How to manufacture a solenoid tube
Fiber laser welding with specified conditions for overlap welding addresses thermal distortion and spatter issues in solenoid tube manufacturing, enhancing quality and reducing costs by minimizing surface deformation and spatter adhesion.
Patent Information
- Application Number
- JP2020039526
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-03-20
- Filing Date
- 2020-03-09
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2040-03-09
AI Technical Summary
Existing methods for manufacturing solenoid tubes, such as TIG welding and laser welding described in Patent Documents 1 and 2, result in thermal distortion and spatter adhesion, leading to increased costs and poor quality due to the need for high precision machining and strict quality control.
The method involves overlap welding using fiber laser welding on both the first and second magnetic members with specified conditions to minimize thermal distortion and spatter adhesion, ensuring high efficiency and ease of process management.
This approach reduces surface deformation and spatter adhesion, improving quality and reducing process costs while maintaining the integrity of the solenoid tube's inner surface, with minimal distortion and no visible spatter deposits.
Smart Images

Figure 0007567177000005 
Figure 0007567177000006 
Figure 0007567177000007
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for manufacturing a solenoid tube, and more particularly to a method for manufacturing a solenoid tube by welding. [Background technology]
[0002] In general, electromagnetic valves called solenoids are used to control the flow rate of fluids, etc. The main structure of a solenoid includes a tubular member having a structure in which a non-magnetic part called a tube is sandwiched between magnetic materials, a coil arranged on the outer periphery of the tube, and a movable iron core made of magnetic material housed inside the tube. 1, the tube has a structure in which a first magnetic member 10 (fixed magnetic pole) made of a tubular member made of a magnetic material and a second magnetic member 12 (magnetic rear part) also made of a tubular member made of a magnetic material are connected by a tubular non-magnetic member 11 (guide pipe) with a small space between them to create a non-magnetic region. A magnetic circuit is formed between the tube and the movable iron core by passing an electric current through a coil arranged on the outer circumferential surface side of the tube, and the position of the movable iron core is controlled by controlling the electric current, which moves the rod connected to the movable iron core, thereby turning the valve on and off.
[0003] Conventionally, TIG welding has been used to join the first and second magnetic members to the non-magnetic member. However, with TIG welding, the heat from welding causes the tube to deform, deteriorating the sliding properties of the movable iron core, which requires high-precision machining of the inner diameter after welding, resulting in a significant increase in costs.
[0004] To solve this problem, Patent Document 1 describes a method of joining a stator (corresponding to a first magnetic member), a yoke (corresponding to a second magnetic member), and a ring (corresponding to a non-magnetic member) by laser welding. It is said that the laser welding described in Patent Document 1 does not require machining of the inner diameter of the tube after welding. Furthermore, Patent Document 2 describes a structure in which a non-magnetic member is fitted to the inner periphery of a first magnetic member and a second magnetic member. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2012-38780 A [Patent Document 2] JP 2014-73018 A Summary of the Invention [Problem to be solved by the invention]
[0006] In Patent Document 1, the welding on the first magnetic member side is performed by lap welding, which is easy to manage and is efficient. However, for the second magnetic member side, the inner peripheral surface of the second magnetic member side, which is the sliding surface of the movable iron core, may be distorted due to the heat caused by welding, so butt welding with the end of the non-magnetic member is performed. However, as described in Patent Document 1, strict quality control is required for butt welding. Specifically, it was found that if there is processing variation on the end surface of the non-magnetic member or the stepped portion of the first magnetic member, imperfect parts will occur in the weld, making it necessary to increase the processing accuracy, which is a major factor in increasing costs.
[0007] In addition, Patent Document 1 does not provide any detailed description of laser welding, and it is unclear what type of laser welding is used. However, as described in detail later, the laser welding in Patent Document 1 is considered to be, for example, YAG laser welding, which is often used in this type of laser welding. When the inventors tried overlap welding with YAG laser welding, they found that a considerable laser output was required to ensure the required welding strength, and that there was a risk of distortion of the inner peripheral surface of the second magnetic member. Furthermore, they found that a large amount of spatter adhered to the welded surface, resulting in poor appearance.
[0008] The structure of Patent Document 2 is said to solve the above-mentioned distortion problem of Patent Document 1, but it requires a major design change and cannot be easily adopted.
