Negative electrode for all-solid-state battery
By controlling the particle and pore shape parameters of Si-based particles in all-solid-state batteries, the resistance in the low SOC region is minimized, addressing the volume change issue and enhancing ion diffusivity.
Patent Information
- Application Number
- JP2021207995
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-12-22
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2041-12-22
AI Technical Summary
Si-based negative electrode active materials in all-solid-state batteries experience large volume changes during charging and discharging, leading to increased battery resistance in the low state of charge (SOC) region.
The negative electrode includes Si-based particles with controlled particle shape parameter x=D90/D50 greater than 37.9 and pore shape parameter y=p1/p2 less than 0.0035, where D90 and D50 represent particle diameters, and p1 and p2 represent pore volume and diameter, respectively, to reduce battery resistance.
This configuration suppresses volume changes and enhances ion diffusivity, resulting in reduced battery resistance in the low SOC region.
Smart Images

Figure 0007567769000003 
Figure 0007567769000004 
Figure 0007567769000005
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a negative electrode for an all-solid-state battery. [Background technology]
[0002] An all-solid-state battery is a battery that has a solid electrolyte layer between a positive electrode layer and a negative electrode layer, and has the advantage that it is easier to simplify safety devices compared to liquid batteries that have an electrolyte solution containing a flammable organic solvent.
[0003] For example, Patent Document 1 discloses an all-solid-state battery having a negative electrode active material layer containing a Si-based negative electrode active material, in which the negative electrode active material layer has a specific amount of voids in a region of 0.3 μm around the surface of the Si-based negative electrode active material. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2021-103656 A Summary of the Invention [Problem to be solved by the invention]
[0005] It is known that Si-based negative electrode active materials are used in all-solid-state batteries. Although Si-based negative electrode active materials have a large theoretical capacity and are effective in increasing the energy density of batteries, they have a large volume change during charging and discharging, which may cause fluctuations in the restraining pressure of the all-solid-state battery. In this regard, by providing voids as in Patent Document 1, the volume change of the Si-based negative electrode active material can be suppressed, but a new problem arises in that the battery resistance increases in the low charging rate (SOC: State of Charge) region.
[0006] The present disclosure has been made in view of the above circumstances, and has as its main object to provide a negative electrode for an all-solid-state battery capable of reducing the battery resistance in a low SOC region. [Means for solving the problem]
[0007] The negative electrode for an all-solid-state battery according to the present disclosure includes a negative electrode active material, The negative electrode active material contains Si-based particles having pores, The Si-based particles having pores are x represented by the formula (1): x=D90 / D50 [wherein D90 represents the cumulative 90% particle size (μm) in the volume-based particle size distribution of the Si-based particles, and D50 represents the cumulative 50% particle size (μm) in the volume-based particle size distribution of the Si-based particles] is 37.9 or more, and The negative electrode for an all-solid-state battery is characterized in that y, represented by formula (2): y=p1 / p2 (wherein p1 represents the cumulative pore volume (cc / g) in a log differential pore volume distribution curve obtained by a DFT method for the Si-based particles, and p2 represents the pore diameter (nm) having the highest abundance ratio in the log differential pore volume distribution curve), satisfies 0.0035 or less. Effect of the Invention
[0008] According to the present disclosure, it is possible to provide a negative electrode for an all-solid-state battery capable of reducing the battery resistance in a low SOC region. [Brief description of the drawings]
[0009] [Figure 1] FIG. 1 is a schematic cross-sectional view showing an example of an all-solid-state battery according to the present disclosure. [Diagram 2] FIG. 2 shows an example of a log differential pore volume distribution curve obtained by the DFT method using the adsorption isotherm of a Si-based particle having pores. [Diagram 3] FIG. 3 is a diagram in which the values of the particle shape parameter x and the pore shape parameter y of the pore-containing Si particles of Examples 1 to 6 and Comparative Examples 2 to 8 are plotted. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] [Negative electrode for all-solid-state batteries] The negative electrode for an all-solid-state battery according to the present disclosure includes a negative electrode active material, The negative electrode active material contains Si-based particles having pores, The Si-based particles having pores are x represented by the formula (1): x=D90 / D50 [wherein D90 represents the cumulative 90% particle size (μm) in the volume-based particle size distribution of the Si-based particles, and D50 represents the cumulative 50% particle size (μm) in the volume-based particle size distribution of the Si-based particles] is 37.9 or more, and The particle is characterized in that y expressed by the formula (2): y=p1 / p2 (wherein p1 represents the cumulative pore volume (cc / g) in a log differential pore volume distribution curve obtained by a DFT method for the Si-based particles, and p2 represents the pore diameter (nm) having the highest abundance ratio in the log differential pore volume distribution curve) satisfies 0.0035 or less.
