Aluminum alloy extrusions
A controlled Cr, Fe, and Si aluminum alloy extrusion forms a corrosion-resistant oxide film using corrosion as a driving force, addressing the limitations of conventional methods by enhancing durability and recyclability.
Patent Information
- Application Number
- JP2023221426
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-12-27
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-12-27
AI Technical Summary
Conventional corrosion prevention methods for aluminum alloys are expensive, uneven application can lead to corrosion, and may reduce recyclability, while Zn thermal spraying has environmental concerns, necessitating a highly corrosion-resistant single-layer aluminum alloy solution.
An aluminum alloy extrusion containing controlled amounts of Cr, Fe, and Si, with specific intermetallic compound distributions, forms a Cr-containing oxide film using corrosion as a driving force for enhanced corrosion resistance.
The alloy achieves long-lasting corrosion resistance without multilayer treatments, maintaining material integrity and recyclability, while preventing corrosion product clogging and appearance issues.
Smart Images

Figure 0007566121000001 
Figure 0007566121000002 
Figure 0007566121000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an aluminum alloy extrusion material. [Background technology]
[0002] Aluminum is known as a metal with relatively good corrosion resistance, but when it is exposed to a salty environment, the oxide film breaks down and corrosion occurs. In this case, corrosion tends to progress in the thickness direction of the material, penetrating the material in a relatively short time and causing defects such as a decrease in material strength and leakage of contents. For this reason, some kind of corrosion prevention treatment is necessary when using aluminum. Common corrosion prevention methods include surface treatment using a coating with excellent environmental resistance, and a method of extending the lifespan by controlling the corrosion pattern to a planar shape using Zn spraying and diffusion treatment.
[0003] Patent Document 1 discloses a method for producing a laminated metal material, in which a surface treatment agent is applied to the surface of an aluminum alloy to form an oxide film having corrosion resistance, and then a resin film is laminated onto the oxide film. Patent Document 2 discloses an extruded material of an aluminum-zinc alloy, on which an anodized coating is formed that exhibits excellent corrosion resistance even in an environment in which water vapor is present. Patent Document 3 discloses a tube made of a hollow extruded aluminum material, the surface of which is formed of a diffusion layer of a metal that is less noble than the tube (aluminum). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] WO2011 / 052520 paragraph (0062)~(0069) [Patent Document 2] JP2014-037557A, paragraph (0001) [Patent Document 3] JP 2004-324998 A, paragraph (0057) Summary of the Invention [Problem to be solved by the invention]
[0005] Although conventional corrosion prevention methods have excellent performance, surface treatments and multi-layer materials are expensive. In addition, uneven application of surface treatments can lead to corrosion. There is also a risk of corrosion occurring if the product is scratched by external factors during use in the market. In addition, from the perspective of realizing a carbon-neutral society, which has been attracting attention in recent years, there is also the issue that surface treatment and Zn thermal spraying reduce recyclability. For these reasons, it was necessary to develop a highly corrosion-resistant aluminum alloy that could be used as a single layer without using such corrosion prevention methods.
[0006] SUMMARY OF THE PRESENT EMBODIMENT An object of the present invention is to provide an aluminum alloy having high corrosion resistance. [Means for solving the problem]
[0007] The inventors discovered that, when manufacturing an extruded material made of an aluminum alloy to which Cr, Fe, and Si have been added, the manufacturing conditions are controlled to densely distribute Cr-containing compounds, and even if corrosion occurs on the alloy surface, the corrosion acts as a driving force to cover the corroded areas with a highly corrosion-resistant film containing Cr, thereby suppressing the progression of corrosion.
[0008] The aluminum alloy extrusion material of the present invention contains 0.05% by mass or more and 1.00% by mass or less of Cr, 0.05% by mass or more and 1.00% by mass or less of Fe, 0.05% by mass or more and 1.50% by mass or less of Si, with the balance being Al and unavoidable impurities, in which Fe and Si satisfy the relationship 0.8Fe≦Si, and an intermetallic compound containing Cr having a circle equivalent diameter of 0.01 μm or more and less than 5.00 μm is formed within a range of 10,000 μm in an ED-TD parallel plane. 2 The present invention is characterized in that there are 10 or more intermetallic compounds per observation field, and further, there are less than 3 intermetallic compounds per observation field having an equivalent circle diameter of 10 μm or more. ED is the extrusion direction, and TD is the transverse direction perpendicular to ED and the thickness direction (normal direction). The ED-TD parallel plane is a plane parallel to ED and TD that is formed by scraping the surface of the extruded material.
[0009] Cr: 0.05 mass% or more and 1.00 mass% or less Cr densely distributes compounds that contain Cr, and when the compounds are decomposed by slight corrosion, Cr concentrates on the surface of the alloy and forms an oxide film containing Cr with excellent corrosion resistance in the corroded area, improving the corrosion resistance of the alloy. If the Cr content is less than 0.05 mass%, sufficient corrosion resistance (formation of a highly corrosion-resistant oxide film containing Cr) cannot be obtained, and if it exceeds 1.00 mass%, coarse intermetallic compounds are formed during casting, reducing extrudability.
[0010] Fe: 0.05% by mass or more and 1.00% by mass or less Fe is distributed as intermetallic compounds such as Al-Fe and Al-Fe-Si, but by adjusting the manufacturing conditions of these compounds containing Fe, it is possible to dope Cr into the Fe sites, and to densely distribute the intermetallic compounds containing Cr. If the Fe content is less than 0.05 mass%, the manufacturing cost will be high, and if it exceeds 1.00 mass%, coarse intermetallic compounds will be generated during casting, reducing extrudability.
