Air filter media including relofted spunbond webs and methods of making and using same
Relofted spunbond nonwoven webs with specific solidity and quality factors address the balance of low resistance and high efficiency in air filtration by breaking fiber-to-fiber bonds, enhancing filtration performance.
Patent Information
- Application Number
- JP2023000328
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-01-05
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2038-08-03
AI Technical Summary
Existing air filter media face challenges in achieving a balance between low air flow resistance and high particulate filtration efficiency, particularly in high-loft spunbond nonwoven webs, where improvements in quality factor and dust retention capacity are needed.
The development of relofted spunbond nonwoven webs with a solidity of less than 8.0% to 3.0% and a quality factor of at least 0.30, achieved through processes like needle punching or hydroentangling, which break existing fiber-to-fiber bonds to increase loft and enhance filtration properties.
The relofted webs exhibit significant reductions in air flow resistance while maintaining or slightly increasing permeability, resulting in improved quality factors and dust retention capacities, making them suitable for high-efficiency air filtration.
Smart Images

Figure 0007566057000003 
Figure 0007566057000004 
Figure 0007566057000005
Abstract
Description
[Background technology]
[0001] Air filter media is widely used to remove particulate matter from the air. Summary of the Invention
[0002] In a broad summary, disclosed herein is a relofted spunbond nonwoven web exhibiting a solidity of less than 8.0% to at least 3.0% and exhibiting a quality factor of at least 0.30. A method for producing the relofted web is also disclosed. Also disclosed is the use of the relofted web as an air filtration web, for example as a filter medium or layer of a filter medium. These and other aspects will become apparent from the detailed description that follows. However, this broad summary should not be construed to limit the subject matter that may be claimed, whether such subject matter is presented in the claims as originally filed in the application or in claims amended or otherwise presented during the prosecution process. [Brief description of the drawings]
[0003] [Figure 1] 1 is a scanning electron micrograph at 1250x magnification of a portion of an exemplary re-lofted spunbond nonwoven web viewed from the top. [Diagram 2] 4 is a scanning electron micrograph at 740x magnification of another portion of an exemplary re-lofted spunbond nonwoven web viewed from the top. [Diagram 3] 1 is an optical photograph at 20x magnification, viewed from the top, of a portion of an exemplary precursor spunbond nonwoven web from which a re-lofted web may be derived. [Figure 4] 1 is an optical photograph at 20x magnification of a portion of an exemplary re-lofted spunbond nonwoven web viewed from the top. [Diagram 5] FIG. 1 is a perspective view of a portion of an exemplary air filter media comprising a re-lofted spunbond nonwoven web as disclosed herein.
[0004] Like reference numbers in the various figures indicate like elements. Some elements may be presented in the same or equivalent plurals, i.e., even if only one or more representative elements may be designated by a reference number, such reference number shall be understood to apply to all such identical elements. Unless otherwise indicated, all figures and drawings in this document are not to scale and are selected for the purpose of illustrating different embodiments of the present invention. In particular, dimensions of various components are shown for illustrative purposes only, unless otherwise indicated, and no relationship between dimensions of various components should be inferred from the drawings. Terms such as "top", "bottom", "upper", "lower", "upper", "lower", "upper", "front", "rear", "outer", "inner", "upper" and "lower", as well as "first" and "second" may be used in this disclosure, but it should be understood that unless otherwise indicated, these terms are used in a relative sense only.
[0005] The term "generally," as used herein as a qualifier for a property or attribute, means that the property or attribute is readily discernible by one of ordinary skill in the art without a high degree of approximation (e.g., within + / - 20% for quantifiable properties), unless otherwise specified. The term "substantially," unless otherwise specified, means a high degree of approximation (e.g., within + / - 10% for quantifiable properties). The term "essentially" means a very high degree of approximation (e.g., within + / - 2% for quantifiable properties), while the phrase "at least essentially" will be understood to encompass certain instances of "exact" agreement. However, it will be understood that an "exact" agreement, or any other characterization using terms such as, for example, same, equal, identical, uniform, constant, etc., is within normal tolerances or measurement error applicable to a particular situation, rather than requiring absolute precision or perfect agreement. As used herein, terms such as "essentially free" do not exclude the presence of some very low, e.g., 0.1% or less, amounts of material, such as may occur, for example, when using large-scale manufacturing equipment that is subject to routine cleaning procedures. Terms such as "constituted by" are at least as restrictive as the term "adapted for" and require an actual design intent to perform a specified function, not merely a physical ability to do so. All references herein to numerical parameters (dimensions, proportions, etc.) are understood to be calculable using average values derived from multiple measurements of the parameters (unless otherwise specified). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0006] The term "spunbonded" refers to a nonwoven web composed of meltspun fibers, at least a portion of which exhibit fiber-to-fiber bonds, such as those provided by autogenous bonds as described herein below.
[0007] The term "meltspun" refers to fibers formed by extruding filaments through a set of orifices and allowing the filaments to cool and solidify to form fibers, where the filaments pass through an air space (which may include a moving air stream) to aid in cooling the filaments, and through an attenuation (i.e., drawing) unit to at least partially draw the filaments.
[0008] The term "solidity" refers to a dimensionless fraction (usually reported as a percentage) of a fibrous web that represents the percentage of the total volume occupied by solid (e.g., polymeric fiber) materials. Further explanations and methods for obtaining solidity can be found in the Examples section. Loft is 100% minus solidity, which represents the percentage of the total volume of the web that is not occupied by solid materials.
[0009] The term "quality factor" is a figure of merit relating to the overall performance of a filter media in filtering particles from the air, and is defined and discussed later in this specification.
[0010] The term "self-supporting" refers to a spunbond web (whether relofted or not) that exhibits sufficient mechanical integrity to be handled and subjected to conventional web handling processes (e.g., winding, unwinding, etc.).
