Metallized films and film capacitors

The metallized film design addresses high dielectric loss and self-heating in film capacitors by using dual-function fuses, ensuring efficient electrode separation and capacitance maintenance.

JP7567356B2Active Publication Date: 2024-10-16OJI HLDG CORP
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2020177719
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-10-23
Publication Date
2024-10-16
Estimated Expiration
2040-10-23

AI Technical Summary

Technical Problem

Film capacitors with split electrode parts connected by fuses experience high dielectric loss (tanδ) and self-heating, and the effective electrode area is lost when horizontal fuses blow without vertical fuses.

Method used

A metallized film design with divided electrode sections connected via fuses that function as both horizontal and vertical fuses, reducing the number of fuses and minimizing self-heating and electrode area loss.

Benefits of technology

The design suppresses dielectric loss and self-heating, maintaining capacitance by efficiently separating electrodes and reducing unnecessary electrode area loss.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007567356000003
    Figure 0007567356000003
  • Figure 0007567356000004
    Figure 0007567356000004
  • Figure 0007567356000005
    Figure 0007567356000005
Patent Text Reader

Abstract

To provide a metallized film etc., capable of suppressing self-heating when formed into a film capacitor, and suppressing a case in which effective electrode area is lost unnecessarily.SOLUTION: A metallized film comprises a dielectric film. On the dielectric film, an electric introduction part, an insulation margin, and an electrode part positioned between the electric introduction part and insulation margin are formed. The electrode part is divided through a margin part into a large electrode part, a first division electrode part, second division electrode parts, and third division electrode parts which are arranged in order from the electric introduction part to the insulation margin. The large electrode part is connected to the first division electrode through a first fuse part. The first electrode part is connected to two second division electrodes through one second fuse part. The second division electrodes are connected to two third division electrodes through one third fuse.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to metallized films and film capacitors. [Background technology]

[0002] Japanese Patent Laid-Open Publication No. 2005-12082 (Patent Document 1) discloses a metallized film capacitor. In this metallized film capacitor, a pattern of a metal vapor-deposited film is formed on a dielectric film. In this pattern, a plurality of divided small electrode portions are formed via dividing margins. Two adjacent divided small electrode portions in the width direction of the metal vapor-deposited film are connected by a fuse portion (horizontal fuse) extending in the width direction of the metal vapor-deposited film (see Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2005-12082 A Summary of the Invention [Problem to be solved by the invention]

[0004] Generally, in a film capacitor in which split electrodes are connected to each other by fuses, if there are a large number of fuses in a certain area, the dielectric loss (tan δ) of the capacitor when a voltage is applied is large, and the fuses are likely to self-heat. As in the film capacitor disclosed in the above Patent Document 1, heat generation in the film capacitor can be suppressed by connecting adjacent split electrodes to each other only by horizontal fuses. However, if no vertical fuses are provided, if the horizontal fuses blow, the effective electrode area may be lost more than necessary.

[0005] The present invention has been made to solve such problems, and its object is to provide a metallized film etc. that can suppress an increase in dielectric loss (tan δ) and self-heating when used in a film capacitor, improve durability in high-temperature environments, and suppress a situation in which the effective electrode area is lost more than necessary, thereby minimizing the decrease in capacitance of the capacitor. [Means for solving the problem]

[0006] A metallized film according to an aspect of the present invention is a metallized film for a film capacitor. The metallized film includes a dielectric film. An electricity lead-in portion located at one end of the width direction of the metallized film and connected to a metallikon electrode, an insulating margin located at the other end of the width direction of the metallized film, and an electrode portion located between the electricity lead-in portion and the insulating margin are formed on the dielectric film. The electrode portion is divided into a large electrode portion, a first divided electrode portion, a second divided electrode portion, and a third divided electrode portion, which are arranged in order from the electricity lead-in portion toward the insulating margin, via the margin portion. The first, second, and third divided electrode portions are each divided into a plurality of first, second, and third divided electrodes in a direction perpendicular to the width direction of the metallized film, via the margin portion. The number of second divided electrodes present at positions corresponding to one first divided electrode in the direction perpendicular to the width direction of the metallized film is two or more and three or less. The number of third divided electrodes present at positions corresponding to one first divided electrode in the direction perpendicular to the width direction of the metallized film is three or more and six or less. The large electrode portion is connected to a first split electrode via a first fuse. The first split electrode is connected to two second split electrodes via one second fuse. The second split electrode is connected to two third split electrodes via one third fuse.

