Grain-oriented electrical steel sheets and laminated cores
By controlling residual magnetic flux density variations through thermal strain regions and optimizing production conditions, the solution addresses the challenge of achieving low noise and low iron loss in grain-oriented electrical steel sheets, enhancing transformer performance.
Patent Information
- Application Number
- JP2024535485
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2023-02-15
- Filing Date
- 2024-02-14
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2044-02-14
AI Technical Summary
Existing methods to reduce transformer noise and iron loss in grain-oriented electrical steel sheets face challenges such as increased manufacturing costs, larger transformer size, and trade-offs between low noise and low iron loss, particularly due to non-heat-resistant magnetic domain refining which increases hysteresis loss and magnetostriction.
The solution involves controlling the standard deviation of residual magnetic flux density (σBr) to 0.38 or less by introducing linear thermal strain regions on the steel sheet, aligning the magnetization direction with the rolling direction, and optimizing production conditions to minimize variations in residual magnetic flux density.
This approach effectively suppresses transformer noise while maintaining low iron loss, achieving both low noise and low iron loss in transformers by stabilizing residual magnetic flux density variations.
Smart Images

Figure 0007568176000005 
Figure 0007568176000006 
Figure 0007568176000007
Abstract
Description
[Technical field]
[0001] The present invention relates to a grain-oriented electrical steel sheet, in particular a grain-oriented electrical steel sheet suitable as a material for laminated cores for transformers, and a laminated core using the same. [Background technology]
[0002] Grain-oriented electrical steel sheets are used as materials for the iron cores of transformers, etc. In such applications as materials for the iron cores of transformers, it is necessary to suppress energy loss and noise. Here, the energy loss is affected by the iron loss of the grain-oriented electrical steel sheets, and the noise is affected by the magnetostriction characteristics of the grain-oriented electrical steel sheets.
[0003] In recent years, there has been a strong demand for reducing energy loss in transformers and noise during operation in order to comply with energy conservation and environmental regulations, making it extremely important to develop grain-oriented electrical steel sheets with excellent iron loss and magnetostriction properties.
[0004] Here, the iron loss of grain-oriented electrical steel sheet is mainly composed of hysteresis loss and eddy current loss. Methods proposed to improve hysteresis loss include highly orienting the (110)
[0001] crystal orientation, known as the GOSS orientation, in the rolling direction of the steel sheet and reducing impurities in the steel sheet. Methods proposed to improve eddy current loss include increasing the electrical resistance of the steel sheet by adding Si and applying coating tension in the rolling direction of the steel sheet. However, when pursuing further reduction in iron loss of grain-oriented electrical steel sheet, these methods have manufacturing limitations.
[0005] Therefore, magnetic domain refinement technology has been developed as a method to further reduce iron loss in grain-oriented electrical steel sheets. Magnetic domain refinement technology is a method to reduce iron loss, especially eddy current loss, in grain-oriented electrical steel sheets by introducing non-uniformity in magnetic flux through physical means such as forming grooves or introducing localized thermal distortion in steel sheets after final annealing or baking of the insulating coating, thereby refining the width of the 180° magnetic domains (main magnetic domains) formed along the rolling direction.
[0006] For example, Patent Document 1 proposes a technique for improving the iron loss, which was 0.80 W / kg or more, to 0.70 W / kg or less by introducing linear grooves with a width of 300 μm or less and a depth of 100 μm or less into the surface of a steel sheet. Patent Document 2 also proposes irradiating a plasma flame in the sheet width direction of the steel sheet surface after secondary recrystallization to locally introduce thermal strain. The introduction of this thermal strain reduces the iron loss (W 17 / 50 ) has been improved to 0.680W / kg.
[0007] The method of introducing linear grooves as disclosed in Patent Document 1 is called heat-resistant magnetic domain refinement because the magnetic domain refinement effect does not disappear even when stress relief annealing is performed after core forming. On the other hand, the method of introducing thermal strain as disclosed in Patent Document 2 is called non-heat-resistant magnetic domain refinement because the effect of introducing thermal strain is lost due to stress relief annealing.
