Paper-based facing material with mildew-proof function and preparation method thereof

By using surfactants, isothiazolinone anti-mold agents and zinc oxide-loaded calcium carbonate fillers in the preparation process of paper-based finish materials, the problem of insufficient anti-mold performance of paper-based finish materials is solved, and significant results are achieved The antibacterial and mildew-proof effect and material stability are improved.

CN118880665AInactive Publication Date: 2024-11-01ZHEJIANG GRANDRICH PAPER

Patent Information

Application Number
CN202411137894.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing paper-based finishing materials have insufficient anti-mold properties, making it difficult to effectively prevent mold growth and bacterial growth, affecting their service life and aesthetic effect.

Method used

The paper-based finishing materials are prepared by pulping, surfactant, isothiazolinone anti-mold agent, zinc oxide-loaded calcium carbonate filler and wood pulp. , utilize the antibacterial and anti-mold effects of isothiazolinone and zinc oxide to improve the anti-bacterial and anti-mold properties of the material.

Benefits of technology

It significantly improves the antibacterial and mildew-proof properties of paper-based finish materials, extends its service life, avoids the growth of mold and bacteria, keeps the material dry and tidy, and enhances its stability in humid environments.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a paper-based facing material with a mildew-proof function and a preparation method thereof.The preparation method comprises the steps that S100, raw materials including a surfactant, an isothiazolinone mildew preventive, a porous calcium carbonate filler and wood pulp are mixed for pulping, and pulp is obtained; s200, the pulp is put on a net for papermaking, squeezing and drying are conducted, and base paper is obtained; s300, a sizing agent is adopted for teaching raw paper, drying and calendaring are conducted, and the paper-based facing material is obtained; wherein zinc oxide is loaded in the porous calcium carbonate filler. According to the invention, the paper-based facing material with a good mildew-proof effect can be obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of papermaking, and in particular to a paper-based finishing material with mildew-proof function and a preparation method thereof. Background Art

[0002] Paper-based finishing materials are a type of industrial specialty paper processed through a special process. They are also an indispensable raw material in many building materials products, such as low-pressure boards and high-pressure boards used in furniture and cabinets, as well as fireproof boards, floors, wallpapers, etc., which all require paper-based finishing materials to enhance the aesthetics of the products.

[0003] Paper-based decorative materials are usually manufactured through pulping, papermaking, pressing and other processes. Anti-mildew performance is one of the important properties to measure the quality of paper-based decorative materials. How to improve the anti-mildew effect of paper-based decorative materials is a technical problem that technicians in this field are currently committed to solving. Summary of the invention

[0004] One of the problems solved by the present invention is how to provide a paper-based facing material with good mildew-proof effect.

[0005] In order to solve at least one of the above problems, the present invention provides a method for preparing a paper-based facing material with anti-mildew function, the preparation method comprising:

[0006] S100, mixing and pulping raw materials including a surfactant, an isothiazolinone mildew inhibitor, a calcium carbonate filler and wood pulp to obtain a pulp;

[0007] S200, placing the pulp on the screen for papermaking, pressing, and drying to obtain base paper;

[0008] S300, applying sizing agent to base paper, drying and calendering to obtain paper-based finishing material;

[0009] The porous calcium carbonate filler is loaded with zinc oxide.

[0010] In any of the above technical solutions, the surfactant includes at least one of the following or a combination thereof: sodium dodecylbenzene sulfonate, sodium tetrapropylenebenzene sulfonate, sodium fatty alcohol sulfate, xylene sulfonic acid, and condensed sodium naphthalene sulfonate.

[0011] In any of the above technical solutions, the calcium carbonate filler is prepared by the following steps:

[0012] S111, mixing zinc chloride, calcium chloride, and heavy calcium carbonate in water and stirring to obtain a first mixture;

[0013] S112, mixing sodium dodecylbenzene sulfonate and sodium carbonate in water and stirring to obtain a second mixture;

[0014] S113, mixing polyacrylic acid in water and stirring to obtain a third mixture;

[0015] S114, mixing the first mixture, the second mixture and the third mixture to react and obtain calcium carbonate.