[0007] In this metallized film, for example, the first split electrode and the two second split electrodes are connected via one second fuse. The first split electrode and the two second split electrodes are aligned in the width direction (horizontal direction) of the metallized film. The two second split electrodes are aligned in the direction (vertical direction) perpendicular to the width direction of the metallized film. The second fuse connects the first split electrode and the two second split electrodes, and therefore serves as both a horizontal fuse and a vertical fuse. Therefore, with this metallized film, it is not necessary to provide a horizontal fuse and a vertical fuse independently, so that the number of fuses can be reduced and self-heating can be suppressed when the film capacitor is formed. Furthermore, with this metallized film, each of the second fuse and the third fuse also functions as a vertical fuse, so that it is possible to suppress a situation in which the effective electrode area is lost more than necessary.

[0008] In the above metallized film, when the area of ​​the first divided electrode is taken as 1, the area of ​​the second divided electrode may be 1 / 3 or more and 1 / 2 or less, and the area of ​​the third divided electrode may be 1 / 12 or more and 1 / 3 or less.

[0009] Generally, when a metallized film is used to make a film capacitor, two metallized films are superimposed so that the electrical introduction parts are located at the opposite ends. That is, the third divided electrode part of one film is located at a position facing the large electrode part of the other film, and the second divided electrode part of the other film is located at a position facing the first divided electrode part of the other film. In the metallized film according to the present invention, the area of ​​the third divided electrode is smaller than each of the first divided electrode and the second divided electrode. Therefore, with this metallized film, even if a dielectric breakdown occurs in a part of the large electrode part due to an inrush current, the area of ​​the third divided electrode facing the position where the dielectric breakdown occurred is small, so that even if a fuse is blown, the effective electrode area that is lost can be reduced.

[0010] In the metallized film, when the area of ​​the first divided electrode is taken as 1, the area of ​​the third divided electrode may be 1 / 6 or more and 1 / 3 or less.

[0011] In the metallized film, when the width of the first fuse is 1, the width of the second fuse may be 0.6 to 0.9, and the width of the third fuse may be 0.3 to 0.6.

[0012] In this metallized film, the fuse width gradually narrows from the first fuse to the third fuse. Therefore, this metallized film makes it easier for the fuses connecting the split electrodes with smaller areas to blow, thereby preventing an unnecessarily large loss of effective electrode area.

[0013] In the above metallized film, the second fuse may be formed at a position adjacent to two second split electrodes adjacent to each other in a direction perpendicular to the width direction of the metallized film, and adjacent to each of the first split electrodes adjacent to both of the two second split electrodes in the width direction of the metallized film.

[0014] The second fuse is adjacent to each of the first split electrode and the two second split electrodes, and therefore serves as both a horizontal fuse and a vertical fuse. Therefore, with this metallized film, it is not necessary to provide a horizontal fuse and a vertical fuse independently, so the number of fuses can be reduced, and a split electrode in which insulation breakdown has occurred can be electrically separated more efficiently while a current flow path to the split electrodes is secured in the case of a film capacitor, so that the time for which a short-circuit current flows can be shortened and self-heating of the element can be suppressed.

[0015] In the above metallized film, the third fuse may be formed at a position adjacent to two third split electrodes adjacent to each other in a direction perpendicular to the width direction of the metallized film, and adjacent to each of the second split electrodes adjacent to both of the two third split electrodes in the width direction of the metallized film.

[0016] The third fuse is adjacent to each of the second split electrode and the two third split electrodes, and therefore serves as both a horizontal fuse and a vertical fuse. Therefore, with this metallized film, it is not necessary to provide a horizontal fuse and a vertical fuse independently, so the number of fuses can be reduced, and it is possible to electrically separate a split electrode in which insulation breakdown has occurred while securing a current flow path to the split electrodes in a film capacitor, thereby shortening the time for which a short-circuit current flows and suppressing self-heating of the element.

[0017] A film capacitor according to another aspect of the present invention is constructed using the above-described metallized film. Effect of the Invention

[0018] According to the present invention, it is possible to provide a metallized film etc. that can minimize the decrease in capacitance of the capacitor by suppressing self-heating when made into a film capacitor and by suppressing the situation in which the effective electrode area is lost more than necessary. [Brief description of the drawings]