[0008] Non-heat-resistant magnetic domain refinement significantly reduces eddy current loss by introducing localized thermal strain into the steel sheet, but it is known that the introduction of such strain leads to deterioration of magnetic properties, such as increased hysteresis loss and increased magnetostriction. Magnetostriction in particular is known to be one of the noise sources in transformers, and it is also known that the larger the magnetostriction, the greater the noise. Thus, there is a trade-off between the iron loss and noise of transformers in non-heat-resistant magnetic domain refinement materials, so there is a need to develop a method to achieve both low iron loss and low noise.
[0009] In addition to magnetostriction, electromagnetic vibration of the core is known as a cause of transformer noise. The grain-oriented electromagnetic steel sheet with the above-mentioned non-heat-resistant magnetic domain refinement is mainly used as a laminated core (stacked core) for transformers. A schematic diagram of the structure of a laminated core is shown in FIG. 1. A laminated core means a core with a structure in which grain-oriented electromagnetic steel sheets cut into diagonal bars 1 such as legs 11 and yokes 12 are laminated in the plate thickness direction. The left side of FIG. 1 is a plan view of a laminated core placed with the steel plate surface facing up, and examples of XX cross section and YY cross section of the laminated core are shown on the right side of FIG. 1. As shown in FIG. 1, in a laminated core, there are joints 2 between the diagonal bars 1, and magnetic flux circulates inside the steel sheets, so that magnetic flux transfer occurs periodically at these joints 2. During magnetic flux transfer at such joints 2, the ends of the steel sheets are magnetized, so electromagnetic vibration occurs due to the magnetic attraction between the ends and the magnetic repulsion between the layers. Suppression of this electromagnetic vibration has been proposed as a method for improving transformer noise in the past.
[0010] As a method for suppressing noise caused by such electromagnetic vibration, Patent Document 3 proposes making the cross-sectional area of the iron core in the yoke larger than that of the iron core in the legs, while Patent Document 4 proposes a method for suppressing vibration by providing a viscoelastic resin layer between laminated steel plates. [Prior art documents] [Patent documents]
[0011] [Patent Document 1] Special Publication No. 6-22179 [Patent Document 2] Japanese Patent Application Publication No. 7-192891 [Patent Document 3] Japanese Patent Application Publication No. 11-307368 [Patent Document 4] JP 2009-224531 A Summary of the Invention [Problem to be solved by the invention]
[0012] Although the above-mentioned measures to suppress vibrations caused by electromagnetic forces between steel plates can achieve a certain level of effectiveness, they have the following problems: For example, in the method described in Patent Document 3, the transformer itself tends to be large in size because of the structure that ensures a larger cross-sectional area for the yoke than for the legs, which increases the manufacturing cost.
[0013] In addition, the method proposed in Patent Document 4 of providing a viscoelastic resin layer between stacked steel plates reduces the effective cross-sectional area of the steel plates in the legs, so that when comparing iron cores of similar size, each steel plate is excited to a higher magnetic field, resulting in increased loss (iron loss). To avoid this, there is a problem that the iron core must be made larger.
[0014] The present invention has been made in consideration of the above-mentioned circumstances, and has an object to provide a grain-oriented electrical steel sheet and laminated core that have characteristics that can achieve both low iron loss and low noise in a transformer by using a mechanism that differs from the conventional technology, specifically, by suppressing vibrations caused by electromagnetic forces at the joints of the laminated core. [Means for solving the problem]
[0015] The inventors have conducted extensive research to solve the above problems.
[0016] The vibrations of the steel plates at the joints 2 of the iron core include vibrations caused by magnetic forces acting on both end faces of the joints 2, and vibrations caused by magnetic forces acting in the vertical direction of the lamination of the joints 2. When these vibrations were investigated in detail, it was found that the phase of the vertical vibrations differs depending on the position between the layers, and that when the external magnetic field H applied to the legs 11 becomes 0 (zero), the phase shift differs significantly, resulting in an increase in transformer noise.