[0009] The present invention solves the above problems, and aims to provide a method for manufacturing a solenoid tube which enables efficient lap welding with easy work management on both the first magnetic member side and the second magnetic member side, which causes little deformation of the inner surface of the tube due to thermal distortion caused by welding, and which is substantially free of spatter adhesion on the welded surface. [Means for solving the problem]
[0010] The present invention has been made for the above-mentioned purpose. A method for manufacturing a solenoid tube includes a first magnetic member made of a tubular member made of a magnetic material, a second magnetic member made of a tubular member made of a magnetic material and arranged coaxially with the first magnetic member, and a tubular non-magnetic member made of a non-magnetic material and fitted to the outer periphery of the first magnetic member and the second magnetic member to connect the first magnetic member and the second magnetic member, wherein a first step portion is formed on an outer periphery of the first magnetic member at an end portion on the non-magnetic member side, and a second step portion is formed on an outer periphery of the second magnetic member at an end portion on the non-magnetic member side, the first magnetic member and the non-magnetic member are fitted together to have portions that overlap in the circumferential direction at the first step portion, the second magnetic member and the non-magnetic member are fitted together to have portions that overlap in the circumferential direction at the second step portion, and fiber laser welding is performed on the overlapping portions from the outer periphery side to join the first magnetic member and the non-magnetic member, and the second magnetic member and the non-magnetic member are joined together.
[0011] Preferably, the first magnetic member and the non-magnetic member, and the second magnetic member and the non-magnetic member are joined so that the depth of the molten portion by welding is 110% or more of the thickness of the non-magnetic member and 85% or less of the sum of the thickness of the non-magnetic member and the thickness of the second magnetic member directly below the welded portion.
[0012] Also preferably, the fiber laser welding conditions are an output of 270 W to 400 W, a laser irradiation time of 2 seconds to 5 seconds, a downslope of 0.2 seconds to 0.4 seconds, and a peripheral speed of 2 seconds / revolution to 5 seconds / revolution. Effect of the Invention
[0013] According to the present invention, a method for manufacturing a solenoid tube can be provided in which, even when overlap welding, which is easy to control during the process, is performed by fiber laser welding, there is little deformation of the inner peripheral surface of the tube due to thermal distortion caused by welding, and there is substantially no spatter adhesion on the welded surface, making it possible to achieve both improved quality and reduced process costs. Note that, in the present invention, "substantially no spatter adhesion" means that no spatter (particulate adhesion with a particle size of 1 μm to several mm that scatters during welding) can be confirmed when the solenoid tube of the present invention is visually observed from the outer peripheral side. [Brief description of the drawings]
[0014] [Figure 1] 1 is a cross-sectional view showing a solenoid including a tube manufactured using a method for manufacturing a solenoid tube according to an embodiment of the present invention. [Diagram 2] 2 is a cross-sectional view showing a state in which the non-magnetic member 11 and the second magnetic member 12 are welded together. [Diagram 3] 1 is a cross-sectional view showing a tube manufactured using a method for manufacturing a solenoid tube according to an embodiment of the present invention. [Figure 4a] 1 is a photograph showing the appearance of a solenoid according to an embodiment of the present invention. [Figure 4b] 1 is a cross-sectional photograph of a welded portion of a solenoid in an embodiment of the present invention. [Diagram 5] 4 is data showing cylindricity and roundness of a solenoid in an embodiment of the present invention. [Figure 6a] 1 is a photograph showing the appearance of a solenoid according to an embodiment of the present invention and a photograph showing a cross section of a welded portion. [Figure 6b] 1 is a photograph showing the appearance of a solenoid according to an embodiment of the present invention and a photograph showing a cross section of a welded portion. [Figure 7] FIG. 4 is a diagram showing data on solenoid characteristics in an embodiment of the present invention. [Figure 8] 1 is data showing the roundness of solenoids in examples of the present invention and comparative examples. [Figure 9]1 is a cross-sectional photograph of a welded portion of a solenoid in an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Hereinafter, preferred embodiments of the present invention will be described with reference to the drawings.
