Multilayer Ceramic Capacitors
The multilayer ceramic capacitor addresses short circuit risks through optimized external electrode dimensions and surface portion lengths, stabilizing solder wetting and alignment to enhance mounting performance on substrates with reduced areas.
Patent Information
- Application Number
- JP2021186327
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-11-16
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2041-11-16
AI Technical Summary
Conventional LW inversion type multilayer ceramic capacitors face issues with variations in the formation of base and covering conductor layers, leading to inconsistent solder wetting and application of tensile stress, which can cause rotation, tilting, and increased risk of short circuits during mounting on substrates with reduced mounting areas.
The multilayer ceramic capacitor design features specific dimensions and surface portion lengths for external electrodes, ensuring w>l>t, with narrower surface portions to stabilize solder wetting and reduce the risk of short circuits by centering mounting on central portions, thereby improving self-alignment and preventing polarity misalignment.
The design effectively suppresses short circuit defects and enhances mounting stability by controlling solder wetting and stress application, ensuring reliable attachment and alignment on substrates with reduced mounting areas.
Smart Images

Figure 0007567757000002 
Figure 0007567757000003 
Figure 0007567757000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a multilayer ceramic capacitor. [Background technology]
[0002] Conventionally, multilayer ceramic capacitors have been known. A typical multilayer ceramic capacitor has a laminate in a substantially rectangular parallelepiped shape whose length direction L is longer than its width direction W, and external electrodes are provided at both ends of the laminate in the length direction L. Meanwhile, so-called LW-reversed type multilayer ceramic capacitors are also known in which the magnitude relationship between the length direction L and width direction W of the laminate is reversed in order to reduce ESL (see Patent Documents 1 and 2).
[0003] Furthermore, in recent years, as the mounting density of substrates has increased, the mounting area of multilayer ceramic capacitors has decreased. Therefore, the PoP (Package on Package) mounting form has been adopted, and the demand for multilayer ceramic capacitors mounted on the lower end of substrates as LSC (Land Side Capacitor) type has increased. For such LSC (Land Side Capacitor) type mounted multilayer ceramic capacitors, low-profile multilayer ceramic capacitors with a thin thickness in the height direction are required. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2020-57753 A [Patent Document 2] JP 2020-61524 A Summary of the Invention [Problem to be solved by the invention]
[0005] Patent Document 2 discloses an LW-reversed type multilayer ceramic electronic component in which a recess is provided on the edge of at least one of the fourth and fifth surface portions of an external electrode, recessed from the edge toward the first surface portion, and both side portions of the recess in the third direction form covering portions that cover the ridges of the two surfaces in the second direction of the component body.
[0006] However, in the multilayer ceramic electronic component disclosed in Patent Document 2, the area and shape of the coating covering the ridges of the two surfaces in the second direction of the component body may vary due to the formation position and thickness variation of the base conductor layer and the coating conductor layer provided thereon. Here, when mounting an LW-reversed type multilayer ceramic electronic component on a mounting board using solder, depending on the left-right difference in the area and shape of the coating, the wetting of the solder to the coating may change on each surface, and the tensile stress of the solder may be applied differently. This may deteriorate the self-alignment effect. As a result, the multilayer ceramic electronic component may be easily rotated or tilted, and the mountability may be reduced. Note that the distance between the lands of the board on which the LW-reversed type multilayer ceramic electronic component is mounted is short, so the self-alignment effect may deteriorate, and if the multilayer ceramic electronic component rotates significantly, one external electrode may be mounted so as to straddle lands of different polarities, which may cause a short circuit.
[0007] An object of the present invention is to provide an LW reversal type multilayer ceramic capacitor capable of suppressing the occurrence of short circuit defects. [Means for solving the problem]
[0008] The multilayer ceramic capacitor according to the present invention comprises a laminate having a plurality of laminated dielectric layers and a plurality of internal electrode layers laminated on the dielectric layers, the laminate having a first main surface and a second main surface opposing each other in a height direction, a first end face and a second end face opposing each other in a length direction perpendicular to the height direction, and a first side surface and a second side surface opposing each other in a width direction perpendicular to the height direction and the length direction, a first surface portion located on the first end face, a second surface portion located on a portion of the first main surface, and a third surface portion located on a portion of the second main surface. a first external electrode having at least one of a first end surface and a second end surface, a fourth surface portion located on a portion of the first side surface, and a fifth surface portion located on a portion of the second side surface, a sixth surface portion located on the second end surface, at least one of a seventh surface portion located on a portion of the first main surface and an eighth surface portion located on a portion of the second main surface, a ninth surface portion located on a portion of the first side surface, and a tenth surface portion located on a portion of the second side surface, where l is the length in the length direction connecting the first end face and the second end face of the body, w is the length in the width direction connecting the first side face and the second side face, and t is the length in the height direction connecting the first main face and the second main face, there is a dimensional relationship of w>l>t, and when the first external electrode has the second surface portion, the length in the width direction of the second surface portion is smaller than the length in the width direction of the first surface portion, and when the first external electrode has the third surface portion, the length in the width direction of the third surface portion is smaller than the length in the width direction of the first surface portion. When the second external electrode has the seventh surface portion, the width direction length of the seventh surface portion is smaller than the width direction length of the sixth surface portion; when the second external electrode has the eighth surface portion, the width direction length of the eighth surface portion is smaller than the width direction length of the sixth surface portion; the height direction length of the fourth surface portion and the fifth surface portion of the first external electrode is smaller than the height direction length of the first surface portion; and the height direction length of the ninth surface portion and the tenth surface portion of the second external electrode is smaller than the height direction length of the sixth surface portion. Effect of the Invention
[0009] According to the present invention, it is possible to provide an LW-reversed multilayer ceramic capacitor capable of suppressing the occurrence of short-circuit defects. [Brief description of the drawings]
[0010] [Figure 1] 1 is an external perspective view of a multilayer ceramic capacitor according to an embodiment; [Diagram 2] 2 is a view of the multilayer ceramic capacitor shown in FIG. 1, taken along the direction of arrow II when looking at a first side surface side. [Diagram 3] 3 is a view of the multilayer ceramic capacitor shown in FIG. 1, taken along the direction of arrow III when looking at a second side surface side. [Figure 4] 4 is a view of the multilayer ceramic capacitor shown in FIG. 2, looking at a first main surface side along the direction of arrow IV. [Diagram 5] 3 is a view of the multilayer ceramic capacitor shown in FIG. 2, looking at a second main surface side along the direction of arrow V. FIG. [Figure 6] 6 is a cross-sectional view taken along line VI-VI of the multilayer ceramic capacitor shown in FIG. [Figure 7] 7 is a cross-sectional view taken along line VII-VII of the multilayer ceramic capacitor shown in FIG. 6. [Figure 8A] 7 is a cross-sectional view taken along line VIIIA-VIIIA of the multilayer ceramic capacitor shown in FIG. 6, showing a first internal electrode layer. FIG. [Figure 8B] 8 is a cross-sectional view taken along line VIIIB-VIIIB of the multilayer ceramic capacitor shown in FIG. 6, showing a second internal electrode layer. FIG. [Figure 9] 9 is a cross-sectional view taken along line IX-IX of the multilayer ceramic capacitor shown in FIG. 4, showing a first side surface of the laminate. [Figure 10A] 7 is an enlarged view of a portion XA in FIG. 6, showing a cross section of a first external electrode. FIG. [Figure 10B] 7 is an enlarged view of a portion XB in FIG. 6, showing a cross section of a second external electrode. FIG. [Figure 11A]10B is a cross-sectional view showing a modified example of the layer structure of the external electrodes of the multilayer ceramic capacitor according to the embodiment, and corresponds to FIG. 10A. [Figure 11B] 10B is a cross-sectional view showing a modified example of the layer structure of the external electrodes of the multilayer ceramic capacitor according to the embodiment, and corresponds to FIG. 10B. [Figure 12] 3A to 3C are diagrams illustrating intermediate stages in the manufacturing process of the multilayer ceramic capacitor according to the embodiment. [Figure 13] 3A to 3C are diagrams illustrating intermediate stages in the manufacturing process of the multilayer ceramic capacitor according to the embodiment. [Figure 14] 3A to 3C are diagrams illustrating intermediate stages in the manufacturing process of the multilayer ceramic capacitor according to the embodiment. [Figure 15A] 1. FIG. 4 is an external perspective view showing a first modified example of the shape of the external electrodes of the multilayer ceramic capacitor according to the embodiment, and corresponds to FIG. [Figure 15B] 1. FIG. 4 is an external perspective view showing a second modified example of the shape of the external electrodes of the multilayer ceramic capacitor according to the embodiment, and corresponds to FIG. [Figure 15C] FIG. 11 is an external perspective view of the second modified example when viewed from a different angle. [Figure 15D] 15B is a perspective view showing a third modified example of the shape of the external electrodes of the multilayer ceramic capacitor according to the embodiment, and corresponds to FIG. 15B. FIG. [Figure 16A] FIG. 2 is an external perspective view of the multilayer ceramic capacitor of Comparative Example 1, and corresponds to FIG. [Figure 16B] FIG. 8B is a diagram showing a first internal electrode layer of the multilayer ceramic capacitor of the comparative example, and corresponds to FIG. 8A. [Figure 16C] FIG. 8C is a diagram showing a second internal electrode layer of the multilayer ceramic capacitor of the comparative example, and corresponds to FIG. 8B. [Figure 17A] 1. FIG. 4 is an external perspective view of the multilayer ceramic capacitor of Comparative Example 2, which corresponds to FIG. [Figure 17B] FIG. 8B is a diagram showing a first internal electrode layer of the multilayer ceramic capacitor of the comparative example, and corresponds to FIG. 8A. [Figure 17C] FIG. 8C is a diagram showing a second internal electrode layer of the multilayer ceramic capacitor of the comparative example, and corresponds to FIG. 8B. [Figure 18A] 11A and 11B are diagrams for explaining a method for evaluating mountability in an experimental example. [Figure 18B] 11A and 11B are diagrams for explaining a method for evaluating mountability in an experimental example. [Figure 18C] 11A and 11B are diagrams for explaining a method for evaluating mountability in an experimental example. [Figure 18D] 11A and 11B are diagrams for explaining a method for evaluating mountability in an experimental example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, a multilayer ceramic capacitor 1 according to an embodiment of the present disclosure will be described. FIG. 1 is an external perspective view of the multilayer ceramic capacitor 1 of the present embodiment. FIG. 2 is an arrow view of the multilayer ceramic capacitor 1 shown in FIG. 1 when the first side surface WS1 side is seen along the direction of the arrow II. FIG. 3 is an arrow view of the multilayer ceramic capacitor 1 shown in FIG. 1 when the second side surface WS2 side is seen along the direction of the arrow III. FIG. 4 is an arrow view of the multilayer ceramic capacitor 1 shown in FIG. 2 when the first main surface TS1 side is seen along the direction of the arrow IV. FIG. 5 is an arrow view of the multilayer ceramic capacitor 1 shown in FIG. 2 when the second main surface TS2 side is seen along the direction of the arrow V. FIG. 6 is a cross-sectional view of the multilayer ceramic capacitor 1 shown in FIG. 4 taken along the line VI-VI. FIG. 7 is a cross-sectional view of the multilayer ceramic capacitor 1 shown in FIG. 6 taken along the line VII-VII. FIG. 8A is a cross-sectional view of the multilayer ceramic capacitor 1 shown in FIG. 6 taken along the line VIIIA-VIIIA. FIG. 8B is a cross-sectional view of the multilayer ceramic capacitor 1 shown in FIG. 6 taken along the line VIIIB-VIIIB. Fig. 9 is a cross-sectional view taken along line IX-IX of the multilayer ceramic capacitor 1 shown in Fig. 4, showing a first side surface WS1 of the multilayer body 10. Fig. 10A is an enlarged view of portion XA in Fig. 6, showing a cross-section of the first external electrode 40A. Fig. 10B is an enlarged view of portion XB in Fig. 6, showing a cross-section of the second external electrode 40B.
[0012] The multilayer ceramic capacitor 1 includes a laminate 10 and external electrodes 40 .
[0013] 1 to 9 show an XYZ orthogonal coordinate system. The length direction L of the multilayer ceramic capacitor 1 and the laminate 10 corresponds to the Y direction. The width direction W of the multilayer ceramic capacitor 1 and the laminate 10 corresponds to the X direction. The height direction T of the multilayer ceramic capacitor 1 and the laminate 10 corresponds to the Z direction. Here, the cross section shown in FIG. 6 is also referred to as an LT cross section. The cross section shown in FIG. 7 is also referred to as a WT cross section. The cross sections shown in FIGS. 8A and 8B are also referred to as an LW cross section.
[0014] As shown in Figures 1 to 5, the laminate 10 includes a first main surface TS1 and a second main surface TS2 facing each other in a height direction T, a first end surface LS1 and a second end surface LS2 facing each other in a length direction L perpendicular to the height direction T, and a first side surface WS1 and a second side surface WS2 facing each other in a width direction W perpendicular to the height direction T and the length direction L.