[0019] [Figure 1] FIG. 2 is a schematic diagram showing a portion of a plane of a metallized film. [Diagram 2] 2 is an enlarged view that illustrates a schematic view of a portion P1 of FIG. [Diagram 3] 2 is an enlarged view showing a schematic view of a portion P2 of FIG. 1. FIG. [Figure 4] 2 is an enlarged view showing a schematic view of a portion P3 of FIG. 1. FIG. [Diagram 5] FIG. 2 is an enlarged view showing a schematic view of a portion of a metallized film. [Figure 6] FIG. 2 is a diagram for explaining the orientation of two metallized films that are superimposed when manufacturing a film capacitor. [Figure 7] FIG. 13 is a diagram illustrating a schematic view of a portion of a plane of a metallized film in a first modified example. [Figure 8]FIG. 11 is a diagram illustrating a schematic view of a portion of a plane of a metallized film in a second modified example. [Figure 9] FIG. 13 is a diagram illustrating a schematic view of a portion of a plane of a metallized film in a third modified example. [Figure 10] FIG. 13 is a diagram illustrating a schematic view of a portion of a plane of a metallized film in a fourth modified example. [Figure 11] 1 is a diagram showing a part of a plane of a metallized film in Comparative Example 1. FIG. [Figure 12] 13 is a diagram showing a part of a plane of a metallized film in Comparative Example 2. FIG. [Figure 13] 13 is a diagram showing a part of a plane of a metallized film in Comparative Example 3. FIG. [Figure 14] 13 is a diagram showing a part of a plane of a metallized film in Comparative Example 4. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the accompanying drawings. In the drawings, the same or corresponding parts are designated by the same reference characters and their description will not be repeated.

[0021] [1. Composition of metallized film] Fig. 1 is a schematic diagram showing a portion of a plane of metallized film 10 according to the present embodiment. In Fig. 1, only a portion of metallized film 10 in the flow direction is shown. Metallized film 10 is used, for example, in the manufacture of a film capacitor. Hereinafter, the width direction of metallized film 10 will also be simply referred to as the "width direction," and the flow direction of metallized film 10 will also be simply referred to as the "flow direction."

[0022] 1, metallized film 10 includes dielectric film 20. As dielectric film 20, various insulating resins such as polypropylene (PP), polyethylene terephthalate (PET), polyphenylene sulfide (PPS), polyethylene naphthalate (PEN), and polyvinylidene difluoride (PVDF) can be used.

[0023] The thickness of the dielectric film 20 is not particularly limited, but is preferably 0.5 μm to 25 μm, and more preferably 1.5 μm to 10 μm.

[0024] In dielectric film 20, an electrical lead-in portion 30, which is an area where a metal (e.g., aluminum or zinc) is vapor-deposited, is formed at one end, and an insulating margin 40, which is an area where no metal is vapor-deposited, is formed at the other end. When a film capacitor is manufactured using metallized film 10, an electrical lead-in portion 30 is connected to a metallikon electrode.

[0025] An electrode section 50 is formed between the electricity introducing section 30 and the insulating margin 40. The electrode section 50 is formed by evaporating a metal (for example, aluminum or zinc) onto the dielectric film 20.

[0026] The metal forming electrode section 50 and electricity introducing section 30 is not particularly limited, but may be, for example, a metal material such as aluminum (Al), zinc (Zn), tin (Sn), copper (Cu), or an alloy thereof. The thickness of the metal vapor deposition electrode (electrode section 50) is not particularly limited, but is preferably 1 nm to 200 nm. The thickness of the metal vapor deposition film of electricity introducing section 30 is preferably about 2 to 5 times that of the metal vapor deposition electrode. The thickness of the metal vapor deposition electrode may be set according to the resistivity of the metal vapor deposition electrode material so as to obtain the desired electrical characteristics.

[0027] The electrode section 50 is divided into a large electrode section 100, a first divided electrode section 200, a second divided electrode section 300, and a third divided electrode section 400, which are arranged in order from the electricity introducing section 30 toward the insulating margin 40, via a margin section 60, which is an area where no metal is vapor-deposited. Each of the large electrode section 100, the first divided electrode section 200, the second divided electrode section 300, and the third divided electrode section 400 is formed by vapor-depositing a metal.

[0028] First divided electrode portion 200 is divided into multiple first divided electrodes 210 in a direction (flow direction) perpendicular to the width direction of metallized film 10 via margin portion 60. The width direction length of each first divided electrode 210 is, for example, 160% (1.6 times) or more and 180% (1.8 times) or less of the width direction length of large electrode portion 100.

[0029] Second divided electrode portion 300 is divided into a plurality of second divided electrodes 310 in the flow direction of metallized film 10 via margin portion 60. For example, the number of second divided electrodes 310 present at a position corresponding to one first divided electrode 210 in the flow direction of metallized film 10 is two. Note that the number of second divided electrodes 310 present at a position corresponding to one first divided electrode 210 in the flow direction of metallized film 10 does not necessarily have to be two, and may be three. Furthermore, the width direction length of each second divided electrode 310 is, for example, 80% (0.8 times) or more and 120% (1.2 times) or less of the width direction length of first divided electrode 210.

