Polymer electrolyte membrane for redox flow batteries
A polymer electrolyte membrane with optimized mole fractions and molecular weight, incorporating sulfonic acid groups, addresses the challenges of proton conductivity, mechanical strength, and chemical stability in redox flow batteries, ensuring high efficiency and long-term durability.
Patent Information
- Application Number
- JP2020107426
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-06-25
- Filing Date
- 2020-06-23
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2040-06-23
AI Technical Summary
Conventional polymer electrolyte materials for redox flow batteries face challenges in achieving high proton conductivity, active material barrier properties, mechanical strength, and chemical stability, particularly in strong oxidizing atmospheres, leading to issues like membrane swelling, reduced mechanical strength, and insufficient durability.
A polymer electrolyte membrane with specific mole fractions of repeating units derived from aromatic dihalide, diol, and electron-withdrawing groups, combined with a hydrocarbon polymer having a weight average molecular weight of 420,000 or more, and containing sulfonic acid groups, which enhances proton conductivity, mechanical strength, and chemical stability.
The membrane achieves high efficiency, self-discharge suppression, and long-term durability by reducing membrane swelling and improving mechanical properties, while maintaining low active material permeation, thus enhancing the performance of redox flow batteries.
Smart Images

Figure 0007567224000001 
Figure 0007567224000002 
Figure 0007567224000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a polymer electrolyte membrane for a redox flow battery, which is excellent in practical use and can achieve high efficiency and long-term durability of the redox flow battery. [Background technology]
[0002] In recent years, the use of renewable energy sources such as solar and wind power has been increasing. However, the amount of power generated fluctuates greatly due to factors such as solar radiation and wind speed, and there is a demand for large-scale storage battery systems that can stabilize the output of renewable energy, level the power load, and stabilize the power grid. Among these large-scale storage batteries, redox flow batteries are becoming more widely used due to their large capacity, high safety, and excellent durability.
[0003] Redox flow batteries use an oxidation-reduction reaction on electrodes made of active materials such as vanadium, titanium, and manganese, and are repeatedly charged and discharged by pump circulation within the battery. In the case of vanadium-based electrolyte, since only one type of element is used, there is no deterioration of the electrolyte and it can be reused semi-permanently.
[0004] In redox flow batteries, polymer electrolyte membranes are used as a separator that separates two types of electrolytes with different valences. Required properties of polymer electrolyte membranes for redox flow batteries include high proton conductivity, high active material blocking properties to function as a barrier layer that prevents a decrease in battery output and energy efficiency due to active material crossover, chemical stability to withstand a strong oxidizing atmosphere, dimensional stability, and mechanical strength to withstand use.
[0005] Nafion (registered trademark), a perfluorosulfonic acid polymer (manufactured by DuPont), has been widely used as an electrolyte membrane for redox flow batteries. Nafion (registered trademark) is very expensive because it is produced through a multi-stage synthesis, and has the problem of large crossover due to the formation of a cluster structure. In addition, there are problems such as low mechanical strength of the membrane, poor dimensional stability, poor handling, and further problems of waste disposal after use and difficulty in recycling materials. Perfluorosulfonic acid-based membranes have roughly balanced characteristics as polymer electrolyte membranes, but as the practical application of such batteries progresses, further improvement of their characteristics has been required.
[0006] In order to overcome these drawbacks, some efforts have already been made on polymer electrolyte materials based on non-perfluorinated hydrocarbon polymers. As polymer skeletons, aromatic polyether ketones and aromatic polyether sulfones have been actively studied in particular from the viewpoints of heat resistance and chemical stability (Patent Documents 1 to 3, Non-Patent Documents 1 to 3).
[0007] Patent Documents 4 and 5 describe a hydrocarbon-based polymer electrolyte material that combines proton conductivity and methanol blocking properties. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] Japanese Patent Application Publication No. 6-93114 [Patent Document 2] Special Publication No. 2004-528683 [Patent Document 3] US Patent Application Publication No. 2002 / 0091225 [Patent Document 4] JP 2008-66273 A [Patent Document 5] JP 2008-239963 A [Non-patent literature]
[0009] [Non-Patent Document 1] Polymer,1987,vol.28,p-1009 [Non-Patent Document 2] Journal of Membrane Science,83(1993)p-211~220 [Non-Patent Document 3] Macromolecules,1987,vol.20,p-1204 DISCLOSURE OF THEINVENTION [Problem to be solved by the invention]
[0010] When the polymer electrolyte materials described in Patent Documents 1-3 and Non-Patent Documents 1-3 are used in redox flow batteries, increasing the ionic group content to enhance proton conductivity leads to increased swelling of the membrane, which causes problems such as increased crossover of the active material and reduced mechanical strength, making it difficult to achieve both proton conductivity and active material barrier properties and mechanical strength. In addition, there is also a problem with chemical durability, in that the hydrocarbon polymer skeleton decomposes in a strong oxidizing atmosphere.
[0011] When the polymer electrolyte materials described in Patent Documents 4 and 5 are used in redox flow batteries, there is a problem in that the chemical stability is insufficient in the strong oxidizing atmosphere of the redox flow battery.
[0012] As described above, the polymer electrolyte materials according to the prior art are insufficient as a means for improving proton conductivity, active material blocking property, dimensional stability, mechanical strength, and chemical stability, and have not been industrially useful polymer electrolyte materials for redox flow batteries.
[0013] In view of the background of the conventional technology, the present invention provides a polymer electrolyte membrane for redox flow, which has excellent proton conductivity, excellent active material blocking properties, mechanical strength, and chemical stability, and is also highly practical in that it can achieve high efficiency, suppression of self-discharge, and long-term durability when used in a redox flow battery. [Means for solving the problem]
[0014] In order to solve the above problems, the polymer electrolyte membrane for a redox flow battery of the present invention has the following configuration. The polymer electrolyte membrane for redox flow batteries is characterized by using a polymer electrolyte material having a molar fraction of repeating units derived from an aromatic dihalide compound represented by the following general formula (Q1) of 15 mol% or more and 25 mol% or less, a molar fraction of repeating units derived from a compound represented by general formula (Q2) of 25 mol% or more and 35 mol% or less, a molar fraction of repeating units derived from an aromatic diol compound represented by general formula (Q3) of 25 mol% or more and 50 mol% or less, and a molar fraction of repeating units derived from at least one compound selected from compounds represented by general formulas (X-1) and (X-2) of 30 mol% or less, and a weight average molecular weight Mw of 420,000 or more.
[0015] [ka]
[0016] [ka]
[0017] [ka]
[0018] [ka]
[0019] (In general formulas (Q1) to (Q3), X 1 and X 2 is an electron-withdrawing group, Y is an ionic group, Z 1 and Z 2 is halogen, D 3 is oxygen or sulfur, A 3 represents a divalent organic group containing an aromatic ring. 3 has a protecting group. The weight-average molecular weight Mw used here was calculated using N-methyl-2-pyrrolidone solvent (10 mmol L lithium bromide) -1 The weight average molecular weight is determined by gel permeation chromatography using N-methyl-2-pyrrolidone (containing N-methyl-2-pyrrolidone as a mobile phase) as a solvent. The weight average molecular weight is relative to the molecular weight of standard polystyrene.
[0020] The polymer electrolyte membrane for redox flow batteries of the present invention has a tetravalent vanadium concentration of 1.5 mol L at 25°C. -1 , sulfuric acid concentration 3.0mol·L -1 The amount of active material permeated through the aqueous solution is 800×10 -7 It is preferable that the speed is equal to or less than cm / min.
[0021] In the polymer electrolyte membrane for a redox flow battery of the present invention, the polymer electrolyte material preferably contains a hydrocarbon-based polymer having an ionic group.
[0022] In the polymer electrolyte membrane for redox flow batteries of the present invention, the ionic group is preferably a sulfonic acid group.
[0023] In the polymer electrolyte membrane for redox flow batteries of the present invention, the polymer electrolyte material preferably has a sulfonic acid group density of 1.0 to 3.0 mmol / g.
[0024] In the polymer electrolyte membrane for a redox flow battery of the present invention, it is preferable that the polymer electrolyte material does not contain a crosslinked structure. Effect of the Invention
[0025] According to the present invention, it is possible to provide a polymer electrolyte material for redox flow batteries, which is excellent in practical use and can achieve high efficiency, suppression of self-discharge, and long-term durability, and a polymer electrolyte membrane for redox flow batteries using the same. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0026] The present invention will be described in detail below.