[0016] FIG. 1 is a cross-sectional view showing a solenoid including a tube manufactured by a method for manufacturing a solenoid tube according to one embodiment of the present invention. The solenoid 100 includes a first magnetic member 10, a non-magnetic member 11, a second magnetic member 12, a coil 14, a resin member 16, a case 18, a movable core 20, a rod 22, and a spacer 24. The first magnetic member 10 is made of a magnetic material such as mild steel (e.g., SS400). The first magnetic member 10 has an attraction surface 10a that is provided substantially parallel to a plane perpendicular to the axial direction and faces the movable core 20, and includes a portion 10b (on the second magnetic member 12 side of the attraction surface 10a) on whose inner periphery the movable core 20 slides, and a portion 10c on the opposite side of the attraction surface 10a to the second magnetic member 12. In the case where the solenoid is a proportional type solenoid, 10b includes a hollow truncated cone-shaped portion whose outer diameter becomes smaller toward the tip (toward the second magnetic member side) (see FIG. 3). The non-magnetic member 11 is a cylindrical member made of a non-magnetic material such as SUS304. The second magnetic member 12 is made of a magnetic material such as mild steel (e.g., SS400). The second magnetic member 12 has a surface 12a that is substantially parallel to a plane perpendicular to the axial direction and faces the movable core 20, and includes a portion 12b (closer to the first magnetic member than the surface 12a) on whose inner periphery the movable core 20 slides, and a portion 12c that is on the opposite side of the surface 12a to the first magnetic member. The first magnetic member 10 and the second magnetic member 12 have a first step portion 10d and a second step portion 12d on whose outer periphery the non-magnetic member 11 fits, and the non-magnetic member 11 is fitted and welded to the first step portion 10d and the second step portion 12d to form a solenoid tube 200. That is, the solenoid tube 200 has a structure in which the first magnetic member 10 made of a magnetic material and the second magnetic member 12 made of the same magnetic material are connected by the non-magnetic member 11 with a small space therebetween to create a non-magnetic region. The coil 14 is wound around the solenoid tube 200 in a state where it is molded with the resin member 16. The case 18 is formed into a cylindrical shape from a magnetic material such as iron, and is attached to the solenoid tube 200 so as to cover the coil 14 and the resin member 16 from the outside. The movable core 20 is formed into a cylindrical shape, and is housed in the internal space S of the solenoid tube 200. The rod 22 is provided so as to be able to reciprocate within the solenoid tube 200 together with the movable core 20. The spacer 24 is formed, for example, into an annular shape, and is provided on the outer periphery of the rod 22 at one axial end of the movable core 20.
[0017] In such a solenoid 100, when a current is passed through the coil 14, a magnetic field H (shown by a dashed line in FIG. 1) is generated, and the movable core 20, the first magnetic member 10, and the second magnetic member 12 are magnetized. At this time, the first magnetic member 10 and the second magnetic member 12 are connected by the non-magnetic member 11 made of a non-magnetic material with a small space therebetween, so this space becomes a non-magnetic region, and the magnetic flux of the magnetic field H generated by the coil 14 avoids this region and reaches the movable core 20 via the first magnetic member 10 and the second magnetic member 12. This allows the movable core 20 to be strongly magnetized. Before a current is passed through the coil 14, the end face of the movable core 20 on the second magnetic member 12 side is in contact with the surface 12a, but the movable core 20 magnetized by the magnetic field H generated by passing a current through the coil 14 is attracted to the magnetized first magnetic member 10, and the movable core 20 and the rod 22 move inside the tube to the position shown in FIG. 1. The rod 22 is constantly biased toward the surface 12a by a spring (not shown) or the like, and when the supply of current to the coil 14 is stopped, the movable core 20 and the rod 22 move toward the surface 12a.
[0018] When the solenoid 100 is used as a proportional solenoid, the tip of the portion 10b of the first magnetic member 10 is formed in a truncated cone shape, so that the position of the movable core 20 can be controlled by the magnitude of the current flowing through the coil 14 (see FIG. 3).
[0019] Examples of magnetic materials constituting the first magnetic member 10 and the second magnetic member 12 include iron-based materials such as the above-mentioned SS400, as well as magnetic stainless steels such as SUS430, and examples of non-magnetic materials constituting the non-magnetic member 11 include the above-mentioned SUS304, as well as non-magnetic stainless steels such as SUS303, SUS316, and SUS321, Cu-based alloys such as brass and bronze, and aluminum alloys.