[0030] The third divided electrode portion 400 is divided into a plurality of third divided electrodes 410 in the flow direction of the metallized film 10 via margin portions 60. For example, the number of third divided electrodes 410 present at positions corresponding to one first divided electrode 210 in the flow direction of the metallized film 10 is three. The number of third divided electrodes 410 present at positions corresponding to one first divided electrode 210 in the flow direction of the metallized film 10 may be four or more and six or less. The widthwise length of each third divided electrode 410 is, for example, 45% (0.45 times) or more and 55% (0.55 times) or less of the widthwise length of each first divided electrode 210.

[0031] Thus, in metallized film 10, the areas of first divided electrode 210 are largest, followed by second divided electrode 310 and third divided electrode 410. For example, assuming that the area of ​​first divided electrode 210 is 1, the area of ​​second divided electrode 310 is 1 / 3 or more and 1 / 2 or less, and the area of ​​third divided electrode 410 is 1 / 12 or more and 1 / 3 or less. Preferably, the area of ​​third divided electrode 410 is 1 / 6 or more and 1 / 3 or less.

[0032] Fig. 2 is an enlarged view showing a schematic view of a part of portion P1 in Fig. 1. As shown in Fig. 2, the large electrode portion 100 is electrically connected to the first split electrode 210 via the first fuse 70. The width of the first fuse 70 is L1.

[0033] Fig. 3 is an enlarged view showing a schematic view of a part of portion P2 in Fig. 1. As shown in Fig. 3, the first split electrode 210 is electrically connected to two second split electrodes 310 via second fuses 72. That is, the second fuses 72 are formed at positions adjacent to two second split electrodes 310 adjacent to each other in the flow direction and to each of the first split electrodes 210 adjacent to both of the two second split electrodes 310 in the width direction.

[0034] That is, the second fuse 72 serves as a horizontal fuse that electrically connects the first divided electrode 210 and the second divided electrode 310 aligned in the width direction, and as a vertical fuse that electrically connects the two second divided electrodes 310 aligned in the flow direction. Therefore, with the metallized film 10, it is not necessary to provide a horizontal fuse and a vertical fuse independently, so that the number of fuses can be reduced, and when the film capacitor is formed, the effective electrode area is prevented from being lost more than necessary, thereby minimizing the decrease in capacitance of the capacitor. The width of the second fuse 72 is L2.

[0035] Fig. 4 is an enlarged view showing a schematic view of a part of portion P3 in Fig. 1. As shown in Fig. 4, the second split electrode 310 is electrically connected to two third split electrodes 410 via a third fuse 74. That is, the third fuse 74 is formed at a position adjacent to each of the two third split electrodes 410 adjacent to each other in the flow direction and the second split electrode 310 adjacent to both of the two third split electrodes 410 in the width direction.

[0036] That is, the third fuse 74 serves as a horizontal fuse that electrically connects the second divided electrodes 310 and the third divided electrodes 410 arranged in the width direction, and as a vertical fuse that electrically connects the two third divided electrodes 410 arranged in the flow direction. Therefore, with the metallized film 10, it is not necessary to provide a horizontal fuse and a vertical fuse independently, so that the number of fuses can be reduced, and when the film capacitor is formed, the effective electrode area is prevented from being lost more than necessary, thereby minimizing the decrease in capacitance of the capacitor. The width of the third fuse 74 is L3.

[0037] In metallized film 10, first fuse 70, second fuse 72, and third fuse 74 have the widest widths in that order. For example, when width L1 of first fuse 70 is 1, width L2 of second fuse 72 is 0.6 or more and 0.9 or less, and width L3 of third fuse 74 is 0.3 or more and 0.6 or less. In this manner, in metallized film 10, the fuse widths gradually narrow from first fuse 70 to third fuse 74. Therefore, in metallized film 10, fuses connecting split electrodes with smaller areas are more likely to blow, which prevents a situation in which an effective electrode area is lost more than necessary.

[0038] Fig. 5 is an enlarged view showing a schematic view of a portion of metallized film 10. With reference to Fig. 5, for example, assume that second fuse 72 is blown at portion P4. As described above, second fuse 72 and third fuse 74 each function as both a horizontal fuse and a vertical fuse. In this case, the current flowing from first split electrode 210 flows, for example, along the arrow in the figure, through second split electrode 310, third fuse 74, and third split electrode 410 at the bottom of the figure, into second split electrode 310 at the top of the figure.