[0011] As mentioned above, when a Si-based negative electrode active material with voids (pores) is used, the volume change during charging and discharging can be suppressed, but the resistance increases in the low SOC region. In this regard, it is unclear what parameters contribute to reducing the battery resistance for Si-based particles with pores, and there is room for improvement in the performance of all-solid-state batteries that use Si-based particles with pores as the negative electrode active material. In order to obtain an all-solid-state battery negative electrode capable of reducing battery resistance in a low SOC region, the present inventors have focused on the particle shape parameters and pore shape parameters of the Si-based particles having fine pores, which are the raw materials, and have conducted extensive research into the correlation with battery resistance in a low SOC region. As a result, the present inventors have found that the particle shape parameter x of the specific formula (1) consisting of D90 and D50 of the Si-based particles having fine pores, and the pore shape parameter y of the specific formula (2) consisting of the cumulative pore volume p1 and the pore diameter p2 with the highest abundance ratio of the Si-based particles having fine pores, have a high correlation with battery resistance in a low SOC region, as shown in the examples and comparative examples described below, and have completed the present invention. In the present disclosure, by controlling the Si-based particles having pores such that the particle shape parameter x in the formula (1) is 37.9 or more and the pore shape parameter y in the formula (2) is 0.0035 or less, which are highly correlated with the battery resistance in the low SOC region, it is possible to provide a negative electrode for an all-solid-state battery that can reduce the battery resistance in the low SOC region.
[0012] In the present disclosure, the exact reason why the resistance in the low SOC region is low is unclear, but it is presumed as follows. In Si-based particles having pores, if the total particle surface area is too large, it is likely to affect the resistance of the surface reaction, but by controlling D90 / D50 to obtain a particle size distribution with a higher standard deviation, the total particle surface area can be suppressed, and it is believed that the resistance of the surface reaction can be suppressed. Therefore, it is believed that the resistance can be reduced by making D90 / D50 sufficiently large in Si-based particles. In addition, if there are many voids due to pores inside the Si-based particles, it is likely to affect the resistance, but it is believed that the ion diffusivity in the particles can be increased by controlling the ratio between the cumulative pore volume p1 and the pore diameter p2 with the highest abundance ratio, and increasing the pore diameter relative to the cumulative pore volume. Therefore, it is believed that the resistance can be reduced by reducing p1 / p2 to a specific range in Si-based particles. Therefore, it is believed that when D90 / D50 is 37.9 or more and p1 / p2 is 0.0035 or less, the resistance is synergistically reduced.
[0013] (1)Negative electrode active material The negative electrode for an all-solid-state battery disclosed herein includes a negative electrode active material, and the negative electrode active material includes Si-based particles having the specific pores.
[0014] The negative electrode active material may be a Si-based negative electrode active material. Examples of the Si-based negative electrode active material include simple Si, Si alloys, and Si oxides. The Si alloy preferably contains Si element as a main component. The ratio of Si element in the Si alloy may be, for example, 50 mol% or more, 70 mol% or more, or 90 mol% or more. Examples of the Si alloy include Si-Li-based alloys, Si-Al-based alloys, Si-Sn-based alloys, Si-In-based alloys, Si-Ag-based alloys, Si-Pb-based alloys, Si-Sb-based alloys, Si-Bi-based alloys, Si-Mg-based alloys, Si-Ca-based alloys, Si-Ge-based alloys, and Si-Pb-based alloys. The Si alloy may be a two-component alloy or a multi-component alloy of three or more components. The Si alloy may be a Si-Li-based alloy. The Si-based negative electrode active material may be in the form of particles. In the present disclosure, particulate Si-based negative electrode active material is referred to as Si-based particles. The Si-based particles used in the present disclosure may be Si-based particles having pores.