[0011] Si: 0.05 mass% or more and 1.50 mass% or less When Si is contained together with Fe, it favors the formation of Al-Fe-Si intermetallic compounds, which have a smaller cathodic reaction than Al-Fe intermetallic compounds, and forms a highly corrosion-resistant oxide film containing Cr against minor corrosion, improving the corrosion resistance of the alloy. If the Si content is less than 0.05 mass%, a sufficient effect (the formation of a highly corrosion-resistant oxide film containing Cr) cannot be obtained, and if the Si content exceeds 1.50 mass%, the solidus temperature drops and molten metal leaks occur during casting.
[0012] (Relationship between Fe and Si content) Fe and Si have a relationship of 0.8Fe≦Si in terms of mass % in the composition of the aluminum alloy (hereinafter referred to as the relational formula). By satisfying the above relational expression, the formation of Al-Fe-Si intermetallic compounds, which have a smaller cathodic reaction than Al-Fe intermetallic compounds, can be favored, and a highly corrosion-resistant oxide film containing Cr against minor corrosion can be formed, improving the corrosion resistance of the alloy. If the relational expression is not satisfied, the formation of Al-Fe compounds becomes favored, and the corrosion resistance decreases.
[0013] (Distribution of fine intermetallic compounds) ED-TD parallel surface 10000μm 2 Within an observation field per unit area, there are 10 or more intermetallic compounds containing Cr having an equivalent circle diameter of 0.01 μm or more and less than 5.00 μm. By densely distributing fine intermetallic compounds containing Cr, when the intermetallic compounds containing Cr are decomposed by minor corrosion, Cr is concentrated on the surface layer of the alloy, forming an oxide film containing Cr with excellent corrosion resistance in the corroded area, thereby improving the corrosion resistance of the alloy. 2 If the number of particles per observation field is less than 10, it is not possible to form an oxide film containing Cr.
[0014] (Distribution of coarse intermetallic compounds) ED-TD parallel surface 10000μm 2 There are less than three intermetallic compounds with a circle equivalent diameter of 10 μm or more in the observation field per unit area. If a large number of coarse intermetallic compounds having an equivalent circle diameter of 10 μm or more are distributed, they will act as starting points for corrosion and further inhibit the formation of an oxide film containing Cr, thereby reducing the corrosion resistance of the alloy.
[0015] (Corrosion resistance after SWAAT test) The corroded area of the test material subjected to the SWAAT test (Sea Water Acidified Test: conforming to ASTM G85-A) for 24 hours contains Cr in the film. The minor corrosion acts as a driving force to produce a Cr-containing film, improving the corrosion resistance of the alloy.
[0016] The aluminum alloy extruded material of the present invention preferably contains Ti in an amount of 0.05% by mass or more and 1.00% by mass or less. Ti can reduce the progression of corrosion in the thickness direction by distributing layers with different Ti concentrations through the peritectic reaction during casting and the extrusion process. If Ti is less than 0.05 mass%, the improvement in corrosion resistance is low. If Ti is more than 1.00 mass%, coarse intermetallic compounds are formed during casting, reducing extrudability. The aluminum alloy extrusion material of the present invention may further contain any one or more of the following elements: Mn, Mg, Cu, Zr, V, Sr, Sc, and Mo.
[0017] The aluminum alloy extrusion material of the present invention preferably contains 0.10 mass % or more and 2.00 mass % or less of Mn. Mn precipitates as intermetallic compounds such as Al-Mn, Al-Mn-Si, and Al-Mn-Si-Fe compounds, and can improve the material strength of aluminum alloy extrusions. If the Mn content is less than 0.10% by mass, the effect of improving the material strength is low, and if the Mn content exceeds 2.00% by mass, coarse intermetallic compounds are generated during casting, resulting in reduced extrudability.
[0018] The aluminum alloy extruded material of the present invention preferably contains 0.01% by mass or more and 3.00% by mass or less of Mg. Mg is dissolved or Mg 2 It precipitates as an intermetallic compound such as Si, and can improve the material strength of the aluminum alloy extrusion material. If the Mg content is less than 0.01% by mass, the effect of improving the material strength is low, whereas if the Mg content exceeds 3.00% by mass, the material strength of the aluminum alloy extrusion material is too high, making material manufacturing (extrusion) difficult.
[0019] The aluminum alloy extrusion material of the present invention preferably contains Cu in an amount of 0.01% by mass or more and 1.00% by mass or less.
[0020] Cu can improve the material strength of aluminum alloy extrusions through solid solution. If the Cu content is less than 0.01 mass %, the effect of improving the material strength is low, whereas if the Cu content exceeds 1.00 mass %, the material strength of the aluminum alloy extrusion material is too high, making it difficult to manufacture (extrude) the material.
[0021] The aluminum alloy extrusion material of the present invention preferably contains any one or more of the elements Zr, V, Sr, Sc and Mo in an amount of 0.01% by mass or more and 0.50% by mass or less for each element. Zr, V, Sr, Sc, and Mo form intermetallic compounds and can improve the material strength of aluminum alloy extrusions. If the content of Zr, V, Sr, Sc, or Mo is less than 0.05% by mass, the effect of improving the material strength is low, and if the content of Zr, V, Sr, Sc, or Mo exceeds 0.50% by mass, coarse intermetallic compounds are generated during casting, reducing extrudability. Effect of the Invention
[0022] In the aluminum alloy extrusion material of the present invention, intermetallic compounds containing Cr are densely distributed, and a highly corrosion-resistant coating containing Cr is produced using slight corrosion as a driving force, making it possible to maintain corrosion resistance for a long period of time. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] The extruded material according to an embodiment of the present invention contains 0.05% by mass to 1.00% by mass of Cr, 0.05% by mass to 1.00% by mass of Fe, 0.05% by mass to 1.50% by mass of Si, and the balance being Al and unavoidable impurities.
