Superconducting coil and method for manufacturing the same
The superconducting coil design with a release material layer and conductive resin part addresses thermal runaway and diameter issues, ensuring stable magnetic field generation and improved mechanical strength.
Patent Information
- Application Number
- JP2021080194
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-05-11
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2041-05-11
AI Technical Summary
Superconducting coils face issues with thermal runaway due to normal conductivity transitions, increased coil diameter, and insufficient electromagnetic force resistance, which affect their stability and magnetic field generation capabilities.
A superconducting coil design featuring a superconducting wire with a tape-shaped metal substrate, a reinforcing wire, and a conductive resin part with a release material layer to reduce adhesion, allowing current diversion and improved mechanical strength, while maintaining a smaller coil diameter.
The design effectively prevents thermal runaway, enhances electromagnetic force resistance, and stabilizes the coil to generate a strong magnetic field without increasing the coil diameter.
Smart Images

Figure 0007566688000001 
Figure 0007566688000002 
Figure 0007566688000003
Abstract
Description
[Technical field]
[0001] SUMMARY OF THE PRESENT EMBODIMENT An embodiment of the present invention relates to a superconducting coil. [Background technology]
[0002] Superconducting wire has a range of current density, temperature and magnetic field that can maintain the superconducting state, i.e., a critical current density, critical temperature and critical magnetic field. Therefore, even if the wire is in a superconducting state and the electrical resistance becomes almost zero, it does not mean that the current can flow infinitely. When any of the current density, temperature and magnetic field exceeds these critical values, the wire transitions to a normal conducting state. When a current flows through the point where the wire has transitioned to a normal conducting state, the temperature of the coil rises due to Joule heat, and there is a risk of thermal runaway that burns the superconducting wire. The burned superconducting wire will not return to a superconducting state even if it is cooled again, so it will be impossible to restore it as a superconducting coil. Therefore, measures are required to prevent thermal runaway in superconducting coils.
[0003] Therefore, if the superconducting wires of different turns of a superconducting coil are short-circuited between the turns, the current flowing through the part that has transitioned to normal conductivity can be diverted to the superconducting wires of the different turns. By diverting the current through the part that has transitioned to normal conductivity, it is possible to suppress localized heat generation in the part that has transitioned to normal conductivity. In addition, by detecting changes in the voltage or magnetic field of the superconducting coil caused by the current diverting through the part that has transitioned to normal conductivity and reducing the current flowing before thermal runaway occurs, the superconducting coil can be protected from thermal runaway.
[0004] In addition, the superconducting coil generates an electromagnetic force in the superconducting wire due to the magnetic field generated by itself or an external magnetic field. In particular, the electromagnetic force in the direction of expansion in the coil radial direction becomes a tensile stress in the longitudinal direction (circumferential direction), so-called hoop stress, for the superconducting wire. In order to withstand the hoop stress caused by such a strong magnetic field, for example, in the case of REBCO wire (high-temperature superconducting wire), an oxide superconducting layer is formed on a substrate of a high-strength metal such as Hastelloy (registered trademark) or Ni-based alloy such as NiW. However, in a superconducting magnet that generates a strong magnetic field exceeding 10 T, a hoop stress that exceeds the distortion that the superconducting wire can tolerate is generated. Therefore, a technology is known in which a reinforcing wire such as a metal tape is wound around the superconducting wire to share the hoop stress, thereby suppressing the hoop stress to below the distortion that the superconducting wire can tolerate. In order to further improve the mechanical strength of the superconducting coil, it is necessary to use a reinforcing wire with a larger thickness. However, this causes the thickness between the coil turns to increase. For example, when manufacturing a superconducting coil with the same number of turns, the coil diameter will be larger than that of a conventional superconducting coil.Similarly, when manufacturing a superconducting coil with the same coil diameter, the number of turns of the superconducting wire will be smaller than that of a conventional superconducting coil, and the magnetic field that can be generated will be smaller.
[0005] In view of this, a conventional technique is known in which the side surfaces of the superconducting coil and the gaps between the superconducting wires forming the superconducting coil are impregnated with a conductive resin to electrically connect different turns of superconducting wires in the radial direction. Here, insulating tape and a conductive member are wound in layers between the superconducting wires. There is also a release treatment method for releasing the wide surfaces of the superconducting wires and the reinforcing wires. As a release treatment method, a technique is known in which an insulating wire bonded or coated with a fluororesin or the like is used. In addition, a release material that has good releasability from the superconducting wires or the reinforcing wires is used.
[0006] In this conventional technology, when a normal conductive transition occurs in a superconducting wire, a part of the current flowing through the superconducting wire flows to another superconducting wire through the conductive resin and the conductive member. Therefore, it is expected to have an effect of preventing thermal runaway of the superconducting coil. In addition, by inserting a release material between the turns to weaken the adhesive strength between adjacent superconducting wires, the peeling stress generated on the surface of the superconducting wire due to the difference in thermal contraction rate between the impregnated resin and the superconducting wire can be reduced, and peeling deterioration of the superconducting wire can be prevented. In addition, by using a high-strength reinforcing wire made of metal as the conductive member, the mechanical strength of the superconducting coil can be improved. However, in order to obtain such an effect, insulating tape, reinforcing wire, insulating wire bonded or coated with fluororesin, etc., and a conductive resin layer filled between them must be interposed between the superconducting wires, which increases the coil diameter.
[0007] Another conventional technique is a superconducting coil made of superconducting wires, a release tape, and a resin layer formed between them. However, the release tape and the layer of impregnated resin are formed between the superconducting wires, which increases the coil diameter. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] JP 2020-25014 A [Patent Document 2] Patent No. 5395870 [Patent Document 3] International Publication No. 2020 / 067335 Summary of the Invention [Problem to be solved by the invention]
[0009] The problem that the present invention aims to solve is to provide a superconducting coil that can suppress the occurrence of thermal runaway during the normal conducting transition of the superconducting wire while avoiding an unnecessary increase in the coil diameter, and can improve the electromagnetic force resistance performance to stably generate a strong magnetic field. [Means for solving the problem]
[0010] A superconducting coil according to an embodiment of the present invention comprises a superconducting wire having a superconducting layer made of a superconducting material on one of the two surfaces of a tape-shaped metal substrate, a reinforcing wire made of a tape-shaped metal material wound together with the superconducting wire, and a conductive resin part having conductivity impregnated between the superconducting wire and the reinforcing wire, and at least one of the two surfaces of the reinforcing wire is coated with a release material layer that weakens the adhesion between the reinforcing wire and the conductive resin part more than other parts. Effect of the Invention
[0011] According to an embodiment of the present invention, a superconducting coil is provided that can suppress the occurrence of thermal runaway during the normal conducting transition of the superconducting wire while preventing an unnecessary increase in the coil diameter, and can improve the electromagnetic force resistance performance to stably generate a strong magnetic field. [Brief description of the drawings]
[0012] [Figure 1] FIG. 1 is a perspective view showing a superconducting coil according to a first embodiment. [Diagram 2] Cross-sectional view taken along line II-II in FIG. [Diagram 3] FIG. [Figure 4] FIG. [Diagram 5] FIG. [Figure 6] FIG. [Figure 7] FIG. 2 is a cross-sectional view showing the superconducting coil of the first embodiment. [Figure 8] FIG. 3 is a cross-sectional view showing a superconducting coil of Comparative Example 1. [Figure 9]FIG. 4 is a cross-sectional view showing a superconducting coil of Comparative Example 2. [Figure 10] 4 is a cross-sectional view showing superconducting coils of Comparative Examples 3 and 4. FIG. [Figure 11] 4 is a flowchart showing a method for manufacturing a superconducting coil. [Figure 12] FIG. 4 is a cross-sectional view showing a superconducting coil according to a second embodiment. [Figure 13] FIG. 11 is a cross-sectional view showing a reinforcing wire according to a third embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] (First embodiment) Hereinafter, embodiments of a superconducting coil and a method for manufacturing a superconducting coil will be described in detail with reference to the drawings. First, a first embodiment will be described with reference to FIGS.