[0015] The laminate 10 has a substantially rectangular parallelepiped shape. The corners and ridges of the laminate 10 are preferably rounded. The corners are portions where three faces of the laminate 10 intersect, and the ridges are portions where two faces of the laminate 10 intersect. Note that unevenness may be formed on a part or all of the surfaces constituting the laminate 10.
[0016] As shown in Figures 6 and 7, the laminate 10 has an inner layer portion 11, and a first main surface side outer layer portion 12 and a second main surface side outer layer portion 13 arranged to sandwich the inner layer portion 11 in the height direction T.
[0017] The inner layer portion 11 includes a plurality of dielectric layers 20 and a plurality of internal electrode layers 30. The inner layer portion 11 includes the internal electrode layer 30 located closest to the first main surface TS1 side to the internal electrode layer 30 located closest to the second main surface TS2 side in the height direction T. In the inner layer portion 11, the multiple internal electrode layers 30 are arranged facing each other with the dielectric layer 20 interposed therebetween. The inner layer portion 11 is a portion that generates electrostatic capacitance and essentially functions as a capacitor. The inner layer portion 11 is also called an effective layer portion.
[0018] The plurality of dielectric layers 20 are made of a dielectric material. The dielectric material is, for example, a ceramic material. The dielectric material may be, for example, a dielectric ceramic containing a component such as BaTiO3, CaTiO3, SrTiO3, or CaZrO3. When these components are the main components, subcomponents such as Mn compounds, Fe compounds, Cr compounds, Co compounds, and Ni compounds may be added in smaller amounts than the main components depending on the desired properties of the laminate.
[0019] The thickness of the dielectric layer 20 is preferably 0.5 μm or more and 10 μm or less. The number of laminated dielectric layers 20 is preferably 15 to 700. The number of dielectric layers 20 is the total number of the dielectric layers in the inner layer portion 11 and the dielectric layers in the first main surface side outer layer portion 12 and the second main surface side outer layer portion 13.
[0020] The multiple internal electrode layers 30 include multiple first internal electrode layers 31 and multiple second internal electrode layers 32. The first internal electrode layers 31 are disposed on the multiple dielectric layers 20 and are extended to a first end face LS1. The second internal electrode layers 32 are disposed on the multiple dielectric layers 20 and are extended to a second end face LS2. The multiple first internal electrode layers 31 and the multiple second internal electrode layers 32 are alternately disposed in the height direction T of the laminate 10 with the dielectric layer 20 interposed therebetween. The first internal electrode layers 31 and the second internal electrode layers 32 are disposed so as to sandwich the dielectric layer 20 therebetween.
[0021] As shown in FIG. 8A, the first internal electrode layer 31 has a first opposing electrode portion 31A facing the second internal electrode layer 32, and a first extension portion 31B extended from the first opposing electrode portion 31A to a first end face LS1, a portion of the first side face WS1, and a portion of the second side face WS2.
[0022] The first counter electrode portion 31A is located inside the laminate 10. The first extension portion 31B is connected to the first counter electrode portion 31A and is exposed at the first end face LS1, a portion of the first side face WS1, and a portion of the second side face WS2.
[0023] As shown in FIG. 8B, the second internal electrode layer 32 has a second opposing electrode portion 32A facing the first internal electrode layer 31, and a second extension portion 32B extended from the second opposing electrode portion 32A to the second end face LS2, a portion of the first side face WS1, and a portion of the second side face WS2.
[0024] The second counter electrode portion 32A is located inside the laminate 10. The second extension portion 32B is connected to the second counter electrode portion 32A and is exposed at the second end face LS2, a portion of the first side face WS1, and a portion of the second side face WS2.
[0025] Fig. 9 is a cross-sectional view taken along line IX-IX of the multilayer ceramic capacitor 1 shown in Fig. 4, showing a first side surface WS1 of the laminate 10. Note that line IX-IX indicating the position of the cross-sectional view of Fig. 9 is also shown in Fig. 8A and Fig. 8B. As shown in Fig. 9, the first lead portion 31B of the first internal electrode layer 31 and the second lead portion 32B of the second internal electrode layer 32 are exposed on the first side surface WS1 of the laminate 10.
[0026] Also, although not shown in the figure, similar to the first side surface WS1 side, the first extension portion 31B of the first internal electrode layer 31 and the second extension portion 32B of the second internal electrode layer 32 are exposed on the second side surface WS2 side.
[0027] This makes it possible to shorten the distance between the first lead portion 31B of the first internal electrode layer 31 and the second lead portion 32B of the second internal electrode layer 32, thereby shortening the path through which the current flows, thereby reducing the ESL.
[0028] In this embodiment, the first opposing electrode portion 31A and the second opposing electrode portion 32A face each other via the dielectric layer 20, forming a capacitance and exhibiting the characteristics of a capacitor.
[0029] The shapes of the first counter electrode portion 31A and the second counter electrode portion 32A are not particularly limited, but are preferably rectangular. However, the corners of the rectangular shape may be rounded or obliquely formed.
[0030] The shapes of first drawer section 31B and second drawer section 32B are not particularly limited, but are preferably rectangular. However, the corners of the rectangular shape may be rounded or obliquely formed.
[0031] The dimension in the width direction W of the first lead portion 31B is larger than the dimension in the width direction of the first counter electrode portion 31A. The dimension in the width direction W of the second lead portion 32B is larger than the dimension in the width direction of the second counter electrode portion 32A.
[0032] The dimension in the length direction L of the portions of the first lead portion 31B and the second lead portion 32B exposed on the first side surface WS1 is preferably 20 μm or more and 280 μm or less. The dimension in the length direction L of the portions of the first lead portion 31B and the second lead portion 32B exposed on the second side surface WS2 is preferably 20 μm or more and 280 μm or less.
[0033] The first internal electrode layers 31 may all have the same shape, or some of them may have different shapes. For example, the first internal electrode layers 31 arranged near the center in the height direction T among the first internal electrode layers 31 may have a shape as shown in FIG. 8A and be exposed to the first side surface WS1 and the second side surface WS2, while some of the first internal electrode layers 31 arranged near the first main surface side outer layer portion 12 and the second main surface side outer layer portion 13 may not be exposed to the first side surface WS1 and the second side surface WS2. For example, the internal electrode layers may have a shape as shown in FIG. 16B described later.
[0034] The second internal electrode layers 32 may all have the same shape, or may have some different shapes. For example, the second internal electrode layers 32 arranged near the center in the height direction T among the second internal electrode layers 32 may have a shape as shown in FIG. 8B and be exposed to the first side surface WS1 and the second side surface WS2, while some of the second internal electrode layers 32 arranged near the first main surface side outer layer portion 12 and the second main surface side outer layer portion 13 may not be exposed to the first side surface WS1 and the second side surface WS2. For example, the internal electrode layers may have a shape as shown in FIG. 16C described later.
[0035] This allows adjustment of the range in the height direction T (see t1 in FIG. 9) formed by the plurality of first lead portions 31B exposed on a portion of the first side surface WS1 and the range in the height direction T formed by the plurality of first lead portions 31B exposed on a portion of the second side surface WS2. Also, it allows adjustment of the range in the height direction T (see t1 in FIG. 9) formed by the plurality of second lead portions 32B exposed on a portion of the first side surface WS1 and the range in the height direction T formed by the plurality of second lead portions 32B exposed on a portion of the second side surface WS2. As a result, it allows adjustment of the length T1 in the height direction T of each of the fourth surface portion 40A4 and the fifth surface portion 40A5 of the first external electrode 40A described later and the length T1 in the height direction T of the ninth surface portion 40B4 and the tenth surface portion 40B5 of the second external electrode 40B.
[0036] The first internal electrode layer 31 and the second internal electrode layer 32 are made of an appropriate conductive material such as a metal such as Ni, Cu, Ag, Pd, Au, or an alloy containing at least one of these metals. When an alloy is used, the first internal electrode layer 31 and the second internal electrode layer 32 may be made of, for example, an Ag-Pd alloy.
[0037] The thickness of each of the first internal electrode layers 31 and the second internal electrode layers 32 is preferably, for example, about 0.2 μm or more and 2.0 μm or less. The total number of the first internal electrode layers 31 and the second internal electrode layers 32 is preferably 15 or more and 200 or less.
[0038] The first main surface side outer layer portion 12 is located on the first main surface TS1 side of the laminate 10. The first main surface side outer layer portion 12 is an assembly of a plurality of dielectric layers 20 located between the first main surface TS1 and the internal electrode layer 30 closest to the first main surface TS1. That is, the first main surface side outer layer portion 12 is formed of a plurality of dielectric layers 20 located between the first main surface TS1 and the internal electrode layer 30 located closest to the first main surface TS1 side among the plurality of internal electrode layers 30. The dielectric layer 20 used in the first main surface side outer layer portion 12 may be the same as the dielectric layer 20 used in the internal layer portion 11.
[0039] The second main surface side outer layer portion 13 is located on the second main surface TS2 side of the laminate 10. The second main surface side outer layer portion 13 is an assembly of a plurality of dielectric layers 20 located between the second main surface TS2 and the internal electrode layer 30 closest to the second main surface TS2. That is, the second main surface side outer layer portion 13 is formed of a plurality of dielectric layers 20 located between the second main surface TS2 and the internal electrode layer 30 located closest to the second main surface TS2 side among the plurality of internal electrode layers 30. The dielectric layer 20 used in the second main surface side outer layer portion 13 may be the same as the dielectric layer 20 used in the internal layer portion 11.
[0040] As described above, the laminate 10 has a plurality of laminated dielectric layers 20 and a plurality of internal electrode layers 30 laminated on the dielectric layers 20. In other words, the multilayer ceramic capacitor 1 has the laminate 10 in which the dielectric layers 20 and the internal electrode layers 30 are alternately laminated.
[0041] The laminate 10 has a counter electrode portion 11E. The counter electrode portion 11E is a portion where the first counter electrode portion 31A of the first internal electrode layer 31 and the second counter electrode portion 32A of the second internal electrode layer 32 face each other. The counter electrode portion 11E is configured as a part of the inner layer portion 11. FIGS. 8A and 8B show the range of the width direction W and length direction L of the counter electrode portion 11E. The counter electrode portion 11E is also called a capacitor effective portion.
[0042] The laminate 10 has an end surface side outer layer portion. The end surface side outer layer portion has a first end surface side outer layer portion LG1 located on the first end surface LS1 side and a second end surface side outer layer portion LG2 located on the second end surface LS2 side. The first end surface side outer layer portion LG1 is a portion including the dielectric layer 20 and the first lead portion 31B located between the counter electrode portion 11E and the first end surface LS1. That is, the first end surface side outer layer portion LG1 is an aggregate of the portions of the multiple dielectric layers 20 on the first end surface LS1 side and the multiple first lead portions 31B. The second end surface side outer layer portion LG2 is a portion including the dielectric layer 20 and the second lead portion 32B located between the counter electrode portion 11E and the second end surface LS2. That is, the second end face side outer layer portion LG2 is an aggregate of the portions of the multiple dielectric layers 20 on the second end face LS2 side and the multiple second lead portions 32B. Figures 6, 8A, and 8B show the ranges in the length direction L of the first end face side outer layer portion LG1 and the second end face side outer layer portion LG2. The first end face side outer layer portion LG1 and the second end face side outer layer portion LG2 are also called L gaps or end gaps.
[0043] The laminate 10 has a side surface outer layer portion. The side surface outer layer portion has a first side surface outer layer portion WG1 located on the first side surface WS1 side and a second side surface outer layer portion WG2 located on the second side surface WS2 side. The first side surface outer layer portion WG1 is a portion including the dielectric layer 20 located between the counter electrode portion 11E and the first side surface WS1. That is, the first side surface outer layer portion WG1 is an aggregate of the portions of the multiple dielectric layers 20 on the first side surface WS1 side. The second side surface outer layer portion WG2 is a portion including the dielectric layer 20 located between the counter electrode portion 11E and the second side surface WS2. That is, the second side surface outer layer portion WG2 is an aggregate of the portions of the multiple dielectric layers 20 on the second side surface WS2 side. In FIG. 7, FIG. 8A, and FIG. 8B, the ranges in the width direction W of the first side surface outer layer portion WG1 and the second side surface outer layer portion WG2 are shown. The first side surface outer layer portion WG1 and the second side surface outer layer portion WG2 are also called W gaps or side gaps.
[0044] 6 to 8B, when the length in the length direction L connecting the first end face LS1 and the second end face LS2 of the laminate 10 is l, the length in the width direction W connecting the first side face WS1 and the second side face WS2 is w, and the length in the height direction T connecting the first main face TS1 and the second main face TS2 is t, the dimensional relationship between them is w>l>t. This makes it possible to increase the width of the drawn-out portion at the end face of the internal electrode layer 30. In addition, since the distance between the first external electrode 40A and the second external electrode 40B described later can be shortened, the ESL of the multilayer ceramic capacitor 1 can be reduced.
[0045] The length l in the length direction L connecting the first end surface LS1 and the second end surface LS2 of the laminate 10 is preferably 0.05 mm or more and 0.7 mm or less. The length w in the width direction W connecting the first side surface WS1 and the second side surface WS2 of the laminate 10 is preferably 0.15 mm or more and 1.5 mm or less. The length t in the height direction T connecting the first main surface TS1 and the second main surface TS2 of the laminate 10 is preferably 150 μm or less. This allows high-density mounting. The length t in the height direction T connecting the first main surface TS1 and the second main surface TS2 of the laminate 10 is preferably 100 μm or less, more preferably 50 μm or less. This allows higher-density mounting.
