knitting

The knitted fabric uses composite false twisted yarns with controlled torque and crimp development to maintain snag resistance and softness, addressing the issue of fabric degradation after washing.

JP7567638B2Active Publication Date: 2024-10-16TORAY INDUSTRIES INC
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2021071573
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-04-21
Publication Date
2024-10-16
Estimated Expiration
2041-04-21

AI Technical Summary

Technical Problem

Conventional stretch knitted fabrics suffer from reduced snag resistance after repeated washing, compromising their firmness and soft texture.

Method used

A knitted fabric composed of composite false twisted yarns, with specific configurations of conjugated and non-conjugated false twisted yarns, including a torque balance and crimp development rate, enhances snag resistance while maintaining softness and firmness.

Benefits of technology

The fabric achieves excellent snag resistance after repeated washing, retaining its soft texture and firmness, with a balanced crimp structure that prevents yarn protrusion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007567638000001
    Figure 0007567638000001
  • Figure 0007567638000002
    Figure 0007567638000002
  • Figure 0007567638000003
    Figure 0007567638000003
Patent Text Reader

Abstract

To solve snag resistance after repeated washing which is heretofore a problem of a stretchable knitted fabric, and provide a knitted fabric having excellent stiffness and sturdiness, and soft feeling.SOLUTION: A knitted fabric includes a conjugate false twisted yarn, where the conjugate false twisted yarn comprises a yarn including a conjugate false twisted yarn A and a non-conjugate false twisted yarn B, the number of entanglement of the conjugate false twisted yarn is 100 / m or more, the number of torque twisting is 30 T / m or less, and the crimp development rate difference is 5-30%.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a knitted fabric which overcomes the problem of poor snag resistance after repeated washing, which has been a problem with conventional stretch knitted fabrics, and has excellent firmness and soft feel. [Background technology]

[0002] Knitted fabrics have excellent characteristics such as a soft texture and stretchability compared to woven fabrics, and are therefore widely used in various clothing applications such as sports and casual outerwear. In recent years, knitted fabrics using polyurethane yarns and bimetal yarns have been increasingly used to give knitted fabrics even higher stretchability. However, knitted fabrics using polyurethane are suitable for innerwear, but are not suitable for outerwear because they lack firmness and show the body lines too much. In addition, knitted fabrics using conjugate yarns in which different polymers are bonded side-by-side have been proposed (see Patent Document 1). This method certainly allows knitted fabrics with excellent firmness to be obtained, but the constituent yarns form protruding parts on the fiber surface, and the snag resistance was not taken into consideration at all. Knitted fabrics have a major problem in that the constituent yarns form loops and protrude onto the knitted fabric surface, making them more susceptible to snags than woven fabrics. Various studies have been conducted to improve the snag resistance of knitted fabrics. For example, a method of twisting the yarns constituting the knitted fabric has been proposed to increase the binding force of the yarns appearing on the knitted fabric surface (see Patent Document 2). However, the knitted fabric obtained by the above method has a problem that the soft texture and stretchability, which are inherent characteristics of the knitted fabric, are lost. In addition, a low-torque composite yarn is obtained by intertwining a composite yarn of a false-twisted yarn having a torque in the S direction and a false-twisted yarn having a torque in the Z direction, thereby obtaining a knitted fabric having snag resistance (see Patent Document 3). This method certainly makes it possible to obtain a knitted fabric having snag resistance, but this effect is the effect before washing, and after repeated washing, the balance of the yarn shape of the two yarns is lost, and one of the yarns tends to protrude from the knitted fabric surface, resulting in a decrease in snag resistance. In reality, the snag resistance of stretch knitted sewn products often deteriorates after home washing, and there was an urgent need to solve this problem. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2020-186503 A [Patent Document 2] JP 2003-247149 A [Patent Document 3] Patent No. 5155162 Summary of the Invention [Problem to be solved by the invention]

[0004] An object of the present invention is to provide a knitted fabric which overcomes the problem of poor snag resistance after repeated washing, which has been a problem with stretch knitted fabrics, and which has excellent firmness and a soft feel. [Means for solving the problem]

[0005] In order to solve the above problems, the knitted fabric of the present invention has the following configuration. A knitted fabric comprising a composite false-twisted yarn, the composite false-twisted yarn being composed of a yarn strip containing a conjugate false-twisted yarn A and a non-conjugate false-twisted yarn B, the composite false-twisted yarn having an entanglement number of 100 or more / m, a torque twist number of 30 T / m or less, and a crimp expression difference of 5 to 30%.

[0006] In the knitted fabric of the present invention, the composite false twist yarn is preferably composed of a false twist yarn having torque in the S direction and a false twist yarn having torque in the Z direction.

[0007] In the knitted fabric of the present invention, the conjugate false twist yarn A is preferably composed of polybutylene terephthalate and polyethylene terephthalate.

[0008] In the knitted fabric of the present invention, the conjugate false twist yarn A preferably has an eccentric core-sheath cross section.