[0020] A method for manufacturing the solenoid tube 200 according to one embodiment of the present invention will now be described.
[0021] 2, one end side of the non-magnetic member 11 is fitted into the second step portion 12d of the second magnetic member 12. Next, fiber laser welding is performed from the outer periphery side on the portion where the non-magnetic member 11 and 12b of the second magnetic member 12 overlap (for example, position A), to weld the non-magnetic member 11 and the second magnetic member 12 together.
[0022] Next, as shown in Figure 3, the movable core 20, rod 22, and spacer 24 are accommodated on the inner side of the second magnetic member 12 to which the non-magnetic member 11 is joined by welding, and the other end of the non-magnetic member 11 is fitted into the first step portion 10d of the first magnetic member 10. Fiber laser welding is then performed from the outer side at the portion where the non-magnetic member 11 and 10c of the first magnetic member 10 overlap (for example, position B), to weld the non-magnetic member 11 and the first magnetic member 10.
[0023] The welding of the first magnetic member 10 and the non-magnetic member 11, and the welding of the second magnetic member 12 and the non-magnetic member 11 are performed so that the melted portion by welding does not penetrate the non-magnetic member 11 and does not penetrate the first magnetic member 10 and the second magnetic member 12, respectively, but in order to ensure a reliable joining and to avoid the risk of distortion of the inner circumferential surface, it is preferable to perform the welding so that the penetration depth (depth of the melted portion) is 110% or more of the thickness of the non-magnetic member 11, 85% or less of the sum of the thickness of the non-magnetic member 11 and the thickness of the first magnetic member 10 directly below the welded portion, and 85% or less of the sum of the thickness of the non-magnetic member 11 and the thickness of the second magnetic member 12 directly below the welded portion. It is more preferable that the penetration depth is 80% or less of the sum of the thickness of the non-magnetic member 11 and the thickness of the first magnetic member 10 directly below the welded portion, and 80% or less of the sum of the thickness of the non-magnetic member 11 and the thickness of the second magnetic member 12 directly below the welded portion.
[0024] The series of assembly steps of fitting the non-magnetic member 11 into the second magnetic member 12, accommodating members such as the movable core 20, and fitting the non-magnetic member 11 into the first magnetic member 10 may be performed first, and then the fiber laser welding of the two locations A and B may be performed successively. The order of the steps may be determined according to the shape of each part, etc.
[0025] In FIG. 3, position B does not contact the back side of the inner circumferential surface of the tube on which the movable iron core 20 slides, so in Patent Document 1, the corresponding portion is laser welded. However, position A contacts just the back side of the inner circumferential surface of the tube on which the movable iron core 20 slides, and if the tube is deformed (distorted) by the heat of welding, the sliding property of the movable iron core 20 deteriorates. In Patent Document 1, in order to prevent this inner circumferential surface from being distorted by the heat of welding, the second magnetic member 12 side is welded at the butt joint (position C). Patent Document 1 does not provide a detailed description of laser welding. The only thing that can be read is that when the second magnetic member 12 and the non-magnetic member 11 are overlap-welded, there is a risk that the inner circumferential surface of the second magnetic member 12 will be distorted, but when butt-welded, there will be no distortion. Butt welding allows welding not only in the depth direction but also in the circumferential direction (surface direction), so the output can be relatively low and the penetration depth required for welding can be made shallow. As shown in the examples described later, in order to deepen the penetration depth and ensure the required welding strength in overlap welding using a YAG laser, the output must be significantly increased, and there is a risk of the inner circumferential surface of the second magnetic member 12 being distorted. Therefore, it is presumed that the laser welding in Patent Document 1 is performed using a high-output laser such as a YAG laser. However, in butt welding, if there is a gap between the non-magnetic member 11 and the step portion 12d at position C, the welding may be incomplete, and high part precision is required to avoid creating a gap, and strict process control is required, which is a factor in increasing costs. Therefore, the inventors have studied a welding method that can obtain the required penetration depth at low output even when overlap welding is performed at position A, and have found that by adopting fiber laser welding and performing welding under specified conditions, it is possible to weld with a welding strength that satisfies the required sealing characteristics and pressure resistance characteristics without causing significant distortion and deformation of the inner circumferential surface of the tube.
