2B] FIG. 2B is an enlarged view of a portion A5 enclosed by a dashed line in FIG. 2A. [Figure 2C] FIG. 2C is an enlarged view of a portion B5 enclosed by a dashed line in FIG. 2A. [Figure 3A] FIG. 3A is a schematic enlarged view of one fiber in the ion permeable membrane 1 according to an embodiment of the present invention, in which the average fiber diameter of the fiber substrate 3 is 0.8 times the average particle diameter of the ion conductor particles 2. [Figure 3B] FIG. 3B is a cross-sectional view of the fiber shown in FIG. 3A taken along line IIIB-IIIB. [Figure 3C] FIG. 3C is a schematic enlarged view of one fiber in the ion permeable membrane 1 according to an embodiment of the present invention, in which the average fiber diameter of the fiber substrate 3 is larger than the average particle diameter of the ion conductor particles 2. [Figure 3D] FIG. 3D is a cross-sectional view of the fiber shown in FIG. 3C taken along line IIID-IIID. [Figure 3E] FIG. 3E is a schematic enlarged view of one fiber in the ion permeable membrane 1 according to an embodiment of the present invention, in which the average fiber diameter of the fiber substrate 3 is 0.2 times or less the average particle diameter of the ion conductor particles 2. [Figure 3F] FIG. 3F is a cross-sectional view of the fiber shown in FIG. 3E taken along line IIIF-IIIF. [Figure 4A] FIG. 4A is a schematic diagram showing a method for evaluating the ion permeability function. [Figure 4B] FIG. 4B is a schematic diagram showing a method for evaluating the ion permeability function. [Diagram 5] FIG. 5 is a table summarizing the results of the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] Hereinafter, an ion-permeable membrane according to an embodiment of the present invention will be described with reference to the drawings. In the following description, the same components are denoted by the same reference numerals, and the description will be omitted as appropriate. In addition, in this specification, the terms "average fiber diameter" and "average particle diameter" each refer to a median diameter.

[0017] FIG. 1A shows a schematic diagram of an ion-permeable membrane 1 according to an embodiment of the present invention, FIG. 1B shows an enlarged view of the A1 portion surrounded by a dashed line in FIG. 1A, FIG. 1C shows a cross-sectional view taken along line IC-IC shown in FIG. 1B, and FIG. 1D shows an enlarged view of the B1 portion surrounded by a dashed line in FIG. 1A.

[0018] As shown in FIG. 1B, the ion-permeable membrane 1 includes ion-conductor particles 2, a fiber substrate 3 (shown in a dot pattern), and a filler 4 (shown in a mesh pattern) containing a water-soluble polymer compound. Compared to the conventional technology, which is a sintered body of ion-conductor particles, the ion-permeable membrane 1 includes not only the ion-conductor particles 2 but also the fiber substrate 3 and the filler 4, and thus exhibits flexibility, and can process a large amount of raw liquid at high speed without breaking. As shown in FIG. 1C, the ion-conductor particles 2 have a portion embedded in the fiber substrate 3 (hereinafter, sometimes referred to as the "embedded portion") 2a (the portion surrounded by the dashed line in FIG. 1C) and a portion exposed from the fiber substrate 3 (hereinafter, sometimes referred to as the "exposed portion") 2b. As shown in FIG. 1C, the fiber substrate 3 has a recessed shape by the amount of the embedded portion 2a at the joint portion with the ion-conductor particles 2. The exposed portion 2b provides the ion permeability of the ion permeable membrane 1, while the embedded portion 2a fixes the ion conductor particles 2 to the fiber substrate 3, thereby preventing the ion conductor particles 2 from falling off even when, for example, a large amount of raw liquid is treated at high speed.

[0019] As shown in FIG. 1D, in the ion permeable membrane 1, exposed portions 2b of a plurality of ion conductor particles 2 are connected to each other from the upper surface 1a to the lower surface 1b of the ion permeable membrane 1 in the thickness direction Z of the ion permeable membrane 1 (hereinafter, the connected portions are referred to as "connecting portions 1c"). The connecting portions 1c become ion conductive paths as shown by the dashed dotted lines in FIG. 1D, and the ion permeable membrane 1 has an ion permeability function. In addition, since the ion permeable membrane 1 includes the fiber base material 3, it is possible to effectively form unevenness on the upper surface 1a and the lower surface 1b of the ion permeable membrane 1, and it is possible to increase the contact area with the object to be treated by the ion permeable membrane (the liquid contact area if the object is a liquid such as seawater), and to promote the movement of ions.