[0039] That is, in metallized film 10, even if second fuse 72 is blown at portion P4, the area of ​​second split electrode 310 at the upper part in the figure is not immediately lost from the effective electrode area. In this way, according to metallized film 10, second fuse 72 and third fuse 74 each function not only as a horizontal fuse but also as a vertical fuse, so that it is possible to prevent the effective electrode area from being lost more than necessary.

[0040] FIG. 6 is a diagram for explaining the orientation of two metallized films 10 that are superposed when manufacturing a film capacitor 5. As shown in FIG. 6, when the metallized films 10 are used to form a film capacitor 5, the two metallized films 10 are superposed so that the electrical lead-in portions 30 are located at the opposite ends. That is, the third divided electrode portion 400 of one film is located at a position facing the large electrode portion 100 of the other film, and the second divided electrode portion 300 of the other film is located at a position facing the first divided electrode portion 200 of the other film. In the metallized film 10, the area of ​​the third divided electrode 410 is smaller than each of the first divided electrode 210 and the second divided electrode 310. Therefore, according to the metallized film 10, even if a dielectric breakdown occurs in a part of the large electrode portion 100 due to an inrush current, the area of ​​the third divided electrode portion 400 facing the position where self-healing or the like occurs is small, so that the loss of the effective electrode area can be suppressed.

[0041] [2. Features] As described above, in the metallized film 10 according to the present embodiment, for example, the first split electrode 210 and the two second split electrodes 310 are connected via one second fuse 72. The first split electrode 210 and the two second split electrodes 310 are arranged in the width direction (horizontal direction) of the metallized film 10. The two second split electrodes 310 are arranged in the flow direction (vertical direction) of the metallized film 10. The second fuse 72 connects the first split electrode 210 and the two second split electrodes 310, and therefore serves as both a horizontal fuse and a vertical fuse. Therefore, according to the metallized film 10, it is not necessary to provide a horizontal fuse and a vertical fuse independently, so that the number of fuses can be reduced and self-heating can be suppressed when the film capacitor 5 is formed. In addition, according to the metallized film 10, each of the second fuse 72 and the third fuse 74 also functions as a vertical fuse, so that it is possible to suppress a situation in which the effective electrode area is lost more than necessary.

[0042] [3. Modifications] Although the embodiment has been described above, the present invention is not limited to the above embodiment, and various modifications are possible without departing from the spirit of the present invention.

[0043] <3-1> 7 is a schematic diagram of a portion of a plane of metallized film 10A in the first modified example. As shown in Fig. 7, the number of second divided electrodes 310A present at a position corresponding to one first divided electrode 210A in the flow direction of metallized film 10A may be three.

[0044] <3-2> Fig. 8 is a schematic diagram showing a portion of a plane of metallized film 10B in the second modified example. As shown in Fig. 8, the relative position of each third divided electrode 410B to first divided electrode 210B in the flow direction differs from that in metallized film 10 according to the above embodiment. The relative position of the third divided electrode to the first divided electrode in the flow direction may be as shown in Fig. 8.

[0045] <3-3> FIG. 9 is a schematic diagram showing a part of a plane of a metallized film 10C in a third modified example. As shown in FIG. 9, the widthwise length of each of the first divided electrode portion 200C, the second divided electrode portion 300C, and the third divided electrode portion 400C may be the same. In this case, the widthwise length of the large electrode portion 100C is preferably 1 / 5 or more and 1 / 4 or less of the widthwise length of the metallized film 10C. For example, when the widthwise length of the large electrode portion 100C is 1 / 4 or less of the widthwise length of the metallized film 10C, the loss of the effective electrode area due to dielectric breakdown on the electricity introduction side can be reduced, and the shift of the overlapping divided electrodes can be reduced, so that the divided electrodes separated by dielectric breakdown can be reduced, and the effect of suppressing the decrease in capacitance can be improved. In addition, when the widthwise length of the large electrode portion 100C is 1 / 5 or more of the widthwise length of the metallized film 10C, the area of ​​the divided electrodes to be set can be reduced, and the loss of the effective electrode area at the time of dielectric breakdown can be reduced, and the effect of suppressing the decrease in capacitance can be improved.

[0046] <3-4> Fig. 10 is a schematic diagram of a portion of a plane of metallized film 10D in the fourth modified example. As shown in Fig. 10, in the flow direction of metallized film 10A, the number of second divided electrodes 310D present at positions corresponding to one first divided electrode 210D may be three, and further, the number of third divided electrodes 410D present at positions corresponding to one first divided electrode 210D may be six.