[0026] The conditions for fiber laser welding depend on the material properties and thickness of the portion 12b of the second magnetic member 12 and the non-magnetic member 11, but are set so that the molten portion penetrates the non-magnetic member 11 but does not penetrate the portion 12b of the second magnetic member 12. Specifically, it is preferable that the output is 270 W to 400 W, the laser irradiation time is 2 seconds to 5 seconds, the downslope is 0.2 seconds to 0.4 seconds, and the peripheral speed is 2 seconds / revolution to 5 seconds / revolution.
[0027] Fiber laser welding can be used at a high processing speed (within 3 seconds of tact time) and with a deep penetration depth, and is less affected by heat than conventional laser welding such as YAG laser. According to the present invention, it is possible to manufacture a tube with a circularity of the inner circumferential surface of preferably 10 μm or less, more preferably 10 μm or less and 5 μm or less, with little deformation and no problem with the sliding of the movable iron core. In addition, since the laser light is a continuous wave with a strong and accurately focused beam, it is possible to accurately weld a narrow area, the weld mark is narrow, and the physical distortion caused to the welded part is small. In addition, there is almost no spatter adhesion at the weld mark. However, on the other hand, since the weld mark is narrow, it is relatively unsuitable for butt welding, and there is a risk of incomplete welding in particular if the butt part is not accurately aligned. EXAMPLES
[0028] [Comparison of welding conditions] Example 1 For the welding methods and welding locations in Table 1, the non-magnetic member 11 and the second magnetic member 12 were welded as shown in Figure 2, and the welded state and the deformation of the inner circumferential surface of the second magnetic member 12 were compared and evaluated. The deformation of the inner circumferential surface was evaluated by evaluating the cylindricity and roundness of the inner circumferential surface of the sample. The thickness of the non-magnetic member 11 used in the experiment was 0.68 mm, and the thickness of the second magnetic member 12b portion (equal to the sum of the thickness of the non-magnetic member 11 and the thickness (1.52 mm) directly below the second step portion 12d) was 2.2 mm.
[0029] [Table 1]
[0030] The welding point A is an overlap welding, and C is a butt welding. The welding conditions were adjusted so that the penetration depth was the value in the table (1.0 mm: 147% of the thickness of the non-magnetic member 11 and 45% of the thickness of the second magnetic member 12b, and 1.6 mm: 235% of the thickness of the non-magnetic member 11 and 73% of the thickness of the second magnetic member 12b). Specifically, the fiber laser welding conditions were the output value in the table, the laser irradiation time 3 seconds (one revolution), and the downslope time 0.3 seconds, and the TIG welding conditions were a base current of 80 A, a pulse current of 40 A, a pulse frequency of 100 Hz, a peripheral speed of 20 seconds, and a downslope of 4 seconds. The penetration depth was evaluated by etching the weld cross section with ferric chloride solution and determining the part where the color tone changed as the penetration part.
[0031] For each welded sample, the appearance was evaluated and a sealing test (no air leak when pressurized for 30 seconds with an air pressure of 0.49 to 0.63 MPa was performed, rated as ◯). The results are shown in Table 1. For the appearance of Example 1-1, a photograph of another sample welded under the same conditions is shown in FIG. 4a. As shown in FIG. 3, this sample is a sample in which both the first magnetic member 10 side and the second magnetic member 12 side are welded under the same conditions as Example 1-1. Also, a cross-sectional photograph of the welded portion is shown in FIG. 4b. Also, the cylindricity and roundness of Example 1-1 were evaluated. The results are shown in FIG. 5. The cylindricity and roundness were evaluated using a roundness / cylindricity measuring device at two locations, directly below part A and 9 mm behind part A (second magnetic member 12 side). The cylindricity was 3.5 μm, and the roundness directly below part A was 2.0 μm.