[0014] Reference numeral 1 in Fig. 1 denotes a superconducting coil according to the first embodiment. The superconducting coil 1 described below may use either a high-temperature superconducting wire or a low-temperature superconducting wire, and will exhibit high effectiveness with either wire. However, the following description will be exemplified by the case where a high-temperature superconducting wire that exhibits particularly high effectiveness is used.
[0015] As shown in FIGS. 1 and 2, a superconducting coil 1 of the first embodiment includes a spool 10, a winding portion 11, a conductive resin portion 12, and an insulating plate 13.
[0016] The winding portion 11 is formed by winding one tape-shaped superconducting wire 20 (FIG. 4) and one tape-shaped reinforcing wire 40 (FIG. 5) around a cylindrical winding frame 10.
[0017] Superconducting coil 1 has a central hole 2 (space) penetrating the center of the winding axis. In this embodiment, a direction parallel to the winding axis of winding portion 11 is referred to as coil axis direction 3, a direction in which superconducting wire 20 is wound is referred to as coil circumferential direction 4, and a direction in which superconducting wire 20 is layered by winding is referred to as coil radial direction 5.
[0018] For example, the winding portion 11 is formed in a pancake shape by concentrically winding the superconducting wire 20 and the reinforcing wire 40. Such a coil is called a pancake coil. In this embodiment, a so-called single pancake coil formed in the shape of one pancake is illustrated. Note that this embodiment can also be applied to a so-called double pancake coil formed in the shape of two pancakes. However, the following description illustrates the case where a single pancake shape is used, which exhibits a particularly high effect.
[0019] When one turn is defined as a portion in which the superconducting wire 20 and the reinforcing wire 40 are wound around, a plurality of turns form one winding portion 11. In this embodiment, the space between adjacent turns of the superconducting wire 20 is referred to as a space between coil turns.
[0020] Winding portion 11 is impregnated with conductive resin portion 12 made of a resin having electrical conductivity. This conductive resin portion 12 is solidified in a state in which winding portion 11 is impregnated. The conductive resin portion 12 is impregnated into the gap between superconducting wire 20 and reinforcing wire 40. This conductive resin portion 12 forms detour paths 60A-60D (FIG. 7) that are paths along which an excessive current flowing through superconducting wire 20 is detoured.
[0021] In addition, in the winding portion 11, the superconducting wire 20 and the reinforcing wire 40 are stacked by winding to form a winding side portion. For example, the top and bottom surfaces of the superconducting coil 1 in FIG. 2 are the winding side portion. Each winding side portion is covered with an insulating plate 13, which is a disk-shaped plate member having insulating properties. By covering each winding side portion with an insulating plate 13, other superconducting coils 1 of the same configuration can be stacked in the coil axial direction 3.
[0022] 3, for example, a tape-shaped superconducting wire 20 (thin film wire) in which a plurality of general thin film layers are laminated is used as the superconducting wire 20. The superconducting wire 20 is, for example, a wire such as an REBCO wire containing rare metal oxide (RE oxide).
[0023] Superconducting wire 20 includes stabilization layer 21, metal substrate 22, orientation layer 23, intermediate layer 24, superconducting layer 25, and protective layer 26. However, the types and numbers of layers constituting superconducting wire 20 are not limited to those described above, and may be more or less as necessary.
[0024] Stabilization layer 21 is a layer that covers the entire outer circumferential surface of superconducting wire 20. Stabilization layer 21 is made of a highly conductive metal such as copper or aluminum. Stabilization layer 21 serves as a path for bypassing excess current flowing through superconducting layer 25, thereby preventing thermal runaway.
[0025] The metal substrate 22 is a tape-shaped member and is made of a high-strength metal material such as a nickel-based alloy, stainless steel, or copper.
[0026] The orientation layer 23 is formed on the metal substrate 22. The orientation layer 23 is formed of, for example, magnesium, which orients the intermediate layer 24 on the surface of the metal substrate 22.
[0027] The intermediate layer 24 is formed on the orientation layer 23. The intermediate layer 24 prevents thermal distortion caused by thermal contraction of the metal substrate 22 and the superconducting layer 25.
[0028] The superconducting layer 25 is formed on the intermediate layer 24. In this embodiment, the superconducting layer 25 is provided on one of the two surfaces of the metal substrate 22 via the intermediate layer 24. The superconducting layer 25 is made of a superconducting material, and is formed of, for example, a rare metal oxide (RE oxide).
[0029] Protective layer 26 is formed on superconducting layer 25. Protective layer 26 is formed of, for example, silver, gold, platinum, or the like. Protective layer 26 prevents oxygen contained in superconducting layer 25 from diffusing from superconducting layer 25, and protects superconducting layer 25. Protective layer 26 covers superconducting layer 25.
[0030] As shown in Fig. 4, four surfaces extending parallel to each other along the longitudinal direction of superconducting wire 20, i.e., the outer peripheral surface of superconducting wire 20, are divided into two main surfaces 27, 28 and two end surfaces 29, 30. Here, main surfaces 27, 28 are wide surfaces that are wider than end surfaces 29, 30. End surfaces 29, 30 are surfaces perpendicular to main surfaces 27, 28 and are narrow surfaces that are narrower than main surfaces 27, 28. Of the two main surfaces 27, 28 (both surfaces) of superconducting wire 20, main surface 27 closer to superconducting layer 25 is referred to as a proximal surface, and main surface 28 farther from superconducting layer 25 than the proximal surface is referred to as a distal surface.
[0031] As shown in Fig. 5, the reinforcing wire 40 is formed by a reinforcing plate 41 made of a tape-shaped metal material. The outer peripheral surface of the reinforcing wire 40 is also divided into two wide surfaces, main surfaces 42 and 43, and two narrow surfaces, end surfaces 44 and 45. At least one main surface 42 of the two main surfaces 42 and 43 (both surfaces) of the reinforcing wire 40 is coated with a release material layer 46 that weakens the adhesion between the reinforcing wire 40 and the conductive resin part 12 more than other parts.
[0032] For example, as shown in FIG. 7, in the first embodiment, of the two main surfaces 42, 43 (both surfaces) of the reinforcing wire 40, one of the main surfaces 42 (FIG. 5) that faces the metal substrate 22 of the superconducting wire 20, i.e., the one of the main surfaces 42 that faces the distal surface 28 of the superconducting wire 20, is coated with a release material layer 46.