[0024] Cr: 0.05 mass% or more and 1.00 mass% or less Cr densely distributes compounds that contain Cr, and when the compounds are decomposed by slight corrosion, Cr concentrates on the surface of the alloy and forms an oxide film containing Cr with excellent corrosion resistance in the corroded area, improving the corrosion resistance of the alloy. If the Cr content is less than 0.05 mass%, sufficient corrosion resistance (formation of a highly corrosion-resistant oxide film containing Cr) cannot be obtained, and if it exceeds 1.00 mass%, coarse intermetallic compounds are formed during casting, reducing extrudability.
[0025] Fe: 0.05% by mass or more and 1.00% by mass or less Fe is distributed as intermetallic compounds such as Al-Fe and Al-Fe-Si, but by adjusting the manufacturing conditions, it is possible to dope Cr into the Fe sites of these compounds containing Fe, and to densely distribute the intermetallic compounds containing Cr. If the Fe content is less than 0.05% by mass, the manufacturing cost will increase, and if it exceeds 1.00% by mass, coarse intermetallic compounds will form during casting, reducing extrudability.
[0026] Si: 0.05 mass% or more and 1.50 mass% or less When Si is contained together with Fe, it favors the formation of Al-Fe-Si compounds, which have a smaller cathodic reaction than Al-Fe compounds, and forms an oxide film containing Cr against minor corrosion, improving the corrosion resistance of the alloy. If the Si content is less than 0.05 mass%, a sufficient effect (the formation of a highly corrosion-resistant oxide film containing Cr) cannot be obtained, and if the Si content exceeds 1.50 mass%, the solidus temperature drops and molten metal leaks occur during casting.
[0027] (Relationship between Fe and Si content) Fe and Si have a relationship of 0.8Fe≦Si in terms of mass % in the composition of the aluminum alloy (hereinafter referred to as the relational formula). By satisfying the above relational expression, the formation of Al-Fe-Si compounds, which have a smaller cathodic reaction than Al-Fe compounds, can be made dominant, and an oxide film containing Cr can be formed against minor corrosion, improving the corrosion resistance of the alloy. If the relational expression is not satisfied, the formation of Al-Fe compounds becomes dominant, and the corrosion resistance decreases.
[0028] The extruded material according to the embodiment of the present invention may contain any one or more of Ti, Mn, Mg, Cu, Zr, V, Sr, Sc, and Mo.
[0029] The aluminum alloy extrusion material preferably contains Ti in an amount of 0.05% by mass to 1.00% by mass. Ti can reduce the progression of corrosion in the wall thickness direction by distributing layers with different Ti concentrations through the peritectic reaction during casting and the extrusion process. If Ti is less than 0.05 mass%, the improvement in corrosion resistance is low. An aluminum alloy extrusion material with Ti exceeding 1.00 mass% preferably contains Mn at 0.10 mass% to 2.00 mass%.
[0030] The aluminum alloy extrusion material preferably contains 0.10 mass % or more and 2.00 mass % or less of Mn. Mn precipitates as intermetallic compounds such as Al-Mn, Al-Mn-Si, and Al-Mn-Si-Fe compounds, and can improve the material strength of aluminum alloy extrusions. If the Mn content is less than 0.10% by mass, the effect of improving the material strength is low, and if the Mn content exceeds 2.00% by mass, coarse intermetallic compounds are generated during casting, resulting in reduced extrudability.
[0031] The aluminum alloy extrusion material preferably contains 0.01% by mass or more and 3.00% by mass or less of Mg. Mg can be precipitated as a solid solution or as an intermetallic compound such as Mg2Si, thereby improving the material strength of the aluminum alloy extrusion material. If the Mg content is less than 0.01% by mass, the effect of improving the material strength is low, and if the Mg content exceeds 3.00% by mass, the material strength of the aluminum alloy extrusion material will be too high, making material manufacturing (extrusion processing) difficult.
[0032] The aluminum alloy extrusion material preferably contains Cu in an amount of 0.01% by mass to 1.00% by mass. Cu can improve the material strength of aluminum alloy extrusions through solid solution. If the Cu content is less than 0.01% by mass, the effect of improving the material strength is low, whereas if the Cu content exceeds 1.00% by mass, the material strength of the aluminum alloy extrusion material is too high, making material manufacturing (extrusion processing) difficult.
[0033] The aluminum alloy extrusion preferably contains any one or more of the elements Zr, V, Sr, Sc and Mo in an amount of 0.01% by mass or more and 0.50% by mass or less for each element. Zr, V, Sr, Sc, and Mo form intermetallic compounds and can improve the material strength of aluminum alloy extrusions. If the content of Zr, V, Sr, Sc, or Mo is less than 0.05% by mass, the effect of improving the material strength is low, and if the content of Zr, V, Sr, Sc, or Mo exceeds 0.50% by mass, coarse intermetallic compounds are generated during casting, reducing extrudability.
[0034] (Distribution of fine intermetallic compounds) ED-TD parallel surface 10000μm 2 In the observation field per 100 mm, there are 10 or more intermetallic compounds containing Cr, each having a circle equivalent diameter of 0.01 μm or more and less than 5.00 μm. ED is the extrusion direction, TD is the transverse direction perpendicular to ED and the thickness direction (ND), and the ED-TD parallel plane is the plane parallel to ED and TD formed by scraping the surface of the extruded material.
[0035] By densely distributing fine intermetallic compounds containing Cr, when the intermetallic compounds containing Cr are decomposed by minor corrosion, Cr is concentrated on the surface layer of the alloy, forming an oxide film containing Cr with excellent corrosion resistance in the corroded area, thereby improving the corrosion resistance of the alloy. 2 If the number of particles per observation field is less than 10, it is not possible to form an oxide film containing Cr.