[0009] The knitted fabric of the present invention preferably has a snag of grade 3 or higher after repeated washing. Effect of the Invention

[0010] According to the present invention, it is possible to obtain a knitted fabric which has been able to overcome the snag resistance after repeated washing, which has not been possible with the prior art, and which has excellent firmness and a soft feel. [Brief description of the drawings]

[0011] [Figure 1] 1 is a photograph substituting a drawing showing an example of a fiber cross section of an eccentric sheath-core composite fiber of the present invention. [Diagram 2] 1 is a cross-section of an example of an eccentric sheath-core composite fiber of the present invention, illustrating the position of the center of gravity in the fiber cross section. [Diagram 3] 1 is a fiber cross section for explaining the fiber diameter (D) and minimum thickness (S) in the fiber cross section of an eccentric sheath-core composite fiber of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] It is important that the knitted fabric of the present invention is made of a composite false-twisted yarn containing at least a conjugate false-twisted yarn A and a non-conjugate false-twisted yarn B. The crimp form is different between the conjugate false-twisted yarn and the non-conjugate false-twisted yarn, and the conjugate false-twisted yarn has a finer coil-shaped crimp than the non-conjugate false-twisted yarn, so that it can enter the gaps present in the knitted fabric and reduce the gaps in the knitted fabric. By making the yarn in the knitted fabric less mobile, even if an external force is applied to the knitted fabric by repeated washing, the yarn does not protrude from the knitted fabric surface, and excellent snag resistance can be obtained. Here, a knitted fabric made of a composite false-twisted yarn consisting of a conjugate false-twisted yarn alone or a conjugate false-twisted yarn and a conjugate false-twisted yarn has excellent stretchability, but the coil crimp is likely to protrude from the knitted fabric surface, and the snag resistance is deteriorated. Furthermore, in the case of a non-conjugated false-twisted yarn alone or a composite false-twisted yarn consisting of a non-conjugated false-twisted yarn and a non-conjugated false-twisted yarn, there are many voids in the knitted fabric, the yarns are likely to move with repeated washing, and the crimps in the outer layer of the yarns are likely to protrude, resulting in poor snag resistance.In addition, in the case of a composite false-twisted yarn consisting of a conjugated non-false-twisted yarn and a non-conjugated false-twisted yarn, residual torque is likely to occur, resulting in poor snag resistance.

[0013] It is also important that the number of entanglements in the composite false twist yarn constituting the knitted fabric of the present invention is 100 or more / m. The preferred number of entanglements is 120 to 200 / m. If the number of entanglements is less than 100 / m, the crimps in the outer layer of the yarn tend to protrude, the convergent form cannot be maintained, and snag resistance deteriorates.

[0014] It is also important that the torque twist number of the composite false twist yarn constituting the knitted fabric of the present invention is 30 T / m or less. The preferred torque twist number is 20 T / M or less. If the torque twist number exceeds 30 T / M, during dyeing processing, torque is also generated at the same time as crimp is generated, resulting in large unevenness of the knitted fabric and poor snag resistance.

[0015] It is also important that the crimp expression difference of the composite false-twisted yarn constituting the knitted fabric of the present invention is 5 to 30%. The preferred crimp expression difference is 5 to 20%. If the crimp expression difference is less than 5%, there will be many voids in the knitted fabric, the yarn will be more likely to move with repeated washing, and the crimp of the outer layer of the yarn will be more likely to protrude, resulting in poor snag resistance. If the crimp expression difference exceeds 30%, the non-conjugated false-twisted yarn B will protrude together with the yarn to the surface of the knitted fabric, resulting in poor snag resistance.

[0016] It is also preferred that the composite false twist yarn constituting the knitted fabric of the present invention is composed of a false twist yarn having a torque in the S direction and a false twist yarn having a torque in the Z direction. This preferred embodiment cancels out the false twist torque and makes the knitted crimp flat, making it easier to obtain excellent snag resistance.

[0017] The cross section of the conjugate false twist yarn A used in the present invention is composed of two kinds of polymers. Examples of suitable polymers for obtaining stretchability include polyethylene terephthalate, polyethylene naphthalate, polybutylene terephthalate, polytrimethylene terephthalate, nylon, polylactic acid, thermoplastic polyurethane, and polyphenylene sulfide. The molecular weight of these can be changed to use a high molecular weight polymer for one component and a low molecular weight polymer for the other, or one component can be used as a homopolymer and the other component as a copolymer. In addition, as for combinations of different polymer compositions, various combinations such as polybutylene terephthalate / polyethylene terephthalate, polytrimethylene terephthalate / polyethylene terephthalate, and polytrimethylene terephthalate / polybutylene terephthalate can be mentioned. Among these, in the combination of polybutylene terephthalate and polyethylene terephthalate, a fine coil crimp structure is developed after false twisting, so that the voids in the knitted fabric are reduced. As a result, the knitted fabric is less likely to deform with repeated washing, and one of the yarns does not protrude from the knitted fabric surface, and excellent snag resistance can be obtained, which is preferable.

[0018] The ratio of the two components in the conjugate false twisted yarn A used in the present invention, component A:component B, is preferably in the range of 70:30 to 30:70 (area ratio), more preferably in the range of 65:35 to 45:55.