[0047] [4. Examples, etc.] <4-1. Examples and Comparative Examples> (4-1-1. Example 1-3) In metallized film 10 in Examples 1-3, the split electrode pattern shown in Fig. 1 was formed. That is, in each of Examples 1-3, the ratio of the lengths in the flow direction of first split electrode 210, second split electrode 310, and third split electrode 410 was 1:1 / 2:1 / 3. The length in the flow direction of first split electrode 210 was 4.6 mm. In addition, the ratio of the lengths in the width direction of first split electrode 210, second split electrode 310, and third split electrode 410 was 1:1:1 / 2. The length in the width direction of first split electrode 210 was 8.0 mm.

[0048] In Examples 1 to 3, the relationship between the widths of the fuses was different from one another. In Example 1, when the width of the first fuse 70 was 1, the width of the second fuse 72 was 0.7, and the width of the third fuse 74 was 0.5. The width of the first fuse 70 was 0.35 mm.

[0049] In the second embodiment, assuming that the width of the first fuse 70 is 1, the width of the second fuse 72 is 0.6, and the width of the third fuse 74 is 0.3. The width of the first fuse 70 is 0.35 mm.

[0050] In the third embodiment, assuming that the width of the first fuse 70 is 1, the width of the second fuse 72 is 0.9, and the width of the third fuse 74 is 0.6. The width of the first fuse 70 is 0.35 mm.

[0051] (4-1-2. Example 4) In metallized film 10D in Example 4, the split electrode pattern shown in Fig. 10 was formed. That is, in Example 4, the ratio of the lengths in the flow direction of first split electrode 210D, second split electrode 310D, and third split electrode 410D was 1:1 / 3:1 / 6. The length in the flow direction of first split electrode 210D was 4.6 mm. Moreover, the ratio of the lengths in the width direction of first split electrode 210D, second split electrode 310D, and third split electrode 410D was 1:1:1 / 2. The length in the width direction of first split electrode 210 was 8.5 mm.

[0052] In the fourth embodiment, when the width of the first fuse 70D is taken as 1, the width of the second fuse 72D is 0.7, and the width of the third fuse 74D is 0.5. The width of the first fuse 70D was 0.35 mm.

[0053] (4-1-3. Comparative Example 1) Fig. 11 is a diagram showing a portion of a plane of metallized film 10E in Comparative Example 1. As shown in Fig. 11, in metallized film 10E in Comparative Example 1, a so-called fishnet-type divided electrode pattern was formed by margin portion 60E. In metallized film 10E in Comparative Example 1, a plurality of divided electrodes (segments) was formed by margin portion 60E, and fuses 76E were formed on each of the four sides of each divided electrode.

[0054] (4-1-4. Comparative Example 2) Fig. 12 is a diagram showing a part of a plane of metallized film 10F in Comparative Example 2. As shown in Fig. 12, in metallized film 10F in Comparative Example 2, the ratio of the lengths in the flow direction of first divided electrode 210F, second divided electrode 310F, and third divided electrode 410F was 1:1:1 / 2. The length in the flow direction of first divided electrode 210 was 4.6 mm. In addition, the ratio of the lengths in the width direction of first divided electrode 210F, second divided electrode 310F, and third divided electrode 410F was 1:1:1 / 2. The length in the width direction of first divided electrode 210F was 8.5 mm.

[0055] In Comparative Example 2, when the width of first fuse 70F was taken as 1, the width of second fuse 72F was 0.6, and the width of third fuse 74F was 0.4. The width of first fuse 70F was 0.35 mm.

[0056] (4-1-5. Comparative Example 3) Fig. 13 is a diagram showing a part of a plane of metallized film 10G in Comparative Example 3. As shown in Fig. 13, in metallized film 10G in Comparative Example 3, the ratio of the lengths in the flow direction of first split electrode 210G, second split electrode 310G, and third split electrode 410G was 1:1 / 4:1 / 8. The length in the flow direction of first split electrode 210G was 4.6 mm. In addition, the ratio of the lengths in the width direction of first split electrode 210G, second split electrode 310G, and third split electrode 410G was 1:1:1 / 2. The length in the width direction of first split electrode 210G was 8.5 mm.

[0057] In Comparative Example 3, when the width of first fuse 70G was taken as 1, the width of second fuse 72G was 0.5, and the width of third fuse 74G was 0.3. The width of first fuse 70G was 0.35 mm.