[0027] When conventional sulfonated aromatic polyether ketones and sulfonated aromatic polyether sulfones are used as polymer electrolyte materials, there are problems in that increasing the content of ionic groups in order to enhance proton conductivity causes the membrane to swell, resulting in poor handleability. There are also problems in that the cohesive strength of the polymer molecular chains is low, resulting in poor stability of the polymer higher-order structure, resulting in insufficient mechanical strength and physical durability of the membrane.
[0028] In addition, aromatic polyether ketone (PEK) polymers exhibit crystallinity due to their excellent packing and extremely strong intermolecular cohesive force, and have the property of being completely insoluble in general solvents. In contrast, the polymer electrolyte material of the present invention contains a protecting group in the polymer, thereby reducing the crystallinity of crystalline polymers such as PEK polymers, which have often been difficult to form into films, and thereby imparting solubility to the polymer, making it possible to form films.
[0029] In addition, after being formed into a membrane or the like, some of the protecting groups are deprotected to improve the packing of the molecular chains of the polymer and to impart intermolecular cohesion and crystallinity again, thereby obtaining a polymer electrolyte material with significantly improved hot water resistance, mechanical properties such as tensile strength and elongation, tear strength and fatigue resistance, and active material blocking properties such as vanadium, titanium, manganese, etc. When this production process is performed, the polymer electrolyte membrane of the present invention has the characteristics of being able to simultaneously achieve high proton conductivity, as well as membrane formability (processability), production costs, hot water resistance, active material blocking properties, and mechanical properties.
[0030] Furthermore, the polymer electrolyte membrane obtained by the present invention has a property that it is extremely resistant to tearing even in a hydrated state due to its strong intermolecular cohesive force, i.e., it has high tear strength, and is characterized in that it can achieve extremely excellent long-term durability even in redox flow batteries.
[0031] Furthermore, it has become possible to form a membrane of a crystalline polymer having a low sulfonic acid group density, which could not be used until now due to insufficient solubility, and it has been possible to successfully obtain a polymer electrolyte membrane of the present invention which achieves both proton conductivity and active material blocking effect, and which has excellent hot water resistance, mechanical properties, physical durability, and long-term durability.
[0032] The present inventors have already reported on polymer electrolyte materials containing at least a protecting group and an ionic group. However, in the present invention, they found that the dimensional stability, active material blocking property and long-term durability of the polymer electrolyte material are largely dependent on the structure of the soluble polymer electrolyte material for molding before deprotection. They also attempted to introduce groups containing no protecting groups together with groups containing protecting groups, investigated the ratio of groups containing protecting groups to groups containing no protecting groups, investigated the relationship between the amount of ionic groups and the amount of protecting groups, and investigated in detail the relationship between the structures used and the membrane performance, and thus completed the present invention.
[0033] The polymer electrolyte membrane of the present invention has a tetravalent vanadium (active material) concentration of 1.5 mol L at 25°C. -1 , sulfuric acid concentration 3.0mol·L -1 The amount of active material permeated per unit area through the aqueous solution is 800×10 -7 In redox flow batteries, the lower the active material permeation amount, i.e., the higher the active material barrier property, the more the self-discharge due to active material crossover can be suppressed, and the more the current efficiency and the energy efficiency during repeated charge and discharge can be improved. The vanadium ion (IV valence) permeation amount is -1 , sulfuric acid concentration 3.0mol·L -1 The measurement is performed after immersing the polymer electrolyte membrane in the aqueous solution for 24 hours. -7cm / min or less is preferable, and 200×10 -7 The lower limit is not particularly limited, but from the viewpoint of ensuring proton conductivity, it is preferably 1×10 -7 cm / min or more is preferable, and 10×10 -7 More preferably, the speed is equal to or faster than cm / min.
[0034] The polymer electrolyte membrane for redox flow batteries of the present invention has excellent ion selective permeability, and can simultaneously achieve the above-mentioned low active material permeation amount and high proton conductivity, and is excellent in that it can improve the energy efficiency of charging and discharging.
[0035] In redox flow batteries, especially when the active material is vanadium ions, pentavalent vanadium ions are generated on the positive electrode side during charging. Pentavalent vanadium ions have a very high oxidizing power, so they generally easily decompose hydrocarbon-based polymer electrolyte membranes, making it extremely difficult to achieve both performance and oxidation resistance. Therefore, improving the oxidation resistance of hydrocarbon-based polymer electrolyte membranes is very effective. In order to improve oxidation resistance, a polymer structure design with reduced electron density is necessary, and the present invention has achieved a polymer electrolyte material and polymer electrolyte membrane for redox flow batteries with high oxidation resistance, which are described in detail below.
[0036] The polymer electrolyte material used in the present invention must have a molar fraction of repeating units derived from an aromatic dihalide compound represented by general formula (Q1) of 15 mol% or more and 25 mol% or less, a molar fraction of repeating units derived from a compound represented by general formula (Q2) of 25 mol% or more and 35 mol% or less, a molar fraction of repeating units derived from an aromatic diol compound represented by general formula (Q3) of 25 mol% or more and 50 mol% or less, and a molar fraction of repeating units derived from at least one compound selected from a compound represented by general formula (X-1) or a compound represented by general formula (X-2) of 30 mol% or less. Among these, the molar fraction of repeating units derived from an aromatic dihalide compound represented by general formula (Q1) is more preferably 17 mol% or more and 23 mol% or less, and even more preferably 19 mol% or more and 21 mol% or less, in terms of the balance between proton conductivity, dimensional stability, and mechanical strength. The molar fraction of the repeating unit derived from the aromatic dihalide compound represented by general formula (Q3) is more preferably 30 mol% or more and 45 mol% or less, and even more preferably 35 mol% or more and 40 mol% or less, in terms of the balance between processability, filterability, dimensional stability and mechanical strength. The compounds represented by general formula (X-1) or (X-2) have the effect of improving the processability and filterability of a polymer electrolyte material having a rigid skeleton, and the molar fraction of the repeating unit derived from these compounds varies depending on the usage environment and grade of the electrolyte membrane, so the molar fraction includes 0 mol%.
[0037] If the molar fraction of the repeating unit derived from the aromatic dihalide compound represented by general formula (Q1) is less than 15 mol%, the proton conductivity may be insufficient, and if the molar fraction of the repeating unit is more than 25 mol%, the dimensional stability and molecular weight may be insufficient. If the molar fraction of the repeating unit derived from the aromatic diol compound represented by general formula (Q3) is less than 25 mol%, the processability may be insufficient, and if the molar fraction of the repeating unit is more than 50 mol%, the dimensional stability, mechanical properties, and durability may be insufficient.
[0038] In the polymer electrolyte material used in the present invention, the repeating units derived from the aromatic dihalide compound represented by general formula (Q1) also have the effect of imparting solubility, so when there are many repeating units derived from the aromatic dihalide compound represented by general formula (Q1), it is possible to reduce the copolymerization ratio of the repeating units derived from the aromatic diol compound represented by general formula (Q3). In other words, it is preferable to copolymerize only the amount of repeating units derived from the aromatic diol compound represented by general formula (Q3) required for processability.
[0039] In the present invention, the aromatic polyether polymer means a polymer mainly composed of aromatic rings, in which an ether bond or a thioether bond is included as a mode of linking aromatic ring units. In addition to ether bonds and thioether bonds, direct bonds, ketones, sulfones, various alkylenes, imides, amides, esters, urethanes, and other bonds that are generally used in the formation of aromatic polymers may be present. It is preferable that there are at least one ether or thioether bond per repeating unit of the main constituent. The aromatic ring may include not only a hydrocarbon aromatic ring but also a heterocycle. In addition, some aliphatic units may constitute the polymer together with the aromatic ring unit. The aromatic unit may have any substituent, such as an alkyl group, an alkoxy group, an aromatic group, a hydrocarbon group such as an aryloxy group, a halogen group, a nitro group, a cyano group, an amino group, a halogenated alkyl group, a carboxyl group, a phosphonic acid group, or a hydroxyl group.
[0040] Moreover, the aromatic polyetherketone polymer is a general term for a polymer having at least an ether bond or a thioether bond and a ketone bond in its molecular chain, and includes polyetherketone, polyetherketoneketone, polyetheretherketone, polyetheretherketoneketone, polyetherketoneetherketoneketone, polyetherketonesulfone, polyetherketonephosphineoxide, polyetherketonenitrile, etc., and is not limited to a specific polymer structure. Those containing a small amount of phosphine oxide or nitrile are preferred because the ionic group-containing polymer having a protecting group has sufficient solvent solubility, and those containing a small amount of sulfone are preferred because they have sufficient crystallinity and solvent resistance such as hot water resistance.