[0020] 1B and 1D, the ion-permeable membrane 1 contains a filler 4 (containing a water-resistant water-soluble polymer compound) in a portion other than the ion conductor particles 2 and the fiber substrate 3. This makes it difficult for the target to be treated (such as seawater) to pass through the ion-permeable membrane as is (hereinafter also referred to as the "crossover phenomenon"). This is thought to be because the water-resistant water-soluble polymer compound efficiently repels the target to be treated, preventing it from passing through the ion-permeable membrane as is. By adopting the above-mentioned configuration, the ion-permeable membrane 1 exhibits sufficient mechanical strength and ion-permeable function.

[0021] 1B and 1D, the plurality of fiber base materials 3 are preferably in contact with one another, and more preferably are fused together at the contact portions, thereby improving the mechanical strength of the ion-permeable membrane 1, particularly the breaking elongation, and effectively suppressing cracking and the like.

[0022] FIG. 2A shows a schematic diagram of a spun membrane 5 in a manufacturing process of an ion-permeable membrane 1 according to an embodiment of the present invention, FIG. 2B shows an enlarged view of a portion A5 surrounded by a dashed line in FIG. 2A, and FIG. 2C shows an enlarged view of a portion B5 surrounded by a dashed line in FIG. 2A.

[0023] 2B and 2C, in the state of the spun membrane 5 described later (state after (a) and before (b) in the manufacturing method of the ion-permeable membrane 1 described later), the membrane does not contain the filler 4 and has a large number of voids 6. In this state, the voids 6 are likely to communicate from the upper surface 5a to the lower surface 5b of the spun membrane 5, and the crossover phenomenon is likely to occur.

[0024] The ion conductor particles 2 are, for example, lithium ion conductors such as lithium nitride (LiN), Li 10 GeP2S 12 , (La x ,Li y )TiO z , where x=2 / 3-a, y=3a-2b, z=3-b, 0<a≦1 / 6、0≦b≦0.06、y> 0), Li-substituted NASICON (Na Super Ionic Conductor) type crystal, Li 1+x+y Al x (Ti,Ge) 2-x S y P 3-y O 12 (where 0≦x≦0.6, 0≦y≦0.6) or other materials containing Li (e.g., inorganic compounds) can be used. -4 ~10 -3 Scm -1 The ion conductor particles 2 are not limited to the above materials as long as they have ion conductivity. -7 Scm -1 In the above cases, it is determined that the material has ionic conductivity.

[0025] The average particle size of the ion conductor particles 2 is preferably 50 nm or more and 500 μm or less in order to realize a configuration in which the ion conductor particles 2 have an embedded portion 2a and an exposed portion 2b.

[0026] The ratio of the ion conductor particles 2 to the total volume of the ion conductor particles 2, the fiber base material 3, and the filler 4 is preferably 30% by volume or more. By keeping it in this range, the ion conductor particles 2 are more likely to contact each other in the ion permeable membrane, and the connection parts 1c are more likely to be formed. It is more preferably 35% by volume or more, and even more preferably 40% by volume or more. The ratio is preferably 90% by volume or less. This allows the fiber base material 3 and the filler 4 to occupy a certain volume or more, making it easier to ensure a sufficient breaking elongation and to ensure the embedded parts 2a of the ion conductor particles, thereby preventing the ion conductor particles from falling off. It is more preferably 85% by volume or less, and even more preferably 80% by volume or less.

[0027] The fiber base material 3 preferably has flexibility, which can improve the breaking elongation of the ion-permeable membrane 1. Note that when the breaking elongation measured by the JIS K7161 test method is 1% or more, the material is considered to have flexibility. It is preferable that the fiber base material 3 is hydrophobic. By having hydrophobicity, it is possible to effectively suppress a phenomenon (hereinafter also referred to as "crossover phenomenon") in which the target of treatment by the ion-permeable membrane 1 (such as seawater) passes through the ion-permeable membrane 1 as is. For example, if the water absorption rate measured by the test method of ASTM D-570 is 0.1% or less, the material is determined to be hydrophobic.

[0028] The fiber base material 3 may contain an organic polymer compound. The fiber base material 3 preferably contains 50% by mass or more of an organic polymer compound. This makes the fiber base material 3 more flexible. More preferably, the fiber base material 3 contains 75% by mass or more of an organic polymer compound, and even more preferably, the fiber base material 3 is made of an organic polymer compound. The fiber base material 3 may contain a hydrophobic polymer compound and / or a water-insoluble polymer compound as the organic polymer compound. The fiber base material 3 preferably contains a fluorine-containing polymer containing, for example, one or more monomer units selected from the group consisting of vinylidene fluoride units, tetrafluoroethylene units, and chlorotrifluoroethylene units, and more preferably, the fiber base material 3 is made of the fluorine-containing polymer.