[0033] Further, the other main surface 43 and end surfaces 44, 45 of the reinforcing wire 40 are connected to the conductive resin part 12. In this manner, a part of the outer peripheral surface of the reinforcing wire 40 is electrically connected to the conductive resin part 12. Then, the current that flows in a detouring manner from the superconducting wire 20 to the conductive resin part 12 is easily detouring also to the reinforcing wire 40.
[0034] The superconducting wires 20 and the reinforcing wires 40 are impregnated with and hardened in the conductive resin portion 12. This conductive resin portion 12 fills the gaps between adjacent superconducting wires 20 and reinforcing wires 40, and is also provided on the side portions of the winding.
[0035] The reinforcing wire 40 is fixed to the superconducting wire 20 via the conductive resin part 12, and thus mechanically integrated with the superconducting wire 20, thereby improving the strength of the superconducting wire 20. In other words, when stress is generated in the superconducting wire 20, the reinforcing wire 40 inhibits the deformation, thereby reducing the occurrence of distortion.
[0036] As the material for the reinforcing wire 40, a nickel-based alloy, an alloy such as stainless steel, or a metal material such as copper, silver, or aluminum formed into a tape shape can be suitably used.
[0037] When a part of superconducting wire 20 transitions from a superconducting state to a normal conductive state, conductive resin part 12 forms detours 60A-60D that short-circuit the current in the part that has transitioned to the normal conductive state to a different turn of superconducting wire 20. In other words, conductive resin part 12 functions as detours 60A-60D that pass a current between coil turns and electrically connect superconducting wire 20 at different positions in winding part 11. In this way, the current detours around the part that has transitioned to the normal conductive state, thereby making it possible to suppress local heat generation or thermal runaway in the part that has transitioned to the normal conductive state.
[0038] The resistance values of detours 60A-60D are set to be greater than the resistance value when superconducting wire 20 is in a superconducting state and less than the resistance value when superconducting wire 20 is in a normal conducting state. In this way, a current can be passed through detours 60A-60D only when superconducting wire 20 transitions from a superconducting state to a normal conducting state.
[0039] 6, for example, conductive resin portion 12 may be made by mixing conductive powder 19 into non-conductive resin 18. By changing the proportion or type of conductive powder 19 mixed into conductive resin portion 12, the volume resistivity of conductive resin portion 12 can be easily adjusted.
[0040] As the conductive powder 19, for example, a carbon-based powder such as carbon black, carbon fiber, or graphite is used. Alternatively, a metal-based powder such as metal fine particles, metal oxide, metal fiber, or whiskers may be used as the conductive powder 19. Alternatively, a conductive powder 19 in which fine particles or synthetic fibers are metal-coated may be used. At least one of these conductive powders 19, or a combination of these conductive powders 19, is mixed into the resin 18. Note that the composition of the conductive powder 19 may be different for each position (each section) of the winding portion 11.
[0041] In addition, the resistance value of detours 60A-60D (FIG. 7) can be adjusted by adjusting the amount of conductive resin portion 12 that enters between the turns of adjacent superconducting wire 20 or the amount of conductive resin portion 12 provided on the side portion of the winding.
[0042] Next, a method for manufacturing the superconducting coil 1 will be described with reference to the flow chart of Fig. 11. The above-mentioned drawings will be referred to as appropriate.
[0043] First, in step S1, the manufacturer coats at least one of the two main surfaces 42, 43 (both sides) of the reinforcing wire 40 made of a tape-shaped metal material with a release material layer 46 that weakens the adhesion between the reinforcing wire 40 and the conductive resin part 12, which has conductivity, more than other parts.
[0044] In the next step S2, the manufacturer winds the superconducting wire 20 having the superconducting layer 25 made of a superconducting material provided on one of the two surfaces of the tape-shaped metal substrate 22 together with the reinforcing wire 40.
[0045] In the next step S3, the manufacturer impregnates the space between the superconducting wire 20 and the reinforcing wire 40 with the conductive resin portion 12.
[0046] This completes the method for manufacturing the superconducting coil 1. Note that the above steps are at least a part of the method for manufacturing the superconducting coil 1, and other steps may be included in the method for manufacturing the superconducting coil 1.
[0047] Next, superconducting coil 1 of the first embodiment shown in FIG. 7 will be described in comparison with superconducting coils 51 (51A, 51B) of comparative examples 1 to 4 shown in FIGS.
[0048] 8, in Comparative Example 1 showing the configuration of a general superconducting coil 51, superconducting wire 20 is impregnated with insulating resin portion 52 that has excellent insulating properties and thermal conductivity and is adhesive. Note that the spaces between the coil turns and the surfaces of the side portions of the winding are filled with insulating resin portion 52, except for the portions where minute gaps such as unintended voids occur.
[0049] Impregnation with insulating resin portion 52 is a treatment for the purposes of insulating adjacent superconducting wires 20 from each other, forming a heat transfer path for each turn of superconducting wire 20, and improving the mechanical strength of superconducting coil 51. For insulating resin portion 52, an epoxy resin is preferably used.
[0050] Also, as in superconducting coil 51A of Comparative Example 2 in Fig. 9, insulating member 53 having insulating properties may be inserted between the coil turns. For example, an insulating tape made of polyimide or the like is suitably used for insulating member 53. Tape-shaped insulating member 53 is wound together with superconducting wire 20 to be inserted between the coil turns. By inserting insulating member 53 between the coil turns, it is possible to more reliably insulate the coil turns from each other.
[0051] Here, when a tape-shaped structure (insulating member 53) having a certain thickness is inserted between the coil turns, not limited to insulating member 53 of comparative example 2 in Figure 9, there is a disadvantage that the coil diameter increases by the amount of the thickness.
[0052] For example, in the structure of Comparative Example 1 in FIG. 8, only one resin layer 54 is formed between adjacent superconducting wires 20. In contrast, in the structure of Comparative Example 2 in FIG. 9, two resin layers 54 are formed between adjacent superconducting wires 20. For example, resin layers 54 are formed in the gap between a given insulating member 53 and an adjacent superconducting wire 20 on the inside in the coil radial direction 5, and in the gap between this insulating member 53 and an adjacent superconducting wire 20 on the outside in the coil radial direction 5. In this way, by disposing a tape-shaped structure between the coil turns, the number of resin layers 54 increases, and as a result, the diameter of the coil also increases.
[0053] This increase in the coil diameter is particularly noticeable when resin 52 is applied or spread while winding superconducting wire 20. Furthermore, the increase is more noticeable as the viscosity of resin 52 is higher.
[0054] Even if some means is used to reduce the thickness of each resin layer 54, it is difficult to completely eliminate the thickness of resin layer 54 that has entered the gaps. Even if the thickness of resin layer 54 per turn is small (e.g., 1 μm to 10 μm), when superconducting coil 51 is formed by winding superconducting wire 20 several hundred turns, the diameter of the coil may increase on the order of millimeters.