[0041] The ionic group Y used in the polymer electrolyte material used in the present invention is not particularly limited as long as it is an atomic group having a negative charge, but it is preferable that it has a proton exchange ability. As such functional groups, sulfonic acid groups, sulfonimide groups, sulfate groups, phosphonic acid groups, phosphoric acid groups, and carboxylic acid groups are preferably used. Here, the sulfonic acid group means a group represented by the following general formula (f1), the sulfonimide group means a group represented by the following general formula (f2) [in the general formula, R represents any atomic group. ], the sulfate group means a group represented by the following general formula (f3), the phosphonic acid group means a group represented by the following general formula (f4), the phosphoric acid group means a group represented by the following general formula (f5) or (f6), and the carboxylic acid group means a group represented by the following general formula (f7).
[0042] [ka]
[0043] Such an ionic group includes the functional groups (f1) to (f7) in the form of a salt. The cation that forms the salt may be any metal cation, NR 4 +(R is any organic group) and the like can be mentioned as examples. In the case of a metal cation, the valence and the like are not particularly limited and can be used. Specific examples of preferred metal ions include Li, Na, K, Rh, Mg, Ca, Sr, Ti, Al, Fe, Pt, Rh, Ru, Ir, Pd, and the like. Among them, Na and K are more preferably used as polymer electrolyte materials because they are inexpensive, do not adversely affect solubility, and can be easily proton-substituted.
[0044] The polymer electrolyte material may contain two or more of these ionic groups, and a combination of these groups may be preferable. The combination is appropriately determined depending on the structure of the polymer. Among these, it is more preferable to have at least a sulfonic acid group, a sulfonimide group, and a sulfate group from the viewpoint of high proton conductivity, and it is most preferable to have at least a sulfonic acid group from the viewpoint of hydrolysis resistance.
[0045] Methods for introducing an ionic group into these electrolyte polymers include a method of polymerization using a monomer having an ionic group and a method of introducing an ionic group by a polymer reaction. In the present invention, the method of polymerization using a monomer having an ionic group is used.
[0046] The method of polymerization using a monomer having an ionic group may be to use a monomer having an ionic group in the repeating unit, and if necessary, to introduce a suitable protecting group and perform deprotection after polymerization. Such a method is described, for example, in Journal of Membrane Science, 197, 2002, p. 231-242.
[0047] To explain the method of introducing an ionic group, for example, the introduction of a phosphonic acid group into an aromatic ring can be performed by the method described in Polymer Preprints, 51, 2002, p-750, etc. The introduction of a phosphoric acid group into an aromatic ring can be performed by, for example, phosphorylating an aromatic polymer having a hydroxyl group. The introduction of a carboxylic acid group into an aromatic ring can be performed by, for example, oxidizing an aromatic polymer having an alkyl group or a hydroxyalkyl group. The introduction of a sulfate group into an aromatic ring can be performed by, for example, sulfate-esterifying an aromatic ring having a hydroxyl group. As a method of sulfonating an aromatic ring, i.e., a method of introducing a sulfonic acid group, a method described in, for example, JP-A-2-16126 or JP-A-2-208322 is known.
[0048] Specifically, for example, aromatic rings can be sulfonated by reacting them with a sulfonating agent such as chlorosulfonic acid in a solvent such as chloroform, or by reacting them in concentrated sulfuric acid or fuming sulfuric acid. There are no particular limitations on the sulfonating agent as long as it sulfonates aromatic rings, and sulfur trioxide and the like can also be used. When aromatic rings are sulfonated by this method, the degree of sulfonation can be easily controlled by the amount of sulfonating agent used, the reaction temperature, and the reaction time. Sulfonimide groups can be introduced into aromatic polymers, for example, by reacting sulfonic acid groups with sulfonamide groups.
[0049] In the present invention, the electron-withdrawing group X in the aromatic dihalide compound represented by the general formula (Q1) or (Q2) 1 and X 2 Preferred specific examples of the substituent include ketone, sulfone, phosphine oxide, etc. Preferred examples of the substituent of the phosphine oxide include a methyl group, an ethyl group, a propyl group, an isopropyl group, a cyclopentyl group, a cyclohexyl group, a norbornyl group, a vinyl group, an allyl group, a benzyl group, a phenyl group, a naphthyl group, a phenylphenyl group, etc. In terms of industrial availability, the most preferred substituent is a phenyl group.
[0050] Among these, from the viewpoints of crystallinity, mechanical strength, durability, and dimensional stability, X 1 and X 2 More preferred are aromatic dihalide compounds represented by the following general formulas (Q4) and (Q5), in which is a ketone.
[0051] [ka]
[0052] (In the general formulas (Q4) and (Q5), Z 5 and Z 6 is halogen, M 5 or M 6 represents hydrogen, a metal cation, or an ammonium cation.) Specific examples of the aromatic dihalide compound represented by general formula (Q1) include 3,3'-disulfonate-4,4'-dichlorodiphenyl sulfone, 3,3'-disulfonate-4,4'-difluorodiphenyl sulfone, 3,3'-disulfonate-4,4'-dichlorodiphenyl ketone, 3,3'-disulfonate-4,4'-difluorodiphenyl ketone, 3,3'-disulfonate-4,4'-dichlorodiphenylphenylphosphine oxide, and 3,3'-disulfonate-4,4'-difluorodiphenylphenylphosphine oxide. Among these, as the aromatic active dihalide compound represented by general formula (Q1), 3,3'-disulfonate-4,4'-dichlorodiphenyl ketone and 3,3'-disulfonate-4,4'-difluorodiphenyl ketone are more preferable from the viewpoints of production costs and active material permeation suppression effect, and 3,3'-disulfonate-4,4'-difluorodiphenyl ketone is most preferable from the viewpoint of polymerization activity.
[0053] In addition, examples of aromatic active dihalide compounds represented by general formula (Q2) include 4,4'-dichlorodiphenyl sulfone, 4,4'-difluorodiphenyl sulfone, 4,4'-dichlorodiphenyl ketone, 4,4'-difluorodiphenyl ketone, 4,4'-dichlorodiphenyl phenyl phosphine oxide, and 4,4'-difluorodiphenyl phenyl phosphine oxide. Among these, examples of aromatic dihalide compounds represented by general formula (Q2) include 4,4'-dichlorodiphenyl ketone and 4,4'-difluorodiphenyl ketone, which are more preferred in terms of crystallinity impartation, mechanical strength, and active material permeation suppression effect, and 4,4'-difluorodiphenyl ketone is the most preferred in terms of polymerization activity. These aromatic active dihalide compounds can be used alone, but it is also possible to use multiple aromatic active dihalide compounds in combination.
[0054] Next, the aromatic diol compound represented by the general formula (Q3) used in the present invention will be described. In the present invention, the aromatic diol compound is defined as including a compound having two phenolic -OH groups, as well as a compound having two -SH groups, which are heteroatom analogues of the phenolic -OH groups. Hereinafter, specific examples will be given using phenolic -OH groups, but their heteroatom derivatives can also be preferably used. However, from the viewpoint of production costs, the -OH group can be used more preferably than the -SH group.
[0055] The protecting group used in the aromatic diol compound represented by the general formula (Q3) can be a protecting group generally used in organic synthesis. The protecting group is a substituent that is temporarily introduced on the premise of being removed at a later stage, protects a highly reactive functional group, makes it inactive against subsequent reactions, and can be deprotected to return to the original functional group after the reaction. That is, it is a pair with the functional group to be protected. For example, a t-butyl group may be used as a protecting group for a hydroxyl group, but when the same t-butyl group is introduced into an alkylene chain, it is not called a protecting group. The reaction of introducing a protecting group is called protection (reaction), and the reaction of removing it is called deprotection (reaction).
[0056] Such a protecting reaction is described in detail in, for example, "Protective Groups in Organic Synthesis" by Theodora W. Greene, John Wiley & Sons, Inc., USA, 1981, and these can be preferably used. It is possible to appropriately select a protecting reaction and a deprotecting reaction in consideration of reactivity and yield, stability of the state containing the protecting group, production cost, etc. In addition, the stage at which a protecting group is introduced in a polymerization reaction may be from the monomer stage, the oligomer stage, or the polymer stage, and it can be appropriately selected.