[0029] FIG. 3A is a schematic diagram of an enlarged fiber in the ion-permeable membrane 1 according to the embodiment of the present invention, in which the average fiber diameter of the fiber substrate 3 is 0.8 times the average particle diameter of the ion conductor particles 2, and FIG. 3B is a cross-sectional view of the fiber shown in FIG. 3A along line IIIB-IIIB. As shown in FIG. 3B, the embedded portion 2a of the ion conductor particles 2 is sufficiently secured, so that the ion conductor particles 2 can be firmly fixed to the fiber substrate 3, and the exposed portion 2b of the ion conductor particles 2 is also secured to be sufficiently large. Therefore, the ion conductor particles 2 can be supported in a state where they are sufficiently exposed to the surface of the fiber substrate 3, so that the ion conductor particles 2 can be prevented from falling off and the movement of ions can be promoted. If the embedded portion 2a of the ion conductor particles 2 is 5% or more by volume, it can be said that the embedded portion 2a is sufficiently secured. If the exposed portion 2b of the ion conductor particles 2 is 50% or more by volume, it can be said that the exposed portion 2b is sufficiently secured.

[0030] FIG. 3C is an enlarged schematic view of a single fiber in the ion permeable membrane 1 according to an embodiment of the present invention when the average fiber diameter of the fiber substrate 3 is larger than the average particle diameter of the ion conductor particles 2, and FIG. 3D is a cross-sectional view taken along line III D-IIID of the fiber shown in FIG. 3C. As shown in FIG. 3D, since the embedding portion 2a of the ion conductor particles 2 is sufficiently ensured, the ion conductor particles 2 can be firmly fixed to the fiber substrate 3, and as a result, the dropout of the ion conductor particles 2 can be suppressed. However, since the exposed portion 2b of the ion conductor particles 2 is small, the ion permeation function cannot promote the movement of ions as compared with the cases of FIGS. 3A and 3B.

[0031] FIG. 3E is an enlarged schematic view of a single fiber of the fiber substrate in the ion permeable membrane 1 according to an embodiment of the present invention when the average fiber diameter of the fiber substrate 3 is 0.2 times or less of the average particle diameter of the ion conductor particles 2, and FIG. 3F is a cross-sectional view taken along line III F-IIIF of the fiber shown in FIG. 3E. As shown in FIG. 3F, since the embedding portion 2a of the ion conductor particles 2 is hardly ensured, the ion conductor particles 2 are more likely to drop out as compared with the cases of FIGS. 3A to 3D.

[0032] From the above, when the average fiber diameter of the fiber substrate 3 is A nanometers (nm) and the average particle diameter of the ion conductor particles 2 is B nanometers (nm), it is preferable to satisfy B×0.2 < A < B. More preferably, it is to satisfy B×0.2 < A < B×0.75, and even more preferably, it is to satisfy B×0.2 < A < B×0.5.

[0033] The average length of the fiber substrate 3 is preferably 100 times or more the average fiber diameter of the fiber substrate. Thereby, the mechanical strength of the ion permeable membrane 1, particularly the elongation at break, can be further improved.

[0034] The ratio of the fiber base material 3 to the total volume of the ion conductor particles 2, the fiber base material 3, and the filler 4 is preferably 5% by volume or more. This makes it easier to ensure a sufficient breaking elongation, makes it easier to ensure the embedded parts 2a of the ion conductor particles, and suppresses the ion conductor particles from falling off. It is more preferably 10% by volume or more, and even more preferably 15% by volume or more. The ratio is preferably 65% ​​by volume or less. By keeping the ratio within this range, the ion conductor particles 2 are more likely to come into contact with each other in the ion permeable membrane, and the connection parts 1c are more likely to be formed. The ratio is more preferably 60% by volume or less, and even more preferably 55% by volume or less.

[0035] The filler 4 includes a water-soluble polymer compound. The filler 4 preferably includes 50% by mass or more of the water-soluble polymer compound. More preferably, the filler 4 includes 75% by mass or more of the water-soluble polymer compound, and even more preferably, the filler 4 is made of a water-soluble polymer compound. The water-soluble polymer compound preferably includes at least one selected from the group consisting of polyvinyl alcohol and derivatives thereof, starch and derivatives thereof, cellulose derivatives such as hydroxymethyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, methyl cellulose, and ethyl cellulose, sodium polyacrylate, polyvinylpyrrolidone, casein, gelatin, and derivatives thereof, but is not limited thereto as long as it is a water-soluble polymer compound.