[0032] From Table 1, Figures 4a and 4b, when overlap welding was performed by fiber laser welding, there was no spatter adhesion on the exterior even when welding was performed at an output that could obtain sufficient penetration depth, and the sealing test was also passed. At an output of 500W, some burning was observed on the exterior, but it was within a range that was not problematic. Also, from Figure 5, the tube after fiber laser welding satisfied the cylindricity of 10 μm or less and the roundness of 5 μm or less, and almost no distortion was observed. When butt welding was performed by fiber laser welding, an incompletely welded part (gap) was found in one of the 100 samples produced. It is considered that the gap generated by the processing variation of the non-magnetic member 11 and the variation of the press-fitting work into the rear magnetic pole 12 could not be filled by welding. Furthermore, in the case of TIG welding in Comparative Example 1-2, there was no adhesion on the exterior, but there was a lot of burning, and although an attempt was made to evaluate the cylindricity and roundness, the distortion was too large to measure. Therefore, the inner surface of the tube after TIG welding was processed and then measured, and the cylindricity was 17.1 μm and the roundness was 6.7 μm. In the case of TIG welding, even if butt welding was performed, both the cylindricity and the roundness were significantly deteriorated, and the deformation immediately below the welded part in particular was remarkable.
[0033] Example 2 Welded samples similar to those in Example 1 were produced by changing the fiber laser welding conditions, and the penetration depth and appearance of each sample were evaluated. The welding conditions and evaluation results are shown in Table 2. In this example, the thickness of the non-magnetic member 11 was 0.68 mm, and the thickness of the second magnetic member 12b portion (equal to the sum of the thickness of the non-magnetic member 11 and the thickness (1.52 mm) directly below the second step portion 12d) was 2.2 mm.
[0034] [Table 2]
[0035] As can be seen from Table 2, the penetration depth was 0.8 mm or more and 1.6 mm or less under various welding conditions (118% or more and 235% or less of the thickness of the non-magnetic member 11 and 36% or more and 73% or less of the thickness of the second magnetic member 12b). Regarding the appearance, some burning was observed on the inner circumferential surface under the output condition of 500 W, but this was within the range of no problem, and no spatter adhesion was observed under all conditions.
[0036] Example 3 For the welding method and welding conditions in Table 3, the non-magnetic member 11 and the second magnetic member 12 were welded as shown in FIG. 2, and the weld state, deformation of the inner peripheral surface of the second magnetic member 12, evaluation of appearance, and sealing test were compared and evaluated. The evaluation of the deformation of the inner peripheral surface was performed by evaluating the roundness of the inner peripheral surface of the sample. The appearance evaluation was performed by evaluating the presence or absence of spatter adhesion and burning. The sealing test was also passed (◯) when no air leak was observed when pressurized with an air pressure of 0.49 to 0.63 MPa for 30 seconds. The thickness of the non-magnetic member 11 used in the experiment was 0.67 mm, and the total thickness of the non-magnetic member 11 and the thickness (1.525 mm) directly below the second step portion 12d was 2.195 mm. The roundness was evaluated at the welded portion directly below part A, and the non-welded portion was 10 mm behind part A (second magnetic member 12 side). The welding conditions and evaluation results are shown in Table 3. FIG. 8 shows the measurement results of the roundness, and FIG. 9 shows a cross-sectional view of Example 3-3 as an example of a cross-sectional view of a welded portion.
[0037] [Table 3]
[0038] As can be seen from Table 3, the penetration depth was 0.80 mm or more and 1.83 mm or less under various welding conditions (119% or more and 273% or less of the thickness of the non-magnetic member 11, and 36% or more and 83% or less of the sum of the thickness of the non-magnetic member 11 and the thickness directly below the second step portion 12d). Regarding the appearance, there was no spatter adhesion under all conditions, and the state of the burn was within a range that was not problematic. Regarding the roundness, the roundness was lower than the roundness of TIG welding (after inner surface processing) under all conditions (Comparative Example 1-2, 6.7 μm, also shown in FIG. 8), and especially under conditions of output of 400 W or less, it was 3.5 μm or less, and almost no distortion was observed.
[0039] (Comparative Example) As comparative examples, welded samples similar to those in Example 1 were prepared by changing the YAG laser welding conditions, and the penetration depth and appearance were evaluated. The welding conditions and results are shown in Table 3. The appearance and cross-sectional photographs of Comparative Examples 2-3 and 2-4 are shown in Figures 6a and 6b.
[0040] [Table 4]
[0041] When welding was performed with a peak power (1.8 kW) equivalent to fiber laser welding (output 300 W in Examples 1-1, 2-2, 2-3, and 2-4), the penetration depth was 0.5 mm, did not reach the second magnetic member, and it was not possible to join the non-magnetic member 11 and the second magnetic member 12. Furthermore, as a result of experiments with increased peak power, a lot of spatter adhesion occurred near the welded portion, and particularly the sample with a peak power of 4 kW (fiber laser equivalent output 500 W) had a very large amount of spatter adhesion.