[0057] Specific examples of the protection reaction include a method of protecting / deprotecting a ketone moiety with a ketal moiety, and a method of protecting / deprotecting a ketone moiety with a heteroatom analogue of the ketal moiety, such as a thioketal. These methods are described in Chapter 4 of the aforementioned "Protective Groups in Organic Synthesis." Other examples include a method of protecting / deprotecting between a sulfonic acid and a soluble ester derivative, and a method of introducing a t-butyl group as a soluble group into an aromatic ring and de-t-butylating it with an acid to protect / deprotect the ring. However, the present invention is not limited to these, and can be preferably used. In terms of improving solubility in general solvents and reducing crystallinity, aliphatic groups, especially aliphatic groups containing a cyclic moiety, are preferably used as protecting groups because of their large steric hindrance.
[0058] The position of the functional group to which the protective group is introduced is preferably the main chain of the polymer. Since the protective group is introduced into a polymer with good packing in order to improve processability, the effect of the present invention may not be fully obtained even if the protective group is introduced into the side chain portion of the polymer. Here, the functional group present in the main chain of the polymer is defined as a functional group that breaks the polymer chain when the functional group is deleted. For example, this means that the benzene ring and the benzene ring are broken when the ketone group of an aromatic polyether ketone is deleted.
[0059] In the present invention, a polymer being crystalline means that the polymer has a crystallizable property, that is, the polymer can be crystallized under certain conditions. In addition, a polymer being amorphous means that the polymer is in an amorphous state when used, regardless of the presence or absence of crystallinity of the polymer. The presence or absence of crystallinity of these polymers, and the crystalline and amorphous states can be evaluated by a sharp peak derived from crystals in wide-angle X-ray diffraction (XRD) or a crystallization peak in differential scanning calorimetry (DSC), etc.
[0060] In the present invention, excellent hot water resistance means that the dimensional change (swelling) in high-temperature water is small. If this dimensional change is large, it is not preferable because it may cause membrane damage or increase in resistance during use as a polymer electrolyte membrane. These hot water resistance properties are important properties required for electrolyte polymers used in redox flow batteries.
[0061] As the protection reaction used in the polymer electrolyte material used in the present invention, in terms of reactivity and stability, a method in which a ketone moiety is protected / deprotected with a ketal moiety, or a method in which a ketone moiety is protected / deprotected with a heteroatom analogue of the ketal moiety, such as a thioketal, is more preferable.
[0062] A preferred specific example of the aromatic diol compound represented by general formula (Q3) is at least one selected from the compounds represented by the following general formulae (P1) and (P2).
[0063] [ka]
[0064] (In the general formulas (P1-1) and (P2-1), Ar 1 ~Ar 4 is any divalent arylene group, R 1 and R 2 is at least one group selected from H and an alkyl group; R 3 represents any alkylene group, and E represents O or S. The compounds represented by general formula (P1-1) and general formula (P2-1) may be optionally substituted. Among these, in terms of the odor, reactivity, stability, etc. of the compound, the method in which E is O in the general formulae (P1-1) and (P2-1), that is, the method in which the ketone moiety is protected / deprotected at the ketal moiety, is most preferred.
[0065] R in the aromatic diol compound represented by the general formula (P1-1) used in the present invention 1 and R 2 From the viewpoint of stability, R is preferably an alkyl group, further preferably an alkyl group having 1 to 6 carbon atoms, and most preferably an alkyl group having 1 to 3 carbon atoms. 3 From the viewpoint of stability, R is more preferably an alkylene group having 1 to 7 carbon atoms, and most preferably an alkylene group having 1 to 4 carbon atoms. 3 A specific example of the 2 CH 2 -, -CH(CH 3 )CH 2 -, -CH(CH 3 )CH(CH 3 )-, -C(CH 3 ) 2 CH 2 -, -C(CH 3 ) 2 CH(CH 3 )-, -C(CH 3 ) 2 O(CH 3 )2 -, -CH 2 CH 2 CH 2 -, -CH 2 C(CH 3 ) 2 CH 2 -, etc., but are not limited to these.
[0066] As the polymer electrolyte material used in the present invention, those having at least the above formula (P3) are more preferably used from the viewpoint of stability such as hydrolysis resistance. 3 The alkylene group has 1 to 7 carbon atoms, i.e., n1 H 2n1 (n1 is an integer of 1 to 7), and from the viewpoints of stability and ease of synthesis, it is preferably a group represented by -CH 2 CH 2 -, -CH(CH 3 )CH 2 -, or -CH 2 CH 2 CH 2 - is most preferably at least one selected from the following:
[0067] In the general formulae (P1-1) and (P2-1), Ar 1 ~Ar 4 The preferred organic group for is a phenylene group, a naphthylene group, or a biphenylene group. These may be optionally substituted. As the aromatic polyether polymer of the present invention, the Ar 3 and Ar 4 are both phenylene groups, i.e., it is more preferable to contain an aromatic diol compound represented by the following general formula (P3), and most preferably Ar 3 and Ar 4 Both are p-phenylene groups.
[0068] [ka]
[0069] (In general formula (P3), n1 is an integer of 1 to 7. The constitutional unit represented by general formula (P3) may be optionally substituted.) Suitable specific examples of the aromatic diol compound represented by general formula (P3) used in the present invention include compounds represented by the following general formulas (r1) to (r10), heteroatom analogues of the ketal moiety, and derivatives derived from these dihydric phenol compounds.
[0070] [ka]
[0071] Among these aromatic diol compounds, from the viewpoint of stability, the compounds represented by the general formulae (r4) to (r10) are more preferred, the compounds represented by the general formulae (r4), (r5) and (r9) are even more preferred, and the compound represented by the general formula (r4) is the most preferred.
[0072] In the present invention, the method of protecting the ketone moiety with a ketal includes a method of reacting a precursor compound having a ketone group with a monofunctional and / or difunctional alcohol in the presence of an acid catalyst. For example, it can be produced by reacting the ketone precursor 4,4'-dihydroxybenzophenone with a monofunctional and / or difunctional alcohol, in a solvent such as an aliphatic or aromatic hydrocarbon, in the presence of an acid catalyst such as hydrogen bromide. The alcohol is an aliphatic alcohol having 1 to 20 carbon atoms. An improved method for producing a ketal monomer used in the present invention comprises reacting the ketone precursor 4,4'-dihydroxybenzophenone with a difunctional alcohol in the presence of an alkyl orthoester and a solid catalyst.
[0073] Specific examples of the bifunctional alcohol include, but are not limited to, ethylene glycol, propylene glycol, 2,3-butanediol, 2-methyl-1,2-propanediol, 2-methyl-2,3-butanediol, 2,3-dimethyl-2,3-butanediol, 1,3-propanediol, 2,2-dimethyl-1,3-propanediol, etc. Among these, ethylene glycol, propylene glycol, and 2-methyl-1,2-propanediol are most preferred in terms of stability.
[0074] Alkyl orthoesters include trimethyl orthoformate, triethyl orthoformate, trimethyl orthoacetate, triethyl orthoacetate, tetramethyl orthosilicate, tetraethyl orthosilicate, etc. Also, easily hydrolyzed compounds such as 2,2-dimethoxypropane, 2,2-dimethyl-1,3-dioxolane, which form volatile products such as methanol, ethanol, acetone, etc., can be used in place of the orthoesters.
[0075] The solid catalyst is preferably a particulate acidic alumina-silica compound, most preferably a montmorillonite clay, such as exemplified by the montmorillonite designated K-10 (e.g., Aldrich reagent). Although montmorillonite clay is preferred, other solid acidic catalysts with high surface area can also function effectively as catalysts. These include acidic aluminas, sulfonated polymeric resins, and the like.
[0076] The reaction is carried out by mixing together the ketone precursor, about one equivalent or preferably an excess of the difunctional alcohol, about one equivalent or preferably an excess of the orthoester and at least 1 g of solid catalyst per equivalent of ketone, preferably 10 moles or more of solid catalyst per equivalent of ketone. The reaction is carried out in the presence of an inert solvent if necessary. A large excess of solid can be used since the catalyst is easily removed by filtration for reuse. The reaction is carried out at a temperature from about 25°C to about the boiling point of the orthoester used, preferably at a temperature lower than the boiling point of the orthoester but higher than the boiling point of the orthoester reaction product. For example, when using trimethyl orthoformate (boiling point 102°C) whose reaction products are methanol (boiling point 65°C) and methyl formate (boiling point 34°C), a reaction temperature of about 65°C to 102°C is suitable. Of course, the reaction temperature can be appropriately adjusted when the reaction is carried out under reduced or elevated pressure.
[0077] The most preferred ketal monomer is prepared by heating a mixture of 4,4'-dihydroxybenzophenone, excess glycol, excess trialkyl orthoformate, and about 0.1 to about 5 g of Montmorillonite clay K-10 per gram of ketone, preferably about 0.5 to about 2.5 g of clay per gram of ketone, to distill off the alcohol resulting from the orthoformate. The ketal-containing monomer 2,2-bis(4-hydroxyphenyl)-1,3-dioxolane can be obtained in excellent yields (60% to almost quantitative) within 48 hours of reaction time.