[0015] (2) Si-based particles with fine pores The Si-based particles having pores can suppress the volume change during charging and discharging due to the presence of pores. The porosity of the Si-based particles is not particularly limited, but is, for example, 5% or more and 50% or less. The porosity can be calculated, for example, by observing a scanning electron microscope (SEM) image of the cross section of the Si-based particles and using the following formula. Porosity (%) = 100 × (pore area) / (particle area)
[0016] The Si-based particles having pores used in the present disclosure satisfy x represented by formula (1): x=D90 / D50 [wherein D90 represents the cumulative 90% particle size (μm) in the volume-based particle size distribution of the Si-based particles, and D50 represents the cumulative 50% particle size (μm) in the volume-based particle size distribution of the Si-based particles] of 37.9 or more. The lower limit of x may be 50.0 or more, 100.0 or more, or 200.0 or more. On the other hand, the upper limit of x is not particularly limited, but may be, for example, 232.0 or less. Here, D50 and D90 respectively refer to the cumulative 50% particle size and cumulative 90% particle size in the volume-based particle size distribution measured by a laser diffraction particle size distribution analyzer, and the specific method for determining these values can be the method described in the Examples section below.
[0017] The D50 of the Si-based particles having the pores is not particularly limited as long as it satisfies the above relationship. The D50 may be, for example, 0.331 μm or more, or 0.342 μm or more. On the other hand, the D50 may be, for example, 0.690 μm or less.
[0018] The D90 of the Si-based particles having the pores is not particularly limited as long as it satisfies the above relationship. The D90 may be, for example, 12.556 μm or more, or 56.004 μm or more. On the other hand, the D90 may be, for example, 76.781 μm or less.
[0019] The Si-based particles having pores used in the present disclosure satisfy y of 0.0035 or less, which is expressed by formula (2): y=p1 / p2 [wherein p1 represents the cumulative pore volume (cc / g) in a log differential pore volume distribution curve obtained by a DFT method for the Si-based particles, and p2 represents the pore diameter (nm) having the highest abundance ratio in the log differential pore volume distribution curve]. The upper limit of y may be 0.0030 or less, or may be 0.0025 or less, while the lower limit of y is not particularly limited, and may be, for example, 0.0020 or more. In addition, p1 and p2 can be measured by using a specific surface area measuring device for the Si-based particles having the pores. As a specific method for determining the cumulative pore volume (cc / g) and the pore diameter (nm) having the highest abundance ratio in the log differential pore volume distribution curve obtained by the DFT method of the Si-based particles having the pores of the present disclosure, the method described in the examples described later can be adopted.
[0020] The cumulative pore volume p1 of the Si-based particles having the pores is not particularly limited as long as it satisfies the above relationship. p1 may be, for example, 0.097 cc / g or more, or 0.103 cc / g or more. On the other hand, p1 may be 0.165 cc / g or less.
[0021] The pore diameter p2 at which the Si-based particles having the pores have the highest abundance ratio is not particularly limited as long as it satisfies the above relationship. p2 may be, for example, 39.5 nm or more, or 43.9 nm or more. On the other hand, p2 may be 47.5 nm or less.
[0022] The method for producing the Si-based particles having pores of the present disclosure is not particularly limited as long as the particle shape parameter x and the pore shape parameter y are satisfied. The method for producing the Si-based particles having pores of the present disclosure may be a production method having the following steps 1 to 6, since it can easily produce Si-based particles having pores that simultaneously satisfy the parameters x and y. The production method having the following steps 1 to 6 can easily produce Si-based particles having pores that simultaneously satisfy the parameters x and y by particularly including the following step 3.
[0023] Step 1: A step of pulverizing a Si-based negative electrode active material in a ball mill and adjusting the particle size to a predetermined particle size to obtain Si-based particles. Step 2: A step of placing the obtained Si-based particles in a mortar, adding metallic Li, and mixing the powder at room temperature to obtain Si-Li-based alloy particles. Step 3: A step of adding Si-Li alloy particles to a mesitylene solvent, and then adding dropwise ethanol at 0°C or lower at a constant rate while stirring the mixture at room temperature (25°C). Step 4: Further adding acetic acid dropwise at a constant rate while stirring the mixture. Step 5: filtering the resulting mixture under reduced pressure to recover the powder. Step 6: A step of vacuum drying the recovered powder to remove the solvent and obtain Si-based particles having pores.