[0019] As for the fiber cross-sectional shape of the conjugate false-twisted yarn A, any composite cross-sectional shape may be used, whether it is a side-by-side structure or an eccentric sheath-core structure. However, an eccentric sheath-core cross section is preferred because it reduces cross-sectional deformation during false-twisting, allows uniform crimping of each single yarn, reduces the protrusion of single yarn snarls on the knitted fabric surface, and improves snag resistance.

[0020] Here, the eccentric sheath-core cross section refers to an eccentric sheath-core type having a composite cross section formed by bonding two different polymers, in which the two polymers with different polymer properties are essentially not separated but exist in a bonded state, and the B component completely covers the A component.

[0021] Here, eccentricity refers to the position of the center of gravity of the A component polymer in the cross section of the composite fiber being different from the center of the cross section of the composite fiber. Hereinafter, a specific explanation will be given with reference to FIG. 2. In FIG. 2, the horizontal hatching is the B component, the 30-degree hatching (diagonal lines rising to the right) is the A component, the center of gravity of the A component in the cross section of the composite fiber is the center of gravity a, and the center of gravity of the cross section of the composite fiber is the center of gravity C. Since the center of gravity a and the center of gravity C of the cross section of the composite fiber are separated (eccentric), the fiber is largely curved toward the high shrinkage component after heat treatment. In this way, the high shrinkage component shrinks relatively more strongly than the low shrinkage component, so the eccentric sheath-core composite fiber continues to be curved in the fiber axis direction. As a result, the eccentric sheath-core composite fiber has a three-dimensional spiral structure and exhibits good crimp. Here, the more the center of gravity is separated, the better the crimp is exhibited, and good stretch performance is obtained.

[0022] Furthermore, the ratio S / D of the minimum thickness S of the B component covering the A component in the eccentric core-sheath cross section (hereinafter referred to as "minimum thickness S") to the fiber diameter (diameter of the composite fiber) D is preferably 0.01 to 0.2, and more preferably 0.02 to 0.08.

[0023] This will be explained in more detail using the fiber cross section shown in Figure 3. Here, the thinnest part of the B component in the core-sheath composite fiber has a minimum thickness S.

[0024] Furthermore, it is preferable that the part having a thickness within 1.05 times the minimum thickness S (hereinafter sometimes referred to as the "minimum thickness part") occupies 1 / 3 or more of the entire perimeter of the composite fiber. This preferable embodiment means that component A is present along the contour of the fiber, and compared with a conventional eccentric sheath-core composite fiber of the same area ratio, the present invention has the centers of gravity of the respective components farther apart in the fiber cross section, forming a fine spiral and exhibiting good crimp.

[0025] More preferably, by making the perimeter of the thickness within 1.05 times the minimum thickness S at 2 / 5 or more of the perimeter of the entire fiber, the coil structure of each fiber becomes uniform when crimping occurs, resulting in a knitted fabric with less single-yarn snare and better snag resistance.

[0026] The methods for measuring the minimum thickness S and fiber diameter D are as follows.

[0027] A multifilament made of eccentric sheath-core composite fiber is embedded in an embedding agent such as epoxy resin, and an image is taken of a cross section perpendicular to the fiber direction with a transmission electron microscope (TEM) at a magnification such that 10 or more fibers (locations) can be observed. In this case, if metal dyeing is applied, the contrast of the joint between component A and component B can be made clear by utilizing the dye difference between the polymers. The presence of the joints makes it possible to confirm that the eccentric sheath-core composite fiber is two-component. A circle circumscribing the cross section of 10 single yarns of eccentric sheath-core composite fiber (locations) randomly selected within each image taken is set, and the value obtained by measuring the circumscribing circle diameter corresponds to the fiber diameter D referred to in the present invention. The circle circumscribing the cross section referred to here is a true circle that circumscribs the cross section at two or more points most frequently at two or more points on the cross section taken from a two-dimensionally taken image. The circumscribing circle diameter refers to the diameter of the true circle. In addition, the image in which the fiber diameter D was measured is used to measure the minimum thickness of the B component covering the A component for 10 or more fibers (locations), and the value corresponds to the minimum thickness S referred to in the present invention. Furthermore, these fiber diameters D and minimum thicknesses S are measured in units of μm and rounded off to the nearest third decimal place. The above operations are performed on the images of 10 locations, and the simple number average of the measured values ​​and their ratios (S / D) are calculated. Note that the area of ​​the entire fiber and the areas of the A and B components can be calculated using the images taken above and the image analysis software "WinROOF2015" (Mitani Shoji Co., Ltd.), and then the center of specific gravity and the area ratio can be calculated.