[0036] The water-soluble polymer compound in the filler 4 has water resistance. Here, having water resistance means that it does not substantially dissolve in water. When the water-soluble polymer compound has water resistance, for example, the insolubilization rate, which is the weight ratio before and after boiling for 30 minutes in water 100 times the weight of the initial weight, may be 70% or more. The water-soluble polymer compound becomes water-resistant by being treated for water resistance. Examples of the water-resistant treatment include a reaction that links water-soluble polymer compounds to each other and changes their physical and chemical properties. For example, a water-resistant treated water-soluble polymer compound can be obtained by adding a crosslinking agent (crosslinking agent) depending on the type of water-soluble polymer compound, or by performing a heat treatment or radiation irradiation treatment. The crosslinking agent preferably includes at least one selected from the group consisting of an isocyanate-based crosslinking agent, an epoxy-based crosslinking agent, an oxazoline-based crosslinking agent, an aziridine-based crosslinking agent, and a metal chelate-based crosslinking agent, but is not limited thereto as long as it is a crosslinking agent that can be made water-resistant.

[0037] The filler 4 preferably has flexibility, which can improve the breaking elongation of the ion-permeable membrane 1.

[0038] The ratio of the filler 4 to the total volume of the ion conductor particles 2, the fiber base material 3 and the filler 4 is preferably 30% by volume or less. By keeping it in this range, the ratio of the ion conductor particles 2 increases, and the ion conductor particles 2 are more likely to contact each other in the ion permeable membrane 1, making it easier to form the connection parts 1c. It is more preferably 25% by volume or less, and even more preferably 20% by volume or less. The ratio is preferably 5% by volume or more. This allows the filler 4 to occupy a certain volume or more, making it easier to ensure a sufficient breaking elongation rate and reducing the crossover rate. The ratio is more preferably 10% by volume or more.

[0039] The thinner the thickness of the ion permeable membrane 1 according to the embodiment of the present invention, the more the ion migration can be promoted, but on the other hand, the durability decreases, and therefore the thickness can be designed to be within an optimal range depending on the use conditions of the ion permeable membrane 1. Furthermore, the ion permeable membrane 1 may contain other members in addition to the ion conductor particles 2, the fiber base material 3, and the filler 4, as long as the object of the present invention is achieved.

[0040] The porosity of the ion permeable membrane according to the embodiment of the present invention is preferably 19.0% or less. By setting the porosity to 19.0% or less, the crossover phenomenon can be effectively suppressed. In addition, it becomes easier to form the connection portion 1c, which is an ion conductive path. The porosity is more preferably 15.0% or less. When the ion permeable membrane 1 is composed of ion conductor particles 2, a fiber base material 3, and a filler 4, the porosity can be calculated by the following formula (1). Porosity (%) = 1-Wa / (Va×(D ip ×r ip +D f ×r f +D wr ×r wr ))×100 (1) Here, Wa is the weight (g) of the ion-permeable membrane 1, and Va is the volume (cm 3 ) and D ip is the density of the ionic conductor particle 2 (g / cm 3 ), and r ip is the volume ratio (%) of the ion conductor particles 2 to the total volume of the ion conductor particles 2, the fiber base material 3, and the filler 4, and D f is the density of the fiber base material 3 (g / cm 3 ), and r f is the volume ratio (%) of the fiber base material 3 to the total volume of the ion conductor particles 2, the fiber base material 3, and the filler 4, and D wr is the density of filler 4 (g / cm 3 ), and r wr is the volume ratio (%) of the filler 4 to the total volume of the ion conductor particles 2, the fiber base material 3 and the filler 4.

[0041] The ion-permeable membrane 1 according to the embodiment of the present invention exhibits sufficient mechanical strength and is capable of high-speed processing of a large amount of raw liquid. Specifically, the membrane exhibits mechanical strength with a particle shedding rate of 0% by weight and a breaking elongation rate of 15% or more, which allows the membrane to withstand high-speed processing of a large amount of raw liquid, and also prevents problems such as the membrane being destroyed by pressure or the loss of ion-permeable function.

[0042] The ion permeable membrane 1 according to the embodiment of the present invention has a sufficient ion permeability. Specifically, for example, in the case of the ion permeable membrane 1 using Li ion conductor particles, the ion recovery rate, ion migration rate, and crossover rate described below can be set to 10.0% or more for Li ions, 0.2 mg / hr or more for Li ions, and less than 0.01% for the crossover rate. The above is an example of an ion-permeable membrane using Li-ion conductor particles, but the same applies to cases where ion-conductor particles other than Li-ion are used. For example, in the case of an ion-permeable membrane using Na-ion conductor particles, the ion recovery rate of Na ions can be 10.0% or more, the ion migration rate of Na ions can be 0.2 mg / hr or more, and the crossover rate can be less than 0.01%.

[0043] The ion permeable membrane 1 according to the embodiment of the present invention may be used alone for ion permeation, or may be incorporated into an ion permeation device such as an electrodialysis device. When the ion permeable membrane 1 is incorporated into an ion permeation device, it is possible to realize an ion permeation device and an ion permeation method that are less likely to be destroyed even when high pressure is applied when treating a large amount of raw liquid at high speed, and that significantly suppresses the ion conductor particles 2 from falling off.