[0036] (Distribution of coarse intermetallic compounds) ED-TD parallel surface 10000μm 2 There are less than three intermetallic compounds with a circle equivalent diameter of 10 μm or more in the observation field per unit area. If a large number of coarse intermetallic compounds having an equivalent circle diameter of 10 μm or more are distributed, they will act as starting points for corrosion and further inhibit the formation of an oxide film containing Cr, thereby reducing the corrosion resistance of the alloy.
[0037] (Corrosion of aluminum alloy extrusions) In aluminum alloy extrusions, intermetallic compounds containing Cr are densely distributed, and slight corrosion is the driving force for the formation of a film containing Cr. This Cr-containing oxide film has high corrosion resistance. The condition for confirming the oxide film is to carry out a SWAAT test (Sea Water Acidified Test: conforming to ASTM G85-A) for 24 hours on a test material made of an aluminum alloy of the above composition. After the SWAAT test, corroded areas are generated on the test material, and surface analysis of these corroded areas is carried out in the thickness direction by X-ray photoelectron spectroscopy (hereinafter referred to as XPS). This XPS measurement is carried out by dividing the sputtering time by the SiO 2 Measurements are taken every 1.2 nm in depth (converted into depth), and the oxide film is defined as the area from the surface to the depth direction where the concentrations (intensity) of O and Al are reversed (O>Al on the surface side), and the presence or absence of Cr is confirmed at any measurement point in the oxide film. If Cr is present, a peak appears near 574 eV.
[0038] (Manufacturing method) The method for manufacturing an aluminum alloy extrusion material includes an ingot manufacturing process for manufacturing an ingot, a homogenization process for homogenizing the ingot, and an extrusion process for extruding the ingot.
[0039] (Ingot manufacturing process) The ingot manufacturing process involves producing ingots (slabs) by melting and casting. The ingot is made of an aluminum alloy containing 0.05% by mass to 1.00% by mass of Cr, 0.05% by mass to 1.00% by mass of Fe, 0.05% by mass to 1.50% by mass of Si, and the balance being Al and unavoidable impurities. This aluminum alloy may contain any one or more of Ti, Mn, Mg, Cu, Zr, V, Sr, Sc, and Mo. The aluminum alloy preferably contains 0.05% by mass to 1.00% by mass of Ti. The aluminum alloy preferably contains 0.10% by mass to 2.00% by mass of Mn. The aluminum alloy preferably contains 0.01% by mass to 3.00% by mass of Mg. The aluminum alloy preferably contains 0.01% by mass to 1.00% by mass of Cu. The aluminum alloy preferably contains any one or more of the elements Zr, V, Sr, Sc, and Mo in an amount of 0.01% by mass or more and 0.50% by mass or less for each element. The casting temperature is 700°C or higher and lower than 790°C, and preferably 730°C or higher and lower than 770°C. If the casting temperature is lower than 700°C, the time spent in the crystallization temperature range during casting is long, and coarse intermetallic compounds are generated that cannot be sufficiently crushed in the extrusion process. If the casting temperature is higher than 790°C, production becomes impossible due to molten metal leakage. The cooling rate is 0.1° C. / s or more, and preferably 1° C. / s or more. If the cooling rate during casting is less than 0.1° C. / s, the time spent in the crystallization temperature range during casting is long, and coarse intermetallic compounds that cannot be sufficiently crushed during the extrusion process are generated.
[0040] (homogenization process) In the homogenization step, the ingot is heated to 400° C. or more and less than 600° C., and is maintained in this state, preferably at 430° C. or more and less than 580° C. The holding time is 1 hour or more and 12 hours or less, preferably 3 hours or more and 10 hours or less. Heat treatment of the ingot at a specified temperature causes the precipitation of Al-Fe and Al-Fe-Si intermetallic compounds, and also promotes Cr doping into the Fe sites. If the temperature is less than 400°C, a sufficient effect (homogenization) cannot be obtained, whereas if the temperature is 600°C or higher, the precipitates become coarse or re-dissolve, resulting in a sparse distribution.
[0041] (Extrusion process) The extrusion process is a hot extrusion process. During extrusion, friction between the aluminum and the die generates processing heat, causing the material temperature to rise. The maximum temperature reached during extrusion is, for example, less than 620°C, and preferably less than 580°C. If the temperature exceeds 620°C, the distribution becomes sparse due to the coarsening of the compounds and re-dissolution. The extrusion speed is 0.5 m / s or more, and preferably 0.8 m / s or more. By setting the extrusion speed to 0.5 m / s or more, processing stress can be applied to the material, making it possible to crush coarse intermetallic compounds.
[0042] Through the extrusion process, an aluminum alloy extrusion material made of the aluminum alloy having the above composition is completed. In the manufacturing method of the extruded material, solution treatment, aging treatment, and brazing heat treatment are performed as necessary.
[0043] In the manufacturing method of the aluminum alloy extrusion material according to the embodiment of the present invention, an aluminum alloy containing Cr and an adjusted content ratio of Fe and Si is used as a raw material, and the manufacturing conditions of casting, homogenization, and extrusion temperature are controlled to predominantly generate compounds with small cathodic reactions and suppress coarse crystallized products, thereby preventing the coarse intermetallic compounds from becoming the starting point of corrosion and preventing the formation of a Cr-containing coating.