[0055] Increasing the coil diameter increases the overall size of the superconducting device (not shown) containing the superconducting coil 51, and requires a large space to install the superconducting device. Alternatively, when making a superconducting coil 51 of the same size, the number of turns of the superconducting wire 20 decreases, and the magnetic field that can be generated becomes smaller. Therefore, if the number of turns of the superconducting wire 20 is the same, it is desirable to have a smaller coil diameter.
[0056] 8, when a part of superconducting wire 20 transitions to normal conductivity during current flow, the part where the wire transitions to normal conductivity consumes energy locally, causing a temperature rise and forming a hot spot, which may cause superconducting coil 51 to burn out.
[0057] Superconducting coil 51B of Comparative Example 3 in FIG. 10 differs from Comparative Example 2 in several respects with reference to the prior art. For example, Comparative Example 3 differs from Comparative Example 2 in that conductive resin part 12 is used instead of insulating resin part 52. Comparative Example 3 also differs from Comparative Example 2 in that insulating member 56 with release material obtained by adhering release material 55 to insulating member 53 is used instead of insulating member 53. Comparative Example 3 also differs from Comparative Example 2 in that reinforcing wire 40 is adhered adjacent to superconducting wire 20 via conductive resin part 12. In Comparative Example 3, resin layer 54 made of conductive resin part 12 is formed between superconducting wire 20, reinforcing wire 40, and insulating member 56 with release material.
[0058] Superconducting wire 20 is made up of various layers including superconducting layer 25 stacked on top of one another, and is therefore extremely vulnerable to tensile stress in a direction perpendicular to main surfaces 27, 28 (diameter direction 5 of the coil), i.e., peeling stress. However, during operation of superconducting coil 51B, superconducting wire 20 is subjected to peeling stresses such as thermal stress generated when cooling to the operating temperature and electromagnetic stress generated by excitation. Therefore, when superconducting wire 20 is used for superconducting coil 51B, it is necessary to devise a method for preventing peeling stress from exceeding an allowable value.
[0059] Therefore, release material 55 is disposed between the turns to provide portions that can be released from conductive resin portion 12 at a plurality of locations in coil radial direction 5. In this manner, even if peeling stress is applied, release material 55 and conductive resin portion 12 are released (separated) via release material 55, and therefore the peeling stress applied to superconducting wire 20 is reduced. As a result, deterioration of superconducting wire 20 can be prevented.
[0060] However, in superconducting coil 51B of Comparative Example 3 in FIG. 10, the periphery of insulating member with release material 56 and reinforcing wire 40 arranged between the turns is filled with conductive resin portion 12, so that three resin layers 54 are formed between superconducting wires 20. For example, resin layers 54 are formed in three locations: a gap between superconducting wire 20 and reinforcing wire 40 located on the outside in coil radial direction 5, a gap between reinforcing wire 40 and insulating member with release material 56 located on the outside in coil radial direction 5, and a gap between insulating member with release material 56 and superconducting wire 20 located on the outside in coil radial direction 5. In Comparative Example 3 in FIG. 10, the coil diameter is increased by one in addition to the thickness of insulating member with release material 56 and reinforcing wire 40 themselves, as compared to Comparative Example 2 in FIG. 9.
[0061] 7, in the superconducting coil 1 of the first embodiment, a reinforcing wire 40 is disposed between adjacent superconducting wires 20 in the coil radial direction 5. One main surface 42 of the reinforcing wire 40 is coated with a release material layer 46.
[0062] Here, superconducting coil 1 of the first embodiment has two major differences from Comparative Example 3 (FIG. 10). For example, release material layer 46 having a release effect is formed by coating reinforcing wire 40, not insulating member 53. Also, superconducting wires 20 arranged in radial direction 5 of the coil are not insulated from each other by insulating member 53.
[0063] The release material layer 46 is made of at least one material selected from, for example, fluororesin such as Teflon (registered trademark), paraffin, grease, and silicone oil. In this manner, the work of coating the reinforcing wire material 40 with the release material layer 46 can be easily performed. The release material layer 46 may be formed by combining these materials. Furthermore, the material of the release material layer 46 may be different for each position (each portion) of the winding portion 11.
[0064] As described above, a tape made of an alloy or an elemental metal is preferably used for the reinforcing wire 40. Here, the reinforcing wire 40 is preferably made of a material having a higher Young's modulus than other members constituting the superconducting coil 1, such as the superconducting wire 20 and the conductive resin part 12. In this way, the reinforcing wire 40 reinforces the other members, such as the superconducting wire 20, and becomes able to withstand stresses generated when the superconducting coil 1 is cooled or stresses due to the generated magnetic field. In other words, the mechanical strength of the superconducting coil 1 can be improved.
[0065] Since superconducting wire 20 has a multilayer structure including multiple layers such as superconducting layer 25, reinforcing wire 40 may be made of a material having a Young's modulus similar to that of metal substrate 22, which has the highest mechanical strength among the multiple layers constituting superconducting wire 20. Of course, reinforcing wire 40 may be made of the same material as metal substrate 22.
[0066] When reinforcing wire 40 is made of a conductive material, reinforcing wire 40 can also function as part of detours 60A-60D (FIG. 7) together with conductive resin part 12. In this case, the resistance value of reinforcing wire 40 is set to be greater than the resistance value when superconducting wire 20 is in a superconducting state and less than the resistance value when superconducting wire 20 is in a normal conducting state.
[0067] The release material layer 46 can have a certain effect regardless of whether it is formed on any of the pair of main surfaces 42, 43 of the reinforcing wire 40. Furthermore, the reinforcing wire 40 can function as a part of the detours 60A to 60D together with the conductive resin part 12. Therefore, as shown in Fig. 7, of the pair of main surfaces 42, 43 of the reinforcing wire 40, the release material layer 46 is formed only on the main surface 42 that faces the distal surface 28 of the superconducting wire 20. Furthermore, the release material layer 46 may not be formed on the main surface 43 that faces the proximal surface 27 of the superconducting wire 20.
[0068] Moreover, the electrical resistance of stainless steel, nickel-based alloy, etc. used in metal substrate 22 is higher than the electrical resistance of copper, silver, etc. used in protective layer 26 or stabilizing layer 21. Therefore, as shown in Fig. 7, the electrical resistance of detour 60A, in which current detours from superconducting layer 25 of superconducting wire 20 through proximal surface 27 to reinforcing wire 40, is smaller than the electrical resistance of detour 60B, in which current detours from superconducting layer 25 of superconducting wire 20 through distal surface 28 to reinforcing wire 40.
[0069] Therefore, in the reinforcing wire 40, the release material layer 46 is formed only on the main surface 42 facing the distal surface 28 of the superconducting wire 20. The release material layer 46 is prevented from blocking the current flowing through the detour 60A. In this manner, the electrical resistance when the current detours from the superconducting layer 25 of the superconducting wire 20 to the reinforcing wire 40 can be reduced.
[0070] In the first embodiment, when a normal conducting transition occurs in a part of the superconducting wire 20, a part of the current flowing through the superconducting wire 20 is diverted to a different turn of the superconducting wire 20 via the detours 60A to 60D formed by the conductive resin part 12 and the reinforcing wire 40.
