How paper is made
By simultaneously adding alkenyl succinic anhydride and aluminum sulfate to the pulp slurry, the method enhances sizing properties and minimizes staining in paper production, especially in high ash content papers.
Patent Information
- Application Number
- JP2020207295
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-12-15
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2040-05-21
AI Technical Summary
Conventional paper manufacturing methods using sizing agents do not adequately improve sizing properties and reduce machine staining, particularly when high ash content papers are produced.
Simultaneously adding a mixture of alkenyl succinic anhydride and a water-soluble aluminum compound, such as aluminum sulfate, to the pulp slurry during the papermaking process, optimizing the amounts and timing of addition to enhance sizing properties and minimize staining.
The method improves sizing properties and significantly reduces staining in the papermaking system, particularly in high ash content papers, by effectively stabilizing the alkenyl succinic anhydride hydrolyzate.
Smart Images

Figure 0007567431000001 
Figure 0007567431000002 
Figure 0007567431000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for making paper. [Background technology]
[0002] Generally, paper is produced from a pulp slurry in which pulp fibers are suspended in water, and various chemicals are added to the pulp slurry as necessary in addition to the pulp fibers. The main chemicals used include retention aids, paper strength agents, fillers, sizing agents, and viscosity agents.
[0003] In recent years, efforts to reduce the weight of paper have been underway to reduce logistics costs, etc. One approach to reducing the weight of paper is to increase the content of inorganic particles called fillers in order to improve the whiteness, opacity, and printability of the paper.
[0004] In addition, a sizing agent is added to the pulp slurry in order to increase the water resistance of the paper and suppress ink bleeding. Patent Document 1 discloses a method for manufacturing paper in which a slurry containing a rosin-based sizing agent is used for papermaking. In this method, the addition of an aluminum compound such as aluminum sulfate is considered in order to increase the fixation rate of the sizing agent to the pulp. Patent Document 2 discloses a method for manufacturing paper in which alkenylsuccinic anhydride (ASA) is added as a sizing agent. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2017-8463 A [Patent Document 2] JP 2014-88644 A Summary of the Invention [Problem to be solved by the invention]
[0006] As mentioned above, various paper manufacturing methods using sizing agents have been disclosed. However, in the conventional techniques, the effect of the sizing agent may not be fully obtained, and the reduction of machine stains is not sufficient.
[0007] Therefore, in order to solve such problems of the conventional technology, the present inventors have carried out studies with the aim of improving the sizing properties of paper and reducing contamination in the papermaking system during the paper manufacturing process. [Means for solving the problem]
[0008] As a result of intensive research to solve the above problems, the present inventors have found that by adding a mixture of alkenyl succinic anhydride and a water-soluble aluminum compound, or by simultaneously adding alkenyl succinic anhydride and a water-soluble aluminum compound, in the process of obtaining a pulp slurry, it is possible to improve the sizing ability of paper and reduce staining in the papermaking system during the paper manufacturing process. Specifically, the present invention has the following configuration.
[0009] [1] A method for producing paper, comprising the steps of obtaining a pulp slurry and making paper from the pulp slurry, The method for producing paper, wherein the step of obtaining a pulp slurry includes a step of adding a mixture of alkenyl succinic anhydride and a water-soluble aluminum compound to a dispersion containing pulp and water, or a step of simultaneously adding alkenyl succinic anhydride and a water-soluble aluminum compound to a dispersion containing pulp and water. [2] The method for producing paper according to [1], wherein the water-soluble aluminum compound is aluminum sulfate. [3] The method for producing paper according to [1] or [2], wherein the amount of alkenyl succinic anhydride added is 0.01 to 0.30 parts by mass per 100 parts by mass of the bone dry mass of pulp in the pulp slurry. [4] The step of obtaining a pulp slurry is a step of adding a mixture of an alkenyl succinic anhydride and a water-soluble aluminum compound to a dispersion containing pulp and water, The method for producing paper according to any one of [1] to [3], wherein in the step of adding the mixture, the alkenyl succinic anhydride and the water-soluble aluminum compound are mixed to prepare a mixture, and the mixture is then added to the dispersion within 10 seconds. [5] A method for producing paper according to any one of [1] to [4], wherein in the step of adding a mixture of alkenyl succinic anhydride and a water-soluble aluminum compound to a dispersion containing pulp and water, or in the step of simultaneously adding alkenyl succinic anhydride and a water-soluble aluminum compound to a dispersion containing pulp and water, the amount of the water-soluble aluminum compound added is 0.2 to 38 times the amount of alkenyl succinic anhydride added. [6] The method for producing paper according to any one of [1] to [5], wherein the ash contains light calcium carbonate, and the content of the light calcium carbonate is 80 mass% or more based on the total mass of the ash. Effect of the Invention
[0010] According to the production method of the present invention, the sizing property of paper can be improved and contamination in the papermaking system during the paper production process can be reduced. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The present invention will be described in detail below. The following description of the constituent elements may be based on representative embodiments or specific examples, but the present invention is not limited to such embodiments. In this specification, a numerical range expressed using "~" means a range including the numerical values before and after "~" as the lower and upper limits.