[0044] The ion permeation method may be such that the ion permeable membrane 1 is brought into contact with a solvent such as water, soil, industrial waste, or the like, which contains the desired ions.

[0045] The soil, industrial waste, and the like that are brought into contact with the ion-permeable membrane 1 are preferably wetted with a solvent such as water. When the ion-permeable membrane is brought into contact with a solvent such as water, ion permeation is carried out efficiently. In order to desorb desired ions contained in the solvent such as water, soil, and industrial waste, ultrasonic treatment or bubbling treatment using a micro / nano bubble generator is used in combination as necessary, and ion permeation is carried out more efficiently.

[0046] Next, a method for producing the ion permeable membrane 1 according to an embodiment of the present invention will be described. A method for producing the ion permeable membrane 1 according to an embodiment of the present invention includes the steps of: (a) co-spinning ion conductor particles and a fiber substrate material to obtain a spun membrane; (b) immersing the spun membrane in a solution of a water-soluble polymer compound and drying it; (c) subjecting the water-soluble polymer compound to a water-resistant treatment. The above items (a) to (c) will be explained below.

[0047] (a) Obtaining a spun membrane First, the ion conductor particles 2 and the raw material of the fiber substrate 3 (hereinafter also referred to as "material for the fiber substrate 3", for example, an organic polymer compound) are mixed. At this time, they can be dispersed in a solvent using a kneader, but in the case of a thermoplastic resin, they can also be dry-blended using a powder mixer.

[0048] After mixing as described above, if the material for the fiber substrate 3 is a liquid, the ion conductor particles 2 and the material for the fiber substrate 3 can be spun together by a wet spinning method such as a typical electrospinning method. When spinning by electrospinning, the fiber diameter of the fiber base material 3 can be adjusted by the weight solid content of the material for the fiber base material 3. That is, the fiber diameter of the fiber base material 3 can be made thicker by increasing the weight solid content of the material for the fiber base material 3, and the fiber diameter of the fiber base material 3 can be made thinner by decreasing the weight solid content of the material for the fiber base material 3. Here, in order to sufficiently secure the embedded portions 2a and exposed portions 2b of the ion conductor particles 2, the fiber diameter of the fiber base material 3 may be appropriately adjusted depending on the weight solid content of the material for the fiber base material 3 in relation to the average particle diameter of the ion conductor particles 2. In addition, when the material for the fiber substrate 3 is a dry blend of powders, the ion conductor particles 2 and the material for the fiber substrate 3 can be spun together by a conventional melt spinning method or a spinning method that combines melt spinning and electrospinning. By spinning and depositing, a spun membrane 5 as shown in Figs. 2A to 2C can be obtained.

[0049] (b) Immersing the spun membrane in a solution of a water-soluble polymer compound and drying it. A spun membrane 5 as shown in Figures 2A to 2C is immersed in a solution of a water-soluble polymer compound. The solvent for the solution may be any one or more selected from water, alcohol, and other protic polar solvents. As a method of immersion, for example, the spun membrane 5 obtained as described above can be placed in a liquid tank filled with the solution of the water-soluble polymer compound, thereby immersing it in the solution of the water-soluble polymer material 4. This causes the solution of the water-soluble polymer material to enter and fill the flow path (void 6) inside the spun membrane 5. By using a normal dip coating device, the dipping speed and / or time can be controlled, so that the degree of filling with the solution of the water-soluble polymer compound can also be controlled. Thereafter, the spun membrane 5 can be dried in a normal drying oven. If the drying speed is too fast, warping and / or cracking are likely to occur, so it is preferable to dry as slowly as possible. Regarding the degree of drying, the solvent may be completely removed by evaporation or the like, or a small amount of solvent may remain. For example, it is preferable that the weight change before and after drying is 80% or more of the weight change before and after immersion.

[0050] (c) Water-resistant treatment of water-soluble polymer compounds Water-resistant treatment is performed according to the type of water-soluble polymer compound. For example, in the above (b), a crosslinking agent may be added to the solvent, and after the above (b), a heat treatment or radiation irradiation may be performed to crosslink the water-soluble polymer compound. These may be performed alone or in combination. The heat treatment may be performed simultaneously with the drying in the above (b).

[0051] After the above (c), pressing may be performed using a normal flat plate press or roll press. In this case, the pressing may be performed by applying a temperature to such an extent that the ion conductor particles 2 and the material for the fiber substrate 3 are not melted or altered. For example, the pressing may be performed three or more times at a linear pressure of 0.1 kN / cm or more.