[0017] To investigate further, SST samples were cut from the steel sheets of each layer that constitutes the above iron core, and the hysteresis loops (BH curves, see Figure 2) of each steel sheet were measured. It was found that the magnetic flux density Br(T) remaining in the steel sheets when the external magnetic field H was 0 varied between the steel sheets. In other words, when these steel sheets are stacked, when the external magnetic field is 0 A / m, each stacked steel sheet has a different amount of magnetic flux density, and magnetic attraction / repulsion acts sparsely between the layers at the iron core joints. As a result, irregular vibrations are generated, and this was newly discovered to be the cause of the increase in noise mentioned above.
[0018] The present invention has been made based on the above findings.
[0019] That is, the gist of the present invention is as follows.
[0020] [1] A grain-oriented electrical steel sheet having a plurality of strain regions which extend linearly in a direction transverse to the rolling direction of the steel sheet and are arranged in parallel at intervals in the rolling direction on at least one of the front and back surfaces of the grain-oriented electrical steel sheet, wherein the standard deviation σBr of the residual magnetic flux density Br (the value of the sample magnetic flux density B(T) when the external magnetic field strength H=0) of the hysteresis loop which is drawn when the sample is excited up to 1.7 T with the rolling direction as the magnetization direction is 0.38 or less.
[0021] [2] The grain-oriented electrical steel sheet according to [1] above, wherein the standard deviation σBr is 0.36 or less.
[0022] [3] A laminated core made by stacking multiple grain-oriented electromagnetic steel sheets as described above in [1] or [2]. Effect of the Invention
[0023] According to the present invention, even though it is a non-heat-resistant magnetic domain refinement treated material with linear (thermal) distortion regions formed, it is possible to suppress the variation in residual magnetic flux density. By using the grain-oriented electrical steel sheet of the present invention in a laminated core, it is possible to provide a transformer with low iron loss and low noise. [Brief description of the drawings]
[0024] [Figure 1] FIG. 2 is a schematic diagram showing the structure of a laminated core. [Diagram 2] FIG. 1 is a diagram showing a typical example of a hysteresis loop. [Diagram 3] 1 is a graph showing the effect of σBr on transformer loss. [Figure 4] 1 is a graph showing the effect of σBr on transformer noise. [Diagram 5] FIG. 2 is a diagram showing the concept of a strip threading speed. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0025] The experimental results that led to the completion of the present invention will now be described. (Experiment 1) A steel slab with the composition shown in Table 1 was used, and the surface of the product steel strip of grain-oriented electrical steel sheet with a forsterite coating and an insulating coating (tensile coating) was irradiated with an electron beam to perform magnetic domain refinement treatment. The output of the electron beam was changed between 800 and 1200 W, the beam irradiation interval in the steel sheet running direction was 5 mm, and the beam scanning speed was 80 m / s. Oblique bars were cut from various parts of the sample obtained in this way, and for each oblique bar, the iron loss was measured using the single sheet magnetic measurement method specified in JIS C2556, and the hysteresis loop was measured to calculate the residual magnetic flux density Br (T). After that, from all the oblique bars for which Br was calculated, small groups of oblique bars were selected so that the average value of Br coincided with the population distribution average value and the standard deviation σBr was different, and a three-phase stacked core model transformer (core weight 50 kg) was produced for each small group. For each of the three-phase stacked core model transformers that were fabricated, the iron loss characteristics (transformer loss) were measured when the magnetic flux density in the core legs was 1.7 T at a frequency of 50 Hz. The no-load loss was measured for the iron loss characteristics at 1.7 T and 50 Hz using a wattmeter. At the same time, each model transformer was excited in a soundproof room under conditions of maximum magnetic flux density Bm = 1.7 T and frequency of 50 Hz, and the noise level: dBA (transformer noise) was measured using a sound level meter.
[0026] [Table 1]
[0027] The above-mentioned measurement results of transformer loss and transformer noise were compiled into the effect of σBr on transformer loss, and the results are shown in Figure 3. As shown in Figure 3, the transformer iron loss was roughly the same regardless of σBr. This is thought to be because the oblique angle materials were selected so that the average values of Br were the same, and so the average effect of domain refinement was roughly the same. In other words, it was found that the effect of reducing iron loss due to non-heat-resistant domain refinement applied to steel sheets is not affected by the standard deviation of residual magnetic flux density σBr, as long as the average value of residual magnetic flux density Br is roughly the same.