[0046] The dimensions l, w, and t of the laminate 10 are measured by the following method.
[0047] First, the dimension w of the laminate 10 is measured. Specifically, the dimension w of the laminate 10 is measured with a micrometer at the center position in the length direction L of the laminate ceramic capacitor 1, that is, at a position L / 2 of the laminate ceramic capacitor 1.
[0048] Next, the l dimension and the t dimension of the laminate 10 are measured. First, the same laminate ceramic capacitor 1 as the laminate ceramic capacitor 1 whose w dimension was measured is polished to the center position in the width direction W of the laminate ceramic capacitor 1, that is, to the position W / 2 of the laminate ceramic capacitor 1, so as to be parallel to the LT plane. Then, the LT cross section exposed by polishing is observed with a microscope. The l dimension of the laminate 10 is measured with a microscope at the center position in the height direction T of the laminate 10 in the LT cross section, that is, at the position t / 2 of the laminate 10. The t dimension of the laminate 10 is measured with a microscope at the center position in the length direction L of the laminate 10 in the LT cross section, that is, at the position l / 2 of the laminate 10.
[0049] The external electrode 40 has a first external electrode 40A arranged on the first end face LS1 side, and a second external electrode 40B arranged on the second end face LS2 side.
[0050] The first external electrode 40A is connected to the first internal electrode layer 31. The first external electrode 40A of this embodiment has a first surface portion 40A1 located on the first end face LS1, a second surface portion 40A2 located on a portion of the first main surface TS1, a third surface portion 40A3 located on a portion of the second main surface TS2, a fourth surface portion 40A4 located on a portion of the first side surface WS1, and a fifth surface portion 40A5 located on a portion of the second side surface WS2. It is preferable that the first external electrode 40A has at least one of the second surface portion 40A2 located on a portion of the first main surface TS1 and the third surface portion 40A3 located on a portion of the second main surface TS2, the first surface portion 40A1 located on the first end face LS1, the fourth surface portion 40A4 located on a portion of the first side surface WS1, and the fifth surface portion 40A5 located on a portion of the second side surface WS2.
[0051] The first surface portion 40A1 covers the entire first end face LS1 and is a portion that is connected to the first internal electrode layer 31. Either the second surface portion 40A2 or the third surface portion 40A3 is a portion that is connected to a land of a mounting board.
[0052] The fourth surface portion 40A4 is a portion connected to the first lead portion 31B exposed on the first side surface WS1. The fifth surface portion 40A5 is a portion connected to the first lead portion 31B exposed on the second side surface WS2.
[0053] The second external electrode 40B is connected to the second internal electrode layer 32. The second external electrode 40B of this embodiment has a sixth surface portion 40B1 located on the second end face LS2, a seventh surface portion 40B2 located on a portion of the first main surface TS1, an eighth surface portion 40B3 located on a portion of the second main surface TS2, a ninth surface portion 40B4 located on a portion of the first side surface WS1, and a tenth surface portion 40B5 located on a portion of the second side surface WS2. In addition, it is preferable that the second external electrode 40B has at least one of a seventh surface portion 40B2 located on a portion of the first main surface TS1 and an eighth surface portion 40B3 located on a portion of the second main surface TS2, a sixth surface portion 40B1 located on the second end face LS2, a ninth surface portion 40B4 located on a portion of the first side surface WS1, and a tenth surface portion 40B5 located on a portion of the second side surface WS2.
[0054] The sixth surface portion 40B1 covers the entire second end face LS2 and is a portion that is connected to the second internal electrode layer 32. Either the seventh surface portion 40B2 or the eighth surface portion 40B3 is a portion that is connected to a land of the mounting board.
[0055] The ninth surface portion 40B4 is a portion connected to the second lead portion 32B exposed on the first side surface WS1. The tenth surface portion 40B5 is a portion connected to the second lead portion 32B exposed on the second side surface WS2.
[0056] The length W1 of the second surface portion 40A2 and the third surface portion 40A3 of the first external electrode 40A in the width direction W is smaller than the length W2 of the first surface portion 40A1 in the width direction W. In other words, at both ends of the second surface portion 40A2 and the third surface portion 40A3 of the first external electrode 40A in the width direction W, there are portions where the surface of the laminate 10 is exposed without the external electrodes being formed. In addition, it is preferable that the length W1 of the second surface portion 40A2 and the third surface portion 40A3 of the first external electrode 40A in the width direction W is smaller than the w dimension of the width direction W of the laminate 10. As a result, when the multilayer ceramic capacitor 1 is mounted on the mounting board with solder, the solder is likely to wet the center portion where the second surface portion 40A2 and the third surface portion 40A3 are located, rather than the entire surface of the first surface portion 40A1 of the first external electrode 40A. Therefore, the multilayer ceramic capacitor 1 can be solder-bonded with the center portion in the width direction W as the center, so that the mountability of the multilayer ceramic capacitor 1 can be stabilized. Even if the multilayer ceramic capacitor 1 is rotated significantly on the land, the length W1 of the width direction W of the second surface portion 40A2 and the third surface portion 40A3 of the first external electrode 40A is smaller than the dimension w of the width direction W of the laminate 10, so that it is possible to prevent the multilayer ceramic capacitor 1 from being mounted across lands of different polarity. As a result, it is possible to prevent the occurrence of short circuits.
[0057] The length W1 in the width direction W of each of the second surface portion 40A2 and the third surface portion 40A3 of the first external electrode 40A is preferably, for example, 80% or more and 95% or less of the dimension w in the width direction W of the laminate 10. This can make the effects of the present disclosure more pronounced.
[0058] Furthermore, the length L1 in the length direction L of each of the second surface portion 40A2 and the third surface portion 40A3 of the first external electrode 40A is preferably 20% to 40% of the dimension l in the length direction L of the laminate 10. This not only improves the stability of mounting on the mounting board, but also prevents the multilayer ceramic capacitor 1 from being mounted across lands of different polarity even if the multilayer ceramic capacitor 1 rotates significantly on the land, because the length W1 in the width direction W of the second surface portion 40A2 and the third surface portion 40A3 of the first external electrode 40A is smaller than the dimension w in the width direction W of the laminate 10. As a result, the occurrence of short circuit defects can be prevented.
[0059] The length W1 in the width direction W of the seventh surface portion 40B2 and the eighth surface portion 40B3 of the second external electrode 40B is smaller than the length W2 in the width direction W of the sixth surface portion 40B1. In other words, at both ends of the seventh surface portion 40B2 and the eighth surface portion 40B3 of the second external electrode 40B in the width direction W, there are portions where the surface of the laminate 10 is exposed without the external electrodes being formed. In addition, the length W1 in the width direction W of the seventh surface portion 40B2 and the eighth surface portion 40B3 of the second external electrode 40B is preferably smaller than the w dimension in the width direction W of the laminate 10. As a result, when the multilayer ceramic capacitor 1 is mounted on the mounting board with solder, the solder is likely to wet the center portion where the seventh surface portion 40B2 and the eighth surface portion 40B3 are located, rather than the entire surface of the sixth surface portion 40B1 of the second external electrode 40B. Therefore, the multilayer ceramic capacitor 1 can be solder-bonded with the center portion in the width direction W as the center, and the mountability of the multilayer ceramic capacitor 1 can be stabilized. Even if the multilayer ceramic capacitor 1 is rotated significantly on the land, the length W1 in the width direction W of the seventh surface portion 40B2 and the eighth surface portion 40B3 of the second external electrode 40B is smaller than the dimension w in the width direction W of the laminate 10, so that it is possible to prevent the multilayer ceramic capacitor 1 from being mounted across lands of different polarity. As a result, it is possible to prevent the occurrence of short circuits.
[0060] The length W1 in the width direction W of each of the seventh surface portion 40B2 and the eighth surface portion 40B3 of the second external electrode 40B is preferably, for example, 80% or more and 95% or less of the dimension w in the width direction W of the laminate 10. This can make the effects of the present disclosure more pronounced.
[0061] Furthermore, the length L1 in the length direction L of each of the seventh surface portion 40B2 and the eighth surface portion 40B3 of the second external electrode 40B is preferably 20% to 40% of the dimension l in the length direction L of the laminate 10. This not only improves the stability of mounting on the mounting board, but also prevents the laminated ceramic capacitor 1 from being mounted across lands of different polarity even if the laminated ceramic capacitor 1 rotates significantly on the land, because the length W1 in the width direction W of the seventh surface portion 40B2 and the eighth surface portion 40B3 of the second external electrode 40B is smaller than the dimension w in the width direction W of the laminate 10. As a result, it is possible to prevent the occurrence of short circuit defects.
[0062] The length T1 in the height direction T of the fourth surface portion 40A4 and the fifth surface portion 40A5 of the first external electrode 40A is smaller than the length T2 in the height direction T of the first surface portion 40A1. In other words, at both ends of the height direction T of the fourth surface portion 40A4 and the fifth surface portion 40A5 of the first external electrode 40A, there are portions where the external electrodes are not formed and the surface of the laminate 10 is exposed. In addition, it is preferable that the length T1 in the height direction T of the fourth surface portion 40A4 and the fifth surface portion 40A5 of the first external electrode 40A is smaller than the dimension t in the height direction T of the laminate 10. This suppresses the wetting of the solder onto the first side surface WS1 and the second side surface WS2 (the fourth surface portion 40A4 and the fifth surface portion 40A5 of the first external electrode 40A) of the laminate 10, so that the stress applied in the rotation direction can be suppressed. Therefore, the self-alignment effect is improved, and the mountability of the multilayer ceramic capacitor 1 is stabilized. As a result, the occurrence of short-circuit defects can be prevented.
[0063] The length T1 in the height direction T of each of the fourth surface portion 40A4 and the fifth surface portion 40A5 of the first external electrode 40A is, for example, preferably 40% or more and 80% or less of the dimension t in the height direction T of the laminate 10. More preferably, it is 60% or more and 80% or less.
[0064] The length L2 of each of the fourth surface portion 40A4 and the fifth surface portion 40A5 of the first external electrode 40A in the longitudinal direction L is, for example, preferably 4% to 40% of the dimension l in the longitudinal direction L of the laminate 10. More preferably, it is 10% to 20%.
[0065] The length T1 in the height direction T of the ninth surface portion 40B4 and the tenth surface portion 40B5 of the second external electrode 40B is smaller than the length T2 in the height direction T of the sixth surface portion 40B1. In other words, at both ends of the ninth surface portion 40B4 and the tenth surface portion 40B5 of the second external electrode 40B in the height direction T, there are portions where the surface of the laminate 10 is exposed without the external electrodes being formed. In addition, the length T1 in the height direction T of the ninth surface portion 40B4 and the tenth surface portion 40B5 of the second external electrode 40B is preferably smaller than the t dimension in the height direction T of the laminate 10. This suppresses the wetting of the solder onto the first side surface WS1 and the second side surface WS2 (the ninth surface portion 40B4 and the tenth surface portion 40B5 of the second external electrode 40B) of the laminate 10, thereby suppressing the stress applied in the rotation direction. Therefore, the self-alignment effect is improved, and the mountability of the multilayer ceramic capacitor 1 is stabilized. As a result, the occurrence of short circuit defects can be prevented.
[0066] The length T1 in the height direction T of each of the ninth surface portion 40B4 and the tenth surface portion 40B5 of the second external electrode 40B is, for example, preferably 40% or more and 80% or less of the dimension t in the height direction T of the laminate 10. More preferably, it is 60% or more and 80% or less.
[0067] The length L2 of each of the ninth surface portion 40B4 and the tenth surface portion 40B5 of the second external electrode 40B in the longitudinal direction L is, for example, preferably 4% to 40% of the dimension l in the longitudinal direction L of the laminate 10. More preferably, it is 10% to 20%.
[0068] The shapes of the second surface portion 40A2, the third surface portion 40A3, the seventh surface portion 40B2 and the eighth surface portion 40B3 are not particularly limited, but are preferably rectangular.
[0069] The shapes of the fourth face portion 40A4, the fifth face portion 40A5, the ninth face portion 40B4 and the tenth face portion 40B5 are not particularly limited, but are preferably rectangular.
[0070] The length W2 in the width direction W of the first surface portion 40A1 of the first external electrode 40A and the length T2 in the height direction T of the first surface portion 40A1 of the first external electrode 40A are measured using a microscope. Specifically, the length W2 in the width direction W of the first surface portion 40A1 of the first external electrode 40A is measured at a position half the height direction T of the multilayer ceramic capacitor 1, and the length T2 in the height direction T of the first surface portion 40A1 of the first external electrode 40A is measured at a position half the width direction W of the multilayer ceramic capacitor 1.
[0071] The length W1 in the width direction W of the second surface portion 40A2 and the third surface portion 40A3 of the first external electrode 40A and the length L1 in the length direction L of the second surface portion 40A2 and the third surface portion 40A3 of the first external electrode 40A are measured using a microscope. Specifically, the length W1 in the width direction W of the second surface portion 40A2 and the third surface portion 40A3 of the first external electrode 40A is measured at a position that is 1 / 2 of the length L1 in the length direction L of the second surface portion 40A2 and the third surface portion 40A3 of the first external electrode 40A, and the length L1 in the length direction L of the second surface portion 40A2 and the third surface portion 40A3 of the first external electrode 40A is measured at a position that is 1 / 2 of the width direction W of the multilayer ceramic capacitor 1.