[0058] (4-1-6. Comparative Example 4) Fig. 14 is a diagram showing a portion of a plane of metallized film 10H in Comparative Example 4. As shown in Fig. 14, in metallized film 10H in Comparative Example 4, electrode portion 50H is formed by solidly depositing a metal film on a dielectric film, and a divided electrode pattern is not formed.

[0059] The properties of Examples 1-4 and Comparative Examples 1-4 are shown in Table 1 below.

[0060] [Table 1] <4-2. Manufacturing method> (4-2-1. Examples 1-3 and Comparative Examples 1-3) Each of Examples 1-3 and Comparative Examples 1-3 was manufactured by a common method. Note that, in each of Examples 1-3 and Comparative Examples 1-3, the shape of the divided electrode pattern formed on the dielectric film was different. The manufacturing method common to Examples 1-3 and Comparative Examples 1-3 will be described below.

[0061] An insulating margin and a divided electrode pattern were formed on a PP (polypropylene) film roll with a thickness of 2.3 μm by oil masking using a winding vacuum deposition device (EWE-060) manufactured by ULVAC. Aluminum was deposited to form electrodes on the film, and zinc was deposited to form heavy edges (electrical introduction parts) on the film. This resulted in a metallized film roll with an electrode pattern with an Al metal film resistance of 20 Ω / □ and a Zn metal film resistance of 5 Ω / □. The metallized film roll thus produced was cut to an arbitrary width using a slitter to produce a small reel of metallized film for winding elements with a film width of 30 mm, an insulating margin width of 2.0 mm, and a heavy edge width of 1.5 mm. The elements were wound on the small reel so that the capacitance was 50 μF using a fully automatic metallized film capacitor winding machine (3KAW-N2) manufactured by Kaito Seisakusho, and then pressed and flattened. The flattened element was sprayed with metallicon on the element end faces, and after forming the film electrode extraction part, the element was heat treated at high temperature in a vacuum to harden the element. Leads were attached to the metallicon sprayed part, the element was placed in a resin case, and the gaps were filled with epoxy resin. The resin was then hardened to obtain a film capacitor element for evaluation.

[0062] (4-2-2. Comparative Example 4) An insulating margin was formed on a PP (polypropylene) film roll with a thickness of 2.3 μm by oil masking using an ULVAC winding vacuum deposition device (EWE-060). A divided electrode pattern was not formed. Aluminum was deposited to form electrodes on the film, and zinc was deposited to form heavy edges (electrical introduction parts) on the film. This resulted in a metallized film roll with an electrode pattern with an Al metal film resistance of 20 Ω / □ and a Zn metal film resistance of 5 Ω / □. The metallized film roll thus prepared was wound on a Kaito Manufacturing Co., Ltd. metallized film capacitor fully automatic winding machine (3KAW-N2) to make the capacitance 50 μF, and then pressed and flattened. Metallicon was sprayed on the end faces of the flattened elements, and after forming the film electrode extraction parts, the elements were heat-treated at high temperature in a vacuum to harden them. Leads were attached to the metallikon-sprayed portion, the resultant was placed in a resin case, and the gaps were filled with epoxy resin, which was then cured to obtain a film capacitor element for evaluation.

[0063] <4-3. Testing method> An applied voltage boost test, a short-time voltage withstand test and an accelerated life test were carried out.

[0064] (4-3-1. Applied voltage boost test) A voltage was applied to the film capacitor element for 1 hour while the film capacitor element was heated to 115°C using a thermostatic chamber, and the capacitance of the film capacitor element was then measured. This voltage application test was carried out by gradually increasing the voltage, and the voltage at which the capacitance reduction rate reached 10% and the voltage at which the capacitance reduction rate reached 20% were investigated.

[0065] (4-3-2. Short-time pressure test) A voltage was applied to the film capacitor element at room temperature for 10 seconds, and then the capacitance of the film capacitor element was measured. This voltage application test was carried out by gradually increasing the voltage, and the voltage at which the capacitance reduction rate reached 2% and the voltage at which the capacitance reduction rate reached 5% were investigated.

[0066] (4-3-3. Accelerated life test) A voltage was continuously applied to the film capacitor element while it was heated to 115°C using a thermostatic chamber, and the capacitance of the film capacitor element was measured after the voltage had been applied for a specified period of time. The capacitance reduction rate was measured after 200 hours had elapsed since the voltage application, and after 500 hours had elapsed since the voltage application.

[0067] <4-4. Evaluation results> The evaluation results are shown in Table 2 below.