[0044] In the aluminum alloy extrusion material according to the embodiment of the present invention, fine intermetallic compounds containing Cr are densely distributed, and when the fine intermetallic compounds containing Cr are decomposed by micro-corrosion, an oxide film containing the decomposed Cr and having high corrosion resistance is formed, which allows the aluminum alloy extrusion material to be used for a long period of time even in a single layer. Forming the surface of a conventional aluminum alloy as an anodized film or using a multi-layer material containing a sacrificial anticorrosive material results in high costs. In addition, if the surface treatment is unevenly applied, corrosion may occur. There is also a risk of corrosion occurring if scratches are given due to external factors during use in the market. When Zn spraying is used, corrosion of the sacrificial anode material inevitably occurs due to sacrificial corrosion protection, and if the corrosion products clog the flow path of the device or adhere to the material surface of the device, the performance of the device may be reduced and the appearance of the device may be damaged. In addition, in the case of use such as an air conditioner indoor unit, the corrosion products scatter, which is undesirable. Furthermore, conventional surface treatments and multi-layer materials reduce recyclability. On the other hand, according to the extrusion material according to the embodiment of the present invention, the generation of corrosion products can be suppressed by forming an oxide film containing Cr using corrosion as a driving force, and clogging of the flow path can be prevented, and the function and appearance of the material surface can be maintained well. The extruded material is formed, for example, into a cylindrical shape and used as a piping material, a tube for a heat exchanger, or the like. EXAMPLES
[0045] The corrosion resistance of extruded materials produced by extrusion molding using different materials and manufacturing conditions was evaluated.
[0046] (material) The materials used in the production were one containing Cr, Fe, Si with the balance being Al and unavoidable impurities, and one containing Cr, Fe, Si with the balance being Al and unavoidable impurities, with Ti added. Materials 1 to 9 contain 0.05 mass% or more and 1.00 mass% or less of Cr, 0.05 mass% or more and 1.00 mass% or less of Fe, 0.05 mass% or more and 1.50 mass% or less of Si, and the balance is Al and unavoidable impurities, with the Fe and Si contents satisfying the relationship 0.8Fe≦Si. Materials 10 to 12 contain Cr from 0.05 mass% to 1.00 mass%, Fe from 0.05 mass% to 1.00 mass%, Si from 0.05 mass% to 1.50 mass%, Ti from 0.05 mass% to 1.00 mass%, the balance being Al and unavoidable impurities, and the Fe and Si contents satisfy the relationship 0.8Fe≦Si. Hereinafter, the range of Cr from 0.05 mass% to 1.00 mass%, the range of Fe from 0.05 mass% to 1.00 mass%, the range of Si from 0.05 mass% to 1.50 mass%, and the range of Ti from 0.05 mass% to 1.00 mass% may all be referred to as a first composition range. Materials 35 and 36 contain Cr from 0.05% to 1.00% by mass, Fe from 0.05% to 1.00% by mass, Si from 0.05% to 1.50% by mass, Ti outside the range of 0.05% to 1.00% by mass, the balance being Al and unavoidable impurities, and the Fe and Si contents satisfy the relationship 0.8Fe≦Si. Materials 28 to 33 are materials in which the content of any of Cr, Fe, Si, and Ti is not controlled within the first composition range, and among these, material 32 is a material in which the content of Fe and Si does not satisfy the relationship of 0.8Fe≦Si. Material 34 is a material in which the content of Cr, Fe, and Si is controlled within the first composition range, but the content of Fe and Si does not satisfy the relationship of 0.8Fe≦Si. Table 1 shows the mass percentages of Cr, Fe, Si, and Ti for each material, and the relationship 0.8Fe≦Si.
[0047] [Table 1]
[0048] (Manufacturing method) The manufacturing method of the extruded material includes an ingot manufacturing process for manufacturing an ingot, a homogenization process for homogenizing the ingot, and an extrusion process for extruding the ingot.
[0049] (Ingot manufacturing process) The ingot manufacturing process involves producing ingots (slabs) by melting and casting. The casting temperature is 700°C or higher and lower than 790°C. The cooling rate is 0.1°C / s or more.
[0050] (homogenization process) In the homogenization process, the ingot is heated to a temperature of 400° C. or higher and lower than 600° C. and held for 5 hours.
[0051] (Extrusion process) The extrusion process is a hot extrusion process. During extrusion, friction between the aluminum and the die generates processing heat, causing the material temperature to rise. The maximum temperature reached during extrusion is less than 620°C. The extrusion speed is 0.5 m / s or more.
[0052] The casting temperature, casting cooling rate, homogenization temperature, extrusion temperature, and extrusion rate for each manufacturing method are shown in Table 2. In manufacturing methods A to G, the casting temperature, casting cooling rate, homogenization temperature, extrusion temperature, and extrusion rate are controlled within the above-mentioned ranges, and in manufacturing methods H to L, any of the casting temperature, casting cooling rate, homogenization temperature, extrusion temperature, and extrusion rate is outside the above-mentioned ranges.
[0053] [Table 2]
[0054] Extrusions of aluminum alloys were produced using materials (any of materials 1-12, 28-36) and manufacturing conditions (any of manufacturing methods A-L) to give samples 1-12, 28-36, 41-52, 68-76, 81-100, and 121-130, and the number of compounds, corrosion weight loss, and corrosion depth were measured for each of samples 1-12, 28-36, 41-52, 68-76, 81-100, and 121-130. The extrusions were formed in a cylindrical shape, and their cross sections were rectangular with a length of 1.3 mm and a width of 18.0 mm, and the thickness of each part of the cross section was 0.3 mm.
[0055] A. Number of compounds (distribution state) A thin film was prepared by mechanically polishing and electrolytically polishing a cut-out piece from the sample, and a 10,000 μm thin film was observed on the ED-TD parallel surface using a TEM (transmission electron microscope). 2 The fine compounds and coarse compounds were measured using an observation field of view of 100 μm square. The presence or absence of Cr in the compounds was determined by composition analysis using EPMA for compounds larger than 1 μm and EDS for compounds smaller than 1 μm. Fine compounds are intermetallic compounds having a circle-equivalent diameter of 0.01 μm or more and less than 5.00 μm. Coarse compounds are intermetallic compounds having a circle-equivalent diameter of more than 10 μm. Tables 3 and 4 show the number of fine compounds and coarse compounds.