[0072] The length T1 in the height direction T of the fourth surface portion 40A4 and the fifth surface portion 40A5 of the first external electrode 40A and the length L2 in the length direction L of the fourth surface portion 40A4 and the fifth surface portion 40A5 of the first external electrode 40A are measured using a microscope. Specifically, the length T1 in the height direction T of the fourth surface portion 40A4 and the fifth surface portion 40A5 of the first external electrode 40A is measured at a position that is 1 / 2 of the length L2 in the length direction L of the fourth surface portion 40A4 and the fifth surface portion 40A5 of the first external electrode 40A, and the length L2 in the length direction L of the fourth surface portion 40A4 and the fifth surface portion 40A5 of the first external electrode 40A is measured at a position that is 1 / 2 of the length T1 in the height direction T of the fourth surface portion 40A4 and the fifth surface portion 40A5 of the first external electrode 40A.
[0073] The length W2 in the width direction W of the sixth surface portion 40B1 of the second external electrode 40B and the length T2 in the height direction T of the sixth surface portion 40B1 of the second external electrode 40B are measured using a microscope. Specifically, the length W2 in the width direction W of the sixth surface portion 40B1 of the second external electrode 40B is measured at a position half the length of the height direction T of the multilayer ceramic capacitor 1, and the length T2 in the height direction T of the sixth surface portion 40B1 of the second external electrode 40B is measured at a position half the length of the width direction W of the multilayer ceramic capacitor 1.
[0074] The length W1 in the width direction W of the seventh surface portion 40B2 and the eighth surface portion 40B3 of the second external electrode 40B and the length L1 in the length direction L of the seventh surface portion 40B2 and the eighth surface portion 40B3 of the second external electrode 40B are measured using a microscope. Specifically, the length W1 in the width direction W of the seventh surface portion 40B2 and the eighth surface portion 40B3 of the second external electrode 40B is measured at a position that is 1 / 2 of the length L1 in the length direction L of the seventh surface portion 40B2 and the eighth surface portion 40B3 of the second external electrode 40B, and the length L1 in the length direction L of the seventh surface portion 40B2 and the eighth surface portion 40B3 of the second external electrode 40B is measured at a position that is 1 / 2 of the width direction W of the multilayer ceramic capacitor 1.
[0075] The length T1 in the height direction T of the ninth surface portion 40B4 and the tenth surface portion 40B5 of the second external electrode 40B and the length L2 in the length direction L of the ninth surface portion 40B4 and the tenth surface portion 40B5 of the second external electrode 40B are measured using a microscope. Specifically, the length T1 in the height direction T of the ninth surface portion 40B4 and the tenth surface portion 40B5 of the second external electrode 40B is measured at a position that is 1 / 2 the length T1 in the length direction L of the ninth surface portion 40B4 and the tenth surface portion 40B5 of the second external electrode 40B, and the length L2 in the length direction L of the ninth surface portion 40B4 and the tenth surface portion 40B5 of the second external electrode 40B is measured at a position that is 1 / 2 the length T1 in the height direction T of the ninth surface portion 40B4 and the tenth surface portion 40B5 of the second external electrode 40B.
[0076] 10A, the first external electrode 40A has a first base electrode layer 50A and a first plating layer 60A disposed on the first base electrode layer 50A. The first base electrode layer 50A is disposed on the surface of the laminate 10. The first plating layer 60A is disposed so as to cover the first base electrode layer 50A.
[0077] 10B, the second external electrode 40B has a second base electrode layer 50B and a second plating layer 60B disposed on the second base electrode layer 50B. The second base electrode layer 50B is disposed on the surface of the laminate 10. The second plating layer 60B is disposed so as to cover the second base electrode layer 50B.
[0078] The first base electrode layer 50A and the second base electrode layer 50B include at least one selected from a baked layer, a thin film layer, and the like.
[0079] In this embodiment, the first base electrode layer 50A and the second base electrode layer 50B are thin film layers. The thin film layers are layers on which metal particles are deposited.
[0080] When the first base electrode layer 50A and the second base electrode layer 50B are formed as thin film layers, they are preferably formed by a thin film formation method such as a sputtering method or a vapor deposition method. Here, a sputtered electrode formed by a sputtering method will be described.
[0081] In this embodiment, the first base electrode layer 50A is composed of a first thin film layer 51A formed by a sputtered electrode. The second base electrode layer 50B is composed of a second thin film layer 51B formed by a sputtered electrode. When forming the base electrode layer by a sputtered electrode, it is preferable to form the sputtered electrode directly on the first main surface TS1 and the second main surface TS2 of the laminate 10.
[0082] As shown in Figures 6 and 10A, the first thin film layer 51A formed of a sputtered electrode is disposed on a part of the first main surface TS1 on the first end face LS1 side and on a part of the second main surface TS2 on the first end face LS1 side. Specifically, the first thin film layer 51A is preferably disposed on a part of the first main surface TS1 that is covered by the first external electrode 40A shown in Figure 4. The first thin film layer 51A is preferably disposed on a part of the second main surface TS2 that is covered by the first external electrode 40A shown in Figure 5.
[0083] Furthermore, the first thin film layer 51A is preferably disposed on a part of the first main surface TS1, and is preferably disposed continuously from a part of the first main surface TS1 so as to wrap slightly around a part of the first end surface LS1. The first thin film layer 51A is preferably disposed on a part of the second main surface TS2, and is preferably disposed continuously from a part of the second main surface TS2 so as to wrap slightly around a part of the first end surface LS1.
[0084] For example, as shown in Fig. 12 used in the description of the manufacturing process described later, when a chamfered portion C such as a rounded portion is formed on the ridge line portion of the laminate 10, the first thin film layer 51A is preferably disposed on a part of the first end face LS1 side of the first main surface TS1 and on the chamfered portion C on the first end face LS1 side that is continuous with that part. The first thin film layer 51A is preferably disposed on a part of the second main surface TS2 on the first end face LS1 side and on the chamfered portion C on the first end face LS1 side that is continuous with that part. This makes it easy to form the thin film layer by a sputtering method or the like.
[0085] By the above method, when forming a plating layer, it is possible to control the distance between the first thin film layer 51A arranged on a part of the first end face LS1 and the internal electrode layer 30 exposed on the first end face LS1. Therefore, it becomes easy to deposit a plating layer even on the surface of the laminate 10 between the first thin film layer 51A arranged on a part of the first end face LS1 and the internal electrode layer 30 exposed on the first end face LS1.
[0086] As shown in Figures 6 and 10B, the second thin film layer 51B formed of a sputtered electrode is disposed on a portion of the first main surface TS1 on the second end face LS2 side and on a portion of the second main surface TS2 on the second end face LS2 side. Specifically, the second thin film layer 51B is preferably disposed on a portion of the first main surface TS1 that is covered by the second external electrode 40B shown in Figure 4. The second thin film layer 51B is preferably disposed on a portion of the second main surface TS2 that is covered by the second external electrode 40B shown in Figure 5.
[0087] Furthermore, the second thin film layer 51B is preferably disposed on a part of the first main surface TS1 and a part of the first main surface TS1 that is continuous with the second end surface LS2. The second thin film layer 51B is preferably disposed on a part of the second main surface TS2 and a part of the second main surface TS2 that is continuous with the second end surface LS2.
[0088] For example, as shown in Fig. 12 used in the description of the manufacturing process described later, when a chamfered portion C such as a rounded portion is formed on the ridge line portion of the laminate 10, the second thin film layer 51B is preferably disposed on a part of the first main surface TS1 on the second end face LS2 side and on the chamfered portion C on the second end face LS2 side that is continuous with that part, as shown in Fig. 12 used in the description of the manufacturing process described later. The second thin film layer 51B is preferably disposed on a part of the second main surface TS2 on the second end face LS2 side and on the chamfered portion C on the second end face LS2 side that is continuous with that part, as shown in Fig. 12 used in the description of the manufacturing process described later. This makes it easy to form the thin film layer by a sputtering method or the like.
[0089] By the above method, when forming a plating layer, it is possible to control the distance between the second thin film layer 51B arranged on a part of the second end face LS2 and the internal electrode layer 30 exposed on the second end face LS2. Therefore, it becomes easy to deposit a plating layer even on the surface of the laminate 10 between the second thin film layer 51B arranged on a part of the second end face LS2 and the internal electrode layer 30 exposed on the second end face LS2.
[0090] The thin film layer formed by the sputtered electrode preferably contains at least one metal selected from the group consisting of Mg, Al, Ti, W, Cr, Cu, Ni, Ag, Co, Mo, and V. This can increase the adhesive strength of the external electrode 40 to the laminate 10. The thin film layer may be a single layer or may be formed of multiple layers. For example, it may be formed of a two-layer structure consisting of a layer of Ni-Cr alloy and a layer of Ni-Cu alloy.
[0091] The thickness of the sputtered electrode in the lamination direction connecting the first main surface TS1 and the second main surface TS2 is preferably 50 nm or more and 400 nm or less, and more preferably 50 nm or more and 130 nm or less.
[0092] When forming a base electrode layer by forming a sputtered electrode directly on the first main surface TS1 and the second main surface TS2 of the laminate 10, it is preferable to form a base electrode layer of a baked layer on the first end face LS1 and the second end face LS2, or to directly form a plating layer described later without forming a base electrode layer. In this embodiment, a plating layer described later is directly formed on the first end face LS1 and the second end face LS2 without forming a base electrode layer.
[0093] As described later in a modified example, the first base electrode layer 50A and the second base electrode layer 50B may be baked layers. The baked layer preferably contains a metal component and either a glass component or a ceramic component, or both. The metal component includes at least one selected from, for example, Cu, Ni, Ag, Pd, Ag-Pd alloy, Au, etc. The glass component includes at least one selected from, for example, B, Si, Ba, Mg, Al, Li, etc. The ceramic component may be the same type of ceramic material as the dielectric layer 20, or a different type of ceramic material. The ceramic component includes at least one selected from, for example, BaTiO3, CaTiO3, (Ba,Ca)TiO3, SrTiO3, CaZrO3, etc.
[0094] The baked layer is, for example, a conductive paste containing glass and metal applied to the laminate 10 and baked. The baked layer may be a laminated chip having an internal electrode layer and a dielectric layer and a conductive paste applied to the laminated chip, which are simultaneously baked, or a laminated chip having an internal electrode layer and a dielectric layer is baked to obtain the laminate 10, and then a conductive paste is applied to the laminate 10 and baked. In the case where a laminated chip having an internal electrode layer and a dielectric layer and a conductive paste applied to the laminated chip are simultaneously baked, it is preferable to form the baked layer by baking a material to which a ceramic material is added instead of a glass component. In this case, it is particularly preferable to use the same type of ceramic material as the dielectric layer 20 as the ceramic material to be added. The baked layer may be a multi-layered layer.
[0095] Alternatively, a configuration may be adopted in which a first plating layer 60A and a second plating layer 60B, which will be described later, are disposed directly on the laminate 10 without providing the first base electrode layer 50A and the second base electrode layer 50B.
[0096] The first plating layer 60A is disposed so as to cover the first base electrode layer 50A.
[0097] The second plating layer 60B is disposed so as to cover the second base electrode layer 50B.
[0098] The first plating layer 60A and the second plating layer 60B may contain, for example, at least one selected from Cu, Ni, Sn, Ag, Pd, an Ag-Pd alloy, Au, etc. The first plating layer 60A and the second plating layer 60B may each be formed of a plurality of layers.
[0099] When the base electrode layer is formed of a thin film layer, the plating layer is preferably formed in a three-layer structure of a Cu plating layer as a lower plating layer, a Ni plating layer as a middle plating layer, and a Sn plating layer as an upper plating layer. That is, the first plating layer 60A preferably has a first Cu plating layer 61A, a first Ni plating layer 62A, and a first Sn plating layer 63A. The second plating layer 60B preferably has a second Cu plating layer 61B, a second Ni plating layer 62B, and a second Sn plating layer 63B. However, the first plating layer 60A and the second plating layer 60B are not limited to a three-layer structure and may have other layer configurations.
[0100] The first Cu plating layer 61A is disposed so as to cover the first end face LS1 of the laminate 10 and the first thin film layer 51A as the first base electrode layer 50A disposed on the first main surface TS1 and the second main surface TS2 of the laminate 10. In this embodiment, the first Cu plating layer 61A is further disposed so as to cover the portions where the internal electrode layer 30 is exposed on the first side surface WS1 and the second side surface WS2 of the laminate 10. At this time, the gap between the first thin film layer 51A and the internal electrode layer 30 exposed on the first end face LS1 of the laminate 10 and the gap between the multiple internal electrode layers 30 exposed on the surface of the laminate 10 are narrowly formed, so that the plating layer is also deposited in the regions of these gaps.