[0024] The composition of the Si negative electrode active material, the amount of the Si negative electrode active material, the ball mill rotation speed, and the pulverization time can be appropriately controlled in the step 1. The predetermined particle size can be adjusted to, for example, 300 to 2000 nm.
[0025] The amount of metallic Li, the rotation speed of the mortar, and the mixing time can be appropriately controlled in the step 2. The amount of metallic Li can be adjusted to, for example, 0.8 to 1.4 (mass ratio) relative to the Si-based particles.
[0026] In the step 3, the amount of mesitylene, the temperature of ethanol, the dropping speed, the amount of ethanol, and the rotation speed of the stirrer can be appropriately controlled. The amount of mesitylene can be adjusted to, for example, 25 to 45 (mass ratio) relative to the Si-Li alloy particles. The ethanol temperature can be adjusted to, for example, 0°C or lower. The dropping speed of ethanol can be adjusted to, for example, 1 drop / 2 sec to 1 drop / 6 sec. The amount of ethanol can be adjusted to, for example, 25 to 45 (mass ratio) relative to the Si-Li alloy particles, and may be adjusted to 6.9 to 8.9 (mass ratio). The rotation speed of the stirrer can be adjusted to, for example, 100 to 500 (unit: rpm). In the step 3, by adding mesitylene to the Si-Li alloy particles in advance, the reactivity of ethanol with the Si-Li alloy particles can be controlled, and the fine pore structure can be controlled.
[0027] The amount of acetic acid and the rotation speed of the stirrer can be appropriately controlled in the step 4. The amount of acetic acid can be adjusted to, for example, 45 to 65 (mass ratio) relative to the Si-Li alloy particles.
[0028] The degree of vacuum during vacuum drying and the drying time can be appropriately controlled in step 6. The degree of vacuum may be, for example, −0.1 MPa, and the drying time may be 12 hours or more.
[0029] (3) Other components in the negative electrode The negative electrode for an all-solid-state battery according to the present disclosure may further contain other components in addition to the negative electrode active material. The negative electrode for the all-solid-state battery of the present disclosure may have a negative electrode active material layer on one or both sides of a negative electrode current collector. The negative electrode current collector may have a thickness of, for example, 5 μm to 30 μm. Examples of the material for the negative electrode current collector include SUS, copper, and nickel.
[0030] The negative electrode active material layer may contain at least one of a solid electrolyte, a conductive material, and a binder, in addition to the negative electrode active material, as necessary. The proportion of the negative electrode active material in the negative electrode active material layer is, for example, 20 mass % or more, or may be 30 mass % or more, or may be 40 mass % or more, while the proportion of the negative electrode active material is, for example, 80 mass % or less, or may be 70 mass % or less, or may be 60 mass % or less. The negative electrode active material layer may contain only the Si-based particles having the pores as the negative electrode active material, or may contain other negative electrode active materials. In the latter case, the ratio of the Si-based particles having the pores to the total negative electrode active material may be 50 mass % or more, 70 mass % or more, or 90 mass % or more.
[0031] Examples of the solid electrolyte include inorganic solid electrolytes such as sulfide solid electrolytes, oxide solid electrolytes, nitride solid electrolytes, and halide solid electrolytes. Examples of the sulfide solid electrolyte include solid electrolytes containing Li, X (X is at least one of P, As, Sb, Si, Ge, Sn, B, Al, Ga, and In), and S. The sulfide solid electrolyte may further contain at least one of O and halogen. Examples of the halogen include F, Cl, Br, and I. The sulfide solid electrolyte may be glass (amorphous) or glass ceramics. Examples of the sulfide solid electrolyte include Li2S-P2S5, LiI-Li2S-P2S5, LiI-LiBr-Li2S-P2S5, Li2S-SiS2, Li2S-GeS2, and Li2S-P2S5-GeS2.
[0032] Examples of the conductive material include carbon materials. Examples of the carbon material include particulate carbon materials such as acetylene black (AB) and ketjen black (KB), and fibrous carbon materials such as carbon fiber, carbon nanotubes (CNT), carbon nanofibers (CNF), and vapor grown carbon fiber (VGCF). The conductive material may be vapor grown carbon fiber (VGCF).
