Electrolytic capacitor and method of manufacturing the same
The electrolytic capacitor design with thermal sprayed layers of varying porosity and outer plating reduces ESR, enhancing performance in high frequency applications by increasing contact area and adhesion.
Patent Information
- Application Number
- JP2021569813
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-01-09
- Filing Date
- 2020-12-21
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2040-12-21
AI Technical Summary
Existing multilayer solid electrolytic capacitors have high equivalent series resistance (ESR) due to the tight bonding of electrodes formed by thermal spraying, which limits the reduction of impedance in the high frequency range.
The electrolytic capacitor design includes a laminate structure with external electrodes composed of thermal sprayed layers of varying porosity, where a first thermal sprayed electrode layer is formed on the resin molded body and a second layer with higher porosity is added, along with outer plating layers to reduce contact resistance and ESR.
The design achieves a significant reduction in ESR by increasing the contact area and adhesion between electrodes, thereby improving the capacitor's performance in high frequency applications.
Smart Images

Figure 0007565949000004 
Figure 0007565949000005 
Figure 0007565949000006
Abstract
Description
[Technical field]
[0001] The present invention relates to an electrolytic capacitor and a method for manufacturing an electrolytic capacitor. [Background technology]
[0002] Electrolytic capacitors such as solid electrolytic capacitors are produced, for example, by forming a dielectric layer on the surface of an anode made of a valve metal, and then forming a cathode opposite the anode.
[0003] For example, Patent Document 1 discloses a stacked solid electrolytic capacitor in which a plurality of solid electrolytic capacitor units each having a dielectric film and a solid electrolyte between a pair of electrodes are stacked, one connection end of each of the pair of electrodes faces one side of the stack and is joined to a single conductor, and the other connection end of each of the pair of electrodes faces the other side of the stack and is joined to a single conductor, and at least one of the conductors joined to each of the one electrodes and the conductors joined to each of the other electrodes is formed by spraying a conductive material. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 4-188814 Summary of the Invention [Problem to be solved by the invention]
[0005] In the stacked solid electrolytic capacitor described in Patent Document 1, the conductor to which the electrodes of the units are joined is formed by thermal spraying, so that the electrodes and the conductor are bonded very firmly, and the contact resistance between the electrodes and the conductor is low, resulting in low impedance in the high frequency range, and the ESR (equivalent series resistance) does not increase even if there are a large number of units and the number of contact points increases. However, it can be said that there is room for further improvement in the stacked solid electrolytic capacitor described in Patent Document 1 in terms of lowering the ESR by devising an improved structure for the conductor formed by thermal spraying.
[0006] The present invention has been made to solve the above problems, and has an object to provide an electrolytic capacitor with low ESR and a method for manufacturing the electrolytic capacitor. [Means for solving the problem]
[0007] The electrolytic capacitor of the present invention comprises a rectangular parallelepiped resin molded body having a laminate having a capacitor element including an anode having a dielectric layer on a surface and a cathode facing the anode, and a sealing resin that seals the periphery of the laminate; a first external electrode provided on a first end face of the resin molded body and electrically connected to the anode exposed from the first end face; and a second external electrode provided on a second end face of the resin molded body and electrically connected to the cathode exposed from the second end face, wherein the first external electrode has, in order from the first end face side of the resin molded body, a first sprayed electrode layer and a second sprayed electrode layer in contact with the first sprayed electrode layer and having a higher porosity than the first sprayed electrode layer.
[0008] The method for manufacturing an electrolytic capacitor of the present invention includes the steps of: preparing a rectangular parallelepiped resin molded body having a laminate having a capacitor element including an anode having a dielectric layer on a surface thereof and a cathode facing the anode; and a sealing resin that seals the periphery of the laminate; forming a first external electrode on a first end face of the resin molded body, the first external electrode being electrically connected to the anode exposed from the first end face; and forming a second external electrode on a second end face of the resin molded body, the second external electrode being electrically connected to the cathode exposed from the second end face. The step of forming the first external electrode is characterized in that, in order from the first end face side, a first sprayed electrode layer and a second sprayed electrode layer that is in contact with the first sprayed electrode layer and has a higher porosity than the first sprayed electrode layer are formed by spraying the first end face of the resin molded body. Effect of the Invention
[0009] According to the present invention, an electrolytic capacitor having a low ESR can be provided, and a method for producing the electrolytic capacitor can be provided. [Brief description of the drawings]
[0010] [Figure 1] 1 is a schematic perspective view showing an electrolytic capacitor according to a first embodiment of the present invention. [Diagram 2] 2 is a schematic cross-sectional view showing a portion corresponding to line segment A1-A2 in FIG. [Diagram 3] 3 is a schematic diagram showing an example of a WT surface of a first sprayed electrode layer in FIG. 2. FIG. [Figure 4] 3 is a schematic diagram showing an example of a WT surface of a second sprayed electrode layer in FIG. 2. FIG. [Diagram 5] 1 is a schematic cross-sectional view showing an electrolytic capacitor according to Modification 1 of Embodiment 1 of the present invention. [Figure 6] FIG. 2 is a cross-sectional view illustrating an electrolytic capacitor according to a second embodiment of the present invention. [Figure 7] FIG. 4 is a cross-sectional view illustrating an electrolytic capacitor according to a third embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The electrolytic capacitor of the present invention and the manufacturing method of the electrolytic capacitor of the present invention will be described below. Note that the present invention is not limited to the following configurations, and may be modified as appropriate within the scope of the present invention. In addition, a combination of multiple individual preferred configurations described below also constitutes the present invention.
[0012] Each of the embodiments described below is merely an example, and it goes without saying that partial substitution or combination of the configurations shown in different embodiments is possible. From embodiment 2 onwards, a description of matters common to embodiment 1 will be omitted, and differences will be mainly described. In particular, similar effects due to similar configurations will not be mentioned one after another for each embodiment. In the following description, when there is no particular distinction between each embodiment, it will simply be referred to as the "electrolytic capacitor of the present invention."
[0013] [Embodiment 1] The electrolytic capacitor of the present invention comprises a rectangular parallelepiped resin molded body having a laminate having a capacitor element including an anode having a dielectric layer on a surface thereof and a cathode facing the anode, and a sealing resin sealing the periphery of the laminate, a first external electrode provided on a first end face of the resin molded body and electrically connected to the anode exposed from the first end face, and a second external electrode provided on a second end face of the resin molded body and electrically connected to the cathode exposed from the second end face, wherein the first external electrode has, in order from the first end face side of the resin molded body, a first sprayed electrode layer and a second sprayed electrode layer in contact with the first sprayed electrode layer and having a higher porosity than the first sprayed electrode layer. In the electrolytic capacitor of the present invention, the second external electrode may have, in order from the second end face side of the resin molded body, a first sprayed electrode layer and a second sprayed electrode layer in contact with the first sprayed electrode layer and having a higher porosity than the first sprayed electrode layer. Furthermore, in the electrolytic capacitor of the present invention, the first external electrode and the second external electrode may each have an outer layer plating layer provided on the surface of the second sprayed electrode layer opposite to the first sprayed electrode layer. Such an example will be described below as the electrolytic capacitor of embodiment 1 of the present invention.
[0014] 1 is a schematic perspective view showing an electrolytic capacitor according to embodiment 1 of the present invention. As shown in FIG. 1, electrolytic capacitor 1 has a resin molded body 9, a first external electrode 11, and a second external electrode 13.
[0015] In this specification, the length direction, width direction, and thickness direction of the electrolytic capacitor (resin molded body, first external electrode, or second external electrode) are defined as the directions indicated by arrow L, arrow W, and arrow T, respectively, as shown in Fig. 1 etc. Here, the length direction L, width direction W, and thickness direction T are perpendicular to each other.
[0016] In this specification, in an electrolytic capacitor (resin molded body, first external electrode, or second external electrode), the surface extending along the length direction L and thickness direction T is referred to as the LT surface, the surface extending along the length direction L and width direction W is referred to as the LW surface, and the surface extending along the width direction W and thickness direction T is referred to as the WT surface.
[0017] The resin molding 9 is rectangular and has a first end face 9a and a second end face 9b (both WT faces) facing each other in the longitudinal direction L, a bottom face 9c and a top face 9d (both LW faces) facing each other in the thickness direction T, and a first side face 9e and a second side face 9f (both LT faces) facing each other in the width direction W.
[0018] The first external electrode 11 is provided on the first end face 9a of the resin molding 9, and extends over parts of the bottom face 9c, the top face 9d, the first side face 9e, and the second side face 9f.
[0019] The second external electrode 13 is provided on the second end face 9b of the resin molding 9, and extends over parts of the bottom face 9c, the top face 9d, the first side face 9e, and the second side face 9f.