[0016] In any of the above technical solutions, in S111, the mass ratio of zinc chloride: calcium chloride: heavy calcium carbonate: water is (2-4): (6-8): (14-16): 100.

[0017] In any of the above technical solutions, in S112, the mass ratio of sodium dodecylbenzenesulfonate:sodium carbonate:water=(0.5-1):(4-10):100.

[0018] In any of the above technical solutions, in S113, the mass ratio of polyacrylic acid: water is (6-10):100.

[0019] In any of the above technical solutions, S114 specifically includes:

[0020] The second mixture is added dropwise into the first mixture with simultaneous stirring. After the addition is completed, the mixture is allowed to stand for 15 to 30 minutes. The third mixture is then added dropwise with simultaneous stirring. After the addition is completed, the temperature is raised to 85 to 90° C. and kept warm for 2 to 2.5 hours. The solids are filtered, washed, dried, and heat treated at 300 to 350° C. for 10 to 60 minutes to obtain calcium carbonate.

[0021] In any of the above technical solutions, in S114, the mass ratio is: first mixture: second mixture: third mixture = 100: (80-120): (20-30).

[0022] In any of the above technical solutions, the wood pulp includes bleached coniferous wood pulp and bleached broadleaf wood pulp in a mass ratio of (0.25-0.5):1.

[0023] The present invention also provides a paper-based decorative material with anti-mildew function. The paper-based decorative material with anti-mildew function is obtained by using the preparation method of any of the above technical solutions.

[0024] Beneficial Effects

[0025] The present invention provides a method for preparing a paper-based decorative material with a mildew-proof function. The method firstly uses raw materials including a surfactant, an isothiazolinone mildew-proof agent, a calcium carbonate filler and wood pulp to mix and pulp to obtain a slurry; then the slurry is put on a net for papermaking, pressing and drying to obtain a base paper; finally, a sizing agent is used to sizing the base paper, drying and calendering to obtain a paper-based decorative material. In the slurry prepared by the present invention, an isothiazolinone mildew-proof agent is added.

[0026] Isothiazolinone is mainly composed of two components: 5-chloro-2-methyl-4-isothiazolin-3-one (CIT) and 2-methyl-4-isothiazolin-3-one (MIT). The above two components play a bactericidal role in isothiazolinone. The bactericidal principle of isothiazolinone is to kill by breaking the bonds between bacteria and algae proteins. After contacting with microorganisms, it can quickly and irreversibly inhibit their growth, thereby causing the death of microbial cells. Isothiazolinone fungicides are a heterocyclic structure, and their bactericidal principle mainly relies on the active part on the heterocyclic ring to destroy the DNA molecules in the bacterial cells, making the bacteria inactive.

[0027] The invention adds isothiazolinone mildewproof agent into the slurry, and utilizes the characteristics of isothiazolinone, such as strong stability, low use cost, easy degradation, no residue and good sterilization effect, to give the paper-based facing material better antibacterial and mildewproof performance.

[0028] On this basis, the present invention further adds zinc oxide as an inorganic mildew preventer to the slurry. Zinc oxide not only has good antibacterial and mildew preventive effects, but also as an inorganic material, it has better chemical stability and thermal stability, and can exert antibacterial and mildew preventive effects for a longer period of time.

[0029] In addition, compared with the solution of directly adding zinc oxide to the slurry, the present invention chooses to load zinc oxide on calcium carbonate to achieve antibacterial and mildew-proof effects with calcium carbonate filler containing zinc oxide. The advantage is that it can prevent the agglomeration of nano-scale zinc oxide with smaller particle size in the slurry, ensuring that a smaller amount of zinc oxide can exert a better and more efficient antibacterial and mildew-proof effect. DETAILED DESCRIPTION

[0030] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the following is a detailed description of the specific embodiments of the present invention.

[0031] Unless otherwise specified, the reagents and raw materials used in the present invention can be purchased through commercial channels. The experimental methods in the following examples without specifying specific conditions are selected according to conventional methods and conditions, or according to the product specifications.