[0071] In addition, release material layer 46 provided on reinforcing wire 40 weakens the adhesive force between conductive resin portion 12 and reinforcing wire 40. Therefore, when peeling stress occurs due to the difference in the amount of thermal contraction between superconducting wire 20 and conductive resin portion 12 during cooling of superconducting coil 1, the adhesive surface between release material layer 46 (main surface 42) of reinforcing wire 40 and conductive resin portion 12 is preferentially peeled off, and the peeling stress occurring in superconducting wire 20 can be reduced.
[0072] Furthermore, by directly coating the release material layer 46 onto the reinforcing plate 41, which is the base material of the reinforcing wire 40, it is not necessary to form a resin layer 54 between the reinforcing wire 40 (reinforcing plate 41) and the release material layer 46.
[0073] For example, in the superconducting coil 1 of the first embodiment, resin layers 54 are formed in two locations: in the gap between the superconducting wire 20 and release material layer 46 of the reinforcing wire 40 located outside in the coil radial direction 5, and in the gap between the reinforcing wire 40 and the superconducting wire 20 located outside in the coil radial direction 5. Therefore, in the superconducting coil 1 of the first embodiment, the number of resin layers 54 does not need to be increased as compared to Comparative Example 3 (FIG. 10).
[0074] In the first embodiment, by directly coating the reinforcing plate 41 of the reinforcing wire 40 with the release material layer 46, it becomes unnecessary to provide the insulating member 53. Next, the advantages of this will be described.
[0075] For example, when release material layer 46 is formed by coating with a fluorine-based resin, the thickness of release material layer 46 is very thin, about 1 μm to 10 μm. If release material layer 46 were to be produced alone without coating main surfaces 42, 43 of reinforcing wire 40 with release material layer 46, the strength would be very low due to its thinness. Therefore, it would easily break even with a small tensile force, making it difficult to wind superconducting wire 20 and reinforcing wire 40 together.
[0076] 10, for example, release material 55 having a release effect is formed on the surface of insulating member 53 having a higher mechanical strength than release material 55 to form insulating member 56 with release material. In this comparative example 3, insulating member 56 with release material does not easily break even when a certain tensile force is applied to it. Therefore, it can be wound together with superconducting wire 20 and reinforcing wire 40.
[0077] In the superconducting coil 1 of the first embodiment (FIG. 7), the release material layer 46, which cannot be used alone, is arranged by coating the reinforcing wire 40 rather than on the insulating member 53, thereby eliminating the need to arrange the insulating member 53 used as the base material of the release material 55 in Comparative Example 3 (FIG. 10).
[0078] By manufacturing superconducting coil 1 without disposing release material 55 between superconducting wires 20, the coil diameter can be made smaller than when manufacturing with release material 55 disposed as in Comparative Example 3. For example, if insulating member 53 is a polyimide tape, the thickness is about 10 μm to 100 μm. The coil diameter can be made smaller by the amount of this thickness.
[0079] Next, the effect of providing the bypass paths 60A to 60D using the conductive resin portion 12 to suppress the occurrence of thermal runaway or quenching will be described.
[0080] As the superconducting wire 20 approaches the critical current, which is the limit of the current that can pass through it, an external magnetic field gradually penetrates, destroying the superconducting state locally and causing that portion to transition to a normal conductive state. The flux flow resistance associated with this local normal conductive transition generates heat due to Joule loss. Therefore, if the resistance increases due to a rise in the temperature of the superconducting coil 1, it will induce thermal runaway or quenching.
[0081] Therefore, by providing detours 60A-60D, when local flux flow resistance occurs in a part of superconducting wire 20 due to a normal conducting transition, a part of the current flowing in coil circumferential direction 4 can be diverted to another adjacent turn of superconducting wire 20 via detours 60A-60D. In other words, a part of the current flowing in coil circumferential direction 4 can be diverted in coil radial direction 5. This suppresses the generation of Joule heat, thereby suppressing the occurrence of thermal runaway.
[0082] Here, the current flowing in the coil circumferential direction 4 decreases by the amount that is bypassed. In other words, if the value of the current flowing in the coil circumferential direction 4 is I, and the value of the current bypassed by the bypasses 60A-60D is I', the current flowing in the coil circumferential direction 4 decreases from I to I-I'. In this case, if the resistance of the bypasses 60A-60D is R' and the flux flow resistance is R, the current I' bypassing between the coil turns in the coil radial direction 5 is proportional to R / (R+R').
[0083] In this way, as the flux flow resistance increases, more current is diverted in the coil radial direction 5. This makes it possible to prevent a large amount of current from flowing through a normal conductive portion that has locally transitioned to a normal conductive state, thereby making it possible to suppress the occurrence of thermal runaway or quenching.
[0084] Note that detours 60A-60D may also cause disadvantages. For example, when coil turns are electrically connected via detours 60A-60D, part of the current is diverted to other turns of superconducting wire 20 via detours 60A-60D not only when flux flow resistance occurs but also when superconducting coil 1 is excited from a non-energized state to a rated current value. In other words, part of the current supplied from the power source due to the induced voltage is diverted in the coil radial direction 5.
[0085] After the excitation of the superconducting coil 1 is completed, no induced voltage is generated, so the current flowing through the bypass paths 60A-60D gradually flows in the coil circumferential direction 4, and it takes time for the magnetic field to reach the designed value. Therefore, the lower the resistance between the coil turns, the more current is bypassed during excitation, and the longer the excitation time becomes.
[0086] In other words, it is preferable to set the electrical resistance R' of the bypass paths 60A-60D so that it is small enough to allow a sufficient amount of current to be diverted to the bypass paths 60A-60D when flux flow resistance occurs, and so that it is large enough that the excitation time when the superconducting coil 1 is excited from a non-energized state to the rated current value is not unnecessarily long.
[0087] By reducing the electrical resistance R' between the coil turns, more of the energized current is diverted in the coil radial direction 5. Therefore, the smaller the resistance value of the conductive resin part 12, the larger the current I' that divertes between the coil turns can be. Conversely, the larger the resistance value of the conductive resin part 12, the smaller the current I' that divertes between the coil turns can be.
[0088] Next, the effect of impregnating the winding portion 11 with the conductive resin portion 12 in the superconducting coil 1 of the first embodiment will be described using Comparative Example 4 (FIG. 10). Comparative Example 4 differs in that an insulating resin portion 52 having insulating properties is used instead of the conductive resin portion 12 of Comparative Example 3. Since other parts are similar, Comparative Example 4 will be described using the same FIG. 10 as Comparative Example 3.
[0089] As shown in FIG. 10, in Comparative Example 4, since insulating resin part 52 is used, detours 60A to 60D (FIG. 7) are not formed, and adjacent superconducting wires 20 are not electrically connected to each other in radial direction 5 of the coil.
[0090] In addition, in this comparison example 4, superconducting wire 20 is impregnated with insulating resin part 52, but even when superconducting wire 20 is not impregnated with insulating resin part 52, adjacent superconducting wires 20 are not electrically connected to each other in coil radial direction 5.
[0091] However, in Comparative Example 4, there are cases where a part of the current flowing through superconducting wire 20 is diverted to reinforcing wire 40. For example, there is a case where superconducting wire 20 has a portion in direct contact with reinforcing wire 40. Current flows through this contact portion.