[0011] Disclosed herein is an air filter medium comprising a relofted spunbonded nonwoven web exhibiting a solidity of less than 8.0% to at least 3.0% and a quality factor of at least 0.30. The term "spunbonded" refers to a nonwoven web made of meltspun fibers, at least some of which exhibit fiber-fiber bonding, such as provided by autogenous bonding as described herein below. The term "meltspun" refers to fibers formed by extruding filaments through a set of orifices and allowing the filaments to cool and solidify to form fibers, where the filaments pass through an air space (which may include a moving air stream) to aid in cooling the filaments, and through an attenuation (i.e., drawing) unit to at least partially stretch the filaments. Melt spinning can be distinguished from melt blowing in that melt blowing involves the extrusion of filaments into a converging high velocity air stream introduced by an air blowing orifice located in close proximity to the extrusion orifice.
[0012] The web 10 is a re-lofted spunbond web. The term "re-lofted" refers to a spunbond nonwoven web that has been subjected to a post-treatment process that increases the loft (reduces the solidity) of the spunbond nonwoven web. By definition, a re-lofted web is self-supporting as defined above. As will be discussed in detail later in this specification, a re-lofted spunbond web can be identified and distinguished from a spunbond web that has not been re-lofted by the presence of at least broken fiber-fiber bonds. Exemplary broken fiber-fiber bonds 12 of the fibers 11 of the re-lofted web 10 are indicated in the scanning electron micrographs presented in Figures 1 and 2.
[0013] It has been found that the re-lofting process imparts significant benefits, especially when performed on a spunbond precursor web that is already highly lofted (i.e., as manifested by a solidity of less than 10%). For example, the re-lofted spunbond web may exhibit a significant reduction (e.g., up to 50%) in airflow resistance (as manifested by pressure drop measurements, as discussed in the Examples section herein) compared to the precursor spunbond web. However, the re-lofted spunbond web may exhibit a much smaller increase in the ability of airborne particulates to pass through the web (as manifested by permeability measurements, as discussed in the Examples section herein). This advantageous combination of properties is expressed by the quality factor. The quality factor is a well-known figure of merit often used in air filter media, which takes into account both pressure drop and permeability, as discussed in the Examples section herein. It has been found that re-lofting a high loft spunbond web significantly improves (increases) the quality factor (e.g., up to a factor of 50, 70, or even 90% or more). This is a surprising result considering that high loft spunbond webs often exhibit relatively high quality factors to begin with.Furthermore, re-lofted spunbond webs have been found to have significantly improved dust holding capacity, as evidenced in the examples herein.
[0014] The relofted web 10 is produced by post-treating a precursor spunbond web 9. An exemplary precursor spunbond web 9 is shown in the optical photograph of FIG. 3. The precursor web 9 includes meltspun fibers 11. From the definition and description of meltspun fibers given above, it will be apparent that meltspun fibers and the resulting spunbond webs can be distinguished from meltblown webs (e.g., by the molecular orientation imparted to the meltspun fibers during the attenuation process). Meltspun fibers can also be distinguished from staple fibers, which are typically cut to a desired length, in contrast to meltspun fibers, which are typically continuous except for occasional statistical fiber breaks. Meltspun fibers and spunbond webs can also be distinguished from, for example, carded webs (which typically exhibit significant fiber alignment imparted by the carding process that is not present in spunbond webs), and even airlaid webs, wetlaid webs, and the like.
[0015] The meltspun fibers 11 can be made from any suitable organic polymeric material that can be meltspun. In various embodiments, such fibers can be composed of polyolefins (e.g., polypropylene, polyethylene, etc.), poly(ethylene terephthalate), nylon, and copolymers and / or blends of any of these. In some embodiments, at least some or all of the meltspun fibers 11 are monocomponent fibers. The term "monocomponent" refers to the organic polymeric material of the fiber and means a fiber in which a continuous phase of a homogeneous polymeric composition extends throughout the cross section and length of the fiber. In some advantageous embodiments, the monocomponent fiber can be a polypropylene fiber. The term monocomponent does not require that the organic polymeric component material is the only component of the fiber. Rather, in various embodiments, any suitable additives, such as one or more of antioxidants, plasticizers, processing aids, etc., can be present for any desired purpose. In certain embodiments, the fibers can include an electrostatic additive for the purpose of imparting a stable charge ("electret") to the fiber.
[0016] The monocomponent fibers as defined and described above exclude multicomponent fibers, such as bicomponent fibers. However, in alternative embodiments, at least some or all of the meltspun fibers 11 may be multicomponent fibers comprising at least two phases of different organic polymer compositions. Such fibers may have any suitable configuration selected from, for example, sheath-core, side-by-side, islands-in-the-sea, and the like. In some embodiments, such fibers may include at least one organic polymer phase having a composition that promotes or enhances bonding, e.g., melt bonding, of the meltspun fibers to one another. Multicomponent fibers may suitably include any of the additives described above, e.g., electrostatic additives, in at least one of the fiber phases.
[0017] Meltspun fibers may be produced (e.g., extruded, solidified, and attenuated) and collected using any suitable melt spinning method. In some embodiments, the apparatus and methods set forth in U.S. Pat. No. 8,240,484, the entirety of which is incorporated herein by reference, may be used. As detailed in the '484 patent, the approach disclosed herein allows for the formation of precursor meltspun webs exhibiting relatively high loft, as manifested, for example, by a solidity of less than 8.0%.