[0101] The first Ni plating layer 62A is disposed so as to cover the first Cu plating layer 61 A. The first Sn plating layer 63A is disposed so as to cover the first Ni plating layer 62A. In this embodiment, the first plating layer 60A is directly electrically connected to the first internal electrode layer 31.
[0102] The second Cu plating layer 61B is disposed so as to cover the second end face LS2 of the laminate 10 and the second thin film layer 51B as the second base electrode layer 50B disposed on the first main surface TS1 and the second main surface TS2 of the laminate 10. In this embodiment, the second Cu plating layer 61B is further disposed so as to cover the portions where the internal electrode layer 30 is exposed on the first side surface WS1 and the second side surface WS2 of the laminate 10. At this time, the gap between the second thin film layer 51B and the internal electrode layer 30 exposed on the second end face LS2 of the laminate 10 and the gap between the multiple internal electrode layers 30 exposed on the surface of the laminate 10 are narrowly formed, so that the plating layer is also deposited in the regions of these gaps.
[0103] The second Ni plating layer 62B is disposed so as to cover the second Cu plating layer 61 B. The second Sn plating layer 63B is disposed so as to cover the second Ni plating layer 62B. In this embodiment, the second plating layer 60B is directly electrically connected to the second internal electrode layer 32.
[0104] By providing a plating layer consisting of a Cu plating layer and a Ni plating layer so as to cover the base electrode layer, the base electrode layer is prevented from being eroded by solder when mounting the multilayer ceramic capacitor 1. Furthermore, by further providing an Sn plating layer on the surface of the Ni plating layer, the wettability of the solder when mounting the multilayer ceramic capacitor 1 is improved. This allows the multilayer ceramic capacitor 1 to be easily mounted.
[0105] The thickness of each plating layer is preferably 2 μm or more and 15 μm or less. That is, the average thickness of each of the first Cu plating layer 61A, the first Ni plating layer 62A, the first Sn plating layer 63A, the second Cu plating layer 61B, the second Ni plating layer 62B, and the second Sn plating layer 63B is preferably 2 μm or more and 15 μm or less. More specifically, the average thickness of each of the first Cu plating layer 61A and the second Cu plating layer 61B is more preferably 5 μm or more and 8 μm or less. Also, the average thickness of each of the first Ni plating layer 62A, the first Sn plating layer 63A, the second Ni plating layer 62B, and the second Sn plating layer 63B is more preferably 2 μm or more and 4 μm or less.
[0106] In addition, when the dimension in the length direction connecting the first end face LS1 and the second end face LS2 of the multilayer ceramic capacitor 1 including the laminate 10 and the external electrode 40 is defined as the L dimension, the L dimension is preferably 0.1 mm or more and 0.8 mm or less. In addition, when the dimension in the width direction connecting the first side face WS1 and the second side face WS2 of the multilayer ceramic capacitor 1 is defined as the W dimension, the W dimension is preferably 0.2 mm or more and 1.6 mm or less. In addition, when the dimension in the height direction connecting the first main face TS1 and the second main face TS2 of the multilayer ceramic capacitor 1 is defined as the T dimension, the T dimension is preferably 0.05 mm or more and 0.2 mm or less. The L dimension in the length direction of the multilayer ceramic capacitor 1 of this embodiment is smaller than the W dimension in the width direction of the multilayer ceramic capacitor 1. In addition, in this embodiment, the height direction connecting the first main face TS1 and the second main face TS2 of the multilayer ceramic capacitor 1 is the lamination direction of the dielectric layer 20 and the internal electrode layer 30.
[0107] According to this embodiment, it is possible to suppress the wetting up of the solder on the first side surface WS1 and the second side surface WS2 of the laminate 10 (the fourth surface portion 40A4, the fifth surface portion 40A5, the ninth surface portion 40B4, and the tenth surface portion 40B5 of the external electrode 40). This is because, at the ridges of the first side surface WS1 and the second side surface WS2 of the laminate 10, the external electrodes are not formed, and there are portions where the surface of the laminate 10 is exposed. By suppressing the wetting up of the solder on the first side surface WS1 and the second side surface WS2 of the laminate 10 (the fourth surface portion 40A4, the fifth surface portion 40A5, the ninth surface portion 40B4, and the tenth surface portion 40B5 of the external electrode 40), it is possible to suppress the stress applied in the rotation direction. Therefore, the self-alignment effect is improved, and the mountability of the multilayer ceramic capacitor 1 is stabilized. As a result, it is possible to prevent the occurrence of short-circuit defects and the like. The self-alignment effect is an effect in which, during soldering, a force that reduces the surface area of molten solder, i.e., surface tension, acts on the molten solder, causing the electronic element to move and be positioned as the object of mounting, supported by the molten solder. This self-alignment effect makes it possible to prevent misalignment during mounting.
[0108] Modified examples of the layer structure of the external electrode 40 of the multilayer ceramic capacitor 1 of this embodiment will be described below. In the following description, the same components as those in the above embodiment will be given the same reference numerals, and detailed description will be omitted. Figures 11A and 11B are cross-sectional views showing modified examples of the layer structure of the external electrode 40 of the multilayer ceramic capacitor 1 of this embodiment, and correspond to Figures 10A and 10B.
[0109] In this modification, the configuration of the external electrode 40 is different from that of the above embodiment.
[0110] The first external electrode 40A has a first base electrode layer 50A and a first plating layer 60A. The first base electrode layer 50A of this modification is composed of a first baked layer 52A. The first plating layer 60A of this modification has a first Ni plating layer 62A and a first Sn plating layer 63A.
[0111] The second external electrode 40B has a second base electrode layer 50B and a second plating layer 60B. The second base electrode layer 50B of this modification is composed of a second baked layer 52B. The second plating layer 60B of this modification has a second Ni plating layer 62B and a second Sn plating layer 63B.
[0112] In this modification, the first base electrode layer 50A has, for example, a first surface portion located on the first end face LS1, a second surface portion located on a portion of the first main surface TS1, a third surface portion located on a portion of the second main surface TS2, a fourth surface portion located on a portion of the first side surface WS1, and a fifth surface portion located on a portion of the second side surface WS2, similar to the above-mentioned first external electrode 40A. In this modification, the first base electrode layer 50A is connected to the first internal electrode layer 31.
[0113] The first Ni plating layer 62A is disposed so as to cover the first base electrode layer 50 A. The first Sn plating layer 63A is disposed so as to cover the first Ni plating layer 62A.
[0114] In this modification, the second base electrode layer 50B has, for example, a sixth surface portion located on the second end face LS2, a seventh surface portion located on a portion of the first main surface TS1, an eighth surface portion located on a portion of the second main surface TS2, a ninth surface portion located on a portion of the first side surface WS1, and a tenth surface portion located on a portion of the second side surface WS2, similar to the above-mentioned second external electrode 40B. In this modification, the second base electrode layer 50B is connected to the second internal electrode layer 32.
[0115] The second Ni plating layer 62B is disposed so as to cover the second base electrode layer 50B. The second Sn plating layer 63B is disposed so as to cover the second Ni plating layer 62B.
[0116] The first baked layer 52A constituting the first base electrode layer 50A and the second baked layer 52B constituting the second base electrode layer 50B may be, for example, a conductive paste containing glass and metal applied to the laminate and baked. When the laminated chip before firing and the conductive paste applied to the laminated chip are fired simultaneously, it is preferable to form the baked layer by baking a layer to which a ceramic material is added instead of the glass component. In this case, it is particularly preferable to use the same type of ceramic material as the dielectric layer 20 as the ceramic material to be added.
[0117] When the base electrode layer is formed as a baked layer, the first plating layer 60A and the second plating layer 60B preferably have a two-layer structure in which a Sn plating layer is formed on a Ni plating layer. In this case, the Ni plating layer prevents the base electrode layer from being eroded by solder when mounting the multilayer ceramic capacitor 1. In addition, the Sn plating layer improves the wettability of the solder when mounting the multilayer ceramic capacitor 1. This makes it easier to mount the multilayer ceramic capacitor 1.
[0118] The first plating layer 60A and the second plating layer 60B are not limited to a two-layer structure, and may be formed as a three-layer structure including Cu plating as in the above embodiment, or may have other layer configurations.
[0119] The thickness of each plating layer is preferably 2 μm or more and 15 μm or less. That is, the average thickness of each of the first Ni plating layer 62A, the first Sn plating layer 63A, the second Ni plating layer 62B, and the second Sn plating layer 63B is preferably 2 μm or more and 15 μm or less. More specifically, the average thickness of each of the first Ni plating layer 62A, the first Sn plating layer 63A, the second Ni plating layer 62B, and the second Sn plating layer 63B is more preferably 2 μm or more and 4 μm or less.
[0120] Next, a method for manufacturing the multilayer ceramic capacitor 1 of this embodiment will be described.
[0121] A dielectric sheet for the dielectric layer 20 and a conductive paste for the internal electrode layer 30 are prepared. The conductive paste for the dielectric sheet and the internal electrode includes a binder and a solvent. The binder and the solvent may be known. The paste made of a conductive material is, for example, a metal powder to which an organic binder and an organic solvent are added.
[0122] A conductive paste for the internal electrode layer 30 is printed on the dielectric sheet by, for example, screen printing or gravure printing using a printing plate patterned to have the shape of the internal electrode layer 30 of this embodiment. This prepares a dielectric sheet on which the pattern of the first internal electrode layer 31 is formed and a dielectric sheet on which the pattern of the second internal electrode layer 32 is formed.
[0123] A predetermined number of dielectric sheets on which the pattern of the internal electrode layer is not printed are stacked to form a portion that will become the first main surface side outer layer portion 12 on the first main surface TS1 side. A dielectric sheet on which the pattern of the first internal electrode layer 31 is printed and a dielectric sheet on which the pattern of the second internal electrode layer 32 is printed are alternately stacked on top of the dielectric sheet to form a portion that will become the internal layer portion 11. A predetermined number of dielectric sheets on which the pattern of the internal electrode layer is not printed are stacked on top of the portion that will become the internal layer portion 11 to form a portion that will become the second main surface side outer layer portion 13 on the second main surface TS2 side. In this way, a laminated sheet is produced.
[0124] The laminated sheets are pressed in the lamination direction by means of a hydrostatic press or the like to produce a laminated block.
[0125] The laminated block is cut to a predetermined size to obtain laminated chips. At this time, corners and edges of the laminated chips may be rounded by barrel polishing or the like.
[0126] The laminated chip is fired to produce the laminate 10. The firing temperature depends on the materials of the dielectric layers 20 and the internal electrode layers 30, but is preferably 900° C. or higher and 1400° C. or lower.
[0127] In this embodiment, the base electrode layer is formed of a thin film layer. When forming the base electrode layer of a thin film layer, a thin film layer is formed on the portion of the laminate 10 where the external electrode is to be formed by performing masking or the like. The thin film layer is formed by a thin film formation method such as a sputtering method or a vapor deposition method. In this embodiment, a sputtered electrode is formed as a thin film layer by a sputtering method.
[0128] 12 to 14 are diagrams showing intermediate states in the manufacturing process of the multilayer ceramic capacitor of this embodiment, showing a state after a thin film layer is arranged on the laminate 10 and before a plating layer is arranged. FIG. 12 is a diagram showing a state in which a first thin film layer 51A and a second thin film layer 51B are arranged as thin film layers on the laminate 10, and is a diagram corresponding to the LT cross section of FIG. 6. FIG. 13 is a diagram showing a state in which a first thin film layer 51A is arranged as a thin film layer on the laminate 10, and is a diagram corresponding to the WT cross section of FIG. 7. FIG. 14 is a diagram showing a state in which a first thin film layer 51A and a second thin film layer 51B are arranged on the laminate 10, and is a diagram showing the surface of a first side surface WS1 of the laminate 10, corresponding to FIG. 9.
[0129] The first thin film layer 51A formed of a sputtered electrode is disposed on a part of the first main surface TS1 on the first end face LS1 side and a part of the second main surface TS2 on the first end face LS1 side. The second thin film layer 51B formed of a sputtered electrode is disposed on a part of the first main surface TS1 on the second end face LS2 side and a part of the second main surface TS2 on the second end face LS2 side.
[0130] In this embodiment, the thin film layer formed by the sputtered electrode is disposed on a part of the first main surface TS1 and a part of the second main surface TS2, and is disposed so as to be continuous from a part of the first main surface TS1 and a part of the second main surface TS2 and slightly wrap around a part of the first end surface LS1 and a part of the second end surface LS2. This makes it possible to control the distance between the thin film layer disposed by wrapping around a part of the first end surface LS1 and a part of the second end surface LS2 and the internal electrode layer exposed on the first end surface LS1 and the second end surface LS2. Therefore, it becomes possible to deposit a plating layer on the surface of the laminate 10 between the thin film layer disposed by wrapping around a part of the first end surface LS1 and a part of the second end surface LS2 and the internal electrode layer exposed on the first end surface LS1 and the second end surface LS2.
[0131] Then, a plating layer is formed on the surface of the laminate and the base electrode layer made of the thin film layer. In this embodiment, three plating layers are formed, namely, a Cu plating layer, a Ni plating layer, and a Sn plating layer.
[0132] The plating layer is formed by electrolytic plating, preferably barrel plating.