[0078] Standard isolation techniques can be used to recover the ketal monomer and unreacted ketone, provided that proper care is taken to avoid acidifying the system. Recrystallization or other extensive purification of the isolated reaction product is not necessary before use in the production of polyketals. For example, after diluting the reaction mixture with ethyl acetate solvent, filtering off the solid catalyst, extracting the solution with basic water to remove excess alcohol, removing water with a conventional drying agent such as anhydrous sodium sulfate, removing the solvent and volatiles under vacuum, and then washing the resulting solid with a solvent such as methylene chloride to remove trace contaminants, a reaction product is obtained which contains primarily the ketal monomer, but may still contain some unreacted ketone precursor. However, this reaction product can be used in the production of high molecular weight polyketals without further purification. It can also be recrystallized from a common solvent such as toluene to remove unreacted ketone precursor.
[0079] In the present invention, since the ratio of groups containing a protecting group to groups not containing a protecting group is important, the purity of the ketal monomer is preferably 98% or more, and more preferably 99% or more.
[0080] Next, the aromatic diol compound represented by the general formula (X-1) or (X-2) will be described.
[0081] In the polymer electrolyte material used in the present invention, an aromatic diol compound represented by general formula (X-1) or (X-2) is required from the viewpoint of a group that balances the packing property of the polymer as a soluble polymer electrolyte material for molding before deprotection, and can achieve both crystallinity and processability and filterability. When a ketal group is used as a protecting group, the aromatic diol compound represented by general formula (X-1) has the same structure as a ketone group after deprotection, and can be used with high regularity and crystallinity. From the viewpoint of dimensional stability, production cost, and crystallinity, the aromatic diol compound represented by general formula (X-2) is more preferably an aromatic diol compound represented by formula (X-2) from the viewpoint of high oxidation resistance and filterability. Due to the above effects, the obtained polymer electrolyte material can exhibit excellent performance in mechanical properties, active material blocking properties, long-term durability, etc.
[0082] The polymerization method of the aromatic polyether polymer used in the present invention is not particularly limited as long as it can substantially produce a sufficiently high molecular weight, and for example, it can be synthesized by utilizing the aromatic nucleophilic substitution reaction of an aromatic dihalide compound and an aromatic diol compound. It is also possible to introduce the fifth component by utilizing the aromatic nucleophilic substitution reaction of a halogenated aromatic phenol compound.
[0083] The polymerization of aromatic polyether polymers by aromatic nucleophilic substitution reaction, which is carried out to obtain the polymer electrolyte material used in the present invention, can be carried out by reacting the above-mentioned monomer mixture in the presence of a basic compound to obtain a polymer. The polymerization can be carried out at a temperature range of 0 to 350°C, but preferably at a temperature of 50 to 250°C. If the temperature is lower than 0°C, the reaction tends not to proceed sufficiently, and if the temperature is higher than 350°C, the polymer tends to start to decompose. The reaction can be carried out without a solvent, but is preferably carried out in a solvent. Examples of solvents that can be used include aprotic polar solvents such as N,N-dimethylacetamide, N,N-dimethylformamide, N-methyl-2-pyrrolidone, dimethyl sulfoxide, sulfolane, 1,3-dimethyl-2-imidazolidinone, and hexamethylphosphontriamide, but are not limited to these, and any solvent that can be used as a stable solvent in an aromatic nucleophilic substitution reaction may be used. These organic solvents may be used alone or as a mixture of two or more kinds.
[0084] Examples of the basic compound include sodium hydroxide, potassium hydroxide, sodium carbonate, potassium carbonate, sodium hydrogen carbonate, potassium hydrogen carbonate, and the like, but are not limited to these and can be used as long as it can convert aromatic diols into active phenoxide structures.
[0085] In aromatic nucleophilic substitution reactions, water may be produced as a by-product. In this case, water can be removed from the system as an azeotrope by coexisting toluene or the like in the reaction system, regardless of the polymerization solvent. A water absorbing agent such as a molecular sieve can also be used to remove water from the system. The azeotropic agent used to remove reaction water or water introduced during the reaction is generally any inert compound that does not substantially interfere with the polymerization, co-distills with water, and boils between about 25°C and about 250°C. Common azeotropic agents include benzene, toluene, xylene, chlorobenzene, methylene chloride, dichlorobenzene, trichlorobenzene, and the like. Of course, it is beneficial to select an azeotropic agent whose boiling point is lower than that of the dipolar solvent used. Although an azeotropic agent is commonly used, it is not always necessary when high reaction temperatures, such as temperatures above 200°C, are used, especially when an inert gas is continuously sparged into the reaction mixture. In general, it is desirable to carry out the reaction in an inert atmosphere in the absence of oxygen.
[0086] When the aromatic nucleophilic substitution reaction is carried out in a solvent, it is preferable to charge the monomer so that the concentration of the resulting polymer is 5 to 50% by weight. If the concentration is less than 5% by weight, the degree of polymerization tends to be difficult to increase. On the other hand, if the concentration is more than 50% by weight, the viscosity of the reaction system becomes too high, and post-treatment of the reactants tends to be difficult.
[0087] After the polymerization reaction is completed, the solvent is removed from the reaction solution by evaporation, and the residue is washed as necessary to obtain the desired polymer. Alternatively, the reaction solution can be added to a solvent in which the polymer has low solubility and the by-product inorganic salt has high solubility, thereby removing the inorganic salt, precipitating the polymer as a solid, and filtering the precipitate to obtain the polymer. The recovered polymer is optionally washed with water, alcohol, or other solvents and dried. Once the desired molecular weight is obtained, the halide or phenoxide end groups can be reacted, optionally by introducing a phenoxide or halide end-capping agent to form stable end groups.
[0088] In the present invention, since it is necessary to introduce the protecting group without deprotection until the film formation stage from the viewpoint of processability, it is necessary to carry out polymerization and purification while taking into consideration the conditions under which the protecting group can exist stably. For example, when a ketal is used as the protecting group, the deprotection reaction proceeds under acidic conditions, so the system must be kept neutral or alkaline.
[0089] In the present invention, the method of deprotecting at least a part of the ketone moiety protected by ketal to obtain a ketone moiety is not particularly limited. The deprotection reaction can be carried out in the presence of water and acid under heterogeneous or homogeneous conditions, but from the viewpoint of mechanical strength and solvent resistance, a method of forming into a film or the like and then treating with acid is more preferable. Specifically, the formed film can be deprotected by immersing it in an aqueous hydrochloric acid solution, and the concentration of the acid and the temperature of the aqueous solution can be appropriately selected.
[0090] The weight ratio of the acidic aqueous solution required to the polymer is preferably 1 to 100 times, but a larger amount of water can also be used. The acid catalyst is preferably used at a concentration of 0.1 to 50% by weight of the water present. Suitable acid catalysts include strong mineral acids such as hydrochloric acid, nitric acid, fluorosulfonic acid, sulfuric acid, etc., and strong organic acids such as p-toluenesulfonic acid, trifluoromethanesulfonic acid, etc. The amounts of acid catalyst and excess water, reaction pressure, etc. can be appropriately selected depending on the film thickness of the polymer, etc.
[0091] For example, in the case of a membrane having a thickness of 50 μm, it is possible to easily deprotect almost the entire amount by immersing it in an acidic aqueous solution such as a 6N hydrochloric acid aqueous solution and heating it at 95° C. for 1 to 48 hours. It is also possible to deprotect most of the protecting groups by immersing it in a 1N hydrochloric acid aqueous solution at 25° C. for 24 hours. However, the deprotection conditions are not limited to these, and deprotection may be performed using an acidic gas, an organic acid, or the like, or by heat treatment.
[0092] The weight average molecular weight of the electrolyte material for redox flow batteries used in the present invention must be 420,000 or more. If the weight average molecular weight is low, the mechanical strength becomes insufficient, such as cracks occurring in the molded film, and the chemical stability deteriorates, so that it is preferably 450,000 or more, and more preferably 500,000 or more. On the other hand, the upper limit of the weight average molecular weight is not particularly limited, but if it exceeds 5 million, there may be problems such as insufficient solubility, high solution viscosity, and poor processability. The weight average molecular weight Mw used here indicates the relative weight average molecular weight to the molecular weight of standard polystyrene, determined by gel permeation chromatography using N-methyl-2-pyrrolidone solvent (N-methyl-2-pyrrolidone solvent containing 10 mmol / L of lithium bromide) as the mobile phase. Note that the molecular weight of the polymer electrolyte material obtained by the present invention may be difficult to measure due to its insolubility in solvents, but it is necessary to obtain it from a moldable soluble polymer electrolyte material of the above molecular weight.