[0018] The meltspun fibers may have any suitable average diameter, for example, as determined by optical inspection of a statistically significant number of fibers. In various embodiments, the meltspun fibers may exhibit an average fiber diameter of at least 1, 2, 4, 6, 10, 15, or 20 microns. In further embodiments, the meltspun fibers may exhibit an average fiber diameter of at most 50, 40, 30, 25, 18, or 12 microns. In many embodiments, the meltspun fibers exhibit a monomodal fiber diameter distribution. That is, in such embodiments, the precursor web 9 and the re-lofted web 10 derived therefrom do not include a composite mixture exhibiting separate populations, for example, of fine and coarse fibers. (It is noted that, in general, fiber characteristics, such as, for example, fiber diameter, as described herein, are understood to apply to both the precursor web 9 and the re-lofted web 10 derived therefrom.)
[0019] The precursor web 9 (and the relofted web 10 derived therefrom) is a spunbond web, which means a web that contains at least some fiber-to-fiber bonds. Fiber-to-fiber bonds mean bonds (e.g., melt bonds) between a small number of fibers (typically five or less, most often two) where the fibers contact each other. In fiber-to-fiber bonds, each fiber substantially retains its individual characteristics (e.g., appearance and shape). By definition, fiber-to-fiber bonds are distinct from multi-fiber bonds, which may optionally be present and are discussed later in this specification, in which a large number of fibers are bonded to each other. In many embodiments, the fiber-to-fiber bonds are autogenous. This means fiber-to-fiber melt bonds obtained by subjecting a collection of melt-spun fibers to high temperatures (e.g., as achieved by using an oven and / or a controlled temperature air stream) without applying solid contact pressure on the web. In some embodiments, such bonding may be so-called through-air bonding, performed by directing heated air over and through the web, for example, by use of a controlled heating device as discussed in detail in U.S. Patent Application Publication No. 2008 / 0038976, which is incorporated herein in its entirety for this purpose. In certain embodiments, bonding may be performed by use of the apparatus and methods disclosed in U.S. Patent Application Publication No. 9,976,771, which is incorporated herein in its entirety for this purpose. It will be understood that autogenous bonding, e.g., through-air bonding, can bond fibers to one another to form a self-supporting web without significantly compressing or densifying the web (e.g., without crushing or otherwise significantly reducing the loft of the web). Thus, autogenous bonding and the resulting bonds are distinct from bonds performed by processes such as, for example, calendering, ultrasonic bonding, and the like. In some embodiments, the fiber-fiber bonds may be between monocomponent fibers (e.g., as described in the '771 patent). In other embodiments, the fiber-fiber bonds may be between specific components of multicomponent (e.g., bicomponent) fibers.
[0020] In some embodiments, the spunbond precursor web, and thus the relofted web derived therefrom, may optionally include (in addition to the fiber-fiber bonds described above) multi-fiber area-bonds of the type exemplified by bonds achieved by calendering, ultrasonic bonding, and the like. Exemplary calendered area-bonds 14 are visible in the optical photograph of FIG. 3. As is characteristic of such area bonds, each bond 14 appears to include a large number (e.g., 10 or more) of fiber segments that have been melted and solidified together over a relatively large area such that they have substantially lost their individual characteristics (appearance and shape) in the bonded area. In some embodiments, the spunbond web may include such area bonds at a relatively low concentration. Such a concentration may improve the mechanical integrity of the web without significantly adversely affecting the properties (e.g., filtration performance) of the web. In various embodiments, such area bonds may be present in the precursor web or relofted webs derived therefrom in an area percentage of the web that is greater than 0% but less than 5.0, 4.0, 3.0, 2.5, 2.0, 1.5, 1.0, or 0.5%. As a specific example, the web of Figure 3 includes multi-fiber area bonds that appear to be present in an area percentage estimated to be in the range of 1.3-1.5%.
[0021] In various embodiments, the precursor spunbond nonwoven web from which the re-lofted web is derived may exhibit a solidity of 10.0, 9.0, 8.0, or 7.0% or less (as an average value). In some embodiments, the precursor spunbond nonwoven web from which the re-lofted web is derived may include at least some fibers that have been imparted with an electric charge (e.g., a semi-permanent charge commonly referred to as an electret). In various embodiments, the web may be, for example, corona charged or hydrocharged. In such embodiments, it will be understood that any subsequent re-lofting process should be performed without unacceptably reducing the electret charge. Methods of charging fibers and webs, as well as additives that can improve the ability of fibers to accept and retain an electric charge, are disclosed, for example, in U.S. Pat. Nos. 8,613,795 and 8,790,449, and U.S. Patent Publication No. 2016 / 0206984, all of which are incorporated herein in their entirety for this purpose.
[0022] The relofting process disclosed herein may be carried out on any suitable spunbond web. Spunbond webs that may be particularly suitable include, for example, those of the general type described in US Patent Application Publication No. 20080038976 to Berrigan. If desired, any such medium may be charged to form an electret. In some embodiments, the spunbond web may be a high loft spunbond web. As used herein, this refers to a web that exhibits a solidity of less than 10.0%. Certain high loft spunbond webs (e.g., those with a solidity of less than 8.0%) that may be suitable for relofting, and methods of making such webs, are disclosed in US Patent No. 8,162,153 to Fox, which is incorporated herein by reference in its entirety.
[0023] The precursor spunbond web 9 is subjected to a reloft process to form a reloft web 10. As previously mentioned, the reloft process is a post-treatment step applied to a precursor spunbond web to increase the loft (reduce the solidity) of the web. In this process, a significant percentage (e.g., greater than 5%) of the fiber-fiber bonds are broken such that broken bonds 12 appear, for example, as in FIG. 1. Those skilled in the art will readily appreciate that in conventional handling and processing of spunbond webs, a small number of broken fiber-fiber bonds may occur. However, those skilled in the art of manufacturing and handling spunbond webs will readily appreciate that such a phenomenon, as may occur statistically from time to time in any practical web production process, is distinct from the current example of intentionally breaking a significant percentage of fiber-fiber bonds to increase the loft of the web.