[0068] [Table 2] As shown in Table 2, Comparative Example 1 gave unfavorable results in the applied voltage boost test and the accelerated life test, and Comparative Example 2 gave unfavorable results in the accelerated life test. Comparative Example 3 gave unfavorable results in the applied voltage boost test and the accelerated life test, and Comparative Example 4 gave unfavorable results in all tests. Compared with Comparative Examples 1-4, each of Examples 1-4 obtained stable good results in each test. In particular, Example 3 obtained the best results in most tests (except for the 500-hour accelerated life test). [Industrial Applicability]

[0069] The metallized film of the present invention can be used in various metallized film capacitors. The metallized film capacitor can be used in the following various applications. That is, (1) mobile terminals (mobile phones, portable music players, smartphones, tablet terminals, wearable devices, etc.), (2) personal computers, (3) digital cameras, (4) home appliances (televisions, DVD recorders, refrigerators, washing machines, air conditioners, etc.), (5) car navigation systems, (6) power conditioners for power generation (solar, wind, etc.), (7) LED lighting, (8) automobiles (electric vehicles, hybrid vehicles, plug-in hybrid vehicles, etc.), (9) railroad cars, (10) construction machinery, (11) industrial equipment, (12) other various inverters, etc. Among them, the metallized film capacitor can be used in capacitors used in automobiles and power applications that require high frequency characteristics. [Explanation of symbols]

[0070] 5 film capacitor, 10 metallized film, 20 dielectric film, 30 electrical introduction portion, 40 insulating margin, 50 electrode portion, 60 margin portion, 70 first fuse, 72 second fuse, 74 third fuse, 76E fuse, 100 large electrode portion, 200 first divided electrode portion, 210 first divided electrode, 300 second divided electrode portion, 310 second divided electrode, 400 third divided electrode portion, 410 third divided electrode, P1, P2, P3, P4 portions.

Claims

1. A metallized film for a film capacitor, comprising: A dielectric film is provided, on the dielectric film, an electrical lead-in portion located at one end in a width direction of the metallized film and connected to a metallikon electrode, an insulating margin located at the other end in the width direction, and an electrode portion located between the electrical lead-in portion and the insulating margin, the electrode portion is divided into a large electrode portion, a first divided electrode portion, a second divided electrode portion, and a third divided electrode portion, which are arranged in this order from the electricity introducing portion toward the insulating margin via a margin portion; the first, second, and third divided electrode portions are respectively divided into a plurality of first, second, and third divided electrodes in a direction perpendicular to the width direction via the margin portion; the number of the second divided electrodes present at a position corresponding to one of the first divided electrodes in a direction perpendicular to the width direction is two or more and three or less, the number of the third divided electrodes present at a position corresponding to one of the first divided electrodes in a direction perpendicular to the width direction is 3 or more and 6 or less, the large electrode portion is connected to the first split electrode via a first fuse, the first split electrode is connected to two of the second split electrodes via one second fuse, the second split electrode is connected to two of the third split electrodes via one third fuse, The first, second and third divided electrode portions each have the same length in the width direction, The length of the large electrode portion in the width direction is 1 / 5 or more and 1 / 4 or less of the length of the metallized film in the width direction. Metallized film.

2. 2. The metallized film of claim 1, wherein, when the area of ​​the first divided electrode is 1, the area of ​​the second divided electrode is 1 / 3 or more and 1 / 2 or less, and the area of ​​the third divided electrode is 1 / 12 or more and 1 / 3 or less.

3. 3 . The metallized film of claim 2 , wherein the area of ​​the third divided electrode is equal to or greater than ⅙ and equal to or less than ⅓ of the area of ​​the first divided electrode.

4. The metallized film of claim 2 or claim 3, wherein when the width of the first fuse is 1, the width of the second fuse is 0.6 or more and 0.9 or less, and the width of the third fuse is 0.3 or more and 0.6 or less.

5. The metallized film described in any one of claims 1 to 4, wherein the second fuse is formed at a position adjacent to two second split electrodes adjacent to each other in a direction perpendicular to the width direction, and adjacent to each of the first split electrodes adjacent to both of the two second split electrodes in the width direction.

6. The third fuse is formed at a position adjacent to two third split electrodes adjacent to each other in a direction perpendicular to the width direction, and adjacent to each of the second split electrodes adjacent to both of the two third split electrodes in the width direction.

7. A film capacitor comprising the metallized film according to any one of claims 1 to 6.

Citation Information

Patent Citations

  • A capacitor having safety film

    CN210349582U

  • Vacuum deposited and divided metal coated foil

    JP1992225508A

  • Metallized film capacitor

    JP1996250367A

  • Depositing film and film capacitor using same film and inverter device using same capacitor

    JP2004087648A

  • Metallized film capacitor

    JP2005012082A