[0020] Fig. 2 is a schematic cross-sectional view showing a portion corresponding to line segment A1-A2 in Fig. 1. As shown in Fig. 2, resin molded body 9 has a laminate 30 having a plurality of capacitor elements 20, and sealing resin 8 that seals the periphery of laminate 30. Capacitor elements 20 may be bonded to each other via a conductive adhesive.
[0021] The laminate 30 preferably has a plurality of capacitor elements 20, but may have one capacitor element 20.
[0022] Capacitor element 20 includes an anode 3 having a dielectric layer 5 on its surface, and a cathode 7 facing the anode 3. More specifically, in capacitor element 20, the cathode 7 faces the anode 3 with the dielectric layer 5 interposed therebetween.
[0023] The anode 3 is exposed from a first end surface 9 a of the resin molded body 9 and is electrically connected to a first external electrode 11 .
[0024] The anode 3 has a valve metal substrate 3a at its center and a porous layer (not shown) on its surface, on which a dielectric layer 5 is provided.
[0025] Examples of the valve metal constituting the valve metal base 3a include simple metals such as aluminum, tantalum, niobium, titanium, zirconium, magnesium, silicon, etc., and alloys containing at least one of these metals. Among these, aluminum or an aluminum alloy is preferred.
[0026] The valve metal substrate 3a is preferably in the form of a flat plate, and more preferably in the form of a foil.
[0027] The porous layer is preferably an etched layer that has been etched with hydrochloric acid or the like.
[0028] The thickness of the valve metal base 3a before etching is preferably 60 μm or more, and preferably 180 μm or less. After etching, the thickness of the unetched core of the valve metal base 3a is preferably 10 μm or more, and preferably 70 μm or less. The thickness of the porous layer is designed according to the withstand voltage, electrostatic capacitance, etc. required for the electrolytic capacitor 1, and the total thickness of the porous layers provided on both sides of the valve metal base 3a in the LT plane shown in FIG. 2 is preferably 10 μm or more, and preferably 120 μm or less.
[0029] The dielectric layer 5 is preferably made of an oxide film of the above-mentioned valve metal. For example, when the valve metal substrate 3a is an aluminum foil, the valve metal substrate 3a is anodized in an aqueous solution containing boric acid, phosphoric acid, adipic acid, or a sodium salt or ammonium salt thereof to form an oxide film that becomes the dielectric layer 5. The dielectric layer 5 is formed along the surface of the porous layer, and as a result, the dielectric layer 5 has pores (recesses).
[0030] The thickness of the dielectric layer 5 is designed according to the withstand voltage, capacitance, and the like required for the electrolytic capacitor 1, but is preferably 10 nm or more and 100 nm or less.
[0031] The cathode 7 (here, a cathode extraction layer 7c described later) is exposed from a second end face 9b of the resin molded body 9 and is electrically connected to a second external electrode 13.
[0032] Cathode 7 has a solid electrolyte layer 7a provided on dielectric layer 5, a conductive layer 7b provided on solid electrolyte layer 7a, and a cathode lead layer 7c provided on conductive layer 7b. Since electrolytic capacitor 1 has solid electrolyte layer 7a as a part of cathode 7, it can be said to be a solid electrolytic capacitor.
[0033] The electrolytic capacitor of the present invention may be an electrolytic capacitor having an electrolytic solution instead of a solid electrolyte, or may be an electrolytic capacitor having both a solid electrolyte and an electrolytic solution.
[0034] Examples of materials constituting the solid electrolyte layer 7a include conductive polymers having a skeleton of pyrroles, thiophenes, anilines, etc. Examples of conductive polymers having a skeleton of thiophenes include poly(3,4-ethylenedioxythiophene) (PEDOT), which may be composited with polystyrene sulfonic acid (PSS) as a dopant to form PEDOT:PSS.
[0035] The solid electrolyte layer 7a is formed by, for example, a method of forming a polymer film of poly(3,4-ethylenedioxythiophene) or the like on the surface of the dielectric layer 5 using a treatment liquid containing a monomer such as 3,4-ethylenedioxythiophene, or a method of applying a dispersion liquid of a polymer such as poly(3,4-ethylenedioxythiophene) to the surface of the dielectric layer 5 and then drying it. The solid electrolyte layer 7a is formed in a predetermined region by applying the treatment liquid or dispersion liquid described above to the surface of the dielectric layer 5 by a method such as sponge transfer, screen printing, spray application, dispenser application, inkjet printing, or the like. Note that, as the solid electrolyte layer 7a, it is preferable to form a solid electrolyte layer for an inner layer that fills the pores (recesses) of the dielectric layer 5, and then form a solid electrolyte layer for an outer layer that covers the entire dielectric layer 5.
[0036] The thickness of the solid electrolyte layer 7a is preferably 2 μm or more and preferably 20 μm or less.
[0037] The conductive layer 7b is provided to electrically and mechanically connect the solid electrolyte layer 7a and the cathode lead layer 7c.
[0038] The conductive layer 7b is formed by applying a conductive paste such as a carbon paste, a graphene paste, or a silver paste to the surface of the solid electrolyte layer 7a by a method such as dipping, sponge transfer, screen printing, spray application, dispenser application, or inkjet printing.
[0039] The conductive layer 7b is preferably a carbon layer, a graphene layer, or a silver layer formed as described above. The conductive layer 7b may be a composite layer in which a silver layer is provided on a carbon layer or a graphene layer, or a mixed layer in which a carbon paste or a graphene paste is mixed with a silver paste.
[0040] The thickness of the conductive layer 7b is preferably not less than 2 μm and is preferably not more than 20 μm.
[0041] The cathode lead layer 7c is formed of, for example, a metal foil, a printed electrode layer, a coated electrode layer, or the like.
[0042] When the cathode lead layer 7c is a metal foil, the metal foil is preferably made of at least one metal selected from the group consisting of aluminum, copper, silver, and alloys containing at least one of these metals as a main component. When the metal foil is made of any of the above metals, the resistance of the metal foil is low, and therefore the ESR of the electrolytic capacitor 1 is likely to be low.
[0043] The metal foil may be a metal foil having a surface coated with carbon, titanium, or the like by a film forming method such as sputtering, vapor deposition, etc. Among these, carbon-coated aluminum foil is preferably used.
[0044] The thickness of the metal foil is preferably 20 μm or more and 50 μm or less from the viewpoints of improving the handleability in the manufacturing process, miniaturization, and reducing the ESR.
[0045] When the cathode lead layer 7c is a printed electrode layer, the printed electrode layer is formed in a predetermined region by applying an electrode paste to the surface of the conductive layer 7b by a method such as sponge transfer, screen printing, or inkjet printing.
[0046] When the cathode lead layer 7c is a coated electrode layer, the coated electrode layer is formed in a predetermined region by applying an electrode paste to the surface of the conductive layer 7b by dipping, spray coating, dispenser coating or other method.
[0047] The electrode paste preferably contains silver, copper, or nickel as a main component.
[0048] The printed electrode layer can be thinner than a metal foil. For example, when the printed electrode layer is formed by screen printing, the thickness can be 20 μm or less.
[0049] The cathode extraction layer 7c is preferably provided on the conductive layer 7b while the conductive layer 7b is in a viscous state before drying.
[0050] In the capacitor element 20, an end of the valve metal base 3a located on the second end face 9b side of the resin molded body 9 is sealed with a sealing resin 8. Therefore, the valve metal base 3a is not in direct contact with the solid electrolyte layer 7a or the conductive layer 7b. On the other hand, when an insulating treatment is performed such as being covered with a dielectric layer 5, the end of the valve metal base 3a located on the second end face 9b side of the resin molded body 9 may be covered with the solid electrolyte layer 7a and the conductive layer 7b.
[0051] The sealing resin 8 contains at least a resin, and preferably contains a resin and a filler.
[0052] As the resin, an epoxy resin, a phenol resin, a polyimide resin, a silicone resin, a polyamide resin, a liquid crystal polymer, or the like is preferably used.
[0053] As the filler, silica particles, alumina particles, metal particles, etc. are preferably used.
[0054] The sealing resin 8 may be in a solid or liquid form. As the sealing resin 8, a material containing a solid epoxy resin, a phenol resin, and silica particles is preferably used.
[0055] As a molding method of the resin molded body 9, when a solid sealing resin 8 is used, a resin molding such as compression molding or transfer molding is preferably used, and compression molding is more preferably used. When a liquid sealing resin 8 is used, a molding method such as a dispensing method or a printing method is preferably used. Among them, it is preferable to seal the periphery of the laminate 30 with the sealing resin 8 by compression molding to form the resin molded body 9.