[0093] The chemical structure of the polymer electrolyte material used in the present invention is determined by infrared absorption spectroscopy at 1,030 to 1,045 cm -1 , 1,160~1,190cm -1 S=O absorption, 1,130~1,250cm -1 COC absorption, 1,640-1,660cm -1 The composition ratio of these compounds can be determined by neutralization titration of sulfonic acid groups or elemental analysis. In addition, nuclear magnetic resonance spectroscopy ( 1 The structure can be confirmed by H-NMR, for example, from the aromatic proton peak at 6.8 to 8.0 ppm. 13 C-NMR and solid 13 The positions and arrangement of the sulfonic acid groups can be confirmed using C-NMR.
[0094] The polymer electrolyte material used in the present invention may be insoluble in common organic solvents such as deuterated dimethyl sulfoxide and deuterated chloroform, but it can be measured using deuterated sulfuric acid. This makes it possible to determine whether the polymer is sulfonated at the monomer stage and the sulfonation position is controlled, or whether the sulfonation position is not controlled and the polymer is post-sulfonated. However, if there are no adjacent electron-withdrawing groups such as ketone groups or sulfone groups, the sulfonation reaction will proceed during sample preparation or measurement, making it difficult to determine the exact sulfonation position of the sample.
[0095] The NMR measurement of the chemical structure of such a polymer electrolyte material is carried out by the method described in the Examples.
[0096] The sulfonic acid group in the polymer to be used as the polymer electrolyte material of the present invention may be introduced by block copolymerization or random copolymerization. It can be appropriately selected depending on the chemical structure and crystallinity of the polymer to be used. When fuel barrier properties and low water content are required, random copolymerization is more preferable, and when proton conductivity and high water content are required, block copolymerization is more preferable.
[0097] There is no particular limitation on the method for converting the polymer electrolyte material used in the present invention into a membrane, and possible methods include a method for forming a membrane from a solution state or a method for forming a membrane from a molten state at the stage where the polymer electrolyte material has a protecting group such as ketal, etc. In the former method, for example, a method for forming a membrane can be exemplified by dissolving the polymer electrolyte material in a solvent such as N-methyl-2-pyrrolidone, casting the solution onto a glass plate or the like, and removing the solvent.
[0098] The solvent used for membrane formation may be any solvent that can dissolve the polymer electrolyte material and can be subsequently removed. For example, aprotic polar solvents such as N,N-dimethylacetamide, N,N-dimethylformamide, N-methyl-2-pyrrolidone, dimethyl sulfoxide, sulfolane, 1,3-dimethyl-2-imidazolidinone, hexamethylphosphontriamide, etc., ester-based solvents such as γ-butyrolactone, butyl acetate, etc., carbonate-based solvents such as ethylene carbonate, propylene carbonate, etc., alkylene glycol monoalkyl ethers such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, etc., alcohol-based solvents such as isopropanol, water, and mixtures thereof can be suitably used, with aprotic polar solvents being the most preferred due to their high solubility.
[0099] A preferable method for obtaining a tough membrane is to subject a polymer solution prepared to a required solid content concentration to normal pressure filtration or pressure filtration, etc., and remove foreign matter present in the polymer electrolyte solution. The filter material used here is not particularly limited, but a glass filter or a metal filter is preferable. In this filtration, the minimum filter pore size through which the polymer solution passes is preferably 1 μm or less. If filtration is not performed, foreign matter is allowed to enter, causing membrane breakage or insufficient durability, which is undesirable.
[0100] Next, the obtained polymer electrolyte membrane is preferably heat-treated after at least a part of the ionic group is converted to a metal salt state. If the polymer electrolyte material used is one that is polymerized in the state of a metal salt during polymerization, it is preferable to form a membrane and heat-treat it as it is. The metal of the metal salt may be any metal that can form a salt with sulfonic acid, but from the viewpoint of cost and environmental load, Li, Na, K, Rb, Cs, Mg, Ca, Sr, Ba, Ti, V, Mn, Fe, Co, Ni, Cu, Zn, Zr, Mo, W, etc. are preferable, and among these, Li, Na, K, Ca, Sr, Ba are more preferable, and Li, Na, and K are even more preferable. The temperature of this heat treatment is preferably 150 to 550 ° C, more preferably 160 to 400 ° C, and particularly preferably 180 to 350 ° C.
[0101] The heat treatment time is preferably 10 seconds to 12 hours, more preferably 30 seconds to 6 hours, and particularly preferably 1 minute to 1 hour. If the heat treatment temperature is too low, the fuel permeability suppression effect, elastic modulus, and breaking strength are insufficient. On the other hand, if the heat treatment temperature is too high, the membrane material is likely to deteriorate. If the heat treatment time is less than 10 seconds, the effect of the heat treatment is insufficient. On the other hand, if it exceeds 12 hours, the membrane material is likely to deteriorate. The polymer electrolyte membrane obtained by the heat treatment can be immersed in an acidic aqueous solution as necessary to perform proton replacement. By forming the polymer electrolyte membrane by this method, it becomes possible to achieve a better balance between proton conductivity and active material blocking property, as well as mechanical properties and long-term durability.
[0102] A specific example of a method for converting the polymer electrolyte material used in the present invention into a membrane is to prepare a membrane made of the aromatic polyether polymer by the above-mentioned method, and then deprotect at least a part of the ketone moieties protected by ketal to obtain ketone moieties. This method enables solution membrane formation of a poorly soluble low-sulfonic acid group polymer, and makes it possible to achieve both proton conductivity and active material barrier effect, as well as excellent mechanical properties and dimensional stability.
[0103] In the present invention, the method of deprotecting a part or all of the ketone moieties protected by ketal to obtain ketone moieties is not particularly limited, but includes a method of performing acid treatment after molding. Specifically, the molded membrane can be deprotected by immersing it in an aqueous solution of hydrochloric acid or sulfuric acid, and the concentration of the acid and the temperature of the aqueous solution can be appropriately selected in consideration of the ease of penetration into the molded body. For example, a membrane with a thickness of 50 μm can be easily deprotected by immersing it in an acidic aqueous solution such as a 6N aqueous solution of hydrochloric acid and heating it at 95° C. for 8 hours. However, the conditions for deprotection are not limited to these, and deprotection may be performed using an acidic gas, an organic acid, or the like.
[0104] The thickness of the polymer electrolyte membrane of the present invention is preferably 1 to 2,000 μm. To obtain a membrane strength sufficient for practical use, it is more preferable that the thickness is greater than 1 μm, and to reduce the membrane resistance, i.e., to improve the voltage efficiency, it is preferable that the thickness is less than 2,000 μm. The more preferable range of the thickness is 3 to 500 μm, and the most preferable range is 5 to 250 μm. The thickness can be controlled by the solution concentration or the coating thickness on the substrate.
[0105] In addition, additives such as a crystallization nucleating agent, a plasticizer, a stabilizer, a mold release agent, and an antioxidant, which are used in ordinary polymer compounds, can be added to the polymer electrolyte material used in the present invention, within the scope not contrary to the object of the present invention.
[0106] Furthermore, the polymer electrolyte material used in the present invention may contain various polymers, elastomers, fillers, fine particles, various additives, etc., for the purpose of improving mechanical strength, thermal stability, processability, etc., within the range that does not adversely affect the above-mentioned various properties. Furthermore, the polymer electrolyte material may be reinforced with a microporous membrane, a nonwoven fabric, a mesh, etc.
[0107] The amount of sulfonic acid groups in the polymer electrolyte material can be expressed as a value of sulfonic acid group density (mmol / g). The sulfonic acid group density of the polymer electrolyte material used in the present invention is preferably 1.0 to 3.0 mmol / g in terms of proton conductivity, active material blocking property, and mechanical strength, more preferably 1.1 to 2.5 mmol / g in terms of active material blocking property, and even more preferably 1.2 to 2.0 mmol / g. If the sulfonic acid group density is lower than 1.0 mmol / g, sufficient voltage efficiency may not be obtained due to low proton conductivity, and if it is higher than 3.0 mmol / g, sufficient mechanical strength when water is contained may not be obtained when used as an electrolyte membrane for a fuel cell.