[0028] On the other hand, the measurement results of the above-mentioned transformer noise are summarized as the effect of σBr on the transformer noise, and the results are shown in FIG. 4. As shown in FIG. 4, the transformer noise showed dependency on σBr. The inventors believe that this is because the noise increased due to the increase in the variation of the steel sheet residual magnetic flux when the excitation magnetic field was 0 A / m, which caused irregular vibrations out of phase. In particular, when σBr exceeds 0.38, the noise increases significantly, so if σBr is 0.38 or less, it is possible to improve the transformer noise while maintaining the low iron loss effect due to magnetic domain refinement. As shown in FIG. 4, σBr is more preferably 0.30 or less, even more preferably 0.26 or less, and even more preferably 0.21 or less.
[0029] Hereinafter, preferred embodiments of the present invention will be described in detail. However, the present invention is not limited to the configurations disclosed in the present embodiments, and various modifications are possible without departing from the spirit of the present invention.
[0030] [Grain-oriented electrical steel sheet] In the present invention, the composition of the slab for grain-oriented electrical steel sheet may be any composition that allows secondary recrystallization to occur. When an inhibitor is used, for example, when an AlN-based inhibitor is used, appropriate amounts of Al and N may be contained, and when an MnS·MnSe-based inhibitor is used, appropriate amounts of Mn, Se and / or S may be contained. Of course, both inhibitors may be used in combination. In this case, the preferred contents of Al, N, S and Se are respectively as follows: Al: 0.010~0.065% by mass, N:0.0050~0.0120% by mass, S: 0.005 to 0.030 mass% and Se:0.005~0.030% by mass It is.
[0031] Furthermore, the present invention can also be applied to grain-oriented electrical steel sheets in which the contents of Al, N, S, and Se are limited and no inhibitor is used. In this case, the contents of Al, N, S, and Se are, respectively, Al: less than 0.010% by mass, N: less than 0.0050% by mass, S: less than 0.0050% by mass and Se: less than 0.0050% by mass It is preferable to suppress the
[0032] Representative basic components and optional added components applied to the steel material (slab) for the grain-oriented electrical steel sheet of the present invention will be specifically described below.
[0033] C: 0.08% by mass or less C is added to improve the hot-rolled sheet structure, but if the C content exceeds 0.08 mass%, it becomes difficult to decarburize to 50 mass ppm or less, at which magnetic aging does not occur during the manufacturing process, so the C content is preferably 0.08 mass% or less. Furthermore, since secondary recrystallization occurs even in steel materials that do not contain C, no lower limit is set for the C content.
[0034] Si:2.0~8.0% by mass Although Si is an effective element for increasing the electrical resistance of steel and improving iron loss, if the content is less than 2.0 mass%, the improving effect is not fully exerted, while if the content exceeds 8.0 mass%, the workability and threadability are significantly deteriorated and the magnetic flux density is also reduced. Therefore, the Si content is preferably in the range of 2.0 to 8.0 mass%.
[0035] Mn:0.005~1.0% by mass Mn is an element necessary for improving hot workability, but if the content is less than 0.005 mass%, it is difficult to obtain this effect sufficiently. On the other hand, if the content exceeds 1.0 mass%, the magnetic flux density deteriorates. Therefore, the Mn content is preferably in the range of 0.005 to 1.0 mass%.
[0036] In addition to the above basic components, the following optional additive components, which are known to be effective in improving magnetic properties, may be appropriately contained. Ni: 0.03~1.50% by mass, Sn: 0.01~1.50% by mass, Sb: 0.005~1.50% by mass, Cu:0.03~3.0% by mass, P:0.03~0.50% by mass, Mo: 0.005 to 0.10 mass% and Cr:0.03~1.50% by mass One or more types selected from
[0037] Ni is an effective element for improving the hot-rolled sheet structure and enhancing the magnetic properties. However, if the content is less than 0.03 mass%, the contribution to the magnetic properties is small, while if the content exceeds 1.50 mass%, the secondary recrystallization becomes unstable and the magnetic properties deteriorate. Therefore, the Ni content is preferably in the range of 0.03 to 1.50 mass%.