[0133] The plating layer is arranged so as to cover the exposed portions of the internal electrode layers on the first end face LS1 and the second end face LS2 of the laminate 10. The plating layer is arranged so as to cover the exposed portions of the internal electrode layers on the first side face WS1 and the second side face WS2 of the laminate 10. At this time, by narrowing the gaps between the thin film layer and the internal electrode layers exposed on the surface of the laminate 10 and the gaps between the multiple internal electrode layers exposed on the surface of the laminate 10, the plating layer is also deposited in the regions of these gaps.
[0134] In addition, when it is difficult to control the formation of the plating layer, the plating layer may be formed by masking the portions where the surface of the laminate 10 is to be exposed. This makes it easier to form a plating layer in a desired shape.
[0135] In addition, when the base electrode layer is formed by a baked layer, a conductive paste to be the first base electrode layer is applied to a first surface portion located on the first end face LS1 of the laminate 10, a second surface portion located on a part of the first main surface TS1, a third surface portion located on a part of the second main surface TS2, a fourth surface portion located on a part of the first side surface WS1, and a fifth surface portion located on a part of the second side surface WS2 on the first end face LS1 side of the laminate 10. In addition, a conductive paste to be the second base electrode layer is applied to a sixth surface portion located on the second end face LS2 of the laminate 10, a seventh surface portion located on a part of the first main surface TS1, an eighth surface portion located on a part of the second main surface TS2, a ninth surface portion located on a part of the first side surface WS1, and a tenth surface portion located on a part of the second side surface WS2 on the second end face LS2 side of the laminate 10.
[0136] In addition, the portions where the base electrode layer is not to be formed are masked in advance. After the masking, a conductive paste containing a glass component and a metal is applied to the laminate 10 by a method such as dipping or screen printing. Then, a baking process is performed to form the base electrode layer. The temperature of the baking process at this time is preferably 700°C or more and 900°C or less.
[0137] In addition, when the laminated chip before firing and the conductive paste applied to the laminated chip are fired at the same time, it is preferable to form the fired layer by firing a material to which a ceramic material is added instead of a glass component. In this case, it is particularly preferable to use the same type of ceramic material as that of the dielectric layer 20 as the ceramic material to be added. In this case, the conductive paste is applied to the laminated chip before firing, and the laminated chip and the conductive paste applied to the laminated chip are fired at the same time to form the laminate 10 with the fired layer.
[0138] Thereafter, a plating layer is formed on the surface of the base electrode layer made of the baked layer and the laminate 10. When the base electrode layer is formed of a baked layer, for example, two plating layers, a Ni plating layer and a Sn plating layer, are formed as the plating layer. The plating layer is formed by an electrolytic plating method. As the plating method, barrel plating is preferably used.
[0139] In addition, when it is difficult to control the formation of the plating layer, the plating layer may be formed by masking the portions where the surface of the laminate 10 is to be exposed. This makes it easier to form a plating layer in a desired shape.
[0140] Through these manufacturing steps, the multilayer ceramic capacitor 1 is manufactured.
[0141] The configuration of the external electrodes 40 is not limited to the above configuration. A first modified example of the shape of the external electrodes 40 of the multilayer ceramic capacitor 1 of this embodiment will be described below. In the following description, the same components as those in the above embodiment are given the same reference numerals, and detailed description will be omitted. Fig. 15A is a cross-sectional view showing a first modified example of the shape of the external electrodes 40 of the multilayer ceramic capacitor 1 of this embodiment, and corresponds to Fig. 1.
[0142] In this modification, the shape of the external electrode 40 is different from that of the above embodiment. In this modification, the first external electrode 40A and the second external electrode 40B are disposed on only one of the first principal surface TS1 or the second principal surface TS2.
[0143] For example, the first external electrode 40A of this modification has a first surface 40A1 located on the first end face LS1, a third surface 40A3 located on a portion of the second main surface TS2, a fourth surface 40A4 located on a portion of the first side surface WS1, and a fifth surface 40A5 located on a portion of the second side surface WS2. In other words, the first external electrode 40A of this modification is not formed on the first main surface TS1.
[0144] For example, the second external electrode 40B of this modification has a sixth surface 40B1 located on the second end face LS2, an eighth surface 40B3 located on a portion of the second main surface TS2, a ninth surface 40B4 located on a portion of the first side surface WS1, and a tenth surface 40B5 located on a portion of the second side surface WS2. In other words, the second external electrode 40B of this modification is not formed on the first main surface TS1.
[0145] In this modification, the length W1 in the width direction W of the third surface portion 40A3 of the first external electrode 40A is smaller than the length W2 in the width direction W of the first surface portion 40A1. The length W1 in the width direction W of the third surface portion 40A3 of the first external electrode 40A is smaller than the dimension w in the width direction W of the laminate 10. The length W1 in the width direction W of the eighth surface portion 40B3 of the second external electrode 40B is smaller than the length W2 in the width direction W of the sixth surface portion 40B1. The length W1 in the width direction W of the eighth surface portion 40B3 of the second external electrode 40B is smaller than the dimension w in the width direction W of the laminate 10.
[0146] This configuration also suppresses the deterioration of the self-alignment effect and allows stable mounting. Furthermore, by not arranging the first external electrode 40A and the second external electrode 40B on either the first main surface TS1 or the second main surface TS2, the dimension of the multilayer ceramic capacitor 1 in the height direction T can be reduced, and the multilayer ceramic capacitor 1 can be made even lower in height. Furthermore, by not arranging the first external electrode 40A and the second external electrode 40B on either the first main surface TS1 or the second main surface TS2, the height dimension of the laminate 10 can be secured by the thickness of the external electrode 40. This makes it possible to increase the volume of the effective layer portion of the laminate 10, and to increase the capacitance of the multilayer ceramic capacitor 1.
[0147] The configuration of the external electrode 40 is not limited to the above configuration. A second modified example of the shape of the external electrode 40 of the multilayer ceramic capacitor 1 of this embodiment will be described below. In the following description, the same configurations as those in the above embodiment are given the same reference numerals, and detailed description will be omitted. FIG. 15B is a cross-sectional view showing a second modified example of the shape of the external electrode 40 of the multilayer ceramic capacitor 1 of this embodiment, and corresponds to FIG. 1. FIG. 15C is an external perspective view of this modified example viewed from a different angle so that the first surface portion 40A1 of the first external electrode 40A can be seen.
[0148] In this modification, the shapes of the first surface portion 40A1 of the first external electrode 40A and the sixth surface portion 40B1 of the second external electrode 40B are different from those of the above embodiment.
[0149] The first surface portion 40A1 of this modified example has a first central portion 40A1A, a first extension portion 40A1B extending from the first central portion 40A1A to the first side surface WS1, and a second extension portion 40A1C extending from the first central portion 40A1A to the second side surface WS2.
[0150] The length W3 in the width direction W of the first central portion 40A1A may be smaller than the w dimension in the width direction W of the laminate 10 and may be equal to the length W1 in the width direction W of the second surface portion 40A2 and the third surface portion 40A3 of the first external electrode 40A.
[0151] In addition, the length T2 of the first central portion 40A1A in the height direction T is equal to the dimension t of the laminate 10 in the height direction T, and the first central portion 40A1A is continuously connected to the second surface portion 40A2 and the third surface portion 40A3.
[0152] The first extension 40A1B and the second extension 40A1C extend continuously from the first central portion 40A1A to the first side surface WS1 and the second side surface WS2, and the length T3 of the first extension 40A1B and the second extension 40A1C in the height direction T is smaller than the dimension t in the height direction T of the laminate 10. In other words, at both ends of the height direction T of the first extension 40A1B and the second extension 40A1C, there are portions where the surface of the laminate 10 is exposed without the external electrodes being formed. In this way, since there are portions where the surface of the laminate 10 is exposed, when the multilayer ceramic capacitor 1 is mounted on a mounting board by soldering, the solder is less likely to wet up the entire surface of the first end face LS1, and is more likely to wet up the central portion where the second surface portion 40A2 and the third surface portion 40A3 are located. Therefore, the multilayer ceramic capacitor 1 can be soldered with the central portion in the width direction W as the center, and the mountability of the multilayer ceramic capacitor 1 can be more stable.
[0153] The length T3 in the height direction T of the first extension portion 40A1B and the length T1 in the height direction T of the fourth surface portion 40A4 may be equal to each other, or one of them may be larger. The length T3 in the height direction T of the second extension portion 40A1C and the length T1 in the height direction T of the fifth surface portion 40A5 may be equal to each other, or one of them may be larger.
[0154] The sixth surface portion 40B1 of this modified example has a second central portion 40B1A, a third extension portion 40B1B extending from the second central portion 40B1A to the first side surface WS1, and a fourth extension portion 40B1C extending from the second central portion 40B1A to the second side surface WS2.
[0155] The length W3 in the width direction W of the second central portion 40B1A may be smaller than the w dimension in the width direction W of the laminate 10 and may be equal to the length W1 in the width direction W of the seventh surface portion 40B2 and the eighth surface portion 40B3 of the second external electrode 40B.
[0156] In addition, the length T2 of the second central portion 40B1A in the height direction T is equal to the dimension t of the laminate 10 in the height direction T, and the second central portion 40B1A is continuously connected to the seventh surface portion 40B2 and the eighth surface portion 40B3.
[0157] The third extension 40B1B and the fourth extension 40B1C extend continuously from the second central portion 40B1A to the first side surface WS1 and the second side surface WS2, and the length T3 of the third extension 40B1B and the fourth extension 40B1C in the height direction T is smaller than the dimension t in the height direction T of the laminate 10. In other words, at both ends of the height direction T of the third extension 40B1B and the fourth extension 40B1C, there are portions where the surface of the laminate 10 is exposed without forming external electrodes. In this way, since there are portions where the surface of the laminate 10 is exposed, when the multilayer ceramic capacitor 1 is mounted on a mounting board by soldering, the solder is less likely to wet up the entire surface of the second end face LS2, and is more likely to wet up the central portion where the seventh surface portion 40B2 and the eighth surface portion 40B3 are located. Therefore, the multilayer ceramic capacitor 1 can be soldered around the central portion in the width direction W, and the mountability of the multilayer ceramic capacitor 1 can be more stable.
[0158] The length T3 in the height direction T of the third extension portion 40B1B and the length T1 in the height direction T of the ninth surface portion 40B4 may be equal to each other, or one of them may be greater. The length T3 in the height direction T of the fourth extension portion 40B1C and the length T1 in the height direction T of the tenth surface portion 40B5 may be equal to each other, or one of them may be greater.
[0159] With this configuration as well, it is possible to suppress deterioration of the self-alignment effect and perform stable mounting.
[0160] The configuration of the external electrode 40 is not limited to the above configuration. A third modified example of the shape of the external electrode 40 of the multilayer ceramic capacitor 1 of this embodiment will be described below. In the following description, the same configurations as those in the second modified example are given the same reference numerals, and detailed description will be omitted. Fig. 15D is a cross-sectional view showing the third modified example of the shape of the external electrode 40 of the multilayer ceramic capacitor 1 of this embodiment, and corresponds to Fig. 15B.
[0161] In this modification, the shape of the external electrode 40 is different from that of the second modification. In this modification, the first external electrode 40A and the second external electrode 40B are disposed on only one of the first principal surface TS1 or the second principal surface TS2.
[0162] For example, the first external electrode 40A of this modification has a first surface 40A1 located on the first end face LS1, a third surface 40A3 located on a portion of the second main surface TS2, a fourth surface 40A4 located on a portion of the first side surface WS1, and a fifth surface 40A5 located on a portion of the second side surface WS2. In other words, the first external electrode 40A of this modification is not formed on the first main surface TS1.
[0163] For example, the second external electrode 40B of this modification has a sixth surface 40B1 located on the second end face LS2, an eighth surface 40B3 located on a portion of the second main surface TS2, a ninth surface 40B4 located on a portion of the first side surface WS1, and a tenth surface 40B5 located on a portion of the second side surface WS2. In other words, the second external electrode 40B of this modification is not formed on the first main surface TS1.
[0164] This configuration also makes it possible to suppress deterioration of the self-alignment effect and perform stable mounting, and also provides the same effects as the first and second modifications.
[0165] The multilayer ceramic capacitor 1 of this embodiment provides the following advantages.