[0108] Here, the sulfonic acid group density is the number of moles of sulfonic acid groups introduced per gram of dried polymer electrolyte material, and the larger the value, the larger the amount of sulfonic acid groups. The sulfonic acid group density can be determined by elemental analysis and neutralization titration. Among these, it is preferable to use elemental analysis and calculate from the S / C ratio because of the ease of measurement, but when a sulfur source other than sulfonic acid groups is contained, the ion exchange capacity can also be determined by neutralization titration. The polymer electrolyte material of the present invention includes an embodiment that is a complex consisting of a polymer having an ionic group and other components as described below, and in that case, the sulfonic acid group density is also determined based on the total amount of the complex.
[0109] The polymer electrolyte material used in the present invention may contain other components, such as inactive polymers that do not have electrical conductivity or ion conductivity, or organic or inorganic compounds, as long as the other components do not impair the object of the present invention.
[0110] In the polymer electrolyte material used in the present invention, the content of groups having a protecting group is not particularly limited, but in terms of mechanical properties, active material insulating properties, and chemical stability, it is preferable that the content is as small as possible, and it is most preferable that all of the protecting groups are deprotected. In the polymer electrolyte material of the present invention, the content of the protecting group can be measured by nuclear magnetic resonance spectroscopy (NMR), thermogravimetry (TGA), evolved gas analysis by temperature-programmed thermal desorption-mass spectrometry (TPD-MS), pyrolysis gas chromatography, pyrolysis GC-MS, infrared absorption spectroscopy (IR), etc.
[0111] When the amount of protecting groups contained in the polymer electrolyte material used in the present invention is large, the protecting groups are soluble in solvents, so nuclear magnetic resonance spectroscopy (NMR) is suitable for quantifying the protecting groups. However, when the amount of protecting groups is very small and insoluble in solvents, it may be difficult to accurately quantify them using NMR. In such cases, evolved gas analysis using temperature-programmed thermal desorption-mass spectrometry (TPD-MS), pyrolysis gas chromatography, and pyrolysis GC-MS are suitable quantification methods. EXAMPLES
[0112] The present invention will be described in more detail below with reference to examples, but the present invention is not limited thereto. The conditions for measuring each physical property are as follows. Chemical structural formulae are inserted in the examples, but the chemical structural formulae are inserted for the purpose of helping the reader understand, and do not necessarily accurately represent the chemical structure, exact composition, arrangement, position, number, and molecular weight of the polymerization components of the polymer, and the present invention is not limited thereto.
[0113] (1) Nuclear Magnetic Resonance Spectroscopy (NMR) Under the following measurement conditions: 1H-NMR was performed to confirm the structure and to quantify the molar composition ratio of the ionic group-containing segment (A1) and the ionic group-free segment (A2). The molar composition ratio was calculated from the integral values of the peaks observed at 8.2 ppm (derived from disulfonate-4,4'-difluorobenzophenone) and 6.5 to 8.0 ppm (derived from all aromatic protons excluding disulfonate-4,4'-difluorobenzophenone).
[0114] Equipment: JEOL Ltd. EX-270 Resonance frequency: 270MHz ( 1 H-NMR) Measurement temperature: room temperature Dissolution medium: DMSO-d 6 Internal reference substance: TMS (0ppm) Number of times: 16 (2) Weight average molecular weight The weight average molecular weight of the polymer was measured by GPC. The weight average molecular weight was calculated by standard polystyrene conversion using a Tosoh HLC-8022GPC as an integrated UV detector and differential refractometer, and two Tosoh TSK gel SuperHM-H (inner diameter 6.0 mm, length 15 cm) GPC columns. The measurements were performed in N-methyl-2-pyrrolidone solvent (N-methyl-2-pyrrolidone solvent containing 10 mmol / L lithium bromide) at a sample concentration of 0.1 wt%, a flow rate of 0.2 mL / min, and a temperature of 40°C.
[0115] (3) Film thickness Measurements were performed using a Mitutoyo ID-C112 model set on a Mitutoyo Granite Comparator Stand BSG-20.
[0116] (4) Purity measurement method Quantitative analysis was performed by gas chromatography (GC) under the following conditions. Column: DB-5 (Agilent Technologies, Inc.) L = 30 m Φ = 0.53 mm D = 1.50 μm Carrier: Helium (linear velocity = 35.0 cm / sec) Analysis conditions Inj.temp. 300℃ Detector temp. 320℃ Oven 50℃×1min Rate 10℃ / min Final 300℃×15min SP ratio 50:1 (5) Vanadium ion (IV) permeation rate The electrolyte membrane (6.6 cm) is placed between the H-shaped cells. 2 ) on one side, and 1.5 mol L -1 Magnesium sulfate / 3.5 mol / L sulfuric acid aqueous solution on one side, 1.5 mol L on the other -1 Vanadium(IV) sulfate / 3.5 mol L -1 70 mL of sulfuric acid solution was added to each flask. The flask was stirred at 25°C and 300 rpm using a magnetic stirrer. After 4 days, the concentration of tetravalent vanadium dissolved in the magnesium sulfate solution was measured by measuring the absorbance at 765 nm using a UV spectrophotometer (U-3010, manufactured by Hitachi, Ltd.).
[0117] First, 3.5 mol L of vanadium(IV) sulfate at different concentrations was -1 An aqueous sulfuric acid solution was prepared, and the absorbance was measured using the UV spectrophotometer. A calibration curve was prepared based on the relationship between the concentration and the absorbance, and the concentration of the transmitted tetravalent vanadium was quantified from this calibration curve.
[0118] Next, the amount of tetravalent vanadium ions passing through was calculated by the following formula, where the specific gravity (density) of the aqueous sulfuric acid solution used was the same as that of water.
[0119] Tetravalent vanadium ion transmission (×10 -10 cm 2 / min) = permeated vanadium concentration (mol) / (membrane area (cm 2 ) × permeation time (min) / 1.5 (mol / m 3 ) × film thickness (m) (6) Measurement of dimensional change rate (λxy) by hot water test The composite electrolyte membrane was cut into a square of about 5 cm x about 5 cm, and left to stand for 24 hours in a temperature-controlled, humidity-controlled atmosphere at a temperature of 23°C ± 5°C and a humidity of 50% ± 5%, after which the length in the MD direction and the length in the TD direction (MD1 and TD1) were measured with a caliper. The electrolyte membrane was immersed in hot water at 80°C for 8 hours, and the length in the MD direction and the length in the TD direction (MD2 and TD2) were measured again with a caliper, and the dimensional change rate in the MD direction and the TD direction in the in-plane direction (λMD and λTD) and the dimensional change rate in the in-plane direction (λxy) (%) were calculated from the following formula.
[0120] λMD = (MD2 - MD1) / MD1 × 100 λTD=(TD2-TD1) / TD1×100 λxy=(λMD+λTD) / 2 (7) Ion exchange capacity (IEC) After proton exchange and thorough washing with pure water, the moisture on the surface of the electrolyte membrane was wiped off and it was then vacuum dried at 100°C for 12 hours or more to determine the dry weight. Next, 50 mL of a 5 wt% aqueous solution of sodium sulfate was added to the electrolyte and left to stand for 12 hours to perform ion exchange. Then, 0.01 mol L -1 The resulting sulfuric acid was titrated using an aqueous solution of sodium hydroxide. A commercially available phenolphthalein solution for titration (0.1 w / v%) was added as an indicator, and the end point was the point at which the color turned light reddish purple. Finally, the ion exchange capacity was calculated using the following formula.
[0121] Ion exchange capacity (meq / g) = [concentration of sodium hydroxide solution (mmol / mL) × amount dropped (mL)] / dry weight of sample (g) (8) Tensile strength and elongation measurement The polymer electrolyte membrane sample was left at 25°C and 60% RH for 24 hours, then set in the device and subjected to tensile measurement under the following conditions. The tensile strength and tensile elongation values were taken as the values at the moment when the maximum stress was observed during the test. The elastic modulus was taken as the maximum value calculated using any two points where the difference in strain was 3%. The maximum stress and elastic modulus were calculated as the average value of five tests using the following formula.
[0122] Measuring device: Autograph AG-IS (Shimadzu Corporation) Load: 100N Pulling speed: 10mm / min Test piece: width 5mm x length 50mm Distance between samples: 20 mm Test temperature: 25℃ Number of tests: n=5 (9) Oxidation resistance evaluation Polymer electrolyte membrane (78cm 2 The polymer electrolyte membrane was immersed in 225 mL of a 1.7 mol vanadium solution (SOC 44%) at 75° C. for 30 days, and the tensile strength of the polymer electrolyte membrane was measured before and after immersion by the method described in (8). The tensile strength before immersion was A and the tensile strength after immersion was B. The tensile strength retention rate was calculated by the following formula, and the oxidation resistance was evaluated according to the following criteria.