[0028] The non-conjugate false twist yarn B used in the present invention is not limited as long as it is a thermoplastic polymer that can be false twisted, but polyester, nylon, etc. are particularly preferably used. Examples of polyester include polyethylene terephthalate, polybutylene terephthalate, polypropylene terephthalate, and copolymers of these with sulfonic acid components, dicarboxylic acid components, diol components, or oxycarboxylic acid components, or blends of these polyesters. Among them, if it has an anionic site such as a sulfonic acid group, it is preferable because it has cationic dyeability and can express a natural heathered tone due to interaction with a cationic dye having a cationic site. Specific examples of sulfonic acid groups include 5-sulfoisophthalic acid metal salts, such as lithium salts, sodium salts, potassium salts, rubidium salts, and cesium salts, but are not limited to these. Among them, lithium salts and sodium salts are preferable, and sodium salts in particular can be used preferably because they have excellent crystallinity.

[0029] As for nylon, examples include nylon 6, nylon 66, nylon 610, nylon 56, etc., and nylon 6 and nylon 66, which are excellent in crimp development after false twisting, are particularly preferred.

[0030] In addition, the non-conjugate false twisted yarn B used in the present invention can be selected from those having any shape in cross section, including polygonal types such as round, triangular, flat, hexagonal, L-shaped, T-shaped, W-shaped, octave-shaped, dog-bone, and various types.

[0031] Furthermore, in the polymers of the conjugate false-twisted yarn A and the non-conjugate false-twisted yarn B, inorganic fine particles, organic compounds, and carbon black may be contained as needed, as matting agents such as titanium oxide, flame retardants, lubricants, antioxidants, coloring pigments, etc., within the scope of the invention.

[0032] In the present invention, the fineness of the conjugate false-twisted yarn A and the non-conjugate false-twisted yarn B is preferably 15 to 150 dtex, which gives the knitted fabric firmness and light weight while preventing the knitted fabric from becoming too thick when used as an outer garment. The more preferred fineness is 15 to 40 dtex.

[0033] In the present invention, the single yarn fineness of each of the conjugate false-twisted yarn A and the non-conjugate false-twisted yarn B is preferably 0.3 to 5 dtex in order to impart stretchability and softness to the knitted fabric, and more preferably 0.5 to 3.5 dtex.

[0034] In addition, the ratio of the conjugate false-twisted yarn A to the non-conjugate false-twisted yarn B in the present invention (A / B: mass ratio) is preferably in the range of 20 / 80 to 80 / 20, more preferably in the range of 30 / 70 to 70 / 30, taking into consideration the balance of crimp development.

[0035] Next, a method for producing the knitted fabric of the present invention will be described.

[0036] First, when spinning the raw yarn of the conjugate false twist yarn A used in the present invention, if it has an eccentric core-sheath composite structure, it is preferable to precisely control the sheath thickness of the fiber and the perimeter of the thin skin part, and a method using a distribution plate as exemplified in JP-A-2011-174215, JP-A-2011-208313, and JP-A-2012-136804 is preferably used as a spinning spinneret. When a composite yarn having an eccentric core-sheath type cross section is produced using a conventionally known composite spinneret, it is often very difficult to precisely control the position of the center of gravity of the core and the sheath thickness. For example, if the sheath thickness becomes thin and the core component is exposed, this can cause a decrease in snag due to the protrusion of single yarn snare on the knitted surface during repeated washing, and conversely, if the sheath thickness becomes thick, the crimp expression decreases, which can cause problems such as a decrease in stretch performance.

[0037] Regarding the spinning speed, it is preferable that the amorphous portion is in a highly oriented state in order to improve the crimp expression rate, and the preferred spinning speed is 2,800 to 3,500 m / min.

[0038] In addition, it is preferable to spin a highly oriented undrawn yarn when spinning the raw yarn of the non-conjugate false twisted yarn B used in the present invention. In order to improve the crimp expression rate, it is preferable that the amorphous portion is in a highly oriented state, and the preferred spinning speed is 2,800 to 3,500 m / min.

[0039] Next, in producing the composite false-twist textured yarn used in the present invention, the raw yarn of conjugate false-twisted yarn A and the raw yarn of non-conjugate false-twisted yarn B are false-twisted in different directions (false-twisted in the S direction and false-twisted in the Z direction) and then post-entangled, which is preferable as it results in a composite yarn with low torque, a flat knitting crimp, and excellent snag resistance.

[0040] Any false twisting conditions can be selected. The twister may be of the spindle type, friction disk type, or belt nip type, but the friction disk type is preferred because it allows false twisting at high speed and produces relatively little single yarn snare. In the case of a contact heater, a false twisting temperature of 170 to 220°C is preferred because it can impart strong crimp. The number of false twists is determined by the false twist coefficient (number of false twists (T / M) x fineness (dtex) 0.5 ) in the range of 27,000 to 33,000, which allows for strong crimping. In this case, it is more preferable to set the false twist coefficient of conjugate false twist yarn A higher than the false twist coefficient of non-conjugate false twist yarn B, which makes it easier for the fine coil crimps of conjugate false twist yarn A to enter inside the crimps of non-conjugate false twist yarn B, thereby more effectively filling voids in the knitted fabric.

[0041] As for the entangling conditions, the entangling pressure is preferably 0.25 to 0.5 MPa, taking into consideration the balance between stretchability and convergence.