[0033] Examples of the binder include rubber-based binders such as butylene rubber (BR) and styrene butadiene rubber (SBR), and fluoride-based binders such as polyvinylidene fluoride (PVDF). The binder may be polyvinylidene fluoride (PVDF).
[0034] The thickness of the negative electrode active material layer is, for example, 0.3 μm or more and 1000 μm or less.
[0035] The negative electrode for an all-solid-state battery according to the present disclosure contains a negative electrode active material. As long as the negative electrode active material contains Si-based particles having the specific pores, the negative electrode can be produced by appropriately selecting a conventionally known production method.
[0036] [All-solid battery] FIG. 1 is a schematic cross-sectional view showing an example of an all-solid-state battery according to the present disclosure. The all-solid-state battery 100 includes a battery element 20. The all-solid-state battery 100 may further include an exterior body (not shown). The battery element 20 may be housed in the exterior body. The exterior body may be, for example, a metal case or the like. The exterior body may be, for example, a pouch made of an aluminum laminate film or the like.
[0037] The battery element 20 includes a positive electrode 11, a solid electrolyte layer 13, and a negative electrode 12. The positive electrode 11 includes a positive electrode active material and a solid electrolyte. The negative electrode 12 is the negative electrode for an all-solid-state battery of the present disclosure. The solid electrolyte layer (separator layer) 13 is interposed between the positive electrode 11 and the negative electrode 12. The solid electrolyte layer 13 blocks electronic conduction between the positive electrode 11 and the negative electrode 12. The solid electrolyte layer 13 conducts ions. That is, the solid electrolyte layer 13 ionically connects the positive electrode 11 and the negative electrode 12. The positive electrode 11 and the solid electrolyte layer 13 can be appropriately selected from conventionally known positive electrodes and solid electrolyte layers for all-solid-state batteries. Specific examples of the positive electrode 11 and the solid electrolyte layer 13 include those described in JP-A-2021-103656.
[0038] The all-solid-state battery in the present disclosure may be an all-solid-state lithium battery. The all-solid-state battery may be a primary battery or a secondary battery, and in particular may be a secondary battery. This is because the battery can be repeatedly charged and discharged, and is useful, for example, as an in-vehicle battery. The secondary battery also includes a secondary battery used as a primary battery (used only for the purpose of initial charging).
[0039] The all-solid-state battery in the present disclosure may be a single cell or a stacked battery. The stacked battery may be a monopolar stacked battery (a parallel-connected stacked battery) or a bipolar stacked battery (a series-connected stacked battery). The shape of the all-solid-state battery may be, for example, a coin type, a laminate type, a cylindrical type, or a square type. EXAMPLES
[0040] EXAMPLES The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples.
[0041] [Example 1] (Preparation of Si-based particles with micropores) Step 1: The Si active material (composition: Si metal) was pulverized in a ball mill (rotation speed: 1000 rpm, time: 3 hours) and adjusted to a predetermined particle size (600 nm) to obtain Si-based particles. Step 2: The obtained Si-based particles were placed in a mortar, and metallic Li was added. The powder was mixed at room temperature (mortar rotation speed: 50 rpm, time: 20 minutes) to obtain a Si-Li-based alloy. The Si-based particles and metallic Li were weighed out so that they were contained in the mixture in a mass ratio of Si-based particles:metallic Li = 1:1.2. Step 3: After adding a Si-Li alloy (0.1 parts by mass) to 3.4 parts by mass of mesitylene solvent, the mixture was stirred (stirrer rotation speed: 250 rpm) at room temperature (25°C), and ethanol (3.1 parts by mass) at -5°C was added dropwise at a constant rate (1 drop / 5 sec). Step 4: While the mixture was being stirred (stirrer rotation speed: 250 rpm), acetic acid (5.6 parts by mass) was added dropwise at a constant rate (1 drop / 5 sec). Step 5: The resulting mixture was filtered under reduced pressure to recover the powder. Step 6: The powder was vacuum-dried (vacuum degree: -0.1 MPa, drying time: 12 hours) to remove the solvent, and Si-based particles having pores were obtained.