[0042] [Solenoid characteristics] Example 3 The solenoid tube shown in Fig. 3 was produced according to the manufacturing method described in the embodiment. The welding was performed by overlap welding of parts A and B, and the welding conditions were the same as those of Example 1-1 in Table 1. The solenoid characteristics of the produced tube, such as suction force, sealing, and pressure resistance, were confirmed.
[0043] ·Suction power characteristics First, the attractive force characteristics were evaluated. Measurements were made using an attractive force measuring device, measuring the attractive force against the stroke (movement of the movable iron core) for current values of 0.2A, 0.4A, and 0.6A. The results are shown in Figure 7. For comparison, the data for TIG welded products is shown by the dotted line in Figure 7.
[0044] As can be seen from Fig. 7, in the case of TIG welding, the hysteresis width changes significantly before and after welding, whereas in the case of fiber laser welding, the suction force characteristics change very little before and after welding. This also shows that the effect of thermal distortion in fiber laser welding is small.
[0045] Sealing properties Next, the sealing characteristics were evaluated. An air leak tester was used for the measurement. Air pressure was applied at 0.49 to 0.63 MPa for 30 seconds, and the presence or absence of leaks was checked. It was confirmed that there were no leaks and that the seal was completely sealed.
[0046] Pressure resistance characteristics A burst test was conducted to confirm the static pressure resistance. A hydraulic jack and a pressure gauge were used for the measurements. Even when a high pressure of 80 MPa was applied, there was no oil leakage, and it was confirmed that the static pressure resistance was sufficient. [Industrial Applicability]
[0047] The present invention can provide a method for manufacturing a solenoid tube in which, even when lap welding is performed, which is easy to control the process, there is little deformation of the inner surface of the tube due to thermal distortion caused by welding, and there is substantially no spatter deposit on the welded surface, and the method has industrial applicability in that it makes it possible to achieve both improved quality and reduced process costs. [Explanation of symbols]
[0048] 10 First magnetic member 11 Non-magnetic materials 12 Second magnetic member 14 Coil 16 Resin parts 18 cases 20 Movable core 22 Rod 24 Spacer 100 Solenoid 200 Solenoid tube A, B, C welds
Claims
[Claim 1] A method for manufacturing a solenoid tube having a first magnetic member made of a tubular member made of a magnetic material, a second magnetic member arranged coaxially with the first magnetic member and made of a magnetic material, and a tubular non-magnetic member made of a non-magnetic material, fitted to outer peripheries of the first magnetic member and the second magnetic member, and connecting the first magnetic member and the second magnetic member, comprising: a first step portion is formed on an outer peripheral surface of the first magnetic member at an end portion on the non-magnetic member side, and a second step portion is formed on an outer peripheral surface of the second magnetic member at an end portion on the non-magnetic member side, the first magnetic member and the non-magnetic member are fitted together so as to have portions that overlap in a circumferential direction at the first step portion, and the second magnetic member and the non-magnetic member are fitted together so as to have portions that overlap in a circumferential direction at the second step portion, A method for manufacturing a solenoid tube, characterized in that fiber laser welding is performed on the overlapping portions from the outer periphery under conditions of an output of 270 W to 400 W, a laser irradiation time of 2 to 5 seconds, a downslope of 0.2 to 0.4 seconds, and a peripheral speed of 2 to 5 seconds / periphery, thereby joining the first magnetic member and the non-magnetic member, and the second magnetic member and the non-magnetic member, so that the depth of the molten portion by welding is 110% or more of the thickness of the non-magnetic member and 85% or less of the sum of the thickness of the non-magnetic member and the thickness of the second magnetic member directly below the welded portion, the bead width is 0.66 mm to 1.78 mm, and the circularity of the inner periphery of the solenoid tube is 3.5 μm or less.
Citation Information
Patent Citations
Electromagnet device
JP1987145705A
Solenoid valve
JP1999063281A
Solenoid driven part
JP2001146981A
Method of manufacturing valve device and its manufacturing device