[0056] B. Film analysis of corroded areas of extruded materials The coatings in the corroded areas of the test specimens subjected to the SWAAT test for 24 hours were analyzed. The specimens cut from the extrusions were subjected to the SWAAT test for 24 hours, washed with pure water, and thoroughly dried. The XPS measurement of the surface layer of the specimens was then carried out to determine whether or not Cr was present in the coating. When Cr was detected in the coating, it was rated as good, and when it was not detected, it was rated as bad. Tables 3 and 4 show the results of the coating analysis for each sample, with A indicating good and C indicating bad. The SWAAT test is a cyclic test using 5% NaCl with a pH of 3 as the corrosive solution, with one cycle consisting of spraying at 50°C for 30 minutes and wetting at 50°C for 90 minutes. XPS measurement is the time for sputtering SiO 2 Measurements were taken every 1.2 nm (converted to a depth), and the oxide film was defined as the portion from the surface to the depth direction where the concentrations of O and Al reversed (O>Al on the surface side). The presence or absence of Cr was determined at any measurement point in the oxide film (if Cr was present, a peak would appear at around 574 eV). Samples 1 to 9, 28 to 49, 68 to 90, and 121 to 130 shown in Table 3 are made of aluminum alloys that do not contain Ti, and samples 10 to 12, 35, 36, 50 to 52, 75, 76, and 91 to 100 shown in Table 4 are made of aluminum alloys that contain Ti.
[0057] C. Corrosion loss A test piece of 80 mm length was cut out from the cylindrical extrusion material, and the outer peripheral surface was protected by masking within a range of 180 degrees around the central axis and the end of the cylinder, while the unmasked parts of the outer peripheral surface were exposed and subjected to a corrosion test. The corrosion test was performed in a SWAAT test for 1320 hours, and the weight change (corrosion weight loss) before and after the corrosion test was evaluated. The corrosion weight loss was 5.0 mg / cm 2 A corrosion weight loss of less than 5.0mg / cm is considered good. 2 More than 10.0mg / cm 2 Less than 10.0 mg / cm is considered to be slightly better. 2 Tables 3 and 4 show the evaluation of corrosion weight loss for each of Samples 1 to 12, 28 to 36, 41 to 52, 68 to 76, 81 to 100, and 121 to 130, with A indicating good, B indicating fairly good, and C indicating poor.
[0058] D. Corrosion depth After the specimens cut from the extrusions were loaded for 1320 hours by SWAAT, the corrosion depth of the specimens was evaluated. In this evaluation, the deepest corroded area on the exposed surface of the specimen was identified using a non-contact step gauge, and then the specific area was embedded in resin and polished to expose the cross section. The thinnest thickness t1 of the specimen after corrosion was measured by observation, and the difference between this and the thickness t0 of the specimen measured before the SWAAT test was taken as the corrosion depth (=t0-t1). A corrosion depth of less than 60μm was considered good, 60μm to 120μm was considered fair, and 120μm or more was considered poor. Tables 3 and 4 show the evaluation of the corrosion depth of each of Samples 1 to 12, 28 to 36, 41 to 52, 68 to 76, 81 to 100, and 121 to 130, with A indicating good, B indicating fairly good, and C indicating poor.
[0059] E. Evaluation of corrosion resistance The corrosion resistance of the samples was evaluated from the corrosion weight loss and the corrosion depth. When both the corrosion weight loss and the corrosion depth were evaluated as good (A), the sample was evaluated as good, when one was good (A) and the other was somewhat good (B) or when both were somewhat good (B), the sample was evaluated as somewhat good, and when either was poor (C), the sample was evaluated as poor. Tables 3 and 4 show the evaluations of the corrosion resistance of each of the samples 1 to 12, 28 to 36, 41 to 52, 68 to 76, 81 to 100, and 121 to 130, with A being good, B being somewhat good, and C being poor.
[0060] [Table 3]
[0061] [Table 4]
[0062] As shown in Table 3, samples 1-9, 41-49, and 81-85 contain Cr at 0.05% by mass or more and 1.00% by mass or less, Fe at 0.05% by mass or more and 1.00% by mass or less, Si at 0.05% by mass or more and 1.50% by mass or less, and the balance is Al and unavoidable impurities, and the contents of Fe and Si satisfy the relationship of 0.8Fe≦Si. They were manufactured by any of manufacturing methods A to G in which the manufacturing conditions of casting, homogenization treatment, and extrusion processing (extrusion temperature and extrusion speed) were controlled. As a result, compounds with small cathodic reactions were predominantly generated, and fine intermetallic compounds containing Cr were densely distributed, and coarse crystallized products were suppressed thereon. Furthermore, it was confirmed that the corrosion weight loss was small and the corrosion depth was shallow in the corroded part of the surface layer, and an oxide film containing Cr was formed by decomposition of the intermetallic compounds, and the corrosion resistance was good.
[0063] As shown in Table 4, samples 10-12, 35, 50-52, 75, and 91-95 contain Cr from 0.05% to 1.00% by mass, Fe from 0.05% to 1.00% by mass, Si from 0.05% to 1.50% by mass, Ti from 0.05% to 1.00% by mass, and the balance is Al and unavoidable impurities. The materials 10-12 and 35 in which the Fe and Si contents satisfy the relationship of 0.8Fe≦Si were manufactured by one of manufacturing methods A to G in which the manufacturing conditions of casting, homogenization treatment, and extrusion processing (extrusion temperature and extrusion speed) were controlled. As a result, compounds with small cathodic reactions were predominantly generated, fine intermetallic compounds containing Cr were densely distributed, and coarse crystallized products were suppressed. Furthermore, in the corroded portion of the surface layer, the corrosion loss was small, the corrosion depth was shallow, and an oxide film containing Cr was formed by decomposition of the intermetallic compound, and it was confirmed that the corrosion resistance was good. Although Samples 35 and 75 used Material 35 having a Ti content lower than the first composition range, it was confirmed that the corrosion resistance was good.