[0042] (Preparation of negative electrode) The above-mentioned Si-based particles having fine pores were added in an amount of 50 mass%, sulfide solid electrolyte (10LiI-15LiBr-75 (0.75Li2S-0.25P2S5)) in an amount of 37 mass%, conductive material (VGCF) in an amount of 10 mass%, and binder (PVdF) in an amount of 3 mass% to a dispersion medium (heptane). This dispersion medium was subjected to ultrasonic treatment for 5 minutes using an ultrasonic homogenizer to obtain a negative electrode composite material. The negative electrode composite material was applied to both sides of a current collector foil (Ni foil, thickness 24 μm) and dried, and then roll pressed at a linear pressure of 50 kN / cm. The obtained current collector foil with the negative electrode active material layer (thickness of each layer: 45.3 μm) was punched out to φ11.3 mm (1 cm 2 ) to obtain a negative electrode.
[0043] (Preparation of evaluation battery) Cathode active material (LiNi 1 / 3 Co 1 / 3 Mn 1 / 3A dispersion medium (heptane) was charged with 84.7% by mass of 02), 13.4% by mass of sulfide solid electrolyte (10LiI-15LiBr-75 (0.75Li2S-0.25P2S5)), 1.3% by mass of conductive material (VGCF), and 0.6% by mass of binder (PVdF). This dispersion medium was subjected to ultrasonic treatment for 5 minutes using an ultrasonic homogenizer to obtain a positive electrode composite. The positive electrode composite was applied to a current collector foil (Al foil, thickness 10 μm) and dried, and then roll pressed at a linear pressure of 50 kN / cm. The obtained current collector foil with a positive electrode active material layer (thickness 70.0 μm) was punched out to φ11.3 mm (1 cm 2 ) to obtain a positive electrode.
[0044] A sulfide solid electrolyte (10LiI-15LiBr-75 (0.75Li2S-0.25P2S5)) was added to a dispersion medium (heptane) in an amount of 99.5 mass% and a binder (PVdF) was added to a dispersion medium (heptane) in an amount of 0.5 mass%. This dispersion medium was subjected to ultrasonic treatment for 5 minutes using an ultrasonic homogenizer to obtain a composite material. The obtained composite material was applied to a substrate (Al foil, thickness 20 μm) to a thickness of 15 μm and dried, and then punched out to a diameter of Φ11.3 mm (1 cm 2 ) and a solid electrolyte layer (separator layer, thickness 15.0 μm) were obtained.
[0045] The positive electrode, separator layer, and negative electrode were stacked together with their centers aligned, and a surface pressure of 5 tons / cm was applied. 2 The layers were then sealed with a tabbed laminate and restrained at 5 MPa to produce an evaluation battery (all-solid-state lithium battery). The evaluation battery was produced to have a capacity of 2 mAh.
[0046] [Examples 2 to 6] In step 3 of the preparation of Si-based particles having fine pores in Example 1, Si-based particles having fine pores were prepared in the same manner as in Example 1, except that at least one of the amount of mesitylene, the temperature of ethanol, the dropping rate of ethanol, the amount of ethanol, and the rotation speed of the stirrer was changed. A negative electrode and a battery for evaluation were produced in the same manner as in Example 1 using the obtained Si-based particles having fine pores.
[0047] [Comparative Example 1] A negative electrode and a battery for evaluation were produced in the same manner as in Example 1, except that in the production of the negative electrode of Example 1, Si-based particles without pores were used instead of the Si-based particles with pores.
[0048] [Comparative Examples 2 to 8] In step 3 of the preparation of Si-based particles having fine pores in Example 1, Si-based particles having fine pores were prepared in the same manner as in Example 1, except that at least one of the amount of mesitylene, the temperature of ethanol, the dropping rate of ethanol, the amount of ethanol, and the rotation speed of the stirrer was changed. A negative electrode and a battery for evaluation were produced in the same manner as in Example 1 using the obtained Si-based particles having fine pores.
[0049] [evaluation] (D50 and D90 of Si-based particles) By a wet method, the Si-based particles were dispersed in a water solvent (Si-based particles:water = 1:400 (mass ratio)), and the cumulative 50% particle diameter D50 in the volumetric particle diameter distribution of the Si-based particles and the cumulative 90% particle diameter D90 in the volumetric particle diameter distribution of the Si-based particles were obtained using a laser diffraction particle diameter distribution analyzer (Shimadzu, SALD-2300). From the obtained D50 and D90, the particle shape parameter x = D90 / D50 was calculated. The measurement results of Examples 1 to 6 and Comparative Examples 1 to 8 are shown in Table 1 or Table 2.