[0052] The connection part 1c can be formed by, for example, increasing the ratio of the ion conductor particles 2, the fiber base material 3, and the filler 4 to the total volume to a certain extent (adjusting it to be 30% by volume or more, for example), and pressing the dried spun film 5 with a normal flat plate press or roll press device, thereby forming the connection part 1c, and the porosity can be reduced (for example, 19.0% or less). Another method of formation is to spin and deposit the fibers while applying pressure during the spinning process (a) above. In the case of the electrospinning method, this pressure can be obtained by applying a voltage opposite to the voltage applied to the nozzle on the collector side, and in other spinning methods, it can be obtained by suctioning and collecting the spun fibers on the collector side.

[0053] The method may further include pressing the spun membrane 5 before the above (b). The pressing before the above (b) can be performed in the same manner as described above. By adding the pressing before the above (b), the porosity of the ion-permeable membrane 1 can be easily adjusted. EXAMPLES

[0054] The following examples are provided to more specifically describe the embodiments of the present invention. The embodiments of the present invention are not limited to the following examples, and may be modified as appropriate within the scope of the above and below-described aims, and all of these are included in the technical scope of the embodiments of the present invention.

[0055] Example 1 An ion-permeable membrane was produced by the following production method. As the ion conductor particles, lithium ion conductive glass ceramic powder (manufactured by Ohara, LICGC powder material) was weighed out so that the weight ratio was 72% (60% by volume ratio) of the total with polyvinylidene fluoride resin (manufactured by 3M, Dyneon Fluoropolymer THV221), and these were dissolved in dimethylacetamide (DMA) using a homomixer so that the weight solid content was 50%, while dispersing the ion conductor particles. The dispersion thus prepared was spun by electrospinning at a constant temperature and humidity of 23°C and 50%, applying a high voltage of 20 kV to a metal needle nozzle with an inner diameter of φ720 μm. The spun membrane was produced. The conditions such as the liquid delivery pressure and spinning distance other than those mentioned above were adjusted so that no droplets were generated and the fibers were completely fibrous. The spun membrane thus produced was pressed once using a roll press device at a linear pressure of 0.18 kN / cm to adjust the void ratio, and then cut into a 80 mm square size.

[0056] A polyvinyl alcohol resin (PVA217, manufactured by Kuraray Co., Ltd.) was used as the water-soluble polymer compound, and a crosslinking agent (Orgatics TC-310, manufactured by Matsumoto Fine Chemical Co., Ltd.) was weighed out so that the weight ratio of the crosslinking agent to the polyvinyl alcohol resin was 30%. These were then dissolved in pure water using a homomixer so that the weight solid content was 5%, to prepare a solution of the water-soluble polymer compound.

[0057] Next, the spun membrane and the solution of the water-soluble polymer compound were placed in a glass petri dish, and the spun membrane was immersed in the solution and held in a vacuum container at -0.09 MPa for 24 hours. The spun membrane was then removed and dried in a box-type drying oven with an internal temperature set to 100°C for 2 hours, and then held in the same box-type drying oven with an internal temperature set to 110°C for 3 hours in order to promote crosslinking.

[0058] Thereafter, the spun membrane was subjected to five press treatments using a roll press machine at a press line pressure of 0.18 kN / cm, and then cut into a 50 mm square to obtain the ion permeable membrane of Example 1.

[0059] Next, the evaluation items will be specifically described.

[0060] (Average particle size of ionic conductor particles) The average particle size of the ion conductor particles (lithium ion conductive glass ceramic powder) dispersed in water was measured. Specifically, a particle size distribution measuring device (Microtrack Bell, MT-3300EXII) was used to measure the 50% particle size (D50) in the volume-based cumulative fraction obtained by particle size distribution measurement using a laser diffraction / scattering method in accordance with JIS Z8825 (2013). As a result, the average particle size of the ion conductor particles in Example 1 was 400 nm.

[0061] (Average fiber diameter and length of fiber substrate) Using an SEM (Phenom G2Pro scanning electron microscope manufactured by PHENOM-World), 10 images of the surface of the spun membrane immediately after the spinning process were taken at a magnification such that several tens of fibers were visible. Ten fibers were randomly selected from each SEM image, and the fiber diameter and fiber length of the portions of the fiber where ion conductor particles were not embedded were measured for a total of 100 fibers selected from the 10 SEM images. The average fiber diameter (median fiber diameter) of the fiber substrate was calculated from the measured fiber diameter, and was 390 nm. The average length of the fiber substrate was also calculated from the measured fiber length, and was more than 100 times the average fiber diameter.