[0032] Paper-based finishing materials can be used in a variety of application scenarios such as furniture veneer and wallpaper. Anti-mildew performance is one of the important properties to measure the quality of paper-based finishing materials. For example, wallpaper is prone to deformation, mildew, and bacteria after being exposed to moisture. Therefore, how to improve the antibacterial and anti-mildew performance of paper-based finishing materials has always been a technical problem that technicians in this field have been committed to solving.

[0033] In order to solve the above problems, an embodiment of the present invention provides a method for preparing a paper-based facing material with anti-mildew function, the preparation method comprising:

[0034] S100, mixing and pulping raw materials including a surfactant, an isothiazolinone mildew inhibitor, a calcium carbonate filler and wood pulp to obtain a pulp;

[0035] S200, placing the pulp on the screen for papermaking, pressing, and drying to obtain base paper;

[0036] S300, applying sizing agent to base paper, drying and calendering to obtain paper-based finishing material;

[0037] The porous calcium carbonate filler is loaded with zinc oxide.

[0038] The technical solution of the present invention is suitable for preparing interior decoration paper such as furniture veneer, wallpaper, etc. Among them, the isothiazolinone mildewproof agent and zinc oxide give the paper-based finishing material antibacterial and mildewproof properties.

[0039] In the above steps, the surfactant includes at least one of the following or a combination thereof: sodium dodecylbenzene sulfonate, sodium tetrapropylenebenzene sulfonate, sodium fatty alcohol sulfate, xylene sulfonic acid, and condensed sodium naphthalene sulfonate.

[0040] Preferably, the wood pulp used in S100 includes bleached coniferous wood pulp and bleached broadleaf wood pulp in a mass ratio of (0.25-0.5):1.

[0041] The paper-based facing material of the present invention is mainly manufactured by pulping, papermaking, pressing and other processes. Those skilled in the art can select and adjust the equipment, raw materials and process parameters used in pulping, papermaking and pressing according to actual needs.

[0042] Pulping is a key process in the papermaking industry, which separates the fibers from the plant fiber raw materials to obtain paper pulp. The pulping step of the present invention can be carried out by mechanical method, chemical method or chemical mechanical method. The papermaking step uses a bamboo curtain type mesh trough specially used for papermaking to scoop a certain amount of paper pulp, and then swings the mesh trough back and forth or left and right to arrange the pulp fibers in a certain direction to form a paper layer of uniform thickness, i.e., wet paper sheet. The pressing process squeezes the wet paper through a press, which removes excess water from the paper layer and increases the dryness of the paper. The pressure and speed in the pressing process can be selected and adjusted by those skilled in the art according to actual needs.

[0043] It can be understood that the process of using pulp to make paper on the net, press and dry to obtain base paper is a relatively mature existing technology. The selection of specific process parameters for making paper on the net, press and dry has no substantial impact on the realization of the purpose of the present invention.

[0044] Preferably, the beating degree of the wood pulp used in S100 is 30°SR to 45°SR.

[0045] Preferably, in S100, the mass ratio of surfactant: isothiazolinone mildew inhibitor: calcium carbonate filler: wood pulp is (1-2): (2-4): (10-15): 100.

[0046] Further, preferably, in S100, the mass ratio of surfactant:isothiazolinone mildew inhibitor:calcium carbonate filler:wood pulp=1.5:3:12:100.

[0047] One of the improvements made by the present invention over the prior art is to load zinc oxide on calcium carbonate, so as to achieve antibacterial and mildew-proof effects with the calcium carbonate filler containing zinc oxide. The advantage is that it can prevent the agglomeration of nano-scale zinc oxide with a smaller particle size in the slurry, ensuring that a better and more efficient antibacterial and mildew-proof effect is achieved with a smaller amount of zinc oxide. Specifically, the calcium carbonate filler used in the present invention is prepared by the following steps:

[0048] S111, mixing zinc chloride, calcium chloride, and heavy calcium carbonate in water and stirring to obtain a first mixture;

[0049] S112, mixing sodium dodecylbenzene sulfonate and sodium carbonate in water and stirring to obtain a second mixture;

[0050] S113, mixing polyacrylic acid in water and stirring to obtain a third mixture;

[0051] S114, mixing the first mixture, the second mixture and the third mixture to react and obtain calcium carbonate.