[0012] (Paper manufacturing method) The present invention relates to a method for producing paper, comprising a step of obtaining a pulp slurry and a step of making paper from the pulp slurry. Here, the step of obtaining a pulp slurry in the present invention comprises a step of adding a mixture of an alkenyl succinic anhydride and a water-soluble aluminum compound to a dispersion containing pulp and water, or a step of simultaneously adding an alkenyl succinic anhydride and a water-soluble aluminum compound to a dispersion containing pulp and water. In the present invention, by adding a mixture of an alkenyl succinic anhydride and a water-soluble aluminum compound, or simultaneously adding an alkenyl succinic anhydride and a water-soluble aluminum compound in the step of obtaining a pulp slurry, the sizing property of the obtained paper can be improved, and furthermore, the occurrence of stains (machine stains, etc.) in the papermaking system can be suppressed.
[0013] In the process of obtaining a pulp slurry, the sizing property of paper can be improved by using alkenyl succinic anhydride as a sizing agent. Alkenyl succinic anhydride causes fouling in the papermaking process due to the aggregation of the hydrolyzate of alkenyl succinic anhydride. In particular, in the process of producing paper with a high ash content, when the amount of alkenyl succinic anhydride added is increased, the hydrolyzate of alkenyl succinic anhydride and the ash may aggregate, resulting in significant fouling. Thus, since the hydrolyzate of alkenyl succinic anhydride aggregates, it has been thought that sufficient stirring is required after the addition of alkenyl succinic anhydride alone.
[0014] However, the present inventors, in the course of intensively studying the method for producing paper, decided to add a mixture of alkenyl succinic anhydride and a water-soluble aluminum compound to a dispersion containing pulp and water, or to simultaneously add alkenyl succinic anhydride and a water-soluble aluminum compound to a dispersion containing pulp and water. Surprisingly, they found that by adding a mixture of alkenyl succinic anhydride and a water-soluble aluminum compound, or by simultaneously adding alkenyl succinic anhydride and a water-soluble aluminum compound to a dispersion containing pulp and water, it is possible to suppress the aggregation of the hydrolyzate of alkenyl succinic anhydride, and to suppress the occurrence of stains (machine stains, etc.) in the papermaking system. Thus, the present invention is able to achieve both improvement in the sizing property of paper and suppression of the occurrence of stains (machine stains, etc.) in the papermaking system when alkenyl succinic anhydride is used as a sizing agent.
[0015] In the step of obtaining the pulp slurry, the amount of alkenyl succinic anhydride added is preferably 0.01 parts by mass or more, more preferably 0.02 parts by mass or more, even more preferably 0.03 parts by mass or more, even more preferably 0.05 parts by mass or more, even more preferably 0.1 parts by mass or more, and particularly preferably 0.5 parts by mass or more, based on 100 parts by mass of the bone dry mass of the pulp in the pulp slurry. The amount of alkenyl succinic anhydride added is preferably 0.30 parts by mass or less, more preferably 0.25 parts by mass or less, even more preferably 0.24 parts by mass or less, and particularly preferably 0.22 parts by mass or less, based on 100 parts by mass of the bone dry mass of the pulp in the pulp slurry. The amount of alkenyl succinic anhydride added is the amount calculated based on the solid content of alkenyl succinic anhydride. By setting the amount of alkenyl succinic anhydride added within the above range, the sizing property of the paper can be improved more effectively and the stains in the papermaking system can be reduced more effectively.