[0056] The corners of the resin molded body 9 may be rounded. For example, barrel polishing or the like is used as a method for rounding the corners of the resin molded body 9. Since the resin molded body is softer than the ceramic body, it is difficult to round the corners by barrel polishing, but even small rounding can be achieved by adjusting the media specifications such as composition, particle size, and shape, the barrel processing time, and the like.
[0057] The first external electrode 11 is provided on the first end surface 9a of the resin molded body 9, and is electrically connected to the anode 3 exposed from the first end surface 9a.
[0058] The first external electrode 11 has, in this order from the first end surface 9a side of the resin molded body 9, a first sprayed electrode layer 11a and a second sprayed electrode layer 11b.
[0059] The first sprayed electrode layer 11a is provided so as to cover the entire first end surface 9a of the resin molded body 9. Because the first sprayed electrode layer 11a is formed by spraying, the bulk resistance (internal resistance) of the first external electrode 11 is low, and when the electrolytic capacitor 1 is mounted on a wiring board, the contact resistance between the first external electrode 11 and the electrode of the wiring board is low. Furthermore, the adhesion between the first sprayed electrode layer 11a and the resin molded body 9, particularly the anode 3, is improved, and the contact resistance between them is reduced. As a result, the ESR of the electrolytic capacitor 1 is reduced.
[0060] The second sprayed electrode layer 11b is in contact with the first sprayed electrode layer 11a and has a higher porosity than the first sprayed electrode layer 11a. In other words, the second sprayed electrode layer 11b has a larger surface area than the first sprayed electrode layer 11a. Therefore, the provision of the second sprayed electrode layer 11b increases the contact area with the outer layer plating layer 11c described below, making it easier for the outer layer plating layer 11c to adhere to the second sprayed electrode layer 11b, and improving the adhesion between the two. As a result, the ESR of the electrolytic capacitor 1 is reduced.
[0061] The second external electrode 13 is provided on the second end surface 9b of the resin molded body 9, and is electrically connected to the cathode 7 exposed from the second end surface 9b.
[0062] The second external electrode 13 has, in this order from the second end surface 9b side of the resin molded body 9, a first sprayed electrode layer 13a and a second sprayed electrode layer 13b.
[0063] The first sprayed electrode layer 13a is provided so as to cover the entire second end surface 9b of the resin molded body 9. Since the first sprayed electrode layer 13a is formed by spraying, the bulk resistance (internal resistance) of the second external electrode 13 is low, and when the electrolytic capacitor 1 is mounted on a wiring board, the contact resistance between the second external electrode 13 and the electrode of the wiring board is low. Furthermore, the adhesion between the first sprayed electrode layer 13a and the resin molded body 9, particularly the cathode 7, is improved, and the contact resistance between them is reduced. As a result, the ESR of the electrolytic capacitor 1 is reduced.
[0064] The second sprayed electrode layer 13b is in contact with the first sprayed electrode layer 13a and has a higher porosity than the first sprayed electrode layer 13a. In other words, the second sprayed electrode layer 13b has a larger surface area than the first sprayed electrode layer 13a. Therefore, the provision of the second sprayed electrode layer 13b increases the contact area with the outer layer plating layer 13c described below, making it easier for the outer layer plating layer 13c to adhere to the second sprayed electrode layer 13b, and improving the adhesion between the two. As a result, the ESR of the electrolytic capacitor 1 is reduced.
[0065] Fig. 3 is a schematic diagram showing an example of the WT surface of the first sprayed electrode layer in Fig. 2. The first sprayed electrode layer 11a and the first sprayed electrode layer 13a each refer to a sprayed electrode layer in which the porosity on the WT surface is 0% or more and less than 5%, preferably 0%, is continuously arranged in the length direction L. In the first sprayed electrode layer 11a and the first sprayed electrode layer 13a, each of the states in which the porosity on the WT surface is 0% or more and less than 5% may be continuously arranged in the length direction L with the porosity changing, or may be continuously arranged in the length direction L with the porosity not changing. The voids in the first sprayed electrode layer 11a and the first sprayed electrode layer 13a each refer to regions in which the constituent materials originating from the first sprayed electrode layer 11a and the first sprayed electrode layer 13a are not present. The porosity of the WT surface of the first sprayed electrode layer 11a and the first sprayed electrode layer 13a respectively refers to the area ratio of voids to the entire first sprayed electrode layer 11a (including voids) and the entire first sprayed electrode layer 13a (including voids), and is calculated from images of the WT surface taken by CT scan.
[0066] Fig. 4 is a schematic diagram showing an example of the WT surface of the second sprayed electrode layer in Fig. 2. The second sprayed electrode layer 11b and the second sprayed electrode layer 13b each refer to a sprayed electrode layer in which the porosity in the WT surface is 5% or more and less than 100%, preferably 30% or more and 90% or less, is continuously arranged in the length direction L. In the second sprayed electrode layer 11b and the second sprayed electrode layer 13b, each of the states in which the porosity in the WT surface is 5% or more and less than 100% may be continuously arranged in the length direction L with the porosity changing, or may be continuously arranged in the length direction L with the porosity unchanged. In the second sprayed electrode layer 11b and the second sprayed electrode layer 13b, it is preferable that the porosity in the WT surface increases continuously from the resin molded body 9 side to the opposite side to the resin molded body 9. The voids 40 in the second sprayed electrode layer 11b and the second sprayed electrode layer 13b refer to regions where no constituent material originating from the second sprayed electrode layer 11b and the second sprayed electrode layer 13b is present, respectively. The porosity on the WT surface of the second sprayed electrode layer 11b and the second sprayed electrode layer 13b refers to the area ratio of the voids 40 to the entire second sprayed electrode layer 11b (including the voids) and the entire second sprayed electrode layer 13b (including the voids), respectively, and is calculated from an image of the WT surface obtained by a CT scan.
[0067] Images of the WT surfaces of the first sprayed electrode layer 11a, the first sprayed electrode layer 13a, the second sprayed electrode layer 11b, and the second sprayed electrode layer 13b are taken using, for example, a CT scanner "inspeXio SMX-225CT" manufactured by Shimadzu Corporation.
[0068] Sprayed electrode layers such as the first sprayed electrode layer 11a, the first sprayed electrode layer 13a, the second sprayed electrode layer 11b, and the second sprayed electrode layer 13b can be distinguished from electrode layers formed by methods other than spraying by information such as the fact that the outer edges are uneven in a CT scanned image of the WT surface and that oxygen is detected by energy dispersive X-ray analysis (EDX) (i.e., that the layers are oxidized).
[0069] The first sprayed electrode layer 11a and the second sprayed electrode layer 11b preferably contain the same metal as a main component, which reduces the contact resistance between the first sprayed electrode layer 11a and the second sprayed electrode layer 11b, and therefore the ESR of the electrolytic capacitor 1 tends to be low.
[0070] The first sprayed electrode layer 11a and the second sprayed electrode layer 11b each preferably contain copper, nickel, or a nickel-aluminum alloy as a main component, which tends to reduce the contact resistance between the first sprayed electrode layer 11a and the anode 3 compared to when the first sprayed electrode layer 11a contains another metal as a main component, and therefore tends to reduce the ESR of the electrolytic capacitor 1.
[0071] The first sprayed electrode layer 13a and the second sprayed electrode layer 13b preferably contain the same metal as a main component, which reduces the contact resistance between the first sprayed electrode layer 13a and the second sprayed electrode layer 13b, and therefore the ESR of the electrolytic capacitor 1 tends to be low.
[0072] The first sprayed electrode layer 13a and the second sprayed electrode layer 13b each preferably contain copper, nickel, or a nickel-aluminum alloy as a main component, which tends to reduce the contact resistance between the first sprayed electrode layer 13a and the cathode 7 compared to when the first sprayed electrode layer 13a contains another metal as a main component, and therefore tends to reduce the ESR of the electrolytic capacitor 1.
[0073] The metal that is the main component of the first sprayed electrode layer 11a and the second sprayed electrode layer 11b may be different from the metal that is the main component of the first sprayed electrode layer 13a and the second sprayed electrode layer 13b, but it is preferable that they are the same.
[0074] In this specification, the main component of each layer or electrode refers to the component that is contained in the largest amount in each layer or electrode. The main component of each layer or electrode can be confirmed by exposing the LT surface as shown in Figure 2 and then performing elemental analysis such as energy dispersive X-ray analysis.
[0075] The total thickness of the first sprayed electrode layer 11a and the second sprayed electrode layer 11b is preferably 40 μm or more and 120 μm or less. This tends to reduce the ESR of the electrolytic capacitor 1. In addition, the adhesion between the first sprayed electrode layer 11a and the resin molded body 9, in particular, the anode 3, is improved, reducing appearance defects such as peeling and fading of the first sprayed electrode layer 11a.