[0024] A spunbond web can be identified as a reloft web by the presence of a significant number of broken fiber-to-fiber bonds. A reloft web may exhibit other identifying features. For example, in a reloft web, at least a portion of the fibers are physically moved, separated from one another, deformed, rearranged, etc., which may give the web a more fibrillated appearance. In other words, a reloft web may be visually "fluffier" than the precursor web from which it is derived. In fact, a reloft web may be "fluffier" than a typical spunbond web upon casual visual inspection.
[0025] Such characteristics may be particularly evident in embodiments in which the web includes optional multi-fiber area bonds. As evidenced by precursor web 9 as shown in Figure 3, in a typical spunbond web, any multi-fiber area bonds 14 are readily observable as flat areas where the fibers have lost their individual information within the area, with very few or no individual fibers overlying the bonded area. As shown in Figure 4, a re-lofted web derived from such a precursor web may have at least some of the precursor web fibers rearranged such that some or most of the area bonds are at least partially obscured by the overlying fibers.
[0026] In some cases, at least some of the fibers in the reloft web may exhibit characteristics (e.g., stress whitening, stress cracks, crazing, orientation, cross-sectional shrinkage, etc.) that indicate that the fibers have been subjected to significant shear commensurate with the reloft process. Thus, one skilled in the art will appreciate that a reloft spunbond web may be identified by any or all of several characteristics of the individual fibers and / or the web as a whole that result from the reloft process. As discussed below, spunbond webs that have been reloft by methods such as needle punching and / or hydroentangling may be readily identified as having been subjected to such processes by the presence of broken fibers visible (as item 15) in FIG. 2.
[0027] The relofting pattern and area coverage are such that the relofted web exhibits the desired properties in an overall manner averaged over a macroscopic (e.g., at least 10 square cm) area of the web. Thus, properties such as, for example, solidity, particle permeability, pressure drop, quality factor, etc., will be understood to be average properties obtained over a suitable macroscopic area of the relofted web. The term "relofted" requires that at least 30% of the area of the web is relofted, which may result in an overall improvement of, for example, quality factor throughout the web. In various embodiments, at least about 40, 60, 80, 90, 95, 98, or essentially 100% of the area of the web may be relofted. It will be understood that such area percentages are obtained from the ratio of the relofted area of the web (as defined by the perimeter of the relofted area) to the total area of the web.
[0028] In some embodiments, the relofting process may be accomplished by performing multiple localized impingements and penetrations of entities into and / or through the precursor web. In some embodiments, such a relofting process is a needlepunching process. Thus, references herein to relofted and needlepunched webs refer to webs that have been relofted by needlepunching, rather than webs that have been relofted and then needlepunched for some other purpose. Needlepunching refers to the process of penetrating multiple barbed needles into and / or through a mass of fibers and then withdrawing the needles so that the fibers become entangled. Those skilled in the art will appreciate that needlepunching is typically used as a method of mechanically interlocking fibers collected in dry processes such as, for example, carding, garnetting, airlaying (e.g., Landweber), etc. That is, needlepunching is generally considered as a process used to "bond" fibers together to form, for example, a self-supporting web. In contrast, in the present invention, as discussed earlier herein, needlepunching is applied to a nonwoven web that is already bonded and contains fiber-to-fiber bonds, i.e., in this case, needlepunching is used to break at least some of the pre-existing fiber-to-fiber bonds of the spunbond web, as evidenced by what appear to be broken or disrupted bonds 12 in the scanning electron micrograph of the needlepunched web shown in FIG.
[0029] Needle punching has previously been thought to break fibers, as evidenced by the broken fiber ends 15 in the scanning electron micrograph of a needle punched web shown in Figure 2. In fact, needle punching has been cited as adversely affecting filtration efficiency by creating perforations in the web (see, for example, the background art of U.S. Patent No. 7,015,158). It is therefore a surprising result that, in the present invention, needle punching has been found to be a convenient and successful method of re-lofting a spunbond nonwoven precursor web to result in an air filtration web that exhibits increased loft and superior filtration performance, as manifested, for example, by quality factor and dust holding capacity.
[0030] Needle punching can be performed in any suitable manner. Although each individual needle penetration may be considered to affect only a localized zone of the web, it has been found in the present invention that needle punching can be performed such that the needle punched areas collectively result in a re-lofted web (i.e., one or more areas that constitute at least 30% of the total area of the web). This re-lofted web exhibits relatively uniform properties across the length and width of the web or its re-lofted areas. Thus, in various embodiments, the web may be needle punched at a punch density of at least 4, 8, 12, 16, 20, 24, 30, 35, or 40 punches per square centimeter of web. For example, process and equipment parameters such as needle spacing / density, needle strike speed, and speed of advancing the web through the needle punching device can be adjusted as desired to achieve the desired loft increase as well as the desired uniformity. The web may be passed through the needle punch multiple times and / or may be needle punched from both sides of the web, for example, to further improve area uniformity, although this may not be required.
[0031] In some embodiments, the relofting process may be a hydroentangling process. Thus, references herein to relofted and hydroentangled webs refer to webs that have been relofted by hydroentangling, not webs that have been relofted and hydroentangled for some other purpose. Hydroentangling refers to the process of entangling fibers using very fine, high-velocity water jets (rather than barbed needles). Thus, the impinging / penetrating entity in hydroentangling is the water jet, and hydroentangling is sometimes referred to as "hydraulic needling". Those skilled in the art will appreciate that hydroentangling is often used (e.g., instead of needle punching) to mechanically "bond" fibers collected in a dry process, such as, for example, carding, garnetting, air laying (e.g., Landweber). In contrast, as disclosed herein, hydroentangling is applied to nonwoven webs that have already been bonded and contain fiber-fiber bonds, as discussed previously herein. That is, hydroentanglement is used to break at least some of the pre-existing fiber-to-fiber bonds of a spunbond web to result in an air filtration web with improved air filtration properties.