[0016] In the step of adding a mixture of alkenyl succinic anhydride and a water-soluble aluminum compound to a dispersion containing pulp and water, or in the step of simultaneously adding alkenyl succinic anhydride and a water-soluble aluminum compound to a dispersion containing pulp and water, the amount of the water-soluble aluminum compound added is preferably 0.2 times or more, more preferably 0.25 times or more, even more preferably 0.3 times or more, and particularly preferably 0.5 times or more, relative to the amount of alkenyl succinic anhydride added. In addition, the amount of the water-soluble aluminum compound added is preferably 38 times or less, more preferably 20 times or less, even more preferably 10 times or less, and particularly preferably 5 times or less, relative to the amount of alkenyl succinic anhydride added. By setting the amount of the water-soluble aluminum compound and the amount of the alkenyl succinic anhydride added in the step of obtaining a pulp slurry under the above conditions, the sizing property of the paper can be improved more effectively and the staining in the papermaking system can be reduced more effectively.
[0017] The step of obtaining a pulp slurry includes a step of adding a mixture of an alkenyl succinic anhydride and a water-soluble aluminum compound to a dispersion containing pulp and water, or a step of simultaneously adding an alkenyl succinic anhydride and a water-soluble aluminum compound to a dispersion containing pulp and water. Among them, the step of obtaining a pulp slurry preferably includes a step of adding a mixture of an alkenyl succinic anhydride and a water-soluble aluminum compound that is previously mixed. That is, the step of obtaining a pulp slurry preferably includes a step of adding a mixture of an alkenyl succinic anhydride and a water-soluble aluminum compound to a dispersion containing pulp and water.
[0018] When the step of obtaining pulp slurry includes a step of adding a mixture of alkenyl succinic anhydride and a water-soluble aluminum compound to a dispersion containing pulp and water, it is preferable that after mixing the alkenyl succinic anhydride and the water-soluble aluminum compound, the mixture is added to the dispersion immediately.Specifically, it is preferable to add the mixture to the dispersion within 60 seconds, more preferably within 30 seconds, and even more preferably within 10 seconds after mixing the alkenyl succinic anhydride and the water-soluble aluminum compound to form a mixture.In this way, by adding the alkenyl succinic anhydride and the water-soluble aluminum compound to the dispersion containing pulp and water immediately after mixing, it is possible to more effectively reduce stains in the papermaking system.
[0019] The alkenyl succinic anhydride used in the step of obtaining the pulp slurry is preferably added as an emulsion. For example, it is preferable to mix the alkenyl succinic anhydride with cationic starch, and then to make an emulsion solution (emulsion liquid) through an emulsification step, and then to mix this emulsion solution with a water-soluble aluminum compound. By adding the alkenyl succinic anhydride as an emulsion solution (emulsion liquid), the dispersion stability of the alkenyl succinic anhydride can be more effectively improved.
[0020] In addition, before the step of adding a mixture of alkenyl succinic anhydride and a water-soluble aluminum compound to a dispersion containing pulp and water, or before the step of simultaneously adding alkenyl succinic anhydride and a water-soluble aluminum compound to a dispersion containing pulp and water, a step of further mixing a water-soluble aluminum compound may be provided. That is, the step of obtaining a pulp slurry may include a step of adding a mixture of alkenyl succinic anhydride and a water-soluble aluminum compound to a dispersion containing pulp, water, and a water-soluble aluminum compound, or a step of simultaneously adding alkenyl succinic anhydride and a water-soluble aluminum compound to a dispersion containing pulp and water. In addition, the dispersion containing pulp, water, and a water-soluble aluminum compound may further contain an optional component as described below.
[0021] In the emulsion solution of alkenyl succinic anhydride, the particle size of the alkenyl succinic anhydride emulsion particles is preferably 0.1 μm or more, more preferably 0.5 μm or more. The particle size of the alkenyl succinic anhydride emulsion particles is preferably 5 μm or less. The particle size of the alkenyl succinic anhydride emulsion particles is a value measured by observing with an optical microscope.
[0022] In the process of making paper from the pulp slurry (hereinafter also referred to as the papermaking process), any papermaking method such as an acidic papermaking method, a neutral papermaking method, or an alkaline papermaking method can be used. Among them, in the process of making paper from the pulp slurry, it is preferable to use a neutral papermaking method or an alkaline papermaking method. As the papermaking machine, a twin-wire papermaking machine, a gap former papermaking machine, a Fourdrinier papermaking machine, a cylinder papermaking machine, an on-top papermaking machine, a Yankee papermaking machine, or the like can be used. Among them, in the papermaking process, it is preferable to use a twin-wire papermaking machine or a gap former papermaking machine, and it is particularly preferable to use a gap former papermaking machine. The twin-wire papermaking machine and the gap former papermaking machine are papermaking machines of a type in which the raw material is sandwiched between two wires and traveled to dehydrate both above and below. Therefore, the raw material is dehydrated almost evenly on both sides, and the dehydration speed is increased. That is, the twin-wire type papermaking machine and the gap former type papermaking machine have the advantage that high-speed papermaking is possible and the difference in texture between the front and back of the obtained paper is small.