[0052] Preferably, in S111, the mass ratio of zinc chloride:calcium chloride:heavy calcium carbonate:water is (2-4):(6-8):(14-16):100.

[0053] Preferably, in S112, the mass ratio of sodium dodecylbenzenesulfonate:sodium carbonate:water=(0.5-1):(4-10):100.

[0054] Preferably, in S113, the mass ratio of polyacrylic acid to water is (6-10):100.

[0055] More preferably, in S111, the mass ratio of zinc chloride:calcium chloride:heavy calcium carbonate:water is 3:6:15:100.

[0056] More preferably, in S112, the mass ratio of sodium dodecylbenzenesulfonate:sodium carbonate:water=1:8:100.

[0057] More preferably, in S113, the mass ratio of polyacrylic acid to water is 8:100.

[0058] It should be noted that S114 specifically includes: adding the second mixture dropwise into the first mixture and stirring simultaneously, letting it stand for 15 to 30 minutes after the addition is completed, then adding the third mixture dropwise and stirring simultaneously, heating to 85°C to 90°C after the addition is completed, keeping warm for 2 to 2.5 hours, filtering the solids, washing, drying, and heat treating at a temperature of 300°C to 350°C for 10 to 60 minutes to obtain calcium carbonate.

[0059] Preferably, in S114, the mass ratio is: the first mixture: the second mixture: the third mixture = 100: (80-120): (20-30).

[0060] More preferably, in S114, the mass ratio of the first mixture: the second mixture: the third mixture=100:80:20.

[0061] The reasons for using the above steps to prepare calcium carbonate are as follows. Calcium carbonate is divided into heavy calcium carbonate and light calcium carbonate. Among them, heavy calcium carbonate is usually obtained by grinding natural marble, calcite, limestone, etc., while light calcium carbonate is prepared by chemical processing. Heavy calcium carbonate is simple to produce, has low energy consumption, and is low in cost. Light calcium carbonate has the advantages of large specific surface area and rich pore structure, but its cost is relatively high. In order to reduce production costs, the present invention uses heavy calcium carbonate as the core material, and coats the surface of the heavy calcium carbonate with a light calcium carbonate shell through a double decomposition reaction. Taking advantage of the rich pore structure of light calcium carbonate, the calcium carbonate filler can load more zinc oxide on the basis of controlling costs. In addition, zinc oxide is less likely to agglomerate in a loose and porous structure.

[0062] To achieve the above object, the present invention first mixes zinc chloride, calcium chloride and heavy calcium carbonate in water to obtain a first mixture. Then, sodium dodecylbenzene sulfonate and sodium carbonate as surfactants are mixed and stirred in water to obtain a second mixture. By dropping the second mixture into the first mixture and stirring simultaneously, and standing after the dropwise addition, the double decomposition reaction between zinc chloride and calcium chloride and sodium carbonate can be used to deposit a mixed coating layer of calcium carbonate and zinc carbonate on the surface of heavy calcium carbonate. The third mixture is a mixture of polyacrylic acid and water. By further dropping the third mixture and stirring simultaneously, and heating and keeping warm after the dropwise addition, the surface of calcium carbonate can be modified by polyacrylic acid to reduce the surface energy of calcium carbonate and promote its dispersion in pulp.

[0063] Optionally, the average molecular weight of the polyacrylic acid used in the present invention is 200000 to 250000. At the end of the above process, the present invention oxidizes the zinc carbonate into zinc oxide by heat treatment at a temperature of 300°C to 350°C. Preferably, the present invention performs a low-temperature and long-term heat treatment at a temperature of 300°C to 310°C for 40min to 60min to ensure that the zinc carbonate is oxidized into zinc oxide and protect the polyacrylic acid from being damaged by heat.