[0032] Hydroentanglement can be carried out in any suitable manner. Thus, for example, process and equipment parameters such as the spacing density of the water jets, the velocity and pressure of the water, the angle of impact of the water on the web, and the speed at which the web advances through the hydroentanglement device can be adjusted as desired. In particular, the density at which the water jets impact the spunbond web (e.g., as established by the spacing of the water jets and the speed at which the web passes through the hydroentanglement device) can be any suitable value, for example, at least 4, 8, 12, 16, 20, 24, 30, 35, or 40 impacts per square centimeter of web. The web can be passed through the hydroentanglement multiple times and / or can be hydroentangled from both sides of the web, if desired.
[0033] Those skilled in the art will appreciate that processes such as needle punching and hydroentangling can cause fiber entanglements that can act as physical "bonds". Such fiber entanglements can contribute to the integrity / self-supporting nature of the re-lofted web, even if a relatively small number of fiber-to-fiber bonds remain unbroken. However, in many embodiments, a large number of unbroken fiber-to-fiber bonds can still be present in such a re-lofted web.
[0034] The re-lofting process may be performed on any air filtration web for which it is desired to improve filtration performance. However, it has been found that the re-lofting process (however performed) is particularly suited to be performed on webs that already have a relatively high loft. That is, it has been found that re-lofting a high loft web significantly reduces the pressure drop through the web while having a small or negligible effect on the penetration of particles through the web. This results in a significant improvement in the quality factor. When re-lofting was performed on a relatively low loft web (e.g., solidity of 10% or more), the pressure drop was again significantly reduced, but the penetration of particles through the web increased significantly. Thus, the quality factor, which takes into account both of these factors, was not significantly improved.
[0035] Thus, the re-lofting process disclosed herein can use a relatively high loft web to increase the loft to even higher values. This can increase filtration parameters such as quality factor and dust holding capacity. In various embodiments, the precursor web that is re-lofted can exhibit a solidity of less than 10.0, 9.0, 8.0, 7.0, or 6.0%. In various embodiments, the re-lofting process can reduce the solidity by at least 0.1, 0.2, 0.5, 1.0, 1.5, 2.0, 2.5, or 3.0%. (This percentage is expressed relative to the actual solidity itself; i.e., if a precursor web with a solidity of 8.0% is relofted to have a solidity of 6.5%, this is a 1.5% reduction in solidity.) In various embodiments, the relofted web may exhibit a solidity of less than 9.0, 8.0, 7.0, 6.0, 5.0, or 4.0%. In further embodiments, the relofted web may exhibit a solidity of more than 1.0, 2.0, or 3.0%. It should be noted that a significant and useful increase in filtration performance as characterized by quality factor does not necessarily require a significant decrease in measured solidity. Thus, in some cases, a small decrease in solidity, for example, 0.2, 0.1, or even 0.05%, may nevertheless correspond to a useful increase in quality factor. In various embodiments, the re-lofted air filtration web may exhibit a quality factor of at least 0.5, 0.7, 1.0, 1.3, or 1.5.
[0036] The re-lofted web may be of any suitable basis weight. For example, in embodiments where the re-lofting process is a mechanical working process that has an all-over effect on the web, the basis weight may be slightly reduced from the basis weight of the precursor web, otherwise the basis weight may remain relatively unchanged. In various embodiments, the re-lofted web may exhibit a basis weight of 300, 200, 150, 100, 90, or 80 grams per square meter or less. In further embodiments, the re-lofted web may exhibit a basis weight of at least 30, 40, or 50 grams per square meter. It is noteworthy that re-lofting an already high loft air filtration web can significantly increase the dust holding capacity (e.g., by more than two times, as demonstrated in the examples herein) without the web having to have a high basis weight (e.g., 100 grams per square meter or more) or the web having deep embossed (e.g., bag-like) pockets. In various embodiments, the re-lofted air filtration web may exhibit a dust holding capacity of at least 30, 40, 50, or 60 grams per square meter.
[0037] As previously mentioned, in some embodiments, the relofted air filtration web 10 may be pleated. Thus, as shown in the exemplary embodiment of FIG. 5, the relofted air filtration web 10 may provide or be a layer of air filter media 1 that is pleated to include pleats 401 and pleat peaks 402. "Pleated" refers to a substrate (either single layer or multi-layer) that has at least a portion of it folded over itself to form a series of generally parallel, opposing creases, as will be well understood by those skilled in the art. Pleating an air filtration media typically serves to increase the total surface area of the media available within a nominal (planar projected) area. Pleating typically does not significantly change the inherent properties of the media, such as, for example, loft and particle permeability.
[0038] The pleat height and pleat spacing of the pleated web may be in any suitable range. The pleat height (pleat amplitude) is the distance from the upstream peak to the downstream peak along a direction perpendicular to the overall major plane of the pleated web. In various embodiments, the pleat height may be at least 4, 6, 8, 10, 12, 14, 16, 18, 20, 30, or 40 mm. In further embodiments, the pleat height may be at most 110, 90, 70, 50, 35, 25, or 14 mm. The pleat spacing is the distance between the nearest pleat peaks on the same side along a direction in the major plane of the filter media. In various embodiments, the pleat spacing may be at most about 30, 25, 20, 15, 12, 10, 8, 6, or 4 mm. In further embodiments, the pleat spacing may be at least about 3, 5, 7, 9, or 11 mm. The pleats may have any desired radius of curvature, for example, the pleats may have a relatively sinusoidal appearance, or the pleats may be relatively sharply tapered.