[0123] Tensile strength retention rate = B / A ×100 Good: Tensile strength retention rate is 95% or more Acceptable: Tensile strength retention rate is 80% or more and less than 95% Unacceptable: Tensile strength retention rate is less than 80% Synthesis Example 1 Synthesis of 2,2-bis(4-hydroxyphenyl)-1,3-dioxolane (K-DHBP) represented by the following general formula (G1)
[0124] [ka]
[0125] In a 500mL flask equipped with a stirrer, a thermometer and a distillation tube, 49.5g of 4,4'-dihydroxybenzophenone, 134g of ethylene glycol, 96.9g of trimethyl orthoformate and 0.50g of p-toluenesulfonic acid monohydrate were charged and dissolved. The mixture was then stirred at 78-82°C for 2 hours. The internal temperature was then gradually raised to 120°C, and the mixture was heated until the distillation of methyl formate, methanol and trimethyl orthoformate completely stopped. After cooling the reaction solution to room temperature, the reaction solution was diluted with ethyl acetate, the organic layer was washed with 100ml of 5% potassium carbonate aqueous solution and separated, and the solvent was distilled off. 80mL of dichloromethane was added to the residue to precipitate crystals, which were then filtered and dried to obtain 52.0g of 2,2-bis(4-hydroxyphenyl)-1,3-dioxolane. GC analysis of the crystals revealed that they were 99.8% 2,2-bis(4-hydroxyphenyl)-1,3-dioxolane and 0.2% 4,4'-dihydroxybenzophenone.
[0126] Synthesis Example 2 Synthesis of disodium 3,3'-disulfonate-4,4'-difluorobenzophenone represented by the following general formula (G2)
[0127] [ka]
[0128] 109.1 g of 4,4'-difluorobenzophenone (Aldrich reagent) was dissolved in fuming sulfuric acid (50% SO 3 The mixture was reacted at 100°C for 10 hours in 150 mL of ethyl acetate (Wako Pure Chemical Industries, Ltd., reagent). The mixture was then poured little by little into a large amount of water, neutralized with NaOH, and 200 g of salt was added to precipitate the product. The resulting precipitate was filtered and recrystallized from an aqueous ethanol solution to obtain disodium 3,3'-disulfonate-4,4'-difluorobenzophenone represented by the above general formula (G2). The purity was 99.3%. The structure is 1 The product was confirmed by H-NMR. Impurities were quantitatively analyzed by capillary electrophoresis (organic substances) and ion chromatography (inorganic substances). Example 1 Into a 500 mL three-neck flask equipped with a stirrer, a nitrogen inlet tube, and a Dean-Stark trap, 13.82 g of potassium carbonate (Aldrich reagent, 100 mmol), 20.66 g (80 mmol, 50 mol%) of K-DHBP obtained in Synthesis Example 1 as general formula (Q3), 12.02 g (28 mmol, 17.5 mol%) of disodium 3,3'-disulfonate-4,4'-difluorobenzophenone obtained in Synthesis Example 2 as general formula (Q1), and 11.34 g (Aldrich reagent, 52 mmol, 32.5 mol%) of 4,4'-difluorobenzophenone as general formula (Q2) were placed, and after nitrogen replacement, the mixture was dehydrated at 180°C in 90 mL of N-methylpyrrolidone (NMP) and 45 mL of toluene, and then heated to remove toluene, and polymerization was carried out at 200°C for 3 hours. The polymer electrolyte material was obtained by reprecipitation with a large amount of water for purification.
[0129] A 25% by weight N-methylpyrrolidone (NMP) solution containing the polymer electrolyte material was pressure filtered using a glass fiber filter, and then cast onto a glass substrate and dried at 100°C for 4 hours to obtain a polyketal ketone membrane. The membrane was then immersed in a 10% by weight aqueous sulfuric acid solution at 80°C for 24 hours to carry out proton substitution and deprotection reactions, and then thoroughly washed by immersing in a large excess of pure water for 24 hours to obtain a polymer electrolyte membrane for redox flow batteries. (Examples 2 to 13 and Comparative Examples 1 to 3) The same procedure as in Example 1 was carried out except that the types of compounds used and the production conditions were changed as shown in Tables 1 and 2. Comparative Example 4 Various characteristics were evaluated using a commercially available Nafion (registered trademark) 212 membrane (manufactured by DuPont). The Nafion (registered trademark) 212 membrane was immersed in 5% hydrogen peroxide water at 100°C for 30 minutes, then in 5% dilute sulfuric acid at 100°C for 30 minutes, and then thoroughly washed with deionized water at 100°C. Comparative Example 5 Various characteristics were evaluated using a commercially available Nafion (registered trademark) 211 membrane (manufactured by DuPont). The Nafion (registered trademark) 212 membrane was immersed in 5% hydrogen peroxide water at 100°C for 30 minutes, then in 5% dilute sulfuric acid at 100°C for 30 minutes, and then thoroughly washed with deionized water at 100°C.
[0130] [Table 1]
[0131] [Table 2]
[0132] As shown in Tables 1 and 2, the polymer electrolyte membranes of Examples 1 to 13 had lower active material permeability and were superior in dimensional stability, mechanical strength, and oxidation resistance compared to the polymer electrolyte membranes of Comparative Examples 1 to 5. [Industrial Applicability]
[0133] The electrolyte membrane of the present invention is applicable to various electrochemical devices (e.g., fuel cells, water electrolysis devices, chloroalkali electrolysis devices, etc.). Among these devices, the electrolyte membrane is suitable for fuel cells, and is particularly suitable for fuel cells that use an aqueous methanol solution as fuel.
[0134] Applications of the polymer electrolyte fuel cell of the present invention are not particularly limited, but it can be preferably used as a power supply source for mobile devices such as mobile phones, personal computers, PDAs, video cameras, and digital cameras, home appliances such as cordless vacuum cleaners, toys, vehicles such as electric bicycles, motorcycles, automobiles, buses, and trucks, ships, and mobile bodies such as trains, and stationary generators, as a replacement for conventional primary batteries or secondary batteries, or as a hybrid power source with these.
Claims
1. A polymer electrolyte membrane for redox flow batteries, comprising a polymer electrolyte material having a molar fraction of repeating units derived from an aromatic dihalide compound represented by the following general formula (Q1) of 15 mol% or more and 25 mol% or less, a molar fraction of repeating units derived from a compound represented by the following general formula (Q2) of 25 mol% or more and 35 mol% or less, a molar fraction of repeating units derived from an aromatic diol compound represented by the following general formula (Q3) of 20 mol% or more and 50 mol% or less, and a molar fraction of repeating units derived from at least one compound selected from the group consisting of compounds represented by the following general formulas (X-1) and (X-2) of 30 mol% or less, and having a weight average molecular weight Mw of 420,000 or more and 560,000 or less. 【Chemistry 1】 【Chemistry 2】 【Chemistry 3】 【Chemistry 4】 (In general formulas (Q1) to (Q3), 1 and X 2 is an electron-withdrawing group, Y is an ionic group, Z 1 and Z 2 is halogen, D 3 is oxygen or sulfur, A 3 represents a divalent organic group containing an aromatic ring. 3 has a protecting group.)
2. At 25°C, the tetravalent vanadium concentration is 1.5 mol L -1 , sulfuric acid concentration 3.0 mol・L -1 The amount of active material permeated through the aqueous solution is 800×10 -7 2. The polymer electrolyte membrane according to claim 1, wherein the flow rate is 100 s or less.
3. 3. The polymer electrolyte membrane for a redox flow battery according to claim 1, wherein the polymer electrolyte material contains a hydrocarbon-based polymer having an ionic group.
4. 4. The polymer electrolyte membrane for a redox flow battery according to claim 1, wherein the ionic group is a sulfonic acid group.
5. 5. The polymer electrolyte membrane for redox flow batteries according to claim 1, wherein the polymer electrolyte material has a sulfonic acid group density of 1.0 to 3.0 mmol / g.
6. 6. The polymer electrolyte membrane for a redox flow battery according to claim 1, wherein the polymer electrolyte material does not contain a crosslinked structure.
Citation Information
Patent Citations
Polyelectrolyte film and its preparation
JP1994093114A
Fuel cell
JP2004528683A
Polymer electrolyte material and polymer electrolyte molded unit formed of the same, polymer electrolyte membrane, membrane electrode composite, and solid polymer fuel cell
JP2008066273A
Process for producing polymer molded product
JP2008239963A
Ion-conducting sulfonated polymeric materials
US20020091225A1