[0166] (1) The multilayer ceramic capacitor 1 of this embodiment includes a laminate 10 having a plurality of laminated dielectric layers 20 and a plurality of internal electrode layers 30 laminated on the dielectric layers 20, the laminate 10 having a first main surface TS1 and a second main surface TS2 opposing each other in a height direction, a first end face LS1 and a second end face LS2 opposing each other in a length direction perpendicular to the height direction, and a first side surface WS1 and a second side surface WS2 opposing each other in a width direction perpendicular to the height direction and the length direction, a first surface portion 40A1 located on the first end face LS1, a second surface portion 40A2 located in a portion of the first main surface TS1, and a second main surface TS a first external electrode 40A having at least one of a third surface portion 40A3 located in a portion on S2, a fourth surface portion 40A4 located in a portion on the first side surface WS1, and a fifth surface portion 40A5 located in a portion on the second side surface WS2, a sixth surface portion 40B1 located on the second end face LS2, at least one of a seventh surface portion 40B2 located in a portion on the first main surface TS1 and an eighth surface portion 40B3 located in a portion on the second main surface TS2, a ninth surface portion 40B4 located in a portion on the first side surface WS1, and a tenth surface portion 40B5 located in a portion on the second side surface WS2. and a second external electrode 40B having a first end face LS1 and a second end face LS2 of the laminate 10, wherein, assuming that the length in the longitudinal direction connecting the first end face LS1 and the second end face LS2 of the laminate 10 is l, the length in the width direction connecting the first side face WS1 and the second side face WS2 is w, and the length in the height direction connecting the first main face TS1 and the second main face TS2 is t, the dimensional relationship is w>l>t, and when the first external electrode 40A has a second surface portion 40A2, the length W1 in the width direction of the second surface portion 40A2 is smaller than the length W2 in the width direction of the first surface portion 40A1, and when the first external electrode 40A has a third surface portion 40A3 when the second external electrode 40B has a seventh surface portion 40B2, the width direction length W1 of the seventh surface portion 40B2 is smaller than the width direction length W2 of the sixth surface portion 40B1; when the second external electrode 40B has an eighth surface portion 40B3, the width direction length W1 of the eighth surface portion 40B3 is smaller than the width direction length W2 of the sixth surface portion 40B1; and the height direction length T1 of the fourth surface portion 40A4 and the fifth surface portion 40A5 of the first external electrode 40A is smaller than the height direction length T2 of the first surface portion 40A1.The length T1 in the height direction of the ninth surface portion 40B4 and the tenth surface portion 40B5 of the second external electrode 40B is smaller than the length T2 in the height direction of the sixth surface portion 40B1. This makes it possible to provide an LW-reversed multilayer ceramic capacitor that can suppress the occurrence of short-circuit defects.
[0167] For example, the multilayer ceramic capacitor 1 of this embodiment includes a first external electrode 40A having a first surface portion 40A1 located on the first end face LS1, a second surface portion 40A2 located on a portion of the first main surface TS1, a third surface portion 40A3 located on a portion of the second main surface TS2, a fourth surface portion 40A4 located on a portion of the first side surface WS1, and a fifth surface portion 40A5 located on a portion of the second side surface WS2, a sixth surface portion 40B1 located on the second end face LS2, a seventh surface portion 40B2 located on a portion of the first main surface TS1, an eighth surface portion 40B3 located on a portion of the second main surface TS2, a ninth surface portion 40B4 located on a portion of the first side surface WS1, and a tenth surface portion 40B5 located on a portion of the second side surface WS2, and a second external electrode 40B having the same, wherein a widthwise length W1 of the second surface portion 40A2 and the third surface portion 40A3 of the first external electrode 40A is smaller than a widthwise length W2 of the first surface portion 40A1, a widthwise length W1 of the seventh surface portion 40B2 and the eighth surface portion 40B3 of the second external electrode 40B is smaller than a widthwise length W2 of the sixth surface portion 40B1, a heightwise length T1 of the fourth surface portion 40A4 and the fifth surface portion 40A5 of the first external electrode 40A is smaller than a heightwise length T2 of the first surface portion 40A1, and a heightwise length T1 of the ninth surface portion 40B4 and the tenth surface portion 40B5 of the second external electrode 40B is smaller than a heightwise length T2 of the sixth surface portion 40B1.
[0168] For example, the multilayer ceramic capacitor 1 of this embodiment includes a first external electrode 40A having a first surface portion 40A1 located on the first end face LS1, a third surface portion 40A3 located on a portion of the second main surface TS2, a fourth surface portion 40A4 located on a portion of the first side face WS1, and a fifth surface portion 40A5 located on a portion of the second side face WS2, a second external electrode 40B having a sixth surface portion 40B1 located on the second end face LS2, an eighth surface portion 40B3 located on a portion of the second main surface TS2, a ninth surface portion 40B4 located on a portion of the first side face WS1, and a tenth surface portion 40B5 located on a portion of the second side face WS2, a width direction length W1 of the third surface portion 40A3 of the first external electrode 40A is smaller than a width direction length W2 of the first surface portion 40A1, a width direction length W1 of the eighth surface portion 40B3 of the second external electrode 40B is smaller than a width direction length W2 of the sixth surface portion 40B1, a height direction length T1 of the fourth surface portion 40A4 and the fifth surface portion 40A5 of the first external electrode 40A is smaller than a height direction length T2 of the first surface portion 40A1, and a height direction length T1 of the ninth surface portion 40B4 and the tenth surface portion 40B5 of the second external electrode 40B is smaller than a height direction length T2 of the sixth surface portion 40B1.
[0169] (2) In the multilayer ceramic capacitor 1 of this embodiment, when the first external electrode 40A has the second surface portion 40A2, the length W1 in the width direction of the second surface portion 40A2 is smaller than the w dimension of the laminate 10; when the first external electrode 40A has the third surface portion 40A3, the length W1 in the width direction of the third surface portion 40A3 is smaller than the w dimension of the laminate 10; and when the second external electrode 40B has the seventh surface portion 40B2, the length W1 in the width direction of the seventh surface portion 40B2 is When the second external electrode 40B has an eighth surface portion 40B3, the width direction length W1 of the eighth surface portion 40B3 is smaller than the w dimension of the laminate 10, the height direction length T1 of the fourth surface portion 40A4 and the fifth surface portion 40A5 of the first external electrode 40A is smaller than the t dimension of the laminate 10, and the height direction length T1 of the ninth surface portion 40B4 and the tenth surface portion 40B5 of the second external electrode 40B is smaller than the t dimension of the laminate 10. This makes it possible to provide an LW-reversed multilayer ceramic capacitor that can suppress the occurrence of short circuits and perform stable mounting.
[0170] (3) In the multilayer ceramic capacitor 1 of this embodiment, when the first external electrode 40A has the second surface portion 40A2, the second surface portion 40A2 is rectangular, when the first external electrode 40A has the third surface portion 40A3, the third surface portion 40A3 is rectangular, when the second external electrode 40B has the seventh surface portion 40B2, the seventh surface portion 40B2 is rectangular, and when the second external electrode 40B has the eighth surface portion 40B3, the eighth surface portion 40B3 is rectangular. This makes it possible to provide an LW-reversed multilayer ceramic capacitor that can suppress the occurrence of short circuits and perform stable mounting.
[0171] (4) The length t in the height direction connecting the first main surface TS1 and the second main surface TS2 of the laminate 10 of the multilayer ceramic capacitor 1 of this embodiment is 150 μm or less. In such a low-profile multilayer ceramic capacitor, the effects of this embodiment can be appropriately obtained.
[0172] (5) The length t in the height direction connecting the first main surface TS1 and the second main surface TS2 of the laminate 10 of the multilayer ceramic capacitor 1 of this embodiment is 100 μm or less. In such a low-profile multilayer ceramic capacitor, the effects of this embodiment can be appropriately obtained.
[0173] (6) The length t in the height direction connecting the first main surface TS1 and the second main surface TS2 of the laminate 10 of the multilayer ceramic capacitor 1 of this embodiment is 50 μm or less. In such a low-profile multilayer ceramic capacitor, the effects of this embodiment can be appropriately obtained.
[0174] The internal electrode layer 30 has a first internal electrode layer 31 and a second internal electrode layer 32. The first internal electrode layer 31 has a first counter electrode portion 31A located inside the laminate and facing the second internal electrode layer 32, and a first lead portion 31B connected to the first counter electrode portion 31A and exposed to the first end face LS1, a part of the first side face WS1, and a part of the second side face WS2. The second internal electrode layer 32 has a second counter electrode portion 32A located inside the laminate and facing the first internal electrode layer 31, and a second lead portion 32B connected to the second counter electrode portion 32A and exposed to the second end face LS2, a part of the first side face WS1, and a part of the second side face WS2. This makes it possible to shorten the distance between the lead portion of the first internal electrode layer 31 and the lead portion of the second internal electrode layer 32, thereby shortening the path through which the current flows. This makes it possible to reduce the ESL.
[0175] (8) The first external electrode 40A of the multilayer ceramic capacitor 1 of this embodiment has a first base electrode layer 50A and a first plating layer 60A disposed on the first base electrode layer 50A, and the second external electrode 40B has a second base electrode layer 50B and a second plating layer 60B disposed on the second base electrode layer 50B, and the first base electrode layer 50A and the second base electrode layer 50B are sputtered electrodes. This makes it possible to form the external electrodes thin, and a structure is obtained that makes it easy to ensure the thickness of the laminate 10, thereby ensuring the capacitance and strength of the laminate 10.
[0176] <Experimental Example> As a sample of the experimental example, a multilayer ceramic capacitor was fabricated, and the mountability, capacitance, and thickness of the base electrode layer were evaluated.
[0177] First, as a sample of the example, a multilayer ceramic capacitor 1 having the following specifications and shown in Fig. 1 to Fig. 10B was fabricated according to the above-mentioned manufacturing method. As a sample of Comparative Example 1, a multilayer ceramic capacitor 101 having external electrodes 140 (first external electrode 140A, second external electrode 140B) with a normal structure as shown in Fig. 16A was fabricated. As a sample of Comparative Example 2, a multilayer ceramic capacitor 201 having external electrodes 240 (first external electrode 240A, second external electrode 240B) with recesses R recessed from the edges of the external electrodes toward the end faces of the laminate 10 as shown in Fig. 17A was fabricated.
[0178] FIG. 16A is an external perspective view of the multilayer ceramic capacitor 101 of Comparative Example 1, and corresponds to FIG. 1. FIG. 16B is a view showing the first internal electrode layer 131 of the multilayer ceramic capacitor 101 of Comparative Example 1, and corresponds to FIG. 8A. FIG. 16C is a view showing the second internal electrode layer 132 of the multilayer ceramic capacitor 101 of Comparative Example 1, and corresponds to FIG. 8B. FIG. 17A is an external perspective view of the multilayer ceramic capacitor 201 of Comparative Example 2, and corresponds to FIG. 1. FIG. 17B is a view showing the first internal electrode layer 231 of the multilayer ceramic capacitor 201 of Comparative Example 2, and corresponds to FIG. 8A. FIG. 17C is a view showing the second internal electrode layer 232 of the multilayer ceramic capacitor 201 of Comparative Example 2, and corresponds to FIG. 8B. Note that external electrodes are omitted in FIGS. 16B, 16C, 17B, and 17C.
[0179] (Configuration of the embodiment) ·Multilayer ceramic capacitor dimensions: L×W×T=0.520mm×1.000mm×0.100mm Laminate dimensions: L×W×T=0.500mm×0.980mm×0.070mm ·Ceramic material of dielectric layer: BaTiO3 Capacitance: 0.47μF Rated voltage: 4V Internal electrode layer material: Ni Internal electrode layer pattern: the pattern shown in Figures 8A and 8B External electrode structure: Underlying electrode layer: thin film layer (sputtered electrode) Material of the base electrode layer: Two-layer structure of NiCr layer and NiCu layer Thickness of the base electrode layer: principal surface thickness 0.2 μm (thickness of the base electrode layer disposed on each of the first principal surface TS1 and the second principal surface TS2) Plating layer: Three-layer structure of Cu plating, Ni plating, and Sn plating Cu plating thickness: 5.5μm Ni plating thickness: 2.5μm Sn plating thickness: 3.2μm The length W1 in the width direction W of each of the second surface portion 40A2 and the third surface portion 40A3 of the first external electrode 40A is 87% of the dimension w in the width direction W of the laminate 10 (the length W1 in the width direction W of the second surface portion 40A2 and the third surface portion 40A3: 0.85 mm, the dimension w of the laminate 10: 0.980 mm). The length L1 in the longitudinal direction L of each of the second surface portion 40A2 and the third surface portion 40A3 of the first external electrode 40A is 30% of the dimension l in the longitudinal direction L of the laminate 10 (the length L1 in the longitudinal direction L of the second surface portion 40A2 and the third surface portion 40A3: 0.15 mm, the dimension l of the laminate 10: 0.500 mm). The length W1 in the width direction W of each of the seventh surface portion 40B2 and the eighth surface portion 40B3 of the second external electrode 40B is 87% of the dimension w in the width direction W of the laminate 10 (the length W1 in the width direction W of the seventh surface portion 40B2 and the eighth surface portion 40B3: 0.85 mm, the dimension w of the laminate 10: 0.980 mm). The length L1 in the longitudinal direction L of each of the seventh surface portion 40B2 and the eighth surface portion 40B3 of the second external electrode 40B is 30% of the dimension l in the longitudinal direction L of the laminate 10 (the length L1 in the longitudinal direction L of the seventh surface portion 40B2 and the eighth surface portion 40B3: 0.15 mm, the dimension l of the laminate 10: 0.500 mm). The length T1 of each of the fourth surface portion 40A4 and the fifth surface portion 40A5 of the first external electrode 40A in the height direction T is 69% of the dimension t in the height direction T of the laminate 10 (the length T1 of the fourth surface portion 40A4 and the fifth surface portion 40A5 in the height direction T: 0.048 mm, the dimension t of the laminate 10: 0.070 mm). The length L2 of each of the fourth surface portion 40A4 and the fifth surface portion 40A5 of the first external electrode 40A in the longitudinal direction L is 20% of the dimension l of the longitudinal direction L of the laminate 10 (the length L2 of the fourth surface portion 40A4 and the fifth surface portion 40A5 in the longitudinal direction L: 0.1 mm, the dimension l of the laminate 10: 0.500 mm). The length T1 of each of the ninth surface portion 40B4 and the tenth surface portion 40B5 of the second external electrode 40B in the height direction T is 69% of the dimension t in the height direction T of the laminate 10 (the length T1 of the ninth surface portion 40B4 and the tenth surface portion 40B5 in the height direction T: 0.048 mm, the dimension t of the laminate 10: 0.070 mm). The length L2 of each of the ninth surface portion 40B4 and the tenth surface portion 40B5 of the second external electrode 40B in the longitudinal direction L is 20% of the dimension l of the longitudinal direction L of the laminate 10 (the length L2 of the ninth surface portion 40B4 and the tenth surface portion 40B5 in the longitudinal direction L: 0.1 mm, the dimension l of the laminate 10: 0.500 mm).