[0064] Regarding S300, the purpose of sizing is to enhance the anti-permeability of the paper-based finishing material so that the paper-based finishing material can better resist the penetration of liquids such as water and grease, thereby keeping it dry and tidy. In addition, the sizing agent can form a protective film on the surface of the paper-based finishing material, which helps to prevent it from tearing and wrinkling, thereby improving the strength and stability of the paper. The present invention selects the method of surface sizing for sizing, that is: spraying a thin layer of sizing agent on the surface of the paper-based finishing material to form a protective film on the surface of the base paper. The surface sizing process of the present invention is carried out on a papermaking machine. The present invention can use starch, animal glue, synthetic glue and other materials as sizing agents. The amount of sizing agent can be selected and adjusted by those skilled in the art. Preferably, the sizing agent of the present invention is prepared by the following steps:

[0065] S121, enzymatically hydrolyzing starch using α-amylase to obtain enzymatically hydrolyzed starch;

[0066] S122, mixing the defoaming agent, aluminum sulfate, styrene-acrylate copolymer and enzymatic starch, and adding water to prepare a sizing agent with a solid content of 28% to 32% and a pH value of 4.5 to 5.

[0067] Specifically, in S121, the starch is cereal starch or rhizome starch, and the amount of α-amylase used is 200ppm to 400ppm based on the amount of starch added; the enzymatic treatment method is: the α-amylase and starch are mixed and sent into a reactor, 2 to 2.5 times the mass of starch is added with water, and the mixture is reacted for 20 to 30 minutes at a temperature of 75°C to 85°C and a pressure of 40000Pa to 55000Pa, and the solids are extracted and dried at a temperature of 120°C to 130°C.

[0068] Preferably, in S122, the mass ratio of defoaming agent:aluminum sulfate:styrene-acrylate copolymer:enzymatic starch is (0.5-1):(0.5-1):(40-60):100.

[0069] More preferably, in S122, the mass ratio of defoaming agent: aluminum sulfate: styrene-acrylate copolymer: enzymatic starch is 0.5:1:40:100.

[0070] Example 1

[0071] This embodiment provides a paper-based facing material with mildew-proof function, which is prepared by the following steps:

[0072] S1. According to the mass ratio of zinc chloride: calcium chloride: heavy calcium carbonate: water = 3:6:15:100, zinc chloride, calcium chloride and heavy calcium carbonate are mixed and stirred in water to obtain a first mixture;

[0073] S2, mixing sodium dodecylbenzene sulfonate and sodium carbonate in water in a mass ratio of sodium dodecylbenzene sulfonate: sodium carbonate: water = 1:8:100, to obtain a second mixture;

[0074] S3, mixing polyacrylic acid in water at a mass ratio of polyacrylic acid: water = 8:100, to obtain a third mixture;

[0075] S4, adding the second mixture dropwise into the first mixture in a mass ratio of the first mixture: the second mixture: the third mixture = 100:80:20 and stirring simultaneously, standing for 20 minutes after the addition is complete, then adding the third mixture dropwise and stirring simultaneously, heating to 85° C. after the addition is complete, keeping the temperature for 2 hours, filtering the solids, washing once with water, washing once with ethanol, drying, and heat-treating at 310° C. for 40 minutes to obtain a calcium carbonate filler;

[0076] S5, mixing α-amylase and starch into a reactor, adding water twice the mass of starch, reacting for 20 min at a temperature of 80° C. to 85° C. and a pressure of 45000 Pa to 55000 Pa, extracting the solids and drying them at a temperature of 125±3° C., and deactivating the enzyme; wherein the amount of α-amylase used is 200 ppm based on the amount of starch added;

[0077] S6, according to the mass ratio of polyether defoamer: aluminum sulfate: styrene-acrylate copolymer: enzymatic starch = 0.5:1:40:100, the polyether defoamer, aluminum sulfate, styrene-acrylate copolymer and enzymatic starch are mixed, and water is added to prepare a sizing agent with a solid content of 30% and a pH value of 4.5 to 5;

[0078] S7, mixing raw materials including sodium dodecylbenzene sulfonate, isothiazolinone mildew inhibitor, calcium carbonate filler, bleached coniferous pulp and bleached hardwood pulp according to a mass ratio of sodium dodecylbenzene sulfonate: isothiazolinone mildew inhibitor: calcium carbonate filler: bleached coniferous pulp: bleached hardwood pulp = 1.5:3:12:30:70 to obtain a pulp having a beating degree of about 35° SR;

[0079] S8, placing the pulp on the screen for papermaking, pressing, and drying to obtain base paper;

[0080] S9. Use a sizing agent with a mass of 4% of the mass of the base paper to sizing the base paper, dry and calender, and obtain a paper-based facing material.