[0039] If desired, the pleated air filter media 1 (whether in the form of only the relofted air filtration web 10 or in the form of a multi-layer structure in which the web 10 is the filtration layer) may be stabilized in any suitable manner. This may be particularly useful, for example, where the relofting process appreciably reduces the stiffness of the media. Thus, for example, in some embodiments, the air filter media may comprise any suitable pleat-stabilizing item or items. Generally, such elements may take the form of members, strips, filaments, collections of filaments, cardboard sheets with holes, and the like. Such pleat-stabilizing elements may be in contact with (e.g., bonded to) only the peaks of the pleats (such as the exemplary support scrim 403 shown in FIG. 5), or the pleat-stabilizing elements may at least partially follow the pleats of the media and thus be bonded to the walls and / or valleys of the pleats as well. The former type of pleat-stabilizing elements may include, for example, paperboard strips, polymer strands, and the like. The latter types of pleat stabilizing elements may include, for example, chicken wire or chicken wire type metal grids (e.g., applied to the filter media and then pleated therewith), small beads of drizzle glue applied to the pleated media, filaments protruding from the media surface prior to pleating, and the like.
[0040] In some embodiments, the pleated media may be provided with bridging filaments bonded to the pleat peaks on the major side of the media such that they are in discontinuous contact with the pleated media. In some embodiments, the bridging filaments may be of the general type described in U.S. Provisional Patent Application No. 62 / 346179 and WO 2017 / 213926, both of which are incorporated herein in their entireties for this purpose. In some embodiments, the pleated media may be provided with continuous contacting filaments in continuous contact with the pleated media (i.e., pleated with the media). In some embodiments, the continuous contacting filaments may be of the general type described in U.S. Provisional Patent Application No. - / -, Attorney Docket No. 80992US002, entitled PLEATED AIR FILTER WITH REINFORCING FILAMENTS COMPRISING LOCALLY-THINNED BENDING ZONES, which is incorporated herein in its entirety for this purpose.
[0041] If desired, a perimeter support frame 404 may be attached to the major edges of the air filter media 1 (e.g., pleated air filter media 1) including the re-lofted air filtration web 10, for example as shown in an exemplary manner in FIG. 5. Portions of the frame 404 have been omitted in FIG. 5 to show the pleats 401, further emphasizing that FIG. 5 is an exemplary representation and that the particular features of the media 1 (e.g., the shape of the pleat peaks 402) may differ from those depicted. In many advantageous embodiments, the air filter media is rectangular (this term encompasses a square shape) and has four major edges to which the perimeter support frame is attached. Such a frame may provide support and rigidity so that the resulting framed air filter may be installed in a suitable location, such as in the return air duct of an HVAC system, in the compartment of an indoor air cleaner, etc.
[0042] Those skilled in the art will appreciate that high loft spunbond webs (especially very high loft webs, e.g., having a solidity of less than 6.0%) may be prone to compression, for example, when they are wound into bulk and held or stored in that state while awaiting further processing steps. Such compression may be long-term or permanent and may adversely affect filtration performance. However, it may be cumbersome to operate the melt spinning / bonding process directly in-line with the pleating and / or framing process. Thus, it may be difficult to produce a high loft spunbond web and feed it directly into the pleating and / or framing process so that the loft is maintained.
[0043] In contrast, it can be relatively simple to operate a re-lofting process (e.g., a needlepunch operation and / or a hydroentanglement operation) in-line with a pleating and / or framing process. Thus, in some embodiments, the process of re-lofting an air filtration web can be performed in-line with the process of pleating the web and / or the process of framing the web. This advantageously allows the re-lofted web to be input directly into the pleating and / or framing process without the need to reel the re-lofted web into any bulk.
[0044] The re-lofted webs disclosed herein are by definition air filtration webs. This means that the re-lofted webs are purposefully configured to perform particulate filtration of a moving gas stream, specifically, that the re-lofted webs exhibit a quality factor of at least 0.30. (All references to quality factor herein refer to the quality factor obtained by testing with dioctyl phthalate (DOP) unless otherwise specified.) Such re-lofted webs may function alone as air filtration media, or the re-lofted webs may be used as a filtration layer of a multi-layer air filtration media. Re-lofted air filtration webs are distinguished from nonwoven webs that are configured as absorbent materials to absorb liquids, for applications such as hygiene products, diaper construction materials, cleaning wipes, and the like. In particular, re-lofted air filtration webs that are electrically charged to improve their ability to capture particles from air streams are distinguished from webs that are configured to absorb liquids.
[0045] In certain embodiments, the relofted air filtration web (e.g., the charged web) is at least essentially free of hydrophilic fibers, powders, etc. (e.g., cellulosic pulp fibers that are often included in nonwoven webs to facilitate water absorption). As would be expected for an air filtration web, in at least some embodiments, the relofted air filtration web is free of any through holes, through slits, through openings, or generally free of any passageways that would allow airborne particles to pass through the web without encountering any fibers.
[0046] List of exemplary embodiments Embodiment 1 is an air filter media comprising a re-lofted spunbond nonwoven web exhibiting a solidity of less than 8.0% to at least 3.0% and a quality factor of at least 0.30, wherein the re-lofted spunbond nonwoven web is a needlepunched web, a hydroentangled web, or a needlepunched and hydroentangled web.
[0047] Embodiment 2 is the air filter media of embodiment 1, wherein the re-lofted web has a solidity of less than 7.0% to at least 4.0%.
[0048] Embodiment 3 is the air filter media of any one of embodiments 1-2, wherein the re-lofted web comprises at least some of the meltspun fibers that are electrically charged.
[0049] Embodiment 4 is the air filter media of any one of embodiments 1-3, wherein the re-lofted web comprises at least some of the meltspun fibers that are hydrocharged.
[0050] Embodiment 5 is the air filter media of any one of embodiments 1-4, wherein the re-lofted web comprises at least some of the electrically charged meltspun fibers that are monocomponent fibers.