[0076] The total thickness of the first sprayed electrode layer 13a and the second sprayed electrode layer 13b is preferably 40 μm or more and 120 μm or less. This tends to reduce the ESR of the electrolytic capacitor 1. In addition, the adhesion between the first sprayed electrode layer 13a and the resin molded body 9, particularly the cathode 7, is improved, reducing appearance defects such as peeling and fading of the first sprayed electrode layer 13a.
[0077] The total thickness of the first sprayed electrode layer 11a and the second sprayed electrode layer 11b and the total thickness of the first sprayed electrode layer 13a and the second sprayed electrode layer 13b may be the same or different.
[0078] The first external electrode 11 has an outer layer plating layer 11c provided on the surface of the second sprayed electrode layer 11b opposite to the first sprayed electrode layer 11a. By providing the outer layer plating layer 11c, the second sprayed electrode layer 11b, which has a higher porosity than the first sprayed electrode layer 11a, is covered with the relatively dense outer layer plating layer 11c, and the ESR of the electrolytic capacitor 1 tends to be low.
[0079] The outer plating layer 11c and the second sprayed electrode layer 11b preferably contain the same metal as a main component, which reduces the contact resistance between the outer plating layer 11c and the second sprayed electrode layer 11b, and therefore the ESR of the electrolytic capacitor 1 tends to be low.
[0080] The outer plating layer 11c preferably contains copper, nickel, or tin as a main component, which tends to reduce the ESR of the electrolytic capacitor 1. The outer plating layer 11c may have a single-layer structure or a multi-layer structure, but if it has a multi-layer structure, it is preferable that the layer in contact with the second sprayed electrode layer 11b among the multiple layers constituting the outer plating layer 11c contains copper, nickel, or tin as a main component.
[0081] When the outer layer plating layer 11c has a multi-layer structure, the outer layer plating layer 11c may have, in this order from the second sprayed electrode layer 11b side, a first outer layer plating layer 11ca and a second outer layer plating layer 11cb.
[0082] The first outer plating layer 11ca is preferably a so-called nickel plating layer that contains nickel as a main component.
[0083] The second outer plating layer 11cb is preferably a so-called tin plating layer that contains tin as a main component.
[0084] The second external electrode 13 has an outer layer plating layer 13c provided on the surface of the second sprayed electrode layer 13b opposite to the first sprayed electrode layer 13a. By providing the outer layer plating layer 13c, the second sprayed electrode layer 13b, which has a higher porosity than the first sprayed electrode layer 13a, is covered with the relatively dense outer layer plating layer 13c, which tends to reduce the ESR of the electrolytic capacitor 1.
[0085] It is preferable that the outer layer plating layer 13c and the second sprayed electrode layer 13b contain the same metal as a main component, which reduces the contact resistance between the outer layer plating layer 13c and the second sprayed electrode layer 13b, and therefore the ESR of the electrolytic capacitor 1 tends to be low.
[0086] The outer plating layer 13c preferably contains copper, nickel, or tin as a main component, which tends to reduce the ESR of the electrolytic capacitor 1. The outer plating layer 13c may have a single-layer structure or a multi-layer structure, but if it has a multi-layer structure, it is preferable that the layer in contact with the second sprayed electrode layer 13b among the multiple layers constituting the outer plating layer 13c contains copper, nickel, or tin as a main component.
[0087] When the outer layer plating layer 13c has a multi-layer structure, the outer layer plating layer 13c may have, in this order from the second sprayed electrode layer 13b side, a first outer layer plating layer 13ca and a second outer layer plating layer 13cb.
[0088] The first outer plating layer 13ca is preferably a so-called nickel plating layer that contains nickel as a main component.
[0089] The second outer plating layer 13cb is preferably a so-called tin plating layer that contains tin as a main component.
[0090] In the LT plane shown in FIG. 2, the variation in thickness of the first external electrode 11 measured from the first end face 9a of the resin molding 9 and the variation in thickness of the second external electrode 13 measured from the second end face 9b of the resin molding 9 are each preferably 30 μm or less, more preferably 20 μm or less, and even more preferably 5 μm or less.
[0091] The variation in thickness of the first external electrode 11 is determined as follows. First, with the LT surface shown in FIG. 2 exposed, the thickness of the first external electrode 11 is measured at a total of five points, including the bottom surface, the top surface, and three points dividing the area from the bottom surface to the top surface into four equal parts. Then, the difference between the maximum value and the minimum value obtained from the thickness measurements of the first external electrode 11 at these five points is determined as the variation in thickness of the first external electrode 11. Note that even in a non-destructive state where the LT surface shown in FIG. 2 is not exposed, the thickness of the first external electrode 11 can be measured at multiple points by using a fluorescent X-ray thickness gauge, a laser displacement meter, or the like.
[0092] The variation in thickness of the second external electrode 13 is determined in the same manner as the variation in thickness of the first external electrode 11.
[0093] The preferred ranges for each dimension of the electrolytic capacitor 1 are as follows: Dimension in the length direction L: 3.4 mm or more, 3.8 mm or less -Dimension in width direction W: 2.7mm or more, 3.0mm or less - Dimension in thickness direction T: 1.8 mm or more, 2.0 mm or less
[0094] The method for manufacturing an electrolytic capacitor of the present invention includes the steps of: preparing a rectangular parallelepiped resin molded body having a laminate having a capacitor element including an anode having a dielectric layer on a surface thereof and a cathode facing the anode; and a sealing resin that seals the periphery of the laminate; forming a first external electrode on a first end face of the resin molded body, the first external electrode being electrically connected to the anode exposed from the first end face; and forming a second external electrode on a second end face of the resin molded body, the second external electrode being electrically connected to the cathode exposed from the second end face. The step of forming the first external electrode is characterized in that, in order from the first end face side, a first sprayed electrode layer and a second sprayed electrode layer that is in contact with the first sprayed electrode layer and has a higher porosity than the first sprayed electrode layer are formed by spraying the first end face of the resin molded body. In the method for manufacturing an electrolytic capacitor of the present invention, in the step of forming the second external electrode, a first sprayed electrode layer and a second sprayed electrode layer that is in contact with the first sprayed electrode layer and has a higher porosity than the first sprayed electrode layer may be formed in this order from the second end face side by performing thermal spraying on the second end face of the resin molded body. In the step of forming the first external electrode and the step of forming the second external electrode, an outer layer plating layer may be formed on the surface of the second sprayed electrode layer opposite to the first sprayed electrode layer by performing plating treatment after performing the thermal spraying on the first end face and the second end face of the resin molded body, respectively. Such an example will be described below as a method for manufacturing an electrolytic capacitor according to embodiment 1 of the present invention, that is, a method for manufacturing an electrolytic capacitor 1 shown in FIG. 1 and FIG. 2.
[0095] <Process for Producing Resin Molded Body> First, a valve metal substrate 3a having a porous layer on its surface, that is, an anode 3, is prepared. Then, the surface of the porous layer is anodized to form a dielectric layer 5.
[0096] Next, the solid electrolyte layer 7a is formed on the dielectric layer 5 by screen printing or the like. Then, the conductive layer 7b is formed on the solid electrolyte layer 7a by screen printing or the like. Furthermore, the cathode lead layer 7c is formed on the conductive layer 7b by sheet lamination, screen printing or the like. In this way, the cathode 7 having the solid electrolyte layer 7a, the conductive layer 7b, and the cathode lead layer 7c is formed.
[0097] In this manner, capacitor element 20 including anode 3 having dielectric layer 5 on its surface and cathode 7 facing anode 3 is produced.
[0098] Next, a plurality of capacitor elements 20 are stacked to produce a laminate 30. Then, the periphery of the laminate 30 is sealed with sealing resin 8 by compression molding or the like to produce a resin molded body 9. In the resin molded body 9, the anode 3 is exposed from a first end face 9a, and the cathode 7 is exposed from a second end face 9b.
[0099] <Step of forming first external electrode> First, a sprayed electrode layer is formed by spraying the first end face 9a of the resin molded body 9. At this time, for example, by adjusting various spraying conditions, the sprayed electrode layer can be formed, in order from the first end face 9a side, as a first sprayed electrode layer 11a and a second sprayed electrode layer 11b that is in contact with the first sprayed electrode layer 11a and has a higher porosity than the first sprayed electrode layer 11a.
[0100] Examples of the spray material include copper, nickel, nickel-aluminum alloy (95Ni-5Al, Ni-20Al), phosphor bronze (Cu-9Sn), nickel-chromium alloy (Ni-20Cr), nickel-aluminum-molybdenum alloy (Ni-5Al-5Mo), etc. Among them, copper, nickel, or nickel-aluminum alloy is preferable. When copper is used as the spray material, the porosity of the second sprayed electrode layer 11b is likely to be increased compared to when nickel is used.