[0023] In the manufacturing process of the paper of the present invention, the surface of the paper may be subjected to a smoothing treatment in order to improve the surface strength of the paper or to increase the adhesiveness with the adhesive. Such smoothing treatment can be carried out, for example, by pressurizing the paper between reels capable of applying pressure. In addition, when performing the smoothing treatment, the roll that comes into contact with the surface of the paper is preferably a heatable metal roll having a smooth surface.
[0024] The smoothing treatment can also be carried out during the paper making process, for example, by calendaring with a calendar roll having one or more pairs of metal rolls (calendering with a machine calendar), calendaring with a calendar roll having one or more pairs of a metal roll and a resin roll (calendering with a soft calendar), or drying with a Yankee dryer, etc. By using such a manufacturing method, the smoothness of the paper surface is improved, enabling printing with higher accuracy.
[0025] (paper) The present invention may also relate to paper produced by the above-mentioned production method. The paper obtained by the production method of the present invention preferably has a sizing index calculated by the following formula of 5 or more, more preferably 10 or more, and even more preferably 20 or more. In addition, the sizing index is preferably 80 or less, more preferably 75 or less, and even more preferably 70 or less. Sizeability index = Stockigt sizing degree (sec) × 100 / basis weight (g / m 2 ) The Stockigt sizing degree of paper is a value measured in accordance with JIS P 8122.
[0026] The ash content of the paper is preferably 5% by mass or more, more preferably 10% by mass or more, even more preferably 16% by mass or more, even more preferably 22% by mass or more, and particularly preferably 24% by mass or more. The ash content of the paper is preferably 40% by mass or less, and more preferably 35% by mass or less. Thus, the paper obtained by the manufacturing method of the present invention may be high-ash paper. The ash content is a value measured by the ash content test method (525°C combustion method) described in JIS P 8251.
[0027] Here, the ash preferably contains light calcium carbonate. In this case, the content of light calcium carbonate is preferably 80% by mass or more, more preferably 85% by mass or more, and even more preferably 90% by mass or more, based on the total mass of the ash. By setting the content of light calcium carbonate within the above range, it becomes possible to inexpensively produce paper with excellent printability.
[0028] The basis weight of the paper is not particularly limited, but is preferably 20 g / m 2 It is preferable that the thickness is 25 g / m or more. 2 More preferably, the basis weight of the paper is 200 g / m or more. 2 It is preferable that the thickness is less than 170 g / m 2 More preferably, it is 150 g / m or less. 2 It is even more preferable that:
[0029] The thickness of the paper is not particularly limited, but is preferably 25 μm or more, more preferably 30 μm or more, and even more preferably 35 μm or more. The thickness of the paper is preferably 250 μm or less, more preferably 225 μm or less, and even more preferably 200 μm or less.
[0030] (Water-soluble aluminum compounds) In the process of obtaining pulp slurry, a water-soluble aluminum compound is added to a dispersion containing pulp and water together with alkenyl succinic anhydride. The water-soluble aluminum compound functions as a fixing agent for fixing paper strength agents, sizing agents, etc. in the paper. Examples of water-soluble aluminum compounds include polyaluminum chloride (PAC) and aluminum sulfate.
[0031] Among them, the water-soluble aluminum compound is preferably aluminum sulfate. In the step of adding a mixture of alkenyl succinic anhydride and a water-soluble aluminum compound to a dispersion containing pulp and water, or in the step of simultaneously adding alkenyl succinic anhydride and a water-soluble aluminum compound to a dispersion containing pulp and water, the amount of the water-soluble aluminum compound added is preferably 0.2 times or more, more preferably 0.25 times or more, and even more preferably 0.3 times or more, the amount of the alkenyl succinic anhydride added. In addition, the amount of the water-soluble aluminum compound added is preferably 38 times or less, more preferably 20 times or less, and even more preferably 10 times or less, the amount of the alkenyl succinic anhydride added. By setting the amount of the water-soluble aluminum compound and the amount of the alkenyl succinic anhydride added in the above steps under the above conditions, the sizing property of the paper can be more effectively improved and the staining in the papermaking system can be more effectively reduced.