[0062] (Ion-permeable membrane thickness and porosity) The thickness of the ion-permeable membrane cut into a 50 mm square size was measured with a digital micrometer without crushing it so as not to change the density and internal structure, and the weight and density of the raw materials were obtained, and the porosity was calculated from the above formula (1). The volume of the filler in the above formula (1) was calculated using the density of the raw filler material from the weight change between the weight of the spun membrane immediately after cutting into an 80 mm square size and the weight of the spun membrane after holding at 110°C for 3 hours. The measurement results showed that the membrane was 176 μm thick, and the density-volume ratios of the lithium ion conductive glass ceramic powder, fiber substrate material (polyvinylidene fluoride resin), polyvinyl alcohol resin, and crosslinking agent were 3.05 g / cm. 3 49.3% by volume, 1.78g / cm 3 33.1% by volume, 1.25g / cm 3 13.1% by volume and 1.07 g / cm 3 The porosity was 4.6% by volume, and the weight of the ion-permeable membrane was 0.89 g, resulting in a porosity of 12.3%.

[0063] (Elongation at break) The ion-permeable membrane thus produced was cut into a rectangular test piece 10 mm wide and 50 mm long, and the breaking elongation was measured using a tensile tester (AND Corp. RTF-1310). The breaking elongation was found to be 23%.

[0064] (Ion recovery rate, ion migration rate, crossover rate, particle shedding rate) 4A and 4B are schematic diagrams for explaining the evaluation method of the ion permeation function, in which FIG. 4A is a schematic diagram before ion permeation and FIG. 4B is a schematic diagram after ion permeation. The reservoir 7 shown in FIG. 4A was partitioned into the raw liquid side 7a and the recovery side 7b by the 50 mm square ion permeable membrane 1 prepared, and ions 8 were added to the raw liquid side 7a, and only pure water was added to the recovery side 7b. As the ions 8, Li ions, Ni ions, and Co ions were added at a concentration of 100 ppm relative to the pure water. While stirring the raw liquid side 7a with a magnet stirrer, the amount of ions 8 (mg) that had moved to the recovery side 7b was measured every hour for 24 hours using an inductively coupled plasma emission spectrometer (iCAP7400 manufactured by Thermo Fisher Scientific) as shown in FIG. 4B. The ratio (percentage) of the amount of each ion transferred (mg) after 24 hours divided by the initial amount of each ion (mg) in the raw solution was calculated as the recovery rate of each ion (%). The ion transfer rate was calculated by dividing the maximum amount of each ion transferred (mg) measured every hour by the amount of each ion transferred (mg) per hour (mg / hr). The crossover rate was calculated as the ratio (percentage) of the sum of the Ni ion recovery rate and the Co ion recovery rate to the sum of the recovery rates of all ions (Li, Ni, and Co). The Li ion recovery rate was 11.2%, and the Li ion transfer rate was 0.71 mg / hr. On the other hand, the ion recovery rate and ion transfer rate for Ni ions and Co ions were 0.0% and 0.00 mg / hr, respectively, so the crossover rate was 0.00%. In addition, the weight change of the ion permeable membrane was measured before and after this measurement, and the particle shedding rate was calculated as ([weight of ion permeable membrane before measurement (g)] - [weight of ion permeable membrane after measurement (g)]) / [weight of ion permeable membrane before measurement (g)], resulting in a result of 0 weight %. Note that the ion permeable membrane was thoroughly dried after measurement to remove moisture before measuring the weight.

[0065] Comparative Example 1 In Comparative Example 1, a spun membrane was prepared under the same conditions as in Example 1, and the steps after (b) immersing the spun membrane in a solution of a water-soluble polymer compound and drying were omitted. Evaluation was performed in the same manner as in Example 1.

[0066] Comparative Example 2 In Comparative Example 2, an ion-permeable membrane was prepared under the same conditions as in Example 1, but no crosslinking agent was added to the solution of the water-soluble polymer compound, and the holding at 110°C for 3 hours for the purpose of promoting crosslinking was omitted.

[0067] Comparative Example 3 In Comparative Example 3, a lithium ion conductive glass ceramic sintered body (manufactured by OHARA Inc., LICGC sintered body, 50 mm square size) was used as the ion permeable membrane.

[0068] The measurement results for Example 1 and Comparative Examples 1 to 3 are shown in the table of Fig. 5. The mechanical strength (particle shedding rate and breaking elongation rate) and ion permeability (ion recovery rate, ion migration rate, and crossover rate) were judged as follows, with "◯" indicating sufficient performance and "×" indicating poor performance. Regarding the particle shedding rate, 0% by weight was marked as "good" and over 0% by weight was marked as "poor". The breaking elongation rate was rated as "good" if it was 15% or more, and "poor" if it was less than 15%. The ion recovery rate of Li-ions was rated as "good" if it was 10.0% or more, and "bad" if it was less than 10.0%. The ion transfer rate of Li-ions was rated as "good" if it was 0.2mg / hr or more, and "bad" if it was less than 0.2mg / hr. The crossover rate was rated as "good" if it was less than 0.01%, and "bad" if it was 0.01% or more. For the overall evaluation, for the five performance characteristics (i.e., particle shedding rate, breaking elongation rate, Li-ion recovery rate, Li-ion migration rate, and crossover rate), those that were all rated as "Good" were given an A rating, those that received one "B" rating were given, and those that received two or more "B" ratings were given a C rating.