[0101] Examples of the thermal spraying method include plasma spraying, arc spraying, cold spraying, aerosol deposition (AD) method, etc. Among them, plasma spraying is preferable because it is industrially useful.
[0102] When plasma spraying is performed, the first sprayed electrode layer 11a and the second sprayed electrode layer 11b can be formed separately by adjusting various conditions such as blasting before spraying, particle velocity, working gas temperature, number of scans (number of passes), etc. For example, by performing two scans and lowering the particle velocity or gas temperature in the second scan compared to the first scan, the second sprayed electrode layer 11b having a higher porosity than the first sprayed electrode layer 11a can be formed in the second scan.
[0103] Next, the first end face 9a of the resin molded body 9 is sprayed, and then a plating process such as electrolytic plating is performed to form an outer layer plating layer 11c on the surface of the second sprayed electrode layer 11b opposite to the first sprayed electrode layer 11a. At this time, as the outer layer plating layer 11c, a first outer layer plating layer 11ca and a second outer layer plating layer 11cb may be formed in this order from the second sprayed electrode layer 11b side.
[0104] In this manner, a first external electrode 11 is formed on the first end face 9a of the resin molded body 9, and is electrically connected to the anode 3 exposed from the first end face 9a. More specifically, the first external electrode 11 is formed having, in order from the first end face 9a side of the resin molded body 9, a first sprayed electrode layer 11a, a second sprayed electrode layer 11b, and an outer plating layer 11c.
[0105] In the case where a natural oxide film (passivation state) is likely to form on the exposed surface of the anode 3, it has been necessary to previously remove the natural oxide film by pretreatment such as zincate treatment when forming an external electrode on the anode 3. In contrast, when thermal spraying is performed directly on the first end surface 9a of the resin molded body 9 as in this embodiment, the natural oxide film of the anode 3 is physically destroyed and the anode 3 and the first sprayed electrode layer 11a can be directly connected, making it unnecessary to perform pretreatment such as zincate treatment.
[0106] <Step of forming second external electrode> First, a sprayed electrode layer is formed by spraying the second end face 9b of the resin molded body 9. In this case, similarly to the process of forming the first external electrode, for example, by adjusting various spraying conditions, it is possible to form, as the sprayed electrode layer, in order from the second end face 9b side, a first sprayed electrode layer 13a and a second sprayed electrode layer 13b that is in contact with the first sprayed electrode layer 13a and has a higher porosity than the first sprayed electrode layer 13a.
[0107] The spray material may be the same as that used in forming the first sprayed electrode layer 11a and the second sprayed electrode layer 11b. Among them, copper, nickel, or a nickel-aluminum alloy is preferable. When copper is used as the spray material, the porosity of the second sprayed electrode layer 13b is likely to be increased compared to when nickel is used.
[0108] The spraying method may be the same as that used for forming the first sprayed electrode layer 11a and the second sprayed electrode layer 11b. Among them, plasma spraying is preferable because it is industrially useful.
[0109] When plasma spraying is performed, the first sprayed electrode layer 13a and the second sprayed electrode layer 13b can be formed separately by adjusting various conditions such as blasting before spraying, particle velocity, working gas temperature, number of scans (number of passes), etc. For example, by performing two scans and lowering the particle velocity or gas temperature in the second scan compared to the first scan, the second sprayed electrode layer 13b having a higher porosity than the first sprayed electrode layer 13a can be formed in the second scan.
[0110] Next, the second end face 9b of the resin molded body 9 is sprayed, and then a plating process such as electrolytic plating is performed to form an outer layer plating layer 13c on the surface of the second sprayed electrode layer 13b opposite to the first sprayed electrode layer 13a. At this time, as the outer layer plating layer 13c, a first outer layer plating layer 13ca and a second outer layer plating layer 13cb may be formed in this order from the second sprayed electrode layer 13b side.
[0111] In this manner, a second external electrode 13 is formed on the second end face 9b of the resin molded body 9, and is electrically connected to the cathode 7 exposed from the second end face 9b. More specifically, the second external electrode 13 is formed having, in order from the second end face 9b side of the resin molded body 9, a first sprayed electrode layer 13a, a second sprayed electrode layer 13b, and an outer plating layer 13c.
[0112] In the case where a natural oxide film is likely to form on the exposed surface of the cathode 7, it has been conventionally necessary to remove the natural oxide film in advance by a pretreatment such as zincate treatment when forming an external electrode on the cathode 7. In contrast, when thermal spraying is performed directly on the second end surface 9b of the resin molded body 9 as in this embodiment, the natural oxide film of the cathode 7 is physically destroyed and the cathode 7 and the first sprayed electrode layer 13a can be directly connected, making it unnecessary to perform a pretreatment such as zincate treatment.
[0113] The step of forming the first external electrode and the step of forming the second external electrode may be performed at different times or at the same time. When the steps are performed at different times, the order of these steps is not particularly limited.
[0114] In this manner, the electrolytic capacitor 1 shown in FIGS. 1 and 2 is manufactured.
[0115] [Modification 1 of the first embodiment] In the electrolytic capacitor of the first embodiment of the present invention, a composite layer of the second sprayed electrode layer and the outer layer plating layer may be provided inside the second sprayed electrode layer in each of the first external electrode and the second external electrode. Such an example will be described below as an electrolytic capacitor of a first variation of the first embodiment of the present invention. The electrolytic capacitor of the first variation of the first embodiment of the present invention is similar to the electrolytic capacitor of the first embodiment of the present invention, except for the configuration of the second sprayed electrode layer.
[0116] Fig. 5 is a cross-sectional schematic diagram showing an electrolytic capacitor according to Modification 1 of the first embodiment of the present invention. As shown in Fig. 5, in the first external electrode 11 of the electrolytic capacitor 1a, a composite layer 11ba of the second sprayed electrode layer 11b and the outer layer plating layer 11c (here, the first outer layer plating layer 11ca) is provided inside the second sprayed electrode layer 11b. More specifically, the composite layer 11ba is provided in a state in which the constituent material derived from the first outer layer plating layer 11ca exists in the voids of the second sprayed electrode layer 11b. The provision of the composite layer 11ba makes the second sprayed electrode layer 11b dense, and therefore the ESR of the electrolytic capacitor 1a tends to be low.
[0117] The composite layer 11ba may be provided on a part of the second sprayed electrode layer 11b, or may be provided on the entire second sprayed electrode layer 11b. When the composite layer 11ba is provided on a part of the second sprayed electrode layer 11b, the composite layer 11ba is preferably provided in a region of the second sprayed electrode layer 11b that contacts the outer plating layer 11c.
[0118] In the second external electrode 13 of the electrolytic capacitor 1a, a composite layer 13ba of the second sprayed electrode layer 13b and the outer layer plating layer 13c (here, the first outer layer plating layer 13ca) is provided inside the second sprayed electrode layer 13b. More specifically, the composite layer 13ba is provided in a state in which the constituent material derived from the first outer layer plating layer 13ca is present in the voids of the second sprayed electrode layer 13b. The provision of the composite layer 13ba makes the second sprayed electrode layer 13b dense, which tends to reduce the ESR of the electrolytic capacitor 1a.
[0119] The composite layer 13ba may be provided on a part of the second sprayed electrode layer 13b, or may be provided on the entire second sprayed electrode layer 13b. When the composite layer 13ba is provided on a part of the second sprayed electrode layer 13b, the composite layer 13ba is preferably provided in a region of the second sprayed electrode layer 13b that contacts the outer plating layer 13c.
[0120] In the method for manufacturing an electrolytic capacitor according to the first modified example of the first embodiment of the present invention, i.e., the method for manufacturing an electrolytic capacitor 1a shown in Fig. 5, by increasing the porosity of the WT surface of the second sprayed electrode layer 11b, preferably to 30% or more and 90% or less, a portion of the first outer layer plating layer 11ca penetrates into the voids of the second sprayed electrode layer 11b to form a composite layer 11ba. Also, by increasing the porosity of the WT surface of the second sprayed electrode layer 13b, preferably to 30% or more and 90% or less, a portion of the first outer layer plating layer 13ca penetrates into the voids of the second sprayed electrode layer 13b to form a composite layer 13ba.
[0121] [Embodiment 2] In the electrolytic capacitor of the present invention, the first external electrode and the second external electrode may each have an inner layer plating layer provided between the anode and the first sprayed electrode layer, and between the cathode and the first sprayed electrode layer. Such an example will be described below as the electrolytic capacitor of embodiment 2 of the present invention. The electrolytic capacitor of embodiment 2 of the present invention is similar to the electrolytic capacitor of embodiment 1 of the present invention, except for the configurations of the first external electrode and the second external electrode.