[0092] Here, the contact resistance between the superconducting wire 20 and the adjacent reinforcing wire 40 is determined by the contact state of the minute projections and recesses on the surfaces of the superconducting wire 20 and the reinforcing wire 40. The contact resistance also varies depending on the contact area in a microscopic sense. This makes it difficult to adjust the contact resistance. Therefore, the electrical resistance between the superconducting wire 20 and the reinforcing wire 40 differs for each portion of the winding portion 11.
[0093] Furthermore, when superconducting wire 20 is impregnated with insulating resin portion 52, the contact state between superconducting wire 20 and reinforcing wire 40 changes depending on the microscopic thickness distribution of insulating resin portion 52. Therefore, the contact resistance differs depending on the portion of winding portion 11.
[0094] In particular, in a certain portion of the superconducting wire 20, adjacent superconducting wires 20 and reinforcing wires 40 are insulated in the coil radial direction 5. In addition, in another portion, a situation may arise in which adjacent superconducting wires 20 and reinforcing wires 40 are electrically connected. As a result, the magnitude of the current commutated from the superconducting wire 20 to the reinforcing wire 40 differs for each portion of the winding portion 11.
[0095] This may cause a delay in the formation of a magnetic field when a current is applied to superconducting coil 1, since more current than necessary is diverted from superconducting wire 20 to reinforcing wire 40 in a certain portion of winding portion 11. Conversely, in another portion of superconducting wire 20, a necessary amount of current may not be diverted from superconducting wire 20 to reinforcing wire 40. This may cause burning of superconducting coil 51B.
[0096] In the superconducting coil 1 of the first embodiment, before hardening, the conductive resin portion 12, which is a fluid, penetrates between the superconducting wire 20 and the reinforcing wire 40 to form a resin layer 54. Then, fine irregularities on the surfaces of the superconducting wire 20 and the reinforcing wire 40 are filled, and an effect of suppressing the variation in the contact resistance is achieved. Then, the delay in the formation of a magnetic field when a current is applied to the superconducting coil 1 can be reduced, and the risk of the superconducting coil 1 burning can be reduced.
[0097] Next, a path along which the current flowing through superconducting wire 20 is detouring to a superconducting wire 20 adjacent in coil radial direction 5 will be described.
[0098] 7, it is assumed that there is a detour 60C along which a current flows in the radial direction from main surface 28, which is the wide surface of superconducting wire 20, through main surface 42, which is the wide surface of reinforcing wire 40, to an adjacent superconducting wire 20. It is also assumed that there is a detour 60D along which a current flows out from main surface 28 or end surface 29 (FIG. 4) of superconducting wire 20, through conductive resin portion 12 provided on the side surface portion of the winding, to an adjacent superconducting wire 20.
[0099] In the first embodiment (FIG. 7), the insulating member 53 as in Comparative Example 3 (FIG. 10) is not disposed between the turns. Therefore, in the first embodiment, only the release material layer 46 can function to insulate the detour 60C. In other words, if the release material layer 46 has sufficient insulating performance, no current will flow through the detour 60C. On the other hand, if the release material layer 46 does not have sufficient insulating properties, a current may flow through the detour 60C.
[0100] In the first embodiment (FIG. 7), adjacent superconducting wires 20 are electrically connected to each other by detours 60D, so that a current can flow through detours 60D.
[0101] On the other hand, in Comparative Example 4 (FIG. 10), insulating resin part 52 is used, and therefore there is no detour 60D electrically connecting adjacent superconducting wires 20. Therefore, no current flows between adjacent superconducting wires 20.
[0102] In the first embodiment (FIG. 7), whether or not a current flows radially between adjacent superconducting wires 20 depends on whether or not detour 60C is insulated, that is, whether or not release material layer 46 has sufficient electrical insulation.
[0103] For example, if the release material layer 46 is formed to be very thin and does not have sufficient electrical insulation, adjacent superconducting wires 20 may be electrically connected to each other through a bypass 60C that passes through the release material layer 46 and the reinforcing wire 40.
[0104] However, because release material layer 46 has releasability, it is preferentially peeled off from resin layer 54 due to peeling stress caused by thermal contraction during cooling. This peeling changes the contact state with adjacent superconducting wires 20, and furthermore, the contact resistance between reinforcing wire 40 and superconducting wire 20 may differ for each portion of winding portion 11. This may result in a risk that the current is diverted to reinforcing wire 40 more than necessary, or that the necessary amount of current cannot be diverted.
[0105] Conversely, in order to provide sufficient electrical insulation to the release material layer 46, it is conceivable to make the thickness of the release material layer 46 sufficiently large. Alternatively, it is conceivable to overlay an insulating member 53 (FIG. 10) on the release material layer 46. However, this would result in an unnecessarily large coil diameter compared to the superconducting coil 1 of the first embodiment.
[0106] 7, in the superconducting coil 1 of the first embodiment, the superconducting wire 20 is impregnated with the conductive resin portion 12, which provides an electrical connection between the turns and prevents the superconducting coil 1 from burning. In addition, the contact resistance of each portion of the winding portion 11 is made uniform, thereby reducing the distribution of the contact resistance. In addition, the coil diameter is prevented from increasing unnecessarily.
[0107] Next, a quantitative explanation will be given of the difference in coil diameter between superconducting coil 1 of the first embodiment (FIG. 7) and superconducting coil 51B (FIG. 10) of Comparative Example 3. Here, the winding thicknesses of superconducting coils 1 and 51B will be calculated.
[0108] The winding thickness is the total thickness of the members wound around the reel 10, and is calculated by multiplying the thickness per turn of the superconducting wire 20 by the number of turns. When the size of the reel 10 is the same, the coil diameters are the same. Also, the smaller the winding thickness, the smaller the coil diameter.
[0109] For example, the number of turns of superconducting coils 1, 51B is 200. The thickness of superconducting wire 20 is 0.1 mm. The thickness of reinforcing plate 41 of reinforcing wire 40 is 0.1 mm. The thickness of insulating member 53 is 50 μm. The thickness of release material 55 and release material layer 46 is 5 μm. The thickness of resin layer 54 is 5 μm.
[0110] In the superconducting coil 1 (FIG. 7) of the first embodiment, it is assumed that only one of the two main surfaces 42, 43 of the reinforcing wire 40, the main surface 42, is coated with the release material layer .
[0111] In addition, in superconducting coil 51B (FIG. 10) of Comparative Example 3, release material 55 is provided on both wide surfaces (main surfaces) of insulating member 53. However, for the purpose of comparison, calculations are made assuming that release material 55 is provided on only one wide surface of insulating member 53.
[0112] Under the above assumptions, the winding thicknesses of superconducting coil 1 of the first embodiment (FIG. 7) and superconducting coil 51B of Comparative Example 3 (FIG. 10) are calculated.
[0113] In the superconducting coil 1 of the first embodiment (FIG. 7), the thickness per turn is 0.1 mm+0.005 mm+0.005 mm+0.1 mm+0.005 mm=0.215 mm, which is the sum of the thicknesses of the superconducting wire 20, the resin layer 54, the release material layer 46 of the reinforcing wire 40, the reinforcing plate 41 of the reinforcing wire 40, and the resin layer 54. Here, the winding thickness for 200 turns is 0.215 mm×200=43 mm.