[0051] Embodiment 6 is the air filter media of any one of embodiments 1-5, wherein the air filtration web has a quality factor of at least about 0.70.
[0052] Embodiment 7 is the air filter media of any one of embodiments 1-5, wherein the web has a quality factor of at least about 1.0.
[0053] Embodiment 8 is the air filter media of any one of embodiments 1-7, wherein the re-lofted web comprises fiber-to-fiber bonds and also comprises broken fiber-to-fiber bonds.
[0054] Embodiment 9 is the air filter media of any one of embodiments 1-8, wherein the re-lofted web comprises multiple fiber domain bonds present in an area percentage of 2.5% or less.
[0055] Embodiment 10 is the air filter media of any one of embodiments 1-9, wherein the reloft web is a pleated reloft web.
[0056] Embodiment 11 is the air filter media of any one of embodiments 1-10, further comprising a perimeter support frame attached to each of the four major edges of the air filter media.
[0057] Embodiment 12 is the air filter medium of any one of embodiments 1-11, wherein the web is a needle-punched web.
[0058] Embodiment 13 is the air filter medium of any one of embodiments 1-11, wherein the web is a hydroentangled web.
[0059] Embodiment 14 is a method of filtering an airflow stream comprising passing the airflow stream through the air filter media of any one of embodiments 1-13.
[0060] Embodiment 15 is a process for re-lofting a spunbond precursor web, comprising needlepunching and / or hydroentangling a spunbond precursor web having a solidity of 10% or less to produce a re-lofted spunbond air filtration web having a solidity of less than 8.0% to at least 3.0% and a quality factor of at least 0.30.
[0061] Embodiment 16 is the process of embodiment 15, wherein the re-lofting process is a needlepunch process.
[0062] Embodiment 17 is the process of embodiment 15, wherein the relofting process is a hydroentanglement process.
[0063] Embodiment 18 is the process of any one of embodiments 15-17, wherein the relofting process is performed in-line with a subsequent process of pleating the relofted spunbond air filtration web.
[0064] Embodiment 19 is the process of any one of embodiments 15-18, wherein the relofting process is performed in-line with a subsequent process of attaching a perimeter support frame to the main edges of the relofted spunbond air filtration web. EXAMPLES
[0065] Test Method Solidity and Loft Solidity is determined by dividing the measured bulk density of a nonwoven fibrous web by the density of the material that makes up the solid portion of the web. The bulk density of a web can be determined by first measuring the weight of the web (e.g., a 10 cm x 10 cm section). Dividing the measured weight of the web by the area of the web gives the basis weight of the web, expressed in g / m 2 The thickness of a web can be measured by obtaining (e.g., by die cutting) a disk of the web with a diameter of 135 mm and measuring the web thickness by placing a 230 g weight with a diameter of 100 mm centered on the web. The bulk density of a web is determined by dividing the basis weight of the web by the thickness of the web and is reported in g / m 3 It is reported as:
[0066] The solidity is then determined by dividing the bulk density of the nonwoven fibrous web by the density of the material (e.g., polymer) that makes up the solid filaments of the web. The density of the bulk polymer can be measured by standard means if the supplier does not specify the material density. Solidity is a dimensionless fraction that is usually reported as a percentage.
[0067] Loft is typically reported as 100% minus solidity (for example, 7% solidity equals 93% loft).
[0068] Permeability (%), Pressure Drop, and Quality Factor The (particle) penetration, pressure drop, and filtration quality factor (QF) of nonwoven fibrous webs are determined using a challenge aerosol containing DOP (dioctyl phthalate) droplets, delivered at a flow rate of 85 liters / min (unless otherwise indicated) resulting in a face velocity of 14 cm / sec, and evaluated using a TSI® Model 8130 high speed automated filter tester (available from TSI Inc., Shoreview, MN). For the DOP test, the aerosol may contain particles with a diameter of about 0.185 μm, and the automated filter tester may be operated with the heater off and the particle neutralizer on. Calibrated photometers at the inlet and outlet of the filter may be used to measure particle concentration and percent particle penetration through the filter. Pressure drop (ΔP, mmH2O) through the filter may be measured using an MKS pressure transducer (available from MKS Instruments, Wilmington, MA). To calculate QF, the equation: [ka] can be used to calculate the QF from the pressure drop and (particle) permeability.
[0069] Dust Holding Capacity (DHC) The dust holding capacity of a filter (as well as other filtration characteristics such as, for example, the capture efficiency, collection efficiency, and Minimum Efficiency Reporting Value (MERV) of the filter) is measured according to the general method in ASHRAE Standard 52.2 ("Method of Testing General Ventilation Air-Cleaning Devices for Removal Efficiency by Particle Size"). The dust holding capacity test involves configuring the web as a filter (e.g., a pleated and / or framed filter), placing the filter in a test duct, and subjecting the filter to an incremental dust loading step using synthetic dust as set forth in the ASHRAE 52.2 Standard. The dust holding capacity is the total weight of synthetic dust captured by the air filter sample throughout the entire incremental dust loading step. In this case, the samples tested for dust holding capacity were pleated as follows: Therefore, the dust holding capacity of all samples was normalized to the surface area of the air filter sample and is reported in grams of dust per square meter.
[0070] Working Example A high loft spunbond web was obtained. Melt spun fibers were produced and collected generally according to the procedures described in the Examples of US Patent No. 8,240,484. The collected fibers were self-bonded to form a self-supporting spunbond web generally according to the procedures described in US Patent No. 9,976,771, and further area bonded using a calendering process, which is the general approach described in the '484 patent. Area bonds were estimated to be present in an area percentage of the web of approximately 1.5-1.6%. The web was hydrocharged generally according to the procedures disclosed in US Patent Application Publication No. 2012 / 0017910. The web was obtained in two grades: Grade 55, which exhibits a basis weight of approximately 55 grams per square meter and a solidity of approximately 7.5, and Grade 75, which exhibits a basis weight of approximately 75 grams per square meter and a solidity of approximately 7.9. Both grades of material were obtained as flat web samples.