[0081] Example 2

[0082] This embodiment provides a paper-based facing material with mildew-proof function, which is prepared by the following steps:

[0083] S1. Mix α-amylase and starch into a reactor, add water twice the mass of starch, react for 20 min at a temperature of 80° C. to 85° C. and a pressure of 45000 Pa to 55000 Pa, extract the solid and dry it at a temperature of 125±3° C.; wherein, based on the amount of starch added, the amount of α-amylase used is 200 ppm;

[0084] S2, according to the mass ratio of polyether defoamer: aluminum sulfate: styrene-acrylate copolymer: enzymatic starch = 0.5:1:40:100, the polyether defoamer, aluminum sulfate, styrene-acrylate copolymer and enzymatic starch are mixed, and water is added to prepare a sizing agent with a solid content of 30% and a pH value of 4.5 to 5;

[0085] S3. Mix raw materials including sodium dodecylbenzene sulfonate, isothiazolinone mildew inhibitor, zinc oxide, calcium carbonate filler, bleached coniferous pulp and bleached broadleaf pulp in a mass ratio of sodium dodecylbenzene sulfonate: isothiazolinone mildew inhibitor: zinc oxide: calcium carbonate filler: bleached coniferous pulp: bleached broadleaf pulp = 1.5:3:2:10:30:70 to obtain a pulp having a beating degree of about 35° SR; wherein the calcium carbonate filler is heavy calcium carbonate purchased through commercial channels;

[0086] S4, placing the pulp on the screen for papermaking, pressing, and drying to obtain base paper;

[0087] S5. Use a sizing agent with a mass of 4% of the mass of the base paper to sizing the base paper, dry and calender, and obtain a paper-based facing material.

[0088] Example 3

[0089] This embodiment provides a paper-based facing material with mildew-proof function, which is prepared by the following steps:

[0090] S1. Mix α-amylase and starch into a reactor, add water twice the mass of starch, react for 20 min at a temperature of 80° C. to 85° C. and a pressure of 45000 Pa to 55000 Pa, extract the solid and dry it at a temperature of 125±3° C.; wherein, based on the amount of starch added, the amount of α-amylase used is 200 ppm;

[0091] S2, according to the mass ratio of polyether defoamer: aluminum sulfate: styrene-acrylate copolymer: enzymatic starch = 0.5:1:40:100, the polyether defoamer, aluminum sulfate, styrene-acrylate copolymer and enzymatic starch are mixed, and water is added to prepare a sizing agent with a solid content of 30% and a pH value of 4.5 to 5;

[0092] S3, mixing raw materials including sodium dodecylbenzene sulfonate, calcium carbonate filler, bleached coniferous pulp and bleached broadleaf pulp in a mass ratio of sodium dodecylbenzene sulfonate: calcium carbonate filler: bleached coniferous pulp: bleached broadleaf pulp = 1.5:12:30:70 to obtain a pulp having a beating degree of about 35° SR; wherein the calcium carbonate filler is heavy calcium carbonate purchased through commercial channels;

[0093] S4, placing the pulp on the screen for papermaking, pressing, and drying to obtain base paper;

[0094] S5. Use a sizing agent with a mass of 4% of the mass of the base paper to sizing the base paper, dry and calender, and obtain a paper-based facing material.

[0095] Performance Testing

[0096] In the paper-based facing material prepared in Example 1, zinc oxide is loaded on calcium carbonate; in the paper-based facing material prepared in Example 2, zinc oxide is added to the slurry; in the paper-based facing material prepared in Example 3, zinc oxide and isothiazolinone mildew inhibitor are not added.

[0097] The paper-based facing materials of Examples 1-3 were cut into samples 1-3 of 50 mm×50 mm, respectively. For each sample, 100 μL of Aspergillus niger liquid with a concentration of 100 CFU / mL after activation was transferred and evenly coated thereon to obtain test samples 1-3.

[0098] The samples 1-3 to be tested were cultured at 25°C and 80% humidity for 10 days and then the colony growth was observed. Sample 1 corresponding to Example 1 and Sample 2 corresponding to Example 2 did not grow mold. Sample 3 corresponding to Example 3 had a mold spot of about 1.5 mm, which occupied about 1 / 3 of the entire sample area.