[0032] In the step of obtaining a pulp slurry, the water-soluble aluminum compound may be added in several separate portions. For example, in the step of obtaining a pulp slurry, the water-soluble aluminum compound may be added in two separate portions. In this case, it is preferable to add the water-soluble aluminum compound before and after diluting the pulp slurry with white water. When the water-soluble aluminum compound is added in several separate portions, it is sufficient that the alkenyl succinic anhydride is added together with the water-soluble aluminum compound at any of the additions, and when the water-soluble aluminum compound is added in two separate portions, it is preferable that the alkenyl succinic anhydride is added together with the water-soluble aluminum compound at the second addition.
[0033] In the step of obtaining a pulp slurry, a pulp slurry containing an alkenyl succinic anhydride and a water-soluble aluminum compound is obtained. The content of the water-soluble aluminum compound is preferably 0.1 to 3 parts by mass per 100 parts by mass of the bone dry mass of the pulp in the pulp slurry.
[0034] (Inorganic filler) The paper of the present invention contains an inorganic filler. The content of the inorganic filler is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, even more preferably 16 parts by mass or more, even more preferably 22 parts by mass or more, and particularly preferably 24 parts by mass or more, based on 100 parts by mass of the bone dry mass of the pulp. The content of the inorganic filler is preferably 40 parts by mass or less, more preferably 35 parts by mass or less, based on 100 parts by mass of the bone dry mass of the pulp. The inorganic filler also contains light calcium carbonate, and the content of the light calcium carbonate is preferably 80% by mass or more, more preferably 85% by mass or more, and even more preferably 90% by mass or more, based on the total mass of the ash. By setting the content of the light calcium carbonate within the upper range, it becomes possible to inexpensively produce paper with excellent printability.
[0035] The inorganic filler may contain talc. Talc is composed mainly of hydrated magnesium silicate (3MgO·4SiO2·H2O). The inorganic filler may contain fillers other than talc. Examples of inorganic fillers other than talc include inorganic pigments such as heavy calcium carbonate, calcium sulfite, gypsum, kaolin, delaminated kaolin, hydrated silicate, diatomaceous earth, magnesium carbonate, barium carbonate, zinc oxide, titanium dioxide, aluminum hydroxide, calcium hydroxide, magnesium hydroxide, and zinc hydroxide, and organic pigments such as urea-formaldehyde resin fine particles and hollow fine particles. In addition, when waste paper, broke paper, and the like are used as pulp raw materials, fillers contained therein can also be contained. Note that two or more types of inorganic fillers may be mixed and used.
[0036] (Pulp raw material) In the step of obtaining a pulp slurry, first, a dispersion liquid containing pulp and water is obtained. Pulps that can be used in the present invention include, for example, pulp derived from hardwood, pulp derived from softwood, and pulp derived from non-wood. Hardwood kraft pulp includes, for example, unbleached hardwood kraft pulp (LUKP), bleached hardwood kraft pulp (LBKP), semi-bleached hardwood kraft pulp (LSBKP), and sulfite hardwood pulp. Softwood kraft pulp includes, for example, unbleached softwood kraft pulp (NUKP), bleached softwood kraft pulp (NBKP), semi-bleached softwood kraft pulp (NSBKP), and sulfite softwood pulp.
[0037] In addition, the pulp contained in the paper of the present invention preferably contains acacia-derived hardwood pulp. The content of acacia-derived hardwood pulp is preferably 30% by mass or more based on the total mass of the raw materials for the pulp. The content of acacia-derived hardwood pulp may be 30-100% by mass based on the total mass of the raw materials for the pulp, preferably 50-100% by mass, and more preferably 70-100% by mass. By setting the content of acacia-derived pulp within the above range, paper with a small static friction coefficient can be produced. Furthermore, by setting the content of acacia-derived hardwood pulp within the above range, the drying time of the paper in the production process can be shortened.
[0038] Examples of acacia-derived pulp that can be used include pulp obtained from Acacia mangium, A. auriculiformis, A. catechu, A. decurrens, A. holosericea, A. leptocarpa, A. maidenii, A. mearnsii, A. melanoxylon, A. neriifolia, A. silvestris, A. peregrinalis, and hybrids thereof.