[0050] (Pore diameter and cumulative pore volume of Si-based particles) The adsorption isotherm of the Si-based particles having fine pores was measured by a nitrogen gas adsorption method at a gas liquefaction temperature of 77K using a specific surface area measuring device (Quantachrome Nova, manufactured by Anton Paar QuantaTec). FIG. 2 shows an example of a log differential pore volume distribution curve obtained by the DFT method using the adsorption isotherm of a Si-based particle having pores. As shown in Figure 2, in the log differential pore volume distribution curve obtained by the DFT method, the diameter of the first peak, which indicates the index of the pore diameter of the particles having pores, was determined as the pore diameter p2 (nm) with the highest abundance ratio. In addition, the cumulative pore volume in the range of pore diameters equal to or smaller than the minimum diameter of the first peak was determined as the cumulative pore volume p1 (cc / g). The pore shape parameter y = p1 / p2 was calculated from the obtained p1 and p2. The measurement results of Examples 1 to 6 and Comparative Examples 1 to 8 are shown in Table 1 or Table 2.
[0051] (Battery resistance measurement) The direct current internal resistance (DCIR) of the all-solid-state batteries for evaluation obtained in each Example and Comparative Example was measured to determine the discharge resistance. The measurement was performed at 25° C., with the battery being discharged at 4 C for 10 seconds from SOC 20%. <Judgment criteria> 〇: DCIR is 40mΩ or less ×: DCIR exceeds 40mΩ The measurement results of Examples 1 to 6 and Comparative Examples 1 to 8 are shown in Table 1 or Table 2.
[0052] [Table 1]
[0053] [Table 2]
[0054] In Tables 1 and 2, np-Si indicates Si-based particles having pores.
[0055] As shown in Tables 1 and 2, it was confirmed that the DCIR tends to be lower when the particle shape parameter (x = D90 / D50) is large. From this, it is presumed that a particle size distribution with a higher standard deviation is more effective at reducing resistance, and that if the total particle surface area is too large, it will affect the resistance of the surface reaction. In addition, it was confirmed that the DCIR tends to be lower when the pore shape parameter (y = p1 / p2) is small. From this, it is presumed that while having many voids due to pores inside the particle is likely to affect resistance, by increasing the pore diameter, paths for ions and conductivity within the particle are secured.
[0056] FIG. 3 is a diagram in which the values of the particle shape parameter x and the pore shape parameter y of the pore-containing Si particles of Examples 1 to 6 and Comparative Examples 2 to 8 are plotted. As is clear from the performance evaluation results in FIG. 3 and Tables 1 and 2, in Comparative Example 5, although the particle shape parameter x was larger than the predetermined value, the pore shape parameter y was larger than the predetermined value, so the DCIR value was large. In addition, in Comparative Examples 4 and 6, although the pore shape parameter y was smaller than the predetermined value, the particle shape parameter x was smaller than the predetermined value, so the DCIR value was large. From this, it was found that in Si-based particles having pores, controlling both the particle shape parameter x and the pore shape parameter y has a high correlation with the reduction of battery resistance in the low SOC region. [Explanation of symbols]
[0057] 11 Positive electrode 12 Negative electrode 13 Solid electrolyte layer 20 Battery elements 100 solid state battery
Claims
[Claim 1] A negative electrode active material is included, The negative electrode active material contains Si-based particles having pores, The Si-based particles having pores are Formula (1): x = D90 / D50 [wherein D90 represents the cumulative 90% particle size (μm) in the volume-based particle size distribution of the Si-based particles, and D50 represents the cumulative 50% particle size (μm) in the volume-based particle size distribution of the Si-based particles] satisfies 37.9 or more, and Formula (2): y = p1 / p2 [wherein p1 represents the cumulative pore volume (cc / g) in a log differential pore volume distribution curve obtained by a DFT method of the Si-based particles, and p2 represents the pore diameter (nm) having the highest abundance ratio in the log differential pore volume distribution curve] satisfies 0.0035 or less, Negative electrode for all-solid-state batteries.