[0069] As shown in Table 1, Example 1 was given an overall rating of A, and exhibited sufficient mechanical strength and ion permeability. Furthermore, since Example 1 exhibited sufficient ion permeability, it can be determined that an ion conduction path was formed in Example 1 (i.e., in the thickness direction of the ion permeable membrane, the exposed portion was connected from one surface of the ion permeable membrane to the surface opposite to said surface).

[0070] On the other hand, Comparative Example 1 was given an overall rating of B, and the crossover rate was poor. This is believed to be because the composition did not contain a filler containing a water-soluble polymer compound.

[0071] On the other hand, Comparative Example 2 was given an overall rating of C, with poor particle shedding rate and crossover rate. This is thought to be because, although it contained a water-soluble polymer compound, it was not subjected to a water-resistant treatment, so the water-soluble polymer compound did not have water resistance, and the water-soluble polymer material dissolved in water, causing destruction of the ion-permeable membrane, and causing particle shedding and crossover phenomena.

[0072] Comparative Example 3 was given an overall rating of C, and was poor in terms of breaking elongation, Li-ion recovery rate, and Li-ion migration rate. It is believed that the poor breaking elongation in Comparative Example 3 was due to the absence of a fiber base material, and further that the liquid contact area of ​​the ion-permeable membrane surface was small, resulting in poor Li-ion recovery rate and Li-ion migration rate.

[0073] From the above evaluation, it was found that an ion-permeable membrane comprising ion conductor particles, a fibrous substrate, and a filler containing a water-soluble polymer compound, wherein the ion conductor particles have a portion embedded inside the fibrous substrate and a portion exposed from the fibrous substrate, the exposed portion being connected in the thickness direction of the ion-permeable membrane from one surface of the ion-permeable membrane to the surface opposite the one surface, and the water-soluble polymer compound is water-resistant, can be provided that exhibits sufficient mechanical strength and ion permeability. [Industrial Applicability]

[0074] The ion-permeable membrane according to the embodiment of the present invention is more flexible and can achieve a large specific surface area than conventional ion-permeable membranes made of a sintered body, and can therefore be used to selectively allow ion permeation and efficiently recover rare metals, particularly lithium, from waste liquids, waste materials, low-concentration stock solutions, and the like. [Explanation of symbols]

[0075] 1. Ion-permeable membrane 1a Top surface of ion-permeable membrane 1b Underside of ion-permeable membrane 1c Ion permeable membrane connection 2. Ion conductor particles 2a Ion conductor particle embedment portion 2b Exposed portion of ion conductor particle 3. Fiber base material 4 Filling material 5. Spun membrane 5a Top surface of the spinning membrane 5b Lower surface of the spinning membrane 6 void 7. Reservoir 7a Stock solution side of storage tank 7b Reservoir recovery side 8. Aeon

Claims

1. An ion-permeable membrane comprising ion conductor particles, a fiber substrate, and a filler containing a water-soluble polymer compound, the ion conductor particles have a portion embedded in the fiber substrate and a portion exposed from the fiber substrate, the exposed portion is connected from one surface of the ion-permeable membrane to a surface opposite to the one surface in a thickness direction of the ion-permeable membrane, The water-soluble polymer compound has water resistance.

2. 2. The ion-permeable membrane according to claim 1, wherein the ion conductor particles are an inorganic compound containing lithium (Li).

3. The ion-permeable membrane according to claim 1 or 2, wherein the fiber substrate is hydrophobic.

4. The fiber substrate contains a fluorine-containing polymer, The ion-permeable membrane according to any one of claims 1 to 3, wherein the fluorine-containing polymer contains, as a monomer unit, at least one selected from the group consisting of a vinylidene fluoride unit, a tetrafluoroethylene unit, and a chlorotrifluoroethylene unit.

5. Co-spinning the ion conductor particles and a fiber substrate material to obtain a spun membrane; immersing the spun membrane in a solution of a water-soluble polymer compound and drying it; The method for producing the ion-permeable membrane according to any one of claims 1 to 4, further comprising subjecting the water-soluble polymer compound to a water-resistant treatment.

Citation Information

Patent Citations

  • Ion permeable membrane

    JP2021049516A

  • Metal ion recovery device and metal ion recovery method

    WO2015020121A1