[0042] Regarding the yarn processing speed, the faster the speed, the higher the productivity, which is preferable, but in consideration of stable processing, a speed of 100 to 800 (m / min) is preferable.

[0043] The knitted fabric of the present invention can be easily knitted using a normal knitting machine. Filaments and spans other than the composite textured yarn may be interwoven as long as the object of the present invention is not impaired. The knitted fabric structure is not particularly limited, and may be a circular knitted fabric, a weft knitted fabric, or a warp knitted fabric. Preferred examples of circular knitted fabrics and weft knitted fabrics include plain knitted fabrics, flat knitted fabrics, rib knitted fabrics, double knitted fabrics, pearl knitted fabrics, tuck knitted fabrics, floating knitted fabrics, one-sided knitted fabrics, lace knitted fabrics, hair-filled knitted fabrics, knit miss knitted fabrics, and one-sided knotted fabrics. Preferred examples of warp knitted fabrics include single denby knitted fabrics, single atlas knitted fabrics, double cord knitted fabrics, half tricot knitted fabrics, fleece knitted fabrics, and jacquard knitted fabrics. Among these, circular knitted fabrics are particularly preferred in terms of stretchability. Plain knitted fabrics are preferred in terms of light weight.

[0044] The processing step can be carried out according to any dyeing step and conditions. In the knitted fabric of the present invention, the stitch density is preferably within the range of 30 to 100 courses / 2.54 cm and 50 to 130 wales / 2.54 cm.

[0045] Furthermore, the knitted fabric of the present invention may be subjected to various types of additional processing, such as conventional water absorption processing, water repellency processing, nap raising processing, ultraviolet shielding, or processing to impart functions such as antibacterial agents, antiviral agents, deodorizing agents, insect repellents, and retroreflective agents, within the scope of the invention.

[0046] In addition to the normal snag, the knitted fabric of the present invention preferably has a snag of at least grade 3 after repeated washing. Conventional stretch knitted fabrics lose their yarn shape balance after repeated washing, causing yarn stripes to protrude from the knitted fabric surface, resulting in problems with snags. However, by having a snag of at least grade 3 after repeated washing, the snag resistance of actual stretch knitted sewn products can be further improved.

[0047] The stretchability of the knitted fabric of the present invention is preferably 50% or more (preferably 80 to 150%) in terms of warp and weft stretchability measured by method B described in JIS L 1096 (2010).

[0048] The knitted fabric obtained according to the present invention is suitable for use as clothing, such as casual shirts, sports shirts, business shirts, skirts, pants, gym clothes, and the like. EXAMPLES

[0049] The present invention will now be described more specifically with reference to examples. (1) Fineness Using a measuring machine with a frame circumference of 1.0 m, 100 skeins were produced, and the fineness was measured according to the following formula.

[0050] Fineness (dtex) = Weight of skein for 100 uses (g) x 100 (2) Degree of entanglement The degree of entanglement is the number of entangled parts per meter under a tension of 0.1 cN / dtex, and is calculated by inserting a pin into the non-entangled part of the yarn under a tension of 0.02 cN / dtex, moving the pin up and down the length of the yarn over 1 m with a tension of 0.1 cN / dtex, recording the distance traveled as the non-entangled part where the pin moves without resistance, and the part where the pin stops is the entangled part. This process is repeated 30 times, and the degree of entanglement per meter is calculated from the average distance of the non-entangled parts. (3) Difference in crimp occurrence rate Carefully unravel and separate the conjugated false-twisted yarn A and the non-conjugated false-twisted yarn B from the composite twisted yarn in the knitted fabric, and take out 10 pieces of each 6 cm each to use as samples. 1 The sample marked with ) was wrapped in gauze and heat-treated in boiling water at 100°C for 30 minutes without tension. The sample was then removed and air-dried for 24 hours at 35°C and 60% RH. The marked interval (L) after heat treatment was read under a load of 0.02 mN / dtex. This procedure was repeated 10 times, and the average value was taken as the crimp development rate. The difference in the crimp development rate was calculated using the following formula.

[0051] Shrinkage occurrence rate (%) = {(LL 1 ) / L}×100 Crimp development rate difference (%) = (crimp development rate of conjugate false-twisted yarn A) - (crimp development rate of non-conjugate false-twisted yarn B) (4) Torque twist Approximately 75 cm of composite false twist yarn is stretched horizontally, an initial load of 0.02 mN / dtex is hung from the center, and both ends are pulled together. The yarn begins to rotate due to the residual torque, but it is held in this state until the initial load stops, resulting in a twisted yarn. The number of twists over a 25 cm length of the twisted yarn thus obtained is measured with a twist detector under a load of 1 mN / dtex. The obtained number of twists (T / 25 cm) is multiplied by 4 to obtain the torque (T / m). (5) Stretch rate (%) The elongation rate was measured under a load of 1.5 kgf (14.7 N) according to Method B of JIS L 1096 (2010). (6) Snag resistance rating The washing cycle was performed once using a two-tub washing machine with a liquid temperature of 40°C, a wash time of 5 minutes, rinsing at 30°C for 2 minutes twice, and a spin cycle of 30 seconds. Kao's "Attack" (registered trademark) was used as the detergent at 1g / L, with a liquid volume of 40L and a combined weight of 830g for the test cloth and the cotton cloth used as the guide cloth. After repeating this washing process 20 times, the grade was determined according to the JIS L 1058 (2010) D-1 method. A passing grade is 3.5 or above. (7) Stiffness Sensory evaluation involved rating the product on a four-point scale: very good firmness, good firmness, slightly insufficient firmness, and insufficient firmness, with the result closest to the average of the ratings of 10 randomly selected people. (8) Softness In the sensory evaluation, the softness was rated on a four-point scale: very excellent softness, excellent softness, slightly insufficient softness, and insufficient softness, and the result was determined to be closest to the average of the ratings of 10 randomly selected people.