[0039] In the present invention, in addition to softwood kraft pulp and hardwood kraft pulp, various known pulps can be used, such as mechanical pulps such as stone ground pulp (SGP), pressed stone ground pulp (PGW), refiner ground pulp (RGP), thermo ground pulp (TGP), chemi-ground pulp (CGP), groundwood pulp (GP) and thermo mechanical pulp (TMP); disintegrated waste paper pulp, disintegrated and deinked waste paper pulp, or disintegrated, deinked and bleached waste paper pulp produced from brown paper, kraft envelope paper, magazine paper, newspaper paper, flyer paper, office paper, corrugated cardboard, white paper, Kent paper, imitation waste paper, and land certificate paper; and pulp produced chemically or mechanically from non-wood fibers such as kenaf, hemp, and reed. The content of recycled paper pulp relative to the total mass of the paper is preferably less than 30% by mass, more preferably less than 20% by mass, and even more preferably less than 10% by mass.
[0040] The freeness of the pulp raw material used in the present invention is preferably 350 to 650 ml CSF. Before the step of obtaining the pulp slurry, a beating step may be performed as necessary to obtain the above freeness. The freeness is the freeness value measured by a Canadian standard freeness tester in accordance with JIS-P8121 after a sample is disintegrated in a standard disintegrator in accordance with JIS-P8220.
[0041] (optional ingredient) In the present invention, internal additives other than the inorganic fillers described above may be added. Examples of internal additives include various known agents such as paper strength agents such as polyacrylamide and starch, freeness retention improvers such as polyamides, water resistance agents such as polyamides, polyamines and epichlorohydrin, antifoaming agents, basic dyes, acid dyes, anionic direct dyes and cationic direct dyes.
[0042] Furthermore, in the present invention, the raw pulp may contain cationic starch. The content of cationic starch is preferably 0.1 to 15 parts by mass, more preferably 0.1 to 10 parts by mass, relative to 100 parts by mass of the bone dry mass of the raw pulp. The content of cationic starch is the content of cationic starch converted into solid content. By adding cationic starch, the strength of the paper is increased, and paper with good breaking elongation can be obtained. EXAMPLES
[0043] The features of the present invention will be described in more detail below with reference to examples and comparative examples. The materials, amounts used, ratios, processing contents, processing procedures, etc. shown in the following examples can be appropriately changed without departing from the spirit of the present invention. Therefore, the scope of the present invention should not be interpreted as being limited by the specific examples shown below.
[0044] <Method of emulsifying alkenyl succinic anhydride (ASA)> A 100% by mass solution of alkenyl succinic anhydride (Fibran, manufactured by Arakawa Chemical Industry Co., Ltd.) was mixed with a 3% by mass solution of cationic starch (P-3Y, manufactured by Pillar Starch Co., Ltd.), and emulsified for 5 minutes at 5000 rpm using a homogenizer (manufactured by Nippon Seiki Seisakusho Co., Ltd.), to obtain an emulsion of alkenyl succinic anhydride with an alkenyl succinic anhydride component of 1% by mass and an alkenyl succinic anhydride emulsion particle diameter of 2 μm. The particle diameter of the alkenyl succinic anhydride emulsion particle was observed and measured using an optical microscope.
[0045] <Example 1> As the raw pulp, 400 mL of hardwood bleached kraft pulp (LBKP) was used. The pulp slurry was obtained by diluting with water to a pulp concentration of 3% by mass. Aluminium sulfate (solid weight equivalent) of 0.4 parts and cationic starch (P-3Y, manufactured by Pillar Starch Co., Ltd.) (solid weight equivalent) of 1.2 parts were added to 100 parts by mass of bone dry pulp in the pulp slurry to obtain a pre-dilution pulp slurry. The pulp slurry was then diluted with white water to a pulp concentration of 0.5% by mass to obtain a pulp slurry. The emulsion of alkenyl succinic anhydride obtained above was separated into a container and stirred with a simple magnetic stirrer. Aluminium sulfate solution (3% by mass of aluminum sulfate component) was added thereto so that the mass ratio of aluminum sulfate component to alkenyl succinic anhydride was 10:7, and after stirring for 5 seconds, the mixture was immediately added to the diluted pulp slurry using a pipette. In the step of adding the mixture, the mixture of alkenyl succinic anhydride and aluminum sulfate was added so that the aluminum sulfate (solid content equivalent) was 0.2 parts by mass and the alkenyl succinic anhydride (solid content equivalent) was 0.14 parts by mass per 100 parts by mass of bone dry pulp. The mixture was added 10 seconds after dilution with white water. Next, 27 parts by mass of light calcium carbonate (Tamapearl TP-121, manufactured by Okutama Kogyo Co., Ltd.) and 200 ppm of cationic retention agent (ND-300, manufactured by Hymo Co., Ltd.) were added to this pulp slurry per 100 parts by mass of bone dry pulp, and paper was made using a square sheet machine according to a standard method to produce a paper with a basis weight of 60 g / m. 2As a result, handmade paper of
[0046] <Example 2> Handsheets were obtained in the same manner as in Example 1, except that when preparing a mixed solution of alkenyl succinic anhydride and aluminum sulfate, aluminum sulfate was added so that the mass ratio of aluminum sulfate component to alkenyl succinic anhydride was 5:14, and in the step of adding the mixture, the mixed solution of alkenyl succinic anhydride and aluminum sulfate was added in amounts of 0.05 part by mass of aluminum sulfate (solid matter equivalent) and 0.14 part by mass of alkenyl succinic anhydride (solid matter equivalent) per 100 parts by mass of bone dry pulp.