[0064] Samples 28-31, 33, 68-73, 121-125 were produced by using any of materials 28-31 and 33 in which the content of any of Cr, Fe, and Si was outside the first composition range, and by any of production methods A-G in which the production conditions of casting, homogenization, and extrusion (extrusion temperature, extrusion speed) were controlled. Samples 32 and 72 were produced by using material 32 in which the content of Si was outside the first composition range and the content of Fe and Si did not satisfy the relationship of 0.8Fe≦Si, and by any of production methods A and G in which the production conditions of casting, homogenization, and extrusion (extrusion temperature, extrusion speed) were controlled. Samples 34 and 74 were produced as extrusion materials by using material 34 in which the contents of Cr, Fe, and Si were within the first composition range, but the content of Fe and Si did not satisfy the relationship of 0.8Fe≦Si, and by any of production methods A and G in which the production conditions of casting, homogenization, and extrusion (extrusion temperature, extrusion speed) were controlled. Regardless of the control of the manufacturing conditions of casting, homogenization, and extrusion (extrusion temperature, extrusion speed), it was confirmed that the corrosion resistance is low when the content of any of Cr, Fe, and Si is outside the first composition range, or when the content of Fe and Si does not satisfy the relationship of 0.8Fe≦Si. In addition, samples 29, 31, 33, 69, 71, and 73 are materials 29, 31, and 33 in which the content of any of Cr, Fe, and Si is outside the first composition range, and are manufactured by manufacturing methods A and G, respectively, and were not evaluated for corrosion resistance because they are difficult to manufacture. Samples 30 and 70 are materials 30 with a low Fe content, and are manufactured by manufacturing methods A and G, respectively, and were not evaluated for corrosion resistance because they are expensive.
[0065] Samples 126 to 130 were produced by using material 28 having a Cr content outside the first composition range and by one of production methods H to L in which the production conditions of casting, homogenization treatment, and extrusion processing (extrusion temperature and extrusion speed) were not controlled. It was confirmed that the corrosion resistance of the extruded material is low if the production conditions of casting, homogenization treatment, and extrusion processing (extrusion temperature and extrusion speed) are not controlled. Samples 86 to 90 are material 1 containing 0.05% to 1.00% by mass of Cr, 0.05% to 1.00% by mass of Fe, 0.05% to 1.50% by mass of Si, and the remainder being Al and unavoidable impurities, with the Fe and Si contents satisfying the relationship 0.8Fe≦Si, produced by one of production methods H to L in which the production conditions of casting, homogenization treatment, and extrusion processing (extrusion temperature and extrusion speed) are not controlled. It was confirmed that the corrosion resistance of the extruded material is low unless the production conditions of casting, homogenization treatment, and extrusion processing (extrusion temperature and extrusion speed) are controlled.
[0066] Samples 96 to 100 are materials 10 containing 0.05% by mass or more and 1.00% by mass or less of Cr, 0.05% by mass or more and 1.00% by mass or less of Fe, 0.05% by mass or more and 1.50% by mass or less of Si, 0.05% by mass or more and 1.00% by mass or less of Ti, and the balance being Al and unavoidable impurities, and the contents of Fe and Si satisfy the relationship of 0.8Fe≦Si, which are manufactured by one of manufacturing methods H to L in which the manufacturing conditions of casting, homogenizing treatment, and extrusion processing (extrusion temperature and extrusion speed) are not controlled. It was confirmed that the corrosion resistance is low unless the manufacturing conditions of casting, homogenizing treatment, and extrusion processing (extrusion temperature and extrusion speed) are controlled.
[0067] Samples 36 and 76 are extruded materials manufactured from material 36, which contains 0.05% by mass or more and 1.00% by mass or less of Cr, 0.05% by mass or more and 1.00% by mass or less of Fe, 0.05% by mass or more and 1.50% by mass or less of Si, has a Ti content outside the first composition range, and the remainder is Al and unavoidable impurities, and has an Fe and Si content that satisfies the relationship 0.8Fe≦Si, by either manufacturing method A or G, which controls the manufacturing conditions of casting, homogenization treatment, and extrusion processing (extrusion temperature, extrusion speed).Since the Ti content is high and manufacturing is difficult, corrosion resistance was not evaluated. EXAMPLES
[0068] The tensile strength Rm of extruded materials produced using different materials and manufacturing conditions was evaluated.
[0069] (material) The material used to manufacture the extruded material contained Cr, Fe, Si, as well as one or more of the following elements: Ti, Mn, Mg, Cu, Zr, V, Sr, Sc, and Mo, with the remainder being Al and unavoidable impurities. Materials 13 to 27 contain 0.05% to 1.00% by mass of Cr, 0.05% to 1.00% by mass of Fe, 0.05% to 1.50% by mass of Si, the remainder being Al and unavoidable impurities, and the Fe and Si contents satisfy the relationship 0.8Fe≦Si. Materials 13 to 27 also contain 0.05% to 1.00% by mass of Ti, 0.10% to 2.00% by mass of Mn, 0.01% to 3.00% by mass of Mg, 0.01% to 1.00% by mass of Cu, and 0.01% to 0.50% by mass of any one or more of Zr, V, Sr, Sc, and Mo. Hereinafter, the range of 0.10 mass % or more and 2.00 mass % or less of Mn and the range of 0.01 mass % or more and 3.00 mass % or less of Mg may both be referred to as a second composition range. In the materials 37 to 40, the content of either Mn or Mg is outside the second composition range. Table 5 shows the mass percentages of Cr, Fe, Si, Ti, Mn, Mg, Cu, Zr, V, Sr, Sc, and Mo for each of materials 13 to 27 and 37 to 40, and the relationship between the mass percentages of Fe and Si and 0.8Fe≦Si.