[0052] <Example 1> Polyethylene terephthalate and polybutylene terephthalate were fed into a spinneret for eccentric sheath-core composite fibers with a weight composite ratio of 50 / 50 and 48 discharge holes. The polymers merged inside the spinneret to form an eccentric sheath-core composite structure in which the A component polymer was contained in the B component polymer, and the resulting fiber was spun from the spinneret at a spinning speed of 3,000 (m / min) to obtain a conjugate partially oriented yarn with a fineness of 56 dtex, 48 filaments, and an elongation of 130%. In the spinning of Example 1, a spinneret with a distributor plate system was used to obtain the eccentric sheath-core composite fiber shown in Figure 1. The S / D ratio in the fiber cross section was 0.02, and the minimum thickness portion accounted for 40% of the fiber circumference.

[0053] Next, polyethylene terephthalate having a circular cross section copolymerized with 0.3 mol% of 5-sodium sulfoisophthalic acid was spun at a spinning speed of 3,000 (m / min) to obtain a partially oriented polyethylene terephthalate yarn with a fineness of 56 dtex, 48 filaments, and an elongation of 145%.

[0054] Then, using a friction false twist processing machine, the conjugate partially oriented yarn was false twisted in the S direction at a draw ratio of 1.7 times and a false twist coefficient of 29,000 at a processing speed of 400 m / min and a heater temperature of 180°C, and the polyethylene terephthalate partially oriented yarn was false twisted in the Z direction at a draw ratio of 1.8 times and a false twist coefficient of 28,000.After that, an interlace processing was performed at an entanglement pressure of 0.4 MPa, resulting in a composite textured yarn with a fineness of 64 dtex, entanglement number of 125 / m, and a torque twist number of 2 T / m (S direction).

[0055] Next, the composite false twist yarn was used to knit a plain knit circular fabric using a 36G single circular knitting machine. The resulting greige fabric was subjected to continuous open scour at 98°C, dyed in navy blue at 120°C using a cationic dye, and further to a finish set at 170°C, resulting in a fabric weight of 98 g / m 2 A knitted fabric was obtained with 98 courses / 2.54 cm, 58 wales / 2.54 cm, and a crimp expression rate difference of 18% (conjugate: 48%, non-conjugate: 30%).

[0056] The obtained knitted fabric had a warp stretch rate of 78% and a weft stretch rate of 110%, and its snag resistance rating was 4.5 before washing and 4 after 20 washes. Even after repeated washing over a long period of time, the knitted fabric had excellent snag resistance, softness, and firmness.

[0057] <Example 2> In the same manner as in Example 1, a conjugate partially oriented yarn having a fineness of 56 dtex, 48 filaments and an elongation of 130% was obtained.

[0058] Next, nylon 66 having a circular cross section was spun at a spinning speed of 3,200 (m / min) to obtain a nylon 66 drawn yarn having a fineness of 30 dtex, 26 filaments, and an elongation of 60%.

[0059] Then, using a friction false twist processing machine, the conjugate partially oriented yarn was false twisted in the S direction at a draw ratio of 1.7 and a false twist coefficient of 29,000 at a processing speed of 400 m / min and a heater temperature of 180°C, and the nylon 66 oriented yarn was false twisted in the Z direction at a draw ratio of 1.1 and a false twist coefficient of 28,500.After that, an interlace processing was performed at an entanglement pressure of 0.45 MPa, resulting in a composite textured yarn with a fineness of 60 dtex, entanglement number of 155 / m, and a torque twist number of 5 T / m (S direction).

[0060] Next, the composite false twist yarn was used to knit a plain knit circular fabric using a 36G single circular knitting machine. The resulting grey fabric was subjected to continuous open scour at 98°C, dyed navy blue at 100°C using an acid dye, and further subjected to finish setting at 170°C to give a basis weight of 96 g / m 2 A knitted fabric was obtained with 102 courses / 2.54 cm, 61 wales / 2.54 cm, and a crimp expression rate difference of 13% (conjugate: 48%, non-conjugate: 35%).

[0061] The obtained knitted fabric had a warp stretch rate of 85% and a weft stretch rate of 122%, and its snag resistance rating was 4.5 before washing and 4 after 20 washes. Even after repeated washing over a long period of time, the knitted fabric had excellent snag resistance, softness, and firmness.