[0099] The samples 1-3 to be tested were cultured at 25°C and 80% humidity for 20 days and then the colony growth was observed. Sample 1 corresponding to Example 1 did not grow mold. Sample 2 corresponding to Example 2 had a mold spot of about 1.1 mm, which occupied about 1 / 4 of the entire sample area. Sample 3 corresponding to Example 3 had a mold spot of about 2.3 mm, which occupied about 3 / 5 of the entire sample area.

Claims

1. A method for preparing a paper-based facing material with mildew-proof function, characterized in that: The preparation method comprises: S100, mixing and pulping raw materials including a surfactant, an isothiazolinone mildew inhibitor, a calcium carbonate filler and wood pulp to obtain a pulp; S200, placing the slurry on a screen for papermaking, pressing, and drying to obtain base paper; S300, applying sizing agent to the base paper, drying and calendering to obtain the paper-based facing material; Wherein, the porous calcium carbonate filler is loaded with zinc oxide.

2. The preparation method according to claim 1, characterized in that: The surfactant includes at least one of the following or a combination thereof: sodium dodecylbenzene sulfonate, sodium tetrapropylenebenzene sulfonate, sodium fatty alcohol sulfate, xylene sulfonic acid, and condensed sodium naphthalene sulfonate.

3. The preparation method according to claim 1, characterized in that: The calcium carbonate filler is prepared by the following steps: S111, mixing zinc chloride, calcium chloride, and heavy calcium carbonate in water and stirring to obtain a first mixture; S112, mixing sodium dodecylbenzene sulfonate and sodium carbonate in water and stirring to obtain a second mixture; S113, mixing polyacrylic acid in water and stirring to obtain a third mixture; S114, mixing the first mixture, the second mixture and the third mixture to react, to obtain the calcium carbonate.

4. The preparation method according to claim 3, characterized in that: In S111, the mass ratio of zinc chloride:calcium chloride:heavy calcium carbonate:water is (2-4):(6-8):(14-16):

100.

5. The preparation method according to claim 3, characterized in that: In S112, the mass ratio of sodium dodecylbenzenesulfonate:sodium carbonate:water=(0.5-1):(4-10):

100.

6. The preparation method according to claim 3, characterized in that: In S113, the mass ratio of polyacrylic acid to water is (6-10):

100.

7. The preparation method according to claim 3, characterized in that: S114 specifically includes: The second mixture is added dropwise into the first mixture with simultaneous stirring, and after the addition is completed, the mixture is allowed to stand for 15 to 30 minutes, and then the third mixture is added dropwise with simultaneous stirring, and after the addition is completed, the temperature is raised to 85° C. to 90° C. and kept warm for 2 to 2.5 hours, the solids are filtered, washed, dried, and heat-treated at a temperature of 300° C. to 350° C. for 10 to 60 minutes to obtain the calcium carbonate.

8. The preparation method according to claim 7, characterized in that: In S114, the mass ratio is: first mixture: second mixture: third mixture=100:(80-120):(20-30).

9. The preparation method according to any one of claims 1 to 8, characterized in that: The wood pulp comprises bleached coniferous wood pulp and bleached broadleaf wood pulp in a mass ratio of (0.25-0.5):

1.

10. A paper-based facing material with mildew-proof function, characterized in that: The paper-based facing material with anti-mildew function is obtained by the preparation method as described in any one of claims 1 to 9.

Citation Information

Patent Citations

  • Method for preparing antimicrobial material using nano calcium carbonate as substrate

    CN101480194A

  • Calcium silicate filled release body paper and preparation method thereof

    CN105200846A

  • Preparing method of mildew-proof non-woven wall paper

    CN107541981A

  • Paste material for mounting paper painting and calligraphy and preparation method thereof

    CN109370473A

  • Antibacterial silane polyether glue and preparation method thereof

    CN109628047A

Cited By

  • Mildew-proof decorative paper as well as preparation method and application thereof

    CN121161655A

  • A mildew-resistant decorative paper, its preparation method and its application

    CN121161655B