[0070] [Table 5]
[0071] (Manufacturing method) The manufacturing method of the extruded material includes an ingot manufacturing process for manufacturing an ingot, a homogenization process for homogenizing the ingot, and an extrusion process for extruding the ingot. The production method is any one of Production Methods A to L in Table 2 above.
[0072] Extruded materials were produced using the material (any of materials 13-27, 37-40) and manufacturing conditions (any of manufacturing methods A-L) to give samples 13-27, 37-40, 53-67, 77-80, and 101-120, and the strength of each of samples 13-27, 37-40, 53-67, 77-80, and 101-120 was measured. The extrusion material was a pipe material with an inner diameter of 27 mm and an outer diameter of 30 mm, and a test piece according to the tensile test method for metallic materials (JIS Z2241:2011) No. 13B was cut out from this pipe material to measure the tensile strength Rm. Tensile strength Rm of 140 MPa or more was judged as good, 100 MPa or more but less than 140 MPa was judged as fair, and less than 100 MPa was judged as poor. In Table 5, the tensile strength Rm of each of the samples 13 to 27, 37 to 40, 53 to 67, 77 to 80, and 101 to 120 is represented as A for good, B for fair, and C for poor. Furthermore, the measurement of the number of compounds, the film analysis in the corroded parts of the extruded material, and the evaluation of corrosion weight loss, corrosion depth, and corrosion resistance, which were performed in Example 1, were also performed on each of the samples 13 to 27, 37 to 40, 53 to 67, 77 to 80, and 101 to 120 in Example 2, and these measurement values and evaluations are also shown in Table 6.
[0073] [Table 6]
[0074] Samples 13-27, 53-67, and 101-120 were made of any of the materials 13-27 in which the contents of Cr, Fe, Si, Ti, Mn, Mg, Cu, Zr, V, Sr, Sc, and Mo were all controlled to the second composition range, and their tensile strength Rm was good or somewhat good. Among these, samples 13-27, 53-67, 101-105, and 111-115 were made by any of the manufacturing methods A to G in which the manufacturing conditions of casting, homogenization treatment, and extrusion processing (extrusion temperature and extrusion speed) were controlled, and it was confirmed that the corrosion weight loss was small and the corrosion depth was shallow in the corroded part of the surface, and an oxide film containing Cr was formed by decomposition of the intermetallic compound, and the corrosion resistance was good or somewhat good. Samples 106 to 110 and 116 to 120 were produced by Production Methods H to L in which no control was performed on any of the production conditions of casting, homogenization treatment, and extrusion processing (extrusion temperature and extrusion speed), and had poor corrosion resistance.
[0075] Samples 37-40, 77-80 are produced by using any one of the materials 37-40, in which the content of either Mn or Mg is not controlled within the second composition range, and by using any one of the production methods A and G. Among these, samples 37, 39, 77, and 79 had poor tensile strength Rm, but the corrosion resistance was somewhat good because the production conditions of casting, homogenization treatment, and extrusion processing (extrusion temperature and extrusion speed) were controlled. Samples 38, 40, 78, and 80 are produced by using any one of the production methods A and G using materials 38 and 40, in which the content of either Mn or Mg exceeds the second composition range, and were not produced due to poor extrudability.
Claims
1. The alloy contains 0.05% by mass or more and 1.00% by mass or less of Cr, 0.05% by mass or more and 1.00% by mass or less of Fe, 0.05% by mass or more and 1.50% by mass or less of Si, and the balance being Al and inevitable impurities; Fe and Si satisfy the relationship 0.8Fe≦Si, An intermetallic compound containing Cr having a circle equivalent diameter of 0.01 μm or more and less than 5.00 μm is formed on a 10,000 μm area of an ED-TD parallel plane defined as follows: 2 There are 10 or more per observation field, The extruded aluminum alloy material is further characterized in that there are less than three intermetallic compounds having an equivalent circle diameter of 10 μm or more in the observation field. Here, ED is the extrusion direction, TD is the transverse direction perpendicular to the ED and the thickness direction (normal direction), and the ED-TD parallel plane is a plane parallel to the ED and TD that is formed by scraping the surface of the extruded material.
2. 2. The aluminum alloy extrusion material according to claim 1, further comprising 0.05% by mass or more and 1.00% by mass or less of Ti.
3. 3. The aluminum alloy extrusion material according to claim 1 or 2, further comprising any one or more of the following elements: Mn: 0.10% by mass or more and 2.00% by mass or less; Mg: 0.01% by mass or more and 3.00% by mass or less; Cu: 0.01% by mass or more and 1.00% by mass or less; Zr: 0.01% by mass or more and 0.50% by mass or less; V: 0.01% by mass or more and 0.50% by mass or less; Sr: 0.01% by mass or more and 0.50% by mass or less; Sc: 0.01% by mass or more and 0.50% by mass or less; and Mo: 0.01% by mass or more and 0.50% by mass or less.
Citation Information
Patent Citations
Heat exchanger, its manufacturing method, and tube for heat exchanger
JP2004324998A
Extruded aluminum alloy tube for heat exchanger, heat exchanger and method for manufacturing the tube
JP2007070699A
6,000 series aluminum alloy hollow extruded material having excellent high temperature expanded tube formability
JP2011195912A
Structure using aluminum alloy extruded material, and method for joining the same
JP2012040609A
Aluminum-zinc based alloy extrusion material and method for producing teh same
JP2014037557A
Cited By
Preparation method of aluminum alloy reflector bar
CN120571878A
Extruded tube with inner surface straight grooves and tube with inner surface spiral grooves
JP2026061809A
Internally linearly grooved extruded tube stock and internally helically grooved tube
WO2026071246A1