[0062] <Example 3> The A component was polyethylene terephthalate and the B component was polytrimethylene terephthalate. The weight ratio of A component to B component was 50 / 50. They were spun at a spinning speed of 3,000 (m / min) from a side-by-side spinneret with 48 nozzles, resulting in a conjugate partially oriented yarn with a fineness of 90 dtex, 48 filaments, and an elongation of 128%.

[0063] Next, polyethylene terephthalate having a circular cross section was spun at a spinning speed of 3,000 (m / min) to obtain a partially oriented polyethylene terephthalate yarn having a fineness of 56 dtex, 48 filaments, and an elongation of 143%.

[0064] Then, using a friction false twist processing machine, the conjugate partially oriented yarn was false twisted in the S direction at a draw ratio of 1.7 times and a false twist coefficient of 29,000 at a processing speed of 400 m / min and a heater temperature of 180°C, and the polyethylene terephthalate partially oriented yarn was false twisted in the Z direction at a draw ratio of 1.8 times and a false twist coefficient of 29,500.After that, an interlace processing was performed at an entanglement pressure of 0.25 MPa, resulting in a composite textured yarn with a fineness of 94 dtex, entanglement number of 104 pieces / m, and a torque twist number of 3 T / m (S direction).

[0065] Next, the composite false twist yarn was used to knit a plain knit circular fabric using a 36G single circular knitting machine. The resulting greige fabric was subjected to continuous open-weave scouring at 98°C, dyed navy blue at 130°C using a disperse dye, and then finished at 170°C to give a fabric weight of 118 g / m 2 A knitted fabric was obtained with 82 courses / 2.54 cm, 51 wales / 2.54 cm, and a crimp expression rate difference of 6% (conjugate: 42%, non-conjugate: 36%).

[0066] The obtained knitted fabric had a warp stretch rate of 72% and a weft stretch rate of 104%, and a snag resistance rating of grade 4 before washing and grade 3.5 after 20 washes. Even after long-term repeated washing, the knitted fabric had excellent snag resistance, softness, and firmness.

[0067] <Comparative Example 1> In the same manner as in Example 1, two conjugate partially oriented yarns having a fineness of 56 dtex, 48 filaments and an elongation of 130% were obtained.

[0068] The two conjugate partially oriented yarns were then false-twisted in the S direction and Z direction, respectively, using a friction false-twisting machine at a processing speed of 400 m / min, a heater temperature of 180°C, a draw ratio of 1.7 times, and a false-twist coefficient of 29,000, and then interlaced at an entanglement pressure of 0.4 MPa to obtain a composite textured yarn with a fineness of 66 dtex, entanglement number of 124 / m, and a torque twist number of 2 T / m (S direction).

[0069] Next, the composite false twist yarn was used to knit a plain knit circular fabric using a 36G single circular knitting machine. The resulting greige fabric was subjected to continuous open-weave scouring at 98°C, dyed navy blue at 120°C using a disperse dye, and then finished at 170°C to give a fabric weight of 107 g / m 2 A knitted fabric having 105 courses / 2.54 cm, 63 wales / 2.54 cm, and a crimp development rate difference of 0% was obtained.

[0070] The obtained knitted fabric had a warp stretch rate of 87% and a weft stretch rate of 134%, and the snag resistance rating was 3.5 before washing and 2.5 after 20 washings, indicating that the snag resistance decreased with repeated washing. In addition, the softness was excellent, but the firmness was somewhat lacking.

[0071] <Comparative Example 2> Polyethylene terephthalate having a circular cross section was spun at a spinning speed of 3,000 (m / min) to obtain two partially oriented polyethylene terephthalate yarns having a fineness of 56 dtex, 48 filaments, and an elongation of 145%.

[0072] Then, using a friction false twist processing machine, at a processing speed of 400 m / min and a heater temperature of 180°C, one of the polyethylene terephthalate partially oriented yarns was false twisted in the S direction with a draw ratio of 1.7 times and a false twist coefficient of 29,000, and the other polyethylene terephthalate partially oriented yarn was false twisted in the Z direction with a draw ratio of 1.8 times and a false twist coefficient of 28,000, and then interlaced at an entanglement pressure of 0.4 MPa to obtain a composite textured yarn with a fineness of 64 dtex, entanglement number of 118 pieces / m, and a torque twist number of 2 T / m (S direction).

[0073] Next, the composite false twist yarn was used to knit a plain knit circular fabric using a 36G single circular knitting machine. The resulting greige fabric was subjected to continuous open-weave scouring at 98°C, dyed navy blue at 130°C using a disperse dye, and then finished and set at 170°C to give a fabric weight of 98 g / m 2 A knitted fabric having 85 courses / 2.54 cm, 53 wales / 2.54 cm, and a crimp development rate difference of 3% was obtained.

[0074] The obtained knitted fabric had a warp stretch rate of 43% and a weft stretch rate of 77%, and the snag resistance rating was 4.5 before washing and 2.5 after 20 washings, showing that the snag resistance decreased with repeated washing. In addition, the softness was somewhat insufficient, and the firmness was insufficient.