[0071] The flat web samples were re-lofted by needle punching. The needles were provided in 32 rows (in an up-punching configuration with an upper hole plate and a lower hole plate with a vertical spacing of approximately 50 mm between them). Each row spanned a horizontal (cross-web) width of 85 cm across, and the rows were spaced along a down-web extent of 28.5 cm. There were 104 needles in each row (so the needle spacing within a row was approximately 8 mm). The needles were of a common type available under the trade designation F20-9-28-7-B, Needle #5230160, 15x18x30x3.5RB by Foster Needle Co. (Manitowoc, WI). The web was passed through the needle puncher in a continuous fashion at a speed of approximately 1.5 meters per minute. As the web passed through the needle punch unit, it was needle punched at a rate of approximately 150 strokes per minute with a stroke depth of 60 mm. From these parameters, it was estimated that the web was punched at a density of approximately 40 punches per square centimeter of web material. Punching was done from one side only (the top side).
[0072] The increase in web loft was also significantly evident upon casual visual inspection: the relofted web was significantly thicker and "fuzzy" than the as-received web, and very few area bonded regions were still visible; rather, the area bonded regions appeared to be obscured by the fibers that covered them. The relofted web appeared to be very uniform in appearance.
[0073] The solidity and quality factors of these re-lofted samples are presented in Table 1 along with those of the as-obtained web. These were measured on flat web samples. Each data point is the average of multiple measurements. As noted herein, all such measurements were taken over a macroscopic area of the re-lofted web. Thus, the results are global values.
[0074] Dust Holding Capacity (DHC) for re-lofted Grade 55 samples is also included. For the DHC test, samples were pleated to form pleated filters with an overall (nominal) size of 16" x 20", a pleat height of 0.75", and a pleat density of approximately 1.1 pleats per inch. An "as is" (not re-lofted) Grade 55 control sample was similarly pleated. [Table 1]
[0075] As can be seen from Table 1, these re-lofted samples had an improvement in quality factor (% increase compared to the as-obtained sample) from approximately 70% to approximately 80%. The re-lofted sample (Grade 55) tested for dust holding capacity had a very significant improvement in dust holding capacity compared to the "as is" web.
[0076] change Other needle punch conditions The samples were needle punched at various punch densities estimated to range from approximately 30 punches per square cm to approximately 280 punches per square cm. Not all of these samples were characterized for quality factor or dust holding capacity. However, they appear to be physically similar to the samples above, and it was believed that they would perform at least generally similar to (or better than) the examples above.
[0077] Corona Charge A sample was obtained similar to grade 55, but exhibiting a basis weight of approximately 50, and was corona charged using methods conventional in the art, rather than hydrocharged. The sample was re-lofted by needle punching in a manner similar to that described above. The re-lofted sample exhibited a quality factor of approximately 1.0, compared to the as-obtained sample, which exhibited a quality factor of approximately 0.55.
[0078] The foregoing examples are presented for clarity of understanding only, and it is understood that no unnecessary limitations are to be implied by these examples. The tests and test results described in the examples are intended to be illustrative, not predictive, and variations in the test procedures can be expected to produce different results. All quantitative values in the examples are understood to be approximate, taking into account the known tolerances involved in the procedures used. It will be apparent to those skilled in the art that the specific exemplary elements, structures, features, details, configurations, etc. disclosed herein can be modified and / or combined in numerous embodiments. All such variations and combinations are considered by the inventors to be within the scope of the invention as conceived, and not merely representative designs selected to serve as illustrative examples. Thus, the scope of the present invention should not be limited to the specific exemplary structures described herein, but should extend to at least those structures described by the language of the claims and equivalents of those structures. Any elements positively described herein as alternatives may be expressly included or excluded from the claims in any combination as desired. Any of the elements or combinations of elements described herein with open-ended language (e.g., "comprising" and its derivatives) are considered to be further described with closed-ended language (e.g., "consisting of" and its derivatives) and partially closed-ended language (e.g., "consisting essentially of" and its derivatives). Various theories and possible mechanisms may be discussed herein, but such discussion is not intended to limit the claimed subject matter in any way. In the event of any conflict or inconsistency between the description of this specification and the disclosure of any document incorporated herein by reference, but no priority is claimed thereto, the description of this specification shall control.
Claims
1. A process for re-lofting a spunbond precursor web, comprising: needlepunching a spunbond precursor web having a solidity of 10% or less to produce a re-lofted spunbond air filtration web having a solidity of less than 8.0% to at least 3.0% and a quality factor of at least 0.30; Including, the spunbond precursor web comprises fiber-to-fiber bonds; needlepunching the spunbond precursor web to break some of the fiber-to-fiber bonds; A process wherein the re-lofting process is performed in-line with a subsequent process of pleating the re-lofted spunbond air filtration web.
2. A process for re-lofting a spunbond precursor web, comprising: needlepunching a spunbond precursor web having a solidity of 10% or less to produce a re-lofted spunbond air filtration web having a solidity of less than 8.0% to at least 3.0% and a quality factor of at least 0.30; Including, the spunbond precursor web comprises fiber-to-fiber bonds; needlepunching the spunbond precursor web to break some of the fiber-to-fiber bonds; A process wherein the re-lofting process is performed in-line with a subsequent process of attaching a perimeter support frame to the major edges of the re-lofted spunbond air filtration web.
Citation Information
Patent Citations
JP1974031966A
Production of napped especially , light weight flexible fleece material
JP1982042950A
Oil-adsorbable filter material
JP1995051518A
Aligned web filter with pleats
JP2007531617A
High loft spunbond web
JP2012532255A