[0114] Meanwhile, in superconducting coil 51B of Comparative Example 3 (FIG. 10), the thickness per turn is the sum of the thicknesses of superconducting wire 20, resin layer 54, reinforcing plate 41 of reinforcing wire 40, resin layer 54, release material 55, insulating member 53, and resin layer 54, which is 0.1 mm+0.005 mm+0.1 mm+0.005 mm+0.005 mm+0.05 mm+0.005 mm=0.27 mm. Here, the winding thickness for 200 turns is 0.27 mm×200=54 mm.
[0115] In other words, even if superconducting coils 1 and 51B with the same number of turns are manufactured, the winding thickness can be reduced by 11 mm in the first embodiment compared to Comparative Example 3. A winding thickness that is 11 mm smaller means that the radius of superconducting coil 1 is 11 mm smaller. Comparing the diameters results in a difference of 22 mm. Thus, there may be a difference in the coil diameters of superconducting coils 1 and 51B between superconducting coil 1 of the first embodiment (FIG. 7) and superconducting coil 51B of Comparative Example 3 (FIG. 10).
[0116] Here, the coil diameter of the superconducting coil 1 is determined by the current density (A / mm 2) is sometimes used as an index for comparison. The current density is calculated by multiplying the total current value (A) passing through a cross section perpendicular to the circumferential direction of the superconducting coil 1 by the cross-sectional area (mm 2 ) where the cross-sectional area of the winding form 10 is excluded in the calculation. The size of the cross-sectional area of the cross section perpendicular to the circumferential direction of the superconducting coil 1 is calculated by the product of the axial size of the superconducting coil 1 and the winding thickness of the superconducting coil 1. The higher the current density, the more current can be passed through a smaller cross-sectional area. When comparing under the same conditions of the number of turns, current flow, and axial size of the superconducting coil 1, the smaller the winding thickness of the superconducting coil 1, the higher the current density. Therefore, it can be said that the superconducting coil 1 of the first embodiment (FIG. 7) has a higher current density than the superconducting coil 51B of Comparative Example 3 (FIG. 10).
[0117] Furthermore, in the superconducting coil 1 of the first embodiment, the reinforcing wire 40 may be made to have a higher electrical resistance than the conductive resin portion 12. In this way, the current is more actively detouring to the conductive resin portion 12 than to the reinforcing wire 40. The electrical resistance of the detouring path 60D through which the current flows can be adjusted by adjusting the mixture used when forming the conductive resin portion 12.
[0118] 7, the reinforcing wire 40 has a higher electrical resistance than the conductive resin part 12, so that the electrical resistance of a detour 60C that passes through the reinforcing wire 40 is greater than the electrical resistance of a detour 60D that does not pass through the reinforcing wire 40. Note that the reinforcing wire 40 may be designed to have a lower electrical resistance than the conductive resin part 12.
[0119] The following reasoning is valid both when the release material layer 46 has sufficient electrical insulation and when it does not have sufficient electrical insulation. Here, in order to make the effect more pronounced, the following description will be given assuming that the release material layer 46 does not have sufficient electrical insulation.
[0120] The electrical resistance of the bypass 60C is R X The electrical resistance of the detour 60D is R YThe electrical resistance R' in the radial direction between adjacent superconducting wires 20 is expressed as R'=R X ×R Y / (R X +R Y ) shall be expressed as follows.
[0121] Here, the electrical resistance R Y can be continuously changed by changing the ratio of the conductive powder 19 (FIG. 6) contained in the conductive resin portion 12. X Since is determined by the resistance value of the material of the reinforcing wire 40, it is not easy to change it continuously. X >R Y By doing so, the size of R' can be expressed as R Y This makes it easy to vary the value of R' continuously.
[0122] For example, R Y and R X Let the ratio of (R X =γR Y ) When γ=1, R X =R Y When γ>1, R X >R Y When γ<1, R X <R Y In this case, R'=γ×R Y ×R Y / (R Y (1+γ))=(γ / (γ+1))×R Y It becomes.
[0123] Here, when γ>1, consider two cases where γ differs by, say, 10 times. For example, consider the first case when γ=10 and the second case when γ=100. (γ / (γ+1)) approaches 1 asymptomatically as γ increases. Therefore, in the first case, R'=0.91R Y In the second case, R' = 0.99R Y The ratio of R' in both cases is 0.92. In other words, if γ differs by 10 times, R' will differ by 0.92 times.
[0124] On the other hand, when γ<1, consider two cases where γ differs by, say, 10 times. For example, consider the third case where γ=0.1 and the fourth case where γ=0.01. In the third case, R'=0.091R Y In the fourth case, R' = 0.0099R Y The ratio of R' in both cases is 9.19. In other words, if γ differs by a factor of 10, R' will differ by a factor of 9.19.
[0125] In this way, when γ>1, the value of R' is less likely to change due to the influence of the value of γ than when γ<1. In other words, when adjusting the value of R', the electrical resistance R X Electrical resistance R is not significantly affected by differences in the value of Y Depending on the value of , the value of R' can be changed.
[0126] In addition, it is possible to easily adjust the electrical resistance R' in the radial direction between adjacent superconducting wires 20. This makes it possible to easily adjust the magnitude of current I' flowing in the radial direction between adjacent superconducting wires 20. This makes it possible to more reliably avoid burnout of superconducting coil 1.
[0127] According to the first embodiment, a sufficient amount of current, out of the current flowing through superconducting wire 20, is diverted to bypass paths 60A to 60D, thereby making it possible to prevent superconducting coil 1 from burning out.
[0128] In addition, it is possible to reduce peeling stress caused by the difference in the amount of thermal contraction between superconducting wire 20 and conductive resin part 12 when superconducting coil 1 is cooled. Therefore, it is possible to prevent peeling deterioration in superconducting layer 25 of superconducting wire 20.
[0129] Furthermore, the thickness of release material layer 46 is smaller than the thicknesses of superconducting wire 20 and reinforcing wire 40. In this way, superconducting coil 1 can be formed so that its radial thickness does not become large.
[0130] Furthermore, in superconducting coil 1 of the first embodiment (FIG. 7), two resin layers 54 are formed between the turns, so that it is possible to reduce an increase in the coil diameter due to the presence of resin layers 54, compared to superconducting coil 51B (FIG. 10) of comparative example 3. Furthermore, since insulating member 53 is no longer an essential component, it is possible to reduce an increase in the coil diameter.
[0131] Second embodiment Next, a second embodiment will be described with reference to Fig. 12. Note that the same components as those shown in the above-mentioned embodiment will be denoted by the same reference numerals and duplicated description will be omitted.
[0132] 12, in the superconducting coil 1A of the second embodiment, a plurality of reinforcing wires 40, 40A are arranged between the turns of adjacent superconducting wires 20. For example, one reinforcing wire 40 coated with a release material layer 46 and two reinforcing wires 40A not coated with a release material layer 46 are arranged.
[0133] That is, a plurality of reinforcing wires 40, 40A are wound together with the superconducting wire 20, and at least one reinforcing wire 40 among the plurality of reinforcing wires 40, 40A is coated with the release material layer 46.