[0075] <Comparative Example 3> In the same manner as in Example 1, two conjugate partially oriented yarns having a fineness of 56 dtex, 48 filaments and an elongation of 130% were obtained.

[0076] The two conjugate partially oriented yarns were then false-twisted in the S-direction using a friction false-twist processing machine at a processing speed of 400 m / min, a heater temperature of 180°C, a draw ratio of 1.7 times, and a false-twist coefficient of 29,000, and then interlaced at an entanglement pressure of 0.4 MPa to obtain a composite textured yarn with a fineness of 66 dtex, entanglement number of 132 / m, and torque twist number of 42 T / m (S-direction).

[0077] Next, the composite false twist yarn was used to knit a plain knit circular fabric using a 36G single circular knitting machine. The resulting greige fabric was subjected to continuous open-weave scouring at 98°C, dyed navy blue at 120°C using a disperse dye, and then finished at 170°C to give a fabric weight of 110 g / m 2 A knitted fabric having 104 courses / 2.54 cm, 62 wales / 2.54 cm, and a crimp development rate difference of 0% was obtained.

[0078] The obtained knitted fabric had a warp stretch rate of 88% and a weft stretch rate of 138%, and the snag resistance rating was grade 3 before washing and grade 1.5 after 20 washes. Repeated washing caused the unevenness of the knitted fabric surface to increase, and the snag resistance to decrease. In addition, the softness was insufficient, and the firmness was somewhat insufficient.

[0079] <Comparative Example 4> In the same manner as in Example 1, a conjugate partially oriented yarn having a fineness of 56 dtex, 48 filaments and an elongation of 130% was obtained.

[0080] Next, polyethylene terephthalate having a circular cross section was spun at a spinning speed of 3,000 (m / min) to obtain a partially oriented polyethylene terephthalate yarn having a fineness of 56 dtex, 48 filaments, and an elongation of 143%.

[0081] Then, using a friction false twist processing machine, the conjugate partially oriented yarn was false twisted in the S direction at a draw ratio of 1.7 times and a false twist coefficient of 29,000 at a processing speed of 400 m / min and a heater temperature of 180°C, and the polyethylene terephthalate partially oriented yarn was false twisted in the Z direction at a draw ratio of 1.8 times and a false twist coefficient of 29,500.After that, an interlace processing was performed at an entanglement pressure of 0.2 MPa, resulting in a composite textured yarn with a fineness of 93 dtex, entanglement number of 85 pieces / m, and a torque twist number of 10 T / m (S direction).

[0082] Next, the composite false twist yarn was used to knit a plain knit circular fabric using a 36G single circular knitting machine. The resulting greige fabric was subjected to continuous open scour at 98°C, dyed in navy blue at 120°C using a cationic dye, and further subjected to finish setting at 170°C to give a basis weight of 106 g / m 2A knitted fabric was obtained with 95 courses / 2.54 cm, 56 wales / 2.54 cm, and a crimp expression rate difference of 22% (conjugate: 48%, non-conjugate: 26%).

[0083] The obtained knitted fabric had a warp stretch rate of 80% and a weft stretch rate of 115%, and a snag resistance rating of 4.5 before washing and 2.5 after 20 washes. The softness and firmness were excellent, but repeated washing caused the interlacing to come undone, single yarns to protrude from the knitted fabric surface, and the snag resistance to decrease. [Industrial Applicability]

[0084] The knitted fabric of the present invention can be suitably used as clothing for a variety of applications, including casual shirts, sports shirts, business shirts, skirts, pants, gym clothes, and the like. [Explanation of symbols]

[0085] 1. Component A 2 B component a Center of gravity of component A C Center of gravity of composite fiber cross section D fiber diameter S Minimum thickness

Claims

1. A knitted fabric comprising a composite false-twisted yarn, the composite false-twisted yarn being composed of a yarn strip containing a conjugate false-twisted yarn A and a non-conjugate false-twisted yarn B, the composite false-twisted yarn having an entanglement number of 100 or more / m, a torque twist number of 30 T / m or less, and a crimp expression rate difference of 5 to 30%.

2. 2. The knitted fabric according to claim 1, wherein the composite false twist yarn is composed of a false twist yarn having a torque in the S direction and a false twist yarn having a torque in the Z direction.

3. 3. The knitted fabric according to claim 1, wherein the conjugate false twist yarn A is composed of polybutylene terephthalate and polyethylene terephthalate.

4. The knitted fabric according to any one of claims 1 to 3, characterized in that the conjugate false twist yarn A has an eccentric core-sheath cross section.

5. 5. The knitted fabric according to claim 1, wherein the snag after repeated washing is grade 3 or higher.

Citation Information

Patent Citations

  • Osuishoriho

    JP1976055162A

  • Composite yarn and production of woven fabric

    JP1993247757A

  • Woven or knitted fabric, its production and composite yarn

    JP1999043835A

  • Method for producing non-torque false twist yarn

    JP2003166136A

  • Round knitted fabric having excellent snagging resistance

    JP2003247149A