[0122] Fig. 6 is a cross-sectional schematic diagram showing an electrolytic capacitor according to a second embodiment of the present invention. As shown in Fig. 6, the first external electrode 11 of the electrolytic capacitor 2 has an inner layer plating layer 11d provided between the anode 3 and the first sprayed electrode layer 11a. The inner layer plating layer 11d is in contact with the anode 3. The inner layer plating layer 11d is also in contact with the first sprayed electrode layer 11a. When the contact resistance between the anode 3 and the first sprayed electrode layer 11a is high, the provision of the inner layer plating layer 11d reduces the resistance between the anode 3 and the first sprayed electrode layer 11a, and the ESR of the electrolytic capacitor 2 is likely to be reduced.
[0123] The second external electrode 13 of the electrolytic capacitor 2 has an inner layer plating layer 13d provided between the cathode 7 and the first sprayed electrode layer 13a. The inner layer plating layer 13d is in contact with the cathode 7 (here, the cathode lead layer 7c). The inner layer plating layer 13d is also in contact with the first sprayed electrode layer 13a. When the contact resistance between the cathode 7 and the first sprayed electrode layer 13a is high, the provision of the inner layer plating layer 13d reduces the resistance between the cathode 7 and the first sprayed electrode layer 13a, and the ESR of the electrolytic capacitor 2 is likely to be reduced.
[0124] Each of the inner plating layers 11d and 13d preferably contains copper, nickel, or silver as a main component, which makes it easier for the ESR of the electrolytic capacitor 2 to be low.
[0125] When the inner plating layer 11d and the inner plating layer 13d are each a so-called copper plating layer containing copper as a main component, or a so-called silver plating layer containing silver as a main component, the inner plating layer 11d and the inner plating layer 13d each have a single-layer structure. When the inner plating layer 11d and the inner plating layer 13d are each a single-layer structure of a copper plating layer or a silver plating layer, the ESR of the electrolytic capacitor 2 is likely to be low because the interface resistance is low due to the reduced number of interfaces compared to when the inner plating layer 11d and the inner plating layer 13d are a two-layer structure of a nickel plating layer and a silver plating layer. In addition, when the inner plating layer 11d and the inner plating layer 13d are each a copper plating layer or a silver plating layer, the ESR of the electrolytic capacitor 2 is likely to be low compared to when the inner plating layer 11d and the inner plating layer 13d are each a nickel plating layer.
[0126] The copper plating layer or silver plating layer as the inner plating layer 11d is preferably formed by performing a zincate treatment on the first end face 9a of the resin molded body 9, followed by a displacement plating treatment using electroless copper plating or electroless silver plating. The zincate treatment is a treatment for removing oxides on the surface of a metal to be plated and forming a zinc coating on the surface of the metal.
[0127] The copper plating layer or silver plating layer as the inner plating layer 13d can be formed in the same manner as the copper plating layer or silver plating layer as the inner plating layer 11d, but does not need to be subjected to zincate treatment. However, when the cathode lead layer 7c of the cathode 7 contains aluminum as a main component, it is preferable to perform the zincate treatment.
[0128] When the inner plating layer 11d and the inner plating layer 13d are each a copper plating layer, the thickness of the copper plating layer is preferably 0.2 μm or more and 4.0 μm or less, and more preferably 0.5 μm or more and 2.0 μm or less. When the thickness of the copper plating layer is in the above-mentioned range, a sufficient thickness as a plating layer is ensured, and the ESR of the electrolytic capacitor 2 tends to be low.
[0129] When the inner plating layer 11d and the inner plating layer 13d are each a silver plating layer, the thickness of the silver plating layer is preferably 0.1 μm or more and 2.0 μm or less, and more preferably 0.2 μm or more and 1.0 μm or less. When the thickness of the silver plating layer is in the above-mentioned range, the ESR of the electrolytic capacitor 2 tends to be low even if the thickness is relatively small.
[0130] The thickness of the copper plating layer or silver plating layer serving as the inner plating layer 11d is determined as follows. First, a micrograph is taken with the LT surface shown in FIG. 6 exposed, and then a perpendicular line is drawn in the micrograph to the first end face 9a of the resin molded body 9. Next, the thickness determined by the dimension of the perpendicular line is measured for each copper plating layer or silver plating layer provided corresponding to each anode 3. Then, the average value calculated from the thickness measurements at at least five locations is determined as the thickness of the copper plating layer or silver plating layer serving as the inner plating layer 11d.
[0131] The thickness of the copper plating layer or silver plating layer serving as the inner plating layer 13d is determined as follows. First, a micrograph is taken with the LT surface exposed as shown in FIG. 6, and then a perpendicular line is drawn in the micrograph to the second end surface 9b of the resin molded body 9. Next, the thickness determined by the dimension of the perpendicular line is measured for each copper plating layer or silver plating layer provided corresponding to each cathode 7. Then, the average value calculated from the thickness measurements at at least five locations is determined as the thickness of the copper plating layer or silver plating layer serving as the inner plating layer 13d.
[0132] The inner plating layer 11d may be formed by performing a zincate treatment on the first end face 9a of the resin molded body 9, followed by electroless nickel plating and electrolytic silver plating in that order. The inner plating layer 13d may be formed by performing a zincate treatment on the second end face 9b of the resin molded body 9, followed by electroless nickel plating and electrolytic silver plating in that order.
[0133] When the anode 3 (here, the valve action metal base 3a) contains aluminum as a main component, and the first sprayed electrode layer 11a and the second sprayed electrode layer 11b of the first external electrode 11 each contain copper as a main component, the first external electrode 11 preferably has an inner plating layer 11d containing silver as a main component provided between the anode 3 and the first sprayed electrode layer 11a. Since the contact resistance between copper and silver is lower than the contact resistance between copper and aluminum, when the first sprayed electrode layer 11a and the second sprayed electrode layer 11b each contain copper as a main component, the ESR of the electrolytic capacitor 2 is likely to be low if the inner plating layer 11d containing silver as a main component is provided between the anode 3 and the first sprayed electrode layer 11a.
[0134] On the other hand, when the first sprayed electrode layer 11a and the second sprayed electrode layer 11b of the first external electrode 11 each contain nickel or a nickel-aluminum alloy as a main component, it is preferable not to provide the inner plating layer 11d containing silver as a main component. More specifically, when the anode 3 (here, the valve metal base 3a) contains aluminum as a main component and the first sprayed electrode layer 11a and the second sprayed electrode layer 11b of the first external electrode 11 each contain nickel or a nickel-aluminum alloy as a main component, it is preferable that the anode 3 and the first sprayed electrode layer 11a are in contact with each other. Since the contact resistance between nickel or a nickel-aluminum alloy and aluminum is lower than the contact resistance between nickel or a nickel-aluminum alloy and silver, when the first sprayed electrode layer 11a and the second sprayed electrode layer 11b each contain nickel or a nickel-aluminum alloy as a main component, if the inner layer plating layer 11d containing silver as a main component is not provided and the anode 3 and the first sprayed electrode layer 11a are in contact as shown in FIG. 2, the ESR of the electrolytic capacitor 1 is likely to be low.
[0135] In the first external electrode 11 of the electrolytic capacitor 2, a composite layer 11ba of the second sprayed electrode layer 11b and the outer layer plating layer 11c (here, first outer layer plating layer 11ca) may be provided inside the second sprayed electrode layer 11b, as in Variation 1 of Embodiment 1. In the second external electrode 13 of the electrolytic capacitor 2, a composite layer 13ba of the second sprayed electrode layer 13b and the outer layer plating layer 13c (here, first outer layer plating layer 13ca) may be provided inside the second sprayed electrode layer 13b, as in Variation 1 of Embodiment 1.
[0136] The method for manufacturing the electrolytic capacitor of embodiment 2 of the present invention, i.e., the method for manufacturing the electrolytic capacitor 2 shown in FIG. 6, is similar to the method for manufacturing the electrolytic capacitor 1 shown in FIG. 2, except for forming the inner layer plating layer 11d and the inner layer plating layer 13d.
[0137] In the process of forming the first external electrode 11, a plating process is performed on the first end face 9a of the resin molding 9 before thermal spraying, thereby forming an inner layer plating layer 11d between the anode 3 and the first sprayed electrode layer 11a.
[0138] When forming the inner layer plating layer 11d, it is preferable to perform a zincate treatment on the first end face 9a of the resin molded body 9, and then perform a displacement plating treatment using electroless copper plating or electroless silver plating to form a copper plating layer or a silver plating layer.