[0047] <Example 3> Handsheets were obtained in the same manner as in Example 1, except that when preparing a mixed solution of alkenyl succinic anhydride and aluminum sulfate, aluminum sulfate was added so that the mass ratio of the aluminum sulfate component to alkenyl succinic anhydride was 100:14, and in the step of adding the mixture, the mixed solution of alkenyl succinic anhydride and aluminum sulfate was added so that the amount of aluminum sulfate (solid matter equivalent) was 1.0 part by mass and the amount of alkenyl succinic anhydride (solid matter equivalent) was 0.14 part by mass per 100 parts by mass of bone dry pulp.
[0048] <Example 4> Handsheet paper was obtained in the same manner as in Example 1, except that a mixed solution of an emulsion of alkenyl succinic anhydride and aluminum sulfate was not prepared in Example 1, and an emulsion of alkenyl succinic anhydride and aluminum sulfate solution similar to those in Example 1 were added simultaneously to the diluted pulp slurry. In the simultaneous addition step, each solution was added so that aluminum sulfate (solids equivalent) was 0.2 parts by mass and alkenyl succinic anhydride (solids equivalent) was 0.14 parts by mass per 100 parts by mass of bone dry pulp. The emulsion of alkenyl succinic anhydride and aluminum sulfate solution were added simultaneously 10 seconds after dilution with white water.
[0049] <Example 5> A handsheet was obtained in the same manner as in Example 1, except that the mixing time of the emulsion of alkenyl succinic anhydride and aluminum sulfate was changed to 10 seconds when preparing the mixed solution of the emulsion of alkenyl succinic anhydride and aluminum sulfate.
[0050] <Example 6> Handsheets were obtained in the same manner as in Example 1, except that the amount of precipitated calcium carbonate added was changed to 30 parts by mass per 100 parts by mass of bone dry mass of pulp.
[0051] <Example 7> Handsheets were obtained in the same manner as in Example 1, except that when preparing a mixed solution of alkenyl succinic anhydride and aluminum sulfate, aluminum sulfate was added so that the ratio of aluminum sulfate component to alkenyl succinic anhydride was 1:1, and in the step of adding the mixture, the mixed solution of alkenyl succinic anhydride and aluminum sulfate was added so that aluminum sulfate component (solid matter equivalent) was 0.2 part by mass and alkenyl succinic anhydride (solid matter equivalent) was 0.2 part by mass per 100 parts by mass of bone dry pulp.
[0052] <Example 8> Handsheets were obtained in the same manner as in Example 1, except that when preparing a mixed solution of alkenyl succinic anhydride and aluminum sulfate, aluminum sulfate was added so that the ratio of aluminum sulfate component to alkenyl succinic anhydride was 500:14, and in the step of adding the mixture, the mixed solution of alkenyl succinic anhydride and aluminum sulfate was added in such amounts that aluminum sulfate component (solid matter equivalent) was 5.0 parts by mass and alkenyl succinic anhydride (solid matter equivalent) was 0.14 parts by mass per 100 parts by mass of bone dry pulp.
[0053] <Example 9> A handsheet was obtained in the same manner as in Example 1, except that the mixing time of the emulsion of alkenyl succinic anhydride and aluminum sulfate was 60 seconds when preparing the mixed solution of the emulsion of alkenyl succinic anhydride and aluminum sulfate.
[0054] <Example 10> Handsheets were obtained in the same manner as in Example 1, except that the amount of precipitated calcium carbonate added was changed to 40 parts by mass per 100 parts by mass of bone dry mass of pulp.