[0134] A plurality of reinforcing wires 40, 40A are arranged between all of the turns of the superconducting coil 1 A. Note that a plurality of reinforcing wires 40, 40A may be arranged between some of the turns, and a single reinforcing wire 40 may be arranged between the other turns.
[0135] Although a certain degree of effect can be achieved even if all of the multiple reinforcing wires 40 are coated with the release material layer 46, it is desirable that only one of the multiple reinforcing wires 40, 40A arranged between each turn is coated with the release material layer 46.
[0136] If one release material layer 46 is present between superconducting wires 20, an effect of reducing thermal stress occurring in superconducting wire 20 when superconducting coil 1A is cooled is achieved.
[0137] The mechanical strength of the superconducting coil 1A is improved when the multiple reinforcing wires 40, 40A are fixed to each other by the conductive resin part 12. Therefore, the mechanical strength of the superconducting coil 1A is improved by coating only one reinforcing wire 40 with the release material layer 46, which weakens the adhesive strength with the conductive resin part 12, and not coating the other reinforcing wires 40A with the release material layer 46.
[0138] According to the second embodiment, by disposing a plurality of reinforcing wires 40, 40A between turns, it is possible to improve the mechanical strength of the superconducting coil 1. Also, at least one reinforcing wire 40 can form a detour.
[0139] Third embodiment Next, a third embodiment will be described with reference to Fig. 13. Note that the same components as those shown in the above-described embodiment will be denoted by the same reference numerals and duplicated description will be omitted.
[0140] 13, in the reinforcing wire 40B of the third embodiment, both of the two wide surfaces, that is, the main surfaces 42 and 43, are coated with a release material layer 46. The two end surfaces 44 and 45 are not coated with the release material layer 46, and the reinforcing plate 41 is exposed. These end surfaces 44 and 45 are electrically connected to the conductive resin part 12 (FIG. 7).
[0141] When manufacturing this reinforcing wire 40B, first, the entire outer peripheral surface of the reinforcing plate 41 is coated with a release material layer 46. Then, the end faces 44, 45 are cut away to expose the reinforcing plate 41.
[0142] According to the third embodiment, end faces 44, 45, which are part of the outer peripheral surface of reinforcing wire 40, are connected to conductive resin part 12 (FIG. 7). In this manner, reinforcing wire 40 and conductive resin part 12 are electrically connected, so that a current that is diverted from superconducting wire 20 via conductive resin part 12 flows to reinforcing wire 40.
[0143] The superconducting coil has been described based on the first to third embodiments, but the configuration applied in any one of the embodiments may be applied to the other embodiments, or the configurations applied in each embodiment may be combined.
[0144] In the first to third embodiments described above, the superconducting coil 1 has a so-called pancake shape, but may have other shapes. For example, the above-described embodiments can be applied to coils having non-circular shapes such as saddle, elliptical, solid, and solenoid shapes.
[0145] In the above embodiment, the release material layer 46 is coated on a part of the outer peripheral surface of the reinforcing wire 40, but other configurations are also possible. For example, the release material layer 46 may be coated on the entire outer peripheral surface of the reinforcing wire 40.
[0146] According to at least one of the embodiments described above, a release material layer is applied to weaken the adhesion between the reinforcing wire and the conductive resin part compared to other parts, thereby preventing an unnecessary increase in the coil diameter, suppressing the occurrence of thermal runaway when the superconducting wire undergoes a normal conducting transition, and improving the electromagnetic force resistance performance to stably generate a strong magnetic field.
[0147] Although some embodiments of the present invention have been described, these embodiments are presented as examples and are not intended to limit the scope of the invention. These embodiments can be implemented in various other forms, and various omissions, substitutions, modifications, and combinations can be made without departing from the spirit of the invention. These embodiments or modifications thereof are within the scope of the invention and its equivalents as described in the claims, as well as within the scope and spirit of the invention. [Explanation of symbols]
[0148] 1 (1A)...superconducting coil, 2...central hole, 3...coil axial direction, 4...coil circumferential direction, 5...coil radial direction, 10...winding frame, 11...winding portion, 12...conductive resin portion, 13...insulating plate, 18...resin, 19...conductive powder, 20...superconducting wire, 21...stabilization layer, 22...metal substrate, 23...orientation layer, 24...intermediate layer, 25...superconducting layer, 26...protective layer, 27...main surface (proximal surface) , 28...main surface (distal surface), 29, 30...end surface, 40 (40A, 40B)...reinforcing wire, 41...reinforcing plate, 42, 43...main surface, 44, 45...end surface, 46...release material layer, 51 (51A, 51B)...superconducting coil, 52...insulating resin part, 53...insulating member, 54...resin layer, 55...release material, 56...insulating member with release material, 60A, 60B, 60C, 60D...detour.
Claims
1. a superconducting wire having a superconducting layer made of a superconducting material provided on one of both surfaces of a tape-shaped metal substrate; a reinforcing wire made of a tape-shaped metal material wound together with the superconducting wire; a conductive resin portion impregnated between the superconducting wire and the reinforcing wire and having electrical conductivity; Equipped with At least one of the two surfaces of the reinforcing wire is coated with a release layer that weakens the adhesion between the reinforcing wire and the conductive resin portion more than other portions. Superconducting coil.
2. A part of an outer peripheral surface of the reinforcing wire is connected to the conductive resin portion.
2. The superconducting coil according to claim 1.
3. the release material layer is coated on one of the two surfaces of the reinforcing wire material that faces the metal substrate, and the other surface is connected to the conductive resin portion; 3. The superconducting coil according to claim 1 or 2.
4. The thickness of the release material layer is smaller than the thickness of the superconducting wire and the reinforcing wire. The superconducting coil according to any one of claims 1 to 3.
5. The release material layer is made of at least one material selected from the group consisting of fluorine-based resin, paraffin, grease, and silicone oil. The superconducting coil according to any one of claims 1 to 4.
6. The reinforcing wire has a higher Young's modulus than the superconducting wire. The superconducting coil according to any one of claims 1 to 5.
7. A plurality of the reinforcing wires are wound together with the superconducting wire, and at least one of the reinforcing wires is coated with the release material layer. The superconducting coil according to any one of claims 1 to 6.
8. The reinforcing wire has a higher electrical resistance than the conductive resin portion. The superconducting coil according to any one of claims 1 to 7.
9. A step of coating at least one of both surfaces of a reinforcing wire made of a tape-shaped metal material with a release material layer that weakens adhesion between the reinforcing wire and a conductive resin part having conductivity compared to other parts; a step of winding a superconducting wire having a superconducting layer made of a superconducting material on one of both surfaces of a tape-shaped metal substrate together with the reinforcing wire; impregnating a space between the superconducting wire and the reinforcing wire with the conductive resin portion; Including, A method for manufacturing a superconducting coil.
Citation Information
Patent Citations
Method of boring work for deep drawing products
JP1978095870A
Superconducting coil device
JP2010267822A
High-temperature superconducting coil and superconducting magnet device
JP2020025014A
Conductive resin and superconducting coil using the same
JP2020149863A
Superconducting coil device
JP2021061268A