[0139] For example, when the valve metal substrate 3a of the anode 3 is an aluminum foil, the surface of the anode 3 exposed from the first end face 9a of the resin molded body 9 is first etched with an acid mainly composed of nitric acid, and then a zinc coating is formed on the surface to perform a zincate treatment. As the zincate treatment, both single zincate (acid washing) and double zincate (peeling) are preferably performed. Then, a displacement plating treatment is performed using electroless copper plating or electroless silver plating to form a copper plating layer or a silver plating layer as the inner plating layer 11d.
[0140] The plating bath for forming the copper plating layer is preferably a neutral electroless copper plating bath, and the pH value thereof is preferably 7.0 or more and 8.5 or less.
[0141] The plating bath for forming the silver plating layer is preferably a cyanide-containing electroless silver plating bath, and the pH value thereof is preferably 8.0 or more and 9.0 or less.
[0142] In addition, the thickness of the copper plating layer or silver plating layer can be adjusted by adjusting the conditions of electroless copper plating or electroless silver plating, such as the concentration of the plating solution and the plating time.
[0143] In the process of forming the second external electrode 13, a plating process is performed on the second end face 9b of the resin molding 9 before thermal spraying, thereby forming an inner layer plating layer 13d between the cathode 7 and the first sprayed electrode layer 13a.
[0144] When a copper plating layer or a silver plating layer is formed as the inner plating layer 13d, it can be formed in the same manner and under the same conditions as when a copper plating layer or a silver plating layer is formed as the inner plating layer 11d.
[0145] The inner plating layer 11d may be formed by performing a zincate treatment on the first end face 9a of the resin molded body 9, followed by electroless nickel plating and electrolytic silver plating in that order, thereby forming a two-layer structure of a nickel plating layer and a silver plating layer. The inner plating layer 13d may be formed by performing a zincate treatment on the second end face 9b of the resin molded body 9, followed by electroless nickel plating and electrolytic silver plating in that order, thereby forming a two-layer structure of a nickel plating layer and a silver plating layer.
[0146] In each of the above-described embodiments, an outer layer plating layer is provided, but the outer layer plating layer may not be provided. More specifically, in the electrolytic capacitor 1 shown in FIG. 2, the electrolytic capacitor 1a shown in FIG. 5, or the electrolytic capacitor 2 shown in FIG. 6, the outer layer plating layer 11c and the outer layer plating layer 13c may not be provided. In this case, when the second sprayed electrode layer 11b and the second sprayed electrode layer 13b are soldered during mounting on a wiring board, the second sprayed electrode layer 11b and the second sprayed electrode layer 13b have a high porosity, i.e., a large surface area, so that the wettability of the solder is increased.
[0147] [Embodiment 3] In the electrolytic capacitor of the present invention, the second external electrode may have a printed electrode layer provided on the second end face of the resin molded body. In addition, in the electrolytic capacitor of the present invention, the first external electrode and the second external electrode may each have an outer layer plating layer provided on the surface of the second sprayed electrode layer opposite to the first sprayed electrode layer and on the surface of the printed electrode layer opposite to the resin molded body. Such an example will be described below as the electrolytic capacitor of embodiment 3 of the present invention. The electrolytic capacitor of embodiment 3 of the present invention is similar to the electrolytic capacitor of embodiment 1 of the present invention except for the configuration of the second external electrode.
[0148] Fig. 7 is a schematic cross-sectional view showing an electrolytic capacitor according to embodiment 3 of the present invention. As shown in Fig. 7, the second external electrode 13 of the electrolytic capacitor 4 has, in order from the second end face 9b side of the resin molded body 9, a printed electrode layer 13e and an outer plating layer 13c.
[0149] The printed electrode layer 13e is provided on the second end surface 9b of the resin molded body 9, and is in contact with the cathode 7 (here, the cathode lead layer 7c).
[0150] The outer plating layer 13c is provided on the surface of the printed electrode layer 13e opposite to the resin molded body 9.
[0151] The configuration of the second external electrode 13 of the electrolytic capacitor 4 is effective when the main component of the cathode lead layer 7c is other than a valve metal. More specifically, at the second end face 9b of the resin molded body 9, no natural oxide film is formed on the exposed surface of the cathode lead layer 7c, so that the cathode lead layer 7c and the printed electrode layer 13e are directly connected. As a result, the ESR of the electrolytic capacitor 4 tends to be low. In the electrolytic capacitor 4, the main component of the cathode lead layer 7c is preferably silver, copper, nickel, or an alloy containing at least one of these metals.
[0152] In the first external electrode 11 of the electrolytic capacitor 4, as in variant example 1 of embodiment 1, a composite layer 11ba of the second sprayed electrode layer 11b and an outer layer plating layer 11c (here, the first outer layer plating layer 11ca) may be provided inside the second sprayed electrode layer 11b.
[0153] In the first external electrode 11 of the electrolytic capacitor 4, an inner layer plating layer 11d may be provided between the anode 3 and the first sprayed electrode layer 11a as in embodiment 2. In the second external electrode 13 of the electrolytic capacitor 4, an inner layer plating layer 13d may be provided between the cathode 7 and the printed electrode layer 13e as in embodiment 2.
[0154] The manufacturing method of the electrolytic capacitor of embodiment 3 of the present invention, i.e., the manufacturing method of the electrolytic capacitor 4 shown in FIG. 7, is similar to the manufacturing method of the electrolytic capacitor 1 shown in FIG. 2, except that a printed electrode layer 13e is formed instead of the first sprayed electrode layer 13a and the second sprayed electrode layer 13b.
[0155] In the step of forming the second external electrode 13, the electrode paste is applied to the second end surface 9b of the resin molded body 9 by a method such as sponge transfer, screen printing, or inkjet printing to form a printed electrode layer 13e.
[0156] The electrode paste used to form the printed electrode layer 13e preferably contains silver, copper, or nickel as a main component. EXAMPLES
[0157] Examples that more specifically disclose the electrolytic capacitor of the present invention will be described below. In the following examples, a solid electrolytic capacitor will be described as the electrolytic capacitor of the present invention. However, the present invention is not limited to only these examples.
[0158] [Example 1] The solid electrolytic capacitor of Example 1 was produced by the following method.
[0159] <Process for Producing Resin Molded Body> A laminate having the structure shown in FIG. 6 was sealed with a sealing resin containing an epoxy resin and silica particles to produce a resin molded body.
[0160] <Step of forming first external electrode and step of forming second external electrode> First, the first and second end faces of the resin molded body were etched with an acid mainly composed of nitric acid, and then zinc coatings were formed on both end faces to perform a zincate treatment. Then, electroless nickel plating and electrolytic silver plating were sequentially performed on the first and second end faces to form a two-layer structure of a nickel plating layer and a silver plating layer as an inner plating layer.
[0161] Next, the resin molded body was masked so that the first end face and the second end face were exposed, and then plasma spraying was performed to form a sprayed electrode layer covering the inner plating layer. Copper was used as the spray material. In this case, various conditions such as blasting (alumina blasting) before spraying, particle speed, working gas temperature, and number of scans (number of passes) were adjusted to form the sprayed electrode layers on the first end face and the second end face, in order from the first end face side and the second end face side, respectively, a first sprayed electrode layer and a second sprayed electrode layer in contact with the first sprayed electrode layer and having a higher porosity than the first sprayed electrode layer.
[0162] Next, plasma spraying was performed on the first end face and the second end face of the resin molded body, followed by electrolytic nickel plating and electrolytic tin plating, in that order, to form, as outer layer plating layers, a nickel plating layer as a first outer layer plating layer and a tin plating layer as a second outer layer plating layer, in that order, on the surface of the second sprayed electrode layer opposite the first sprayed electrode layer.
[0163] In this manner, the solid electrolytic capacitor of Example 1 was manufactured.
[0164] In the solid electrolytic capacitor of Example 1, the thickness of the sprayed electrode layer, i.e., the total thickness of the first sprayed electrode layer and the second sprayed electrode layer, was 15 μm. The thickness of the sprayed electrode layer was measured using a field emission scanning electron microscope "JSM-7100F" manufactured by JEOL Ltd., with the LT surface exposed by polishing the solid electrolytic capacitor.
[0165] [Examples 2 to 54] The solid electrolytic capacitors of Examples 2 to 54 were manufactured in the same manner as the solid electrolytic capacitor of Example 1, except that the presence or absence of an inner layer plating layer, the sprayed material, and the thickness of the sprayed electrode layer (the total thickness of the first sprayed electrode layer and the second sprayed electrode layer) were changed to the specifications shown in Tables 1 to 3.
[0166] [evaluation] The solid electrolytic capacitors of Examples 1 to 54 were subjected to the following evaluations. The results are shown in Tables 1 to 3.
[0167] <esr> The ESR at 100 kHz was measured using an LCR meter "E4980A" manufactured by KEYSIGHT Corp. The ESR was measured after the formation of the sprayed electrode layer and after the formation of the outer plating layer.