[0055] <Example 11> Handsheets were obtained in the same manner as in Example 1, except that the amount of precipitated calcium carbonate added was changed to 16 parts by mass per 100 parts by mass of bone dry mass of pulp.
[0056] <Example 12> Handsheets were obtained in the same manner as in Example 1, except that the amount of precipitated calcium carbonate added was changed to 7 parts by mass per 100 parts by mass of bone dry mass of pulp.
[0057] <Comparative Example 1> In Example 1, the amount of aluminum sulfate added to the 3% by mass pulp slurry was changed to 0.6 parts by mass per 100 parts by mass of the bone dry mass of pulp in the pulp slurry. The pulp slurry was then diluted with white water in the same manner as in Example 1 to obtain a pulp slurry. Then, to the diluted pulp slurry, only alkenyl succinic anhydride was added in an amount of 0.14 parts by mass per 100 parts by mass of the bone dry mass of pulp. Otherwise, handsheet paper was obtained in the same manner as in Example 1.
[0058] <Comparative Example 2> Handsheet paper was obtained in the same manner as in Example 7, except that rosin (Sizepine N-788, manufactured by Arakawa Chemical Industries, Ltd.) was used instead of alkenyl succinic anhydride.
[0059] <Comparative Example 3> Handsheets were obtained in the same manner as in Comparative Example 2, except that the rosin content in the pulp slurry was changed to 0.3 parts by mass per 100 parts by mass of the bone dry mass of the pulp.
[0060] (evaluation) <Measurement of ash content in paper> The ash content in the paper was measured in accordance with JIS P 8251.
[0061] <Proportion of light calcium carbonate in paper ash> After ashing the paper in accordance with JIS P 8251, the particle size distribution of the ash was measured using Microtrac (MT3000II, manufactured by Microtrac Bell Co., Ltd.). The proportion of light calcium carbonate was calculated with particles having a particle size of 1 to 10 μm being light calcium carbonate and those having a particle size of 11 to 16 μm being talc.
[0062] <Measurement Method of Size Index> The sizing degree was measured, and the size index was calculated by the following formula in accordance with JIS P 8122. Size Index = Sizing Time (seconds) × 100 / Basis Weight (g / m 2 )
[0063] <Soil Evaluation of ASA> After hand-sheeting using a square sheet machine, a metal plate was placed on the wet paper and pressed at 4.2 kgf for 2 minutes. The metal plate was peeled off, and the amount of soil adhesion to the metal plate was visually evaluated in four grades. ◎: Very little 〇: Slightly less △: Slightly more ×: Very much
[0064]
Table 1
[0065]
Table 2
[0066]
Table 3
[0067] In the examples, improvement in sizing degree and reduction of machine soil were achieved simultaneously.
Claims
1. A method for producing paper, comprising the steps of obtaining a pulp slurry and making paper from the pulp slurry, The step of obtaining the pulp slurry includes a step of further diluting a dispersion containing pulp and water with white water, and a step of adding a mixture of an alkenyl succinic anhydride and a water-soluble aluminum compound to the dispersion obtained in the step of diluting with white water, The method for producing paper, wherein in the step of adding the mixture, the alkenyl succinic anhydride and the water-soluble aluminum compound are mixed to form a mixture, and the mixture is added to the dispersion within 10 seconds.
2. The method for producing paper according to claim 1 , wherein the step of obtaining the pulp slurry further comprises the step of adding a water-soluble aluminum compound before the step of diluting with white water.
3. The method for producing paper according to claim 1 or 2, wherein the water-soluble aluminum compound is aluminum sulfate.
4. The method for producing paper according to any one of claims 1 to 3, wherein the amount of the alkenyl succinic anhydride added is 0.01 to 0.30 parts by mass per 100 parts by mass of the bone dry mass of the pulp in the pulp slurry.
5. 5. The method for producing paper according to claim 1, wherein in the step of adding a mixture of alkenyl succinic anhydride and a water-soluble aluminum compound to the dispersion obtained in the step of diluting with white water, the amount of the water-soluble aluminum compound added is 0.2 to 38 times the amount of the alkenyl succinic anhydride added.
6. A method for producing paper described in any one of claims 1 to 5, wherein the ash contained in the paper includes light calcium carbonate, and the content of the light calcium carbonate is 80 mass% or more relative to the total mass of the ash.
Citation Information
Patent Citations
Paper having excellent opacity
JP2002069896A
Method for producing paperboard
JP2007154349A
Method for producing paper
JP2014088644A
Manufacturing method of paper and paper
JP2017008463A