[0180] (Configuration of Comparative Example 1) ·Multilayer ceramic capacitor dimensions: L×W×T=0.520mm×1.000mm×0.100mm ·Ceramic material of dielectric layer: BaTiO3 Capacitance: 0.47μF Rated voltage: 4V Internal electrode layer material: Ni Internal electrode layer pattern: patterns shown in Figures 16B and 16C External electrode structure: Base electrode layer: A layer formed by applying and baking a conductive paste Material of the base electrode layer: Ni Thickness of the base electrode layer: end surface thickness 10 μm, side surface thickness 5 μm, main surface thickness 5 μm (thickness of the base electrode layer disposed on each of the first main surface TS1 and the second main surface TS2) Plating layer: Three-layer structure of Cu plating, Ni plating, and Sn plating Cu plating thickness: 5.5μm Ni plating thickness: 2.5μm Sn plating thickness: 3.2μm
[0181] (Configuration of Comparative Example 2) ·Multilayer ceramic capacitor dimensions: L×W×T=0.520mm×1.000mm×0.100mm ·Ceramic material of dielectric layer: BaTiO3 Capacitance: 0.47μF Rated voltage: 4V Internal electrode layer material: Ni Internal electrode layer pattern: patterns shown in Figures 17B and 17C External electrode structure: Underlying electrode layer: thin film layer (sputtered electrode) Material of the base electrode layer: Two layers: NiCr layer and NiCu layer Thickness of the base electrode layer: principal surface thickness 0.2 μm (thickness of the base electrode layer disposed on each of the first principal surface TS1 and the second principal surface TS2) Plating layer: Three-layer structure of Cu plating, Ni plating, and Sn plating Cu plating thickness: 5.5μm Ni plating thickness: 2.5μm Sn plating thickness: 3.2μm
[0182] Next, the fabricated samples were used to evaluate the mountability.
[0183] (Implementation evaluation) Mountability was evaluated using the sample of the embodiment and the samples of comparative examples 1 and 2. The evaluation was performed using 100 samples for each. Table 1 shows the results of the evaluation of mountability.
[0184] [Table 1]
[0185] In Comparative Example 1, one sample had a rotation failure. In Comparative Example 2, eight samples had a rotation failure. One of them had a large amount of rotation, and one external electrode was mounted so as to straddle lands of different polarity, causing a short circuit. In the sample of Comparative Example 2, the area and shape of the external electrodes covering the ridges of the first and second side portions of the laminate were varied due to variations in the formation position and thickness of the base electrode layer and the plating layer provided thereon, and this is likely to cause changes in the way the solder wets the external electrodes of the first and second side portions, resulting in a large difference in the amount of solder wetting up. As a result, it is presumed that the rotation failure occurred due to differences in the way the tensile stress of the solder was applied to the multilayer ceramic capacitor.
[0186] The evaluation methods used in this experimental example are as follows.
[0187] (Method of evaluating mounting) 18A to 18D are diagrams for explaining a method for evaluating mountability. First, solder (solder composition Sn-3.0Ag-0.5Cu) is printed on each of two lands 310A and 310B arranged on a glass epoxy substrate 300 shown in FIG. 18A. At this time, a solder amount with a thickness of 100 um is printed on each land. As shown in FIG. 18A, the length of the land in the width direction is 1.0 mm, the length of the land in the length direction is 0.3 mm, and the distance between the two lands is 0.2 mm.
[0188] Next, the multilayer ceramic capacitor is placed on the land to which the solder has been applied. At this time, as shown in Fig. 18B, a reference line is taken at the center of the land's width direction so as to be perpendicular to the width direction of the land, and the multilayer ceramic capacitor is placed so that the center of the width direction W of the multilayer ceramic capacitor is located at a position shifted by 0.1 mm in the width direction of the land from the reference line. At this time, the multilayer ceramic capacitor is placed so that the angle θ between the land and the multilayer ceramic capacitor shown in Fig. 18C, that is, the acute angle θ between one of the opposing inner sides of the two lands and the surface of the external electrode of the multilayer ceramic capacitor on the first end face LS1 side or the surface on the second end face LS2 side, is within 5°.
[0189] After that, the external electrodes of the multilayer ceramic capacitor are soldered to the lands by reflow soldering, and the multilayer ceramic capacitor is mounted on the board. After mounting, the mounted state of the multilayer ceramic capacitor is observed, and a case where the angle θ between the land and the multilayer ceramic capacitor is 5° or more is determined to be a rotation defect. Furthermore, as shown in Figure 18D, a case where the multilayer ceramic capacitor is rotated significantly and mounted so that the first external electrode or the second external electrode straddles two lands is determined to be a short circuit defect.
[0190] From the above results, the multilayer ceramic capacitor 1 of this embodiment can suppress the wetting up of the solder on the first side surface WS1 and the second side surface WS2 of the laminate 10, thereby suppressing the stress applied in the rotational direction of the multilayer ceramic capacitor 1. This improves the self-alignment effect, stabilizing the mountability of the multilayer ceramic capacitor 1. As a result, it is possible to prevent short-circuit defects and the like.
[0191] The present invention is not limited to the configurations of the above-mentioned embodiments, and can be appropriately modified and applied within the scope of the present invention. Note that the present invention also includes a combination of two or more of the individual desirable configurations described in the above-mentioned embodiments. [Explanation of symbols]
[0192] 1. Multilayer ceramic capacitors 10 Laminate 11 Inner Layer 12 First main surface side outer layer portion 13 Second main surface outer layer LS1 First end face LS2 Second end face WS1 First Aspect WS2 The Second Side TS1 First main surface TS2 Second main surface l Length in the longitudinal direction w Width direction t Height 20 Dielectric layer 30 Internal electrode layer 31 First internal electrode layer 31A First opposing electrode section 31B First drawer 32 Second internal electrode layer 32A Second opposing electrode part 32B Second drawer 40 External electrode 40A First outer electrode 40A1 First side 40A2 2nd side 40A3 Third side 40A4 4th side 40A5 5th side 40B Second external electrode 40B1 6th side 40B2 7th side 40B3 8th side 40B4 9th side 40B5 10th side 50A First Underlying Electrode Layer 51A First thin film layer 50B Second base electrode layer 51B Second thin film layer 60A First plating layer 60B Second plating layer L Length direction W Width direction T Lamination direction
Claims
1. a laminate having a plurality of laminated dielectric layers and a plurality of internal electrode layers laminated on the dielectric layers, the laminate having a first main surface and a second main surface opposing each other in a height direction, a first end face and a second end face opposing each other in a length direction perpendicular to the height direction, and a first side face and a second side face opposing each other in a width direction perpendicular to the height direction and the length direction; a first external electrode having a first surface portion located on the first end face, at least one of a second surface portion located on a portion of the first main surface and a third surface portion located on a portion of the second main surface, a fourth surface portion located on a portion of the first side surface, and a fifth surface portion located on a portion of the second side surface; a second external electrode having a sixth surface portion located on the second end face, at least one of a seventh surface portion located on a portion of the first main surface and an eighth surface portion located on a portion of the second main surface, a ninth surface portion located on a portion of the first side surface, and a tenth surface portion located on a portion of the second side surface, a length in the longitudinal direction connecting the first end surface and the second end surface of the laminate is l, a length in the width direction connecting the first side surface and the second side surface is w, and a length in the height direction connecting the first main surface and the second main surface is t, where w>l>t is a dimensional relationship between the length in the longitudinal direction connecting the first end surface and the second end surface of the laminate, the first external electrode has the second surface portion, and a length of the second surface portion in a width direction is smaller than a length of the first surface portion in a width direction; a length in a height direction of the fourth surface portion and the fifth surface portion of the first external electrode is smaller than a length in a height direction of the first surface portion, the second external electrode has the seventh surface portion, and a length of the seventh surface portion in a width direction is smaller than a length of the sixth surface portion in a width direction; the ninth surface portion and the tenth surface portion of the second external electrode have lengths in a height direction shorter than the length in a height direction of the sixth surface portion; On the first main surface, a surface of the laminate exposed from a region located between the second surface and the fourth surface.
2. The length in the width direction of the second surface portion is smaller than the w dimension of the laminate, The length of the seventh surface portion in the width direction is smaller than the w dimension of the laminate, a length in a height direction of the fourth surface portion and the fifth surface portion of the first external electrode is smaller than a t dimension of the laminate; 2. The multilayer ceramic capacitor according to claim 1, wherein the lengths of the ninth and tenth surface portions of the second external electrode in the height direction are smaller than the t dimension of the laminate.
3. The second surface portion has a rectangular shape, 3. The multilayer ceramic capacitor according to claim 1, wherein the seventh surface portion has a rectangular shape.
4. 4. The multilayer ceramic capacitor according to claim 1, wherein a length in a height direction connecting said first main surface and said second main surface of said laminate is 150 μm or less.
5. 4. The multilayer ceramic capacitor according to claim 1, wherein a length in a height direction connecting said first main surface and said second main surface of said laminate is 100 μm or less.
6. 4. The multilayer ceramic capacitor according to claim 1, wherein a length in a height direction connecting said first main surface and said second main surface of said laminate is 50 μm or less.
7. The internal electrode layer includes a first internal electrode layer and a second internal electrode layer, the first internal electrode layer is located inside the laminate and has a first opposing electrode portion facing the second internal electrode layer, and a first lead portion connected to the first opposing electrode portion and exposed to the first end face, a portion of the first side face, and a portion of the second side face; The multilayer ceramic capacitor according to any one of claims 1 to 6, wherein the second internal electrode layer has a second opposing electrode portion located inside the laminate and opposing the first internal electrode layer, and a second lead portion connected to the second opposing electrode portion and exposed to the second end face, a portion of the first side face, and a portion of the second side face.
8. the first external electrode has a first base electrode layer and a first plating layer disposed on the first base electrode layer; the second external electrode has a second base electrode layer and a second plating layer disposed on the second base electrode layer, 8. The multilayer ceramic capacitor according to claim 1, wherein the first and second underlying electrode layers are sputtered electrodes.
9. On the first aspect, 2. The multilayer ceramic capacitor according to claim 1, wherein a surface of the laminate is exposed from a region located between the second surface portion and the fourth surface portion.
10. A semiconductor device comprising a plurality of laminated dielectric layers and a plurality of internal electrode layers laminated on the dielectric layers, a first main surface and a second main surface facing each other in a height direction; a first end surface and a second end surface facing each other in a length direction perpendicular to the height direction; a laminate having a first side surface and a second side surface facing each other in a width direction perpendicular to the height direction and the length direction; a first external electrode having a first surface portion located on the first end face, at least one of a second surface portion located on a portion of the first main surface and a third surface portion located on a portion of the second main surface, a fourth surface portion located on a portion of the first side surface, and a fifth surface portion located on a portion of the second side surface; a second external electrode having a sixth surface portion located on the second end face, at least one of a seventh surface portion located on a portion of the first main surface and an eighth surface portion located on a portion of the second main surface, a ninth surface portion located on a portion of the first side surface, and a tenth surface portion located on a portion of the second side surface, a length in the longitudinal direction connecting the first end surface and the second end surface of the laminate is l, a length in the width direction connecting the first side surface and the second side surface is w, and a length in the height direction connecting the first main surface and the second main surface is t, where w>l>t is a dimensional relationship between the length in the longitudinal direction connecting the first end surface and the second end surface of the laminate, the first external electrode has the second surface portion, and a length of the second surface portion in a width direction is smaller than a length of the first surface portion in a width direction; a length in a height direction of the fourth surface portion and the fifth surface portion of the first external electrode is smaller than a length in a height direction of the first surface portion, the second external electrode has the seventh surface portion, and a length of the seventh surface portion in a width direction is smaller than a length of the sixth surface portion in a width direction; the ninth surface portion and the tenth surface portion of the second external electrode have lengths in a height direction shorter than the length in a height direction of the sixth surface portion; On the first aspect, a surface of the laminate exposed from a region located between the second surface and the fourth surface.
Citation Information
Patent Citations
Multilayer capacitor
JP2008300563A
Electronic component and substrate module
JP2012156471A
Multilayer ceramic capacitor
JP2019061997A
Multilayer ceramic electronic component
JP2020057753A
Ceramic electronic component, manufacturing method of ceramic electronic component, and ceramic electronic component mounting circuit board
JP2020061524A