[0168] <Adhesion> By carrying out a cross-cut test on each of the first and second external electrodes in accordance with "JIS K 5600-5-6," the adhesion between the first external electrode and the anode, and the adhesion between the second external electrode and the cathode were evaluated. The evaluation criteria were as follows, covering all the squares engraved on the first and second external electrodes. ○: None of the squares peeled off. △: More than 0% and 5% or less of the squares were peeled off. ×: More than 5% of the squares were peeled off.
[0169] [Table 1]
[0170] [Table 2]
[0171] [Table 3]
[0172] As shown in Tables 1 to 3, the solid electrolytic capacitors of Examples 1 to 54 had low ESR and high adhesion.
[0173] When copper was used as the spray material in forming the sprayed electrode layer as in the solid electrolytic capacitors of Examples 1 to 18, the following was found. When the thickness of the sprayed electrode layer is the same, the specification with "inner layer plating: yes" has a lower ESR than the specification without "inner layer plating: no" Compared to when other thermal spray materials are used, the ESR is more likely to decrease after the formation of the outer plating layer; in other words, the difference between the ESR after the formation of the thermal spray electrode layer and the ESR after the formation of the outer plating layer is more likely to become large.
[0174] When nickel was used as the spray material in forming the sprayed electrode layer as in the solid electrolytic capacitors of Examples 19 to 36, the following was found. When the thickness of the sprayed electrode layer is the same, the "inner layer: without" specification has a lower ESR than the "inner layer: with" specification.
[0175] When a nickel-aluminum alloy was used as the spray material in forming the sprayed electrode layer as in the solid electrolytic capacitors of Examples 37 to 54, the following was found. When the thickness of the sprayed electrode layer is the same, the "inner layer: without" specification has a lower ESR than the "inner layer: with" specification. [Explanation of symbols]
[0176] 1, 1a, 2, 4 electrolytic capacitors 3 Anode 3a Valve metal substrate 5 Dielectric Layer 7 Cathode 7a Solid electrolyte layer 7b Conductive layer 7c Cathode extraction layer 8 Sealing resin 9. Resin molding 9a: First end surface of resin molded body 9b: second end surface of resin molding 9c Bottom surface of resin molded body 9d Top surface of resin molded body 9e First side surface of resin molded body 9f Second side of resin molded body 11 1st external electrode 11a, 13a First sprayed electrode layer 11b, 13b Second sprayed electrode layer 11ba, 13ba composite layer 11c, 13c Outer plating layer 11ca, 13ca 1st outer plating layer 11cb, 13cb Second outer plating layer 11d, 13d Inner plating layer 13 2nd external electrode 13e printed electrode layer 20 Capacitor element 30 Laminate 40 void< / esr>
Claims
1. a rectangular parallelepiped resin molded body including a laminate having a capacitor element including an anode having a dielectric layer on a surface thereof and a cathode facing the anode, and a sealing resin sealing the periphery of the laminate; a first external electrode provided on a first end surface of the resin molded body and electrically connected to the anode exposed from the first end surface; a second external electrode provided on a second end surface of the resin molded body and electrically connected to the cathode exposed from the second end surface, the first external electrode has, in order from the first end surface side of the resin molded body, a first sprayed electrode layer and a second sprayed electrode layer in contact with the first sprayed electrode layer and having a higher porosity than the first sprayed electrode layer; the first external electrode further has an outer layer plating layer provided on a surface of the second sprayed electrode layer opposite to the first sprayed electrode layer, Electrolytic capacitor, characterized in that in the first external electrode, a composite layer of the second sprayed electrode layer and the outer layer plating layer is provided inside the second sprayed electrode layer.
2. 2. The electrolytic capacitor according to claim 1, wherein the second external electrode has, in order from the second end face side of the resin molding, a first sprayed electrode layer and a second sprayed electrode layer in contact with the first sprayed electrode layer and having a higher porosity than the first sprayed electrode layer.
3. An electrolytic capacitor as described in claim 2, wherein the second external electrode further has an outer layer plating layer provided on the surface of the second sprayed electrode layer opposite the first sprayed electrode layer.
4. An electrolytic capacitor as described in Claim 3, wherein in the second external electrode, a composite layer of the second sprayed electrode layer and the outer layer plating layer is provided inside the second sprayed electrode layer.
5. 5. The electrolytic capacitor according to claim 1, wherein the outer plating layer and the second sprayed electrode layer contain the same metal as a main component.
6. 6. The electrolytic capacitor according to claim 1, wherein the outer plating layer contains copper, nickel, or tin as a main component.
7. 7. The electrolytic capacitor according to claim 2, wherein the first external electrode and the second external electrode each have an inner layer plating layer provided between the anode and the first sprayed electrode layer, and between the cathode and the first sprayed electrode layer.
8. The electrolytic capacitor according to claim 7 , wherein the inner plating layer contains copper, nickel, or silver as a main component.
9. 9. The electrolytic capacitor according to claim 1, wherein the first sprayed electrode layer and the second sprayed electrode layer contain the same metal as a main component.
10. 10. The electrolytic capacitor according to claim 9, wherein the first sprayed electrode layer and the second sprayed electrode layer each contain copper, nickel, or a nickel-aluminum alloy as a main component.
11. 11. The electrolytic capacitor according to claim 1, wherein a total thickness of the first sprayed electrode layer and the second sprayed electrode layer is 40 μm or more and 120 μm or less.
12. The anode contains aluminum as a main component, the first sprayed electrode layer and the second sprayed electrode layer of the first external electrode each contain copper as a main component, 2. The electrolytic capacitor according to claim 1, wherein the first external electrode has an inner plating layer that is provided between the anode and the first sprayed electrode layer and contains silver as a main component.
13. The anode contains aluminum as a main component, the first sprayed electrode layer and the second sprayed electrode layer of the first external electrode each contain nickel or a nickel-aluminum alloy as a main component, 2. The electrolytic capacitor according to claim 1, wherein the anode and the first sprayed electrode layer are in contact with each other.
14. 2 . The electrolytic capacitor according to claim 1 , wherein the second external electrode comprises a printed electrode layer provided on the second end surface of the resin molded body.
15. An electrolytic capacitor as described in claim 14, wherein the second external electrode has an outer layer plating layer provided on the surface of the printed electrode layer opposite the resin molded body.
16. a step of producing a rectangular parallelepiped resin molded body including a laminate having a capacitor element including an anode having a dielectric layer on a surface thereof and a cathode facing the anode, and a sealing resin that seals the periphery of the laminate; forming a first external electrode on a first end surface of the resin molded body, the first external electrode being electrically connected to the anode exposed from the first end surface; forming a second external electrode on a second end surface of the resin molded body, the second external electrode being electrically connected to the cathode exposed from the second end surface; In the step of forming the first external electrode, a first sprayed electrode layer and a second sprayed electrode layer that is in contact with the first sprayed electrode layer and has a higher porosity than the first sprayed electrode layer are formed in this order from the first end surface side by spraying the first end surface of the resin molded body, a first end face of the resin molded body having a first external electrode formed thereon, the first end face of the resin molded body being plated after the thermal spraying, thereby forming an outer layer plating layer on a surface of the second sprayed electrode layer opposite to the first sprayed electrode layer, while forming a composite layer of the second sprayed electrode layer and the outer layer plating layer inside the second sprayed electrode layer.
17. 17. The method for manufacturing an electrolytic capacitor according to claim 16, wherein in the step of forming the second external electrode, a first sprayed electrode layer and a second sprayed electrode layer in contact with the first sprayed electrode layer and having a higher porosity than the first sprayed electrode layer are formed in the order from the second end face side by spraying the second end face of the resin molded body.
18. A method for manufacturing an electrolytic capacitor as described in claim 17, wherein in the process of forming the second external electrode, a plating process is performed after the thermal spraying on the second end face of the resin molding, thereby forming an outer layer plating layer on the surface of the second sprayed electrode layer opposite the first sprayed electrode layer.
19. 19. The method for manufacturing an electrolytic capacitor according to claim 17 or 18, wherein in the step of forming the first external electrode and the step of forming the second external electrode, a plating process is performed on the first end face and the second end face of the resin molded body before the thermal spraying, thereby forming an inner layer plating layer between the anode and the first sprayed electrode layer, and between the cathode and the first sprayed electrode layer.
20. The method for producing an electrolytic capacitor according to any one of claims 16 to 19, wherein the thermal spraying is performed by plasma spraying.
Citation Information
Patent Citations
Laminated thin film capacitor
JP1992123413A
Laminated type solid electrolytic capacitor
JP1992188814A
Chip type solid electrolytic capacitor
JP2009076872A
Metallized film capacitor
JP2011249707A
Stacked film capacitor, capacitor module, and power conversion system
JP2015170695A