[0038] In addition, Sn, Sb, Cu, P, Mo, and Cr are also elements that improve magnetic properties, but if the content is less than the lower limit, the effect is insufficient, and if the content exceeds the upper limit, the growth of secondary recrystallized grains is suppressed, resulting in deterioration of magnetic properties. Therefore, it is preferable to set the content of each element within the above range.
[0039] In addition to the above components, the alloy consists of Fe and unavoidable impurities.
[0040] In the manufacture of the grain-oriented electrical steel sheet of the present invention, the steel material (slab) of the grain-oriented electrical steel sheet having the above-mentioned composition is hot-rolled and then hot-rolled sheet annealed. Next, it is cold-rolled once or twice to finish into a steel strip of the final sheet thickness. The steel strip is then decarburized and annealed, coated with an annealing separator mainly composed of MgO, wound into a coil, and subjected to final annealing for the purpose of secondary recrystallization and formation of a forsterite film. The steel strip after the final annealing is then flattened and annealed, and a magnesium phosphate-based tension film is formed to produce a steel strip product.
[0041] The manufacturing method of the grain-oriented electrical steel sheet of the present invention includes a magnetic domain refinement step of introducing thermal strain by energy beam irradiation to the surface of the steel strip of the product sheet, i.e., the grain-oriented electrical steel sheet (steel strip) after the formation of the tensile coating. Even if thermal strain is introduced by energy beam irradiation before the formation of the tensile coating, the thermal strain is relaxed or released by the heat treatment (baking) performed in the formation of the tensile coating, and the desired magnetic domain refinement effect cannot be obtained.
[0042] · Standard deviation σBr of residual magnetic flux density Br is 0.38 or less It is essential that the grain-oriented electrical steel sheet of the present invention has a suppressed variation (deviation) in the residual magnetic flux density Br in the steel sheet. Specifically, it is essential that the standard deviation σBr of the residual magnetic flux density Br in the steel sheet (the value of the sample magnetic flux density B(T) when the strength of the external magnetic field H=0) is 0.38 or less. That is, as described above, if σBr is 0.38 or less, the noise of the transformer can be improved while maintaining the low iron loss effect due to magnetic domain refinement. σBr is preferably 0.36 or less, more preferably 0.34 or less, and even more preferably 0.32 or less. The smaller σBr is, the more significantly the noise of the transformer can be reduced. The lower limit of σBr is not particularly limited, but is theoretically zero.
[0043] The variation in residual magnetic flux density Br, which is the key to this invention, includes those caused by the steel sheet materials such as crystal orientation, internal strain, fine grains, and the amount of precipitates, and those caused by the magnetic domain refinement process, such as the uniformity of thermal strain in the sheet running direction and sheet width direction. Of these, the former has a small effect and is difficult to suppress, but it is effective to suppress the variation in sheet temperature during the rolling and annealing processes.
[0044] On the other hand, the latter is presumed to be caused by a slight change in the heat input form of the energy beam irradiation due to a change in the production line speed during operation. In other words, the greater the amount of thermal strain introduced into the steel sheet, the easier the magnetization reversal becomes, and the lower the residual magnetic flux density Br. Here, in the case of performing the magnetic domain refinement treatment at a constant processing frequency (production line speed / processing interval), if the production line speed changes, the interval of the thermally strained regions existing in the sheet passing direction changes, and the amount of strain per unit area changes depending on the position in the longitudinal direction. As a result, the residual magnetic flux density Br varies in the grain-oriented electrical steel sheet that has been subjected to the magnetic domain refinement treatment. In such a case, it is presumed that it is possible to suppress the variation in Br by changing the amount of heat input according to the production line speed and controlling it so that the amount of strain per unit area is constant.
[0045] On the other hand, if the interval between the thermally distorted regions in the sheet passing direction is constant, the above-mentioned processing frequency changes, and the balance between the scanning and standby times of the energy beam changes. Here, during the beam standby, the energy beam is irradiated onto a beam receiver called a beam collector. If the balance between the scanning and standby times changes, the beam is scattered by fumes and gases generated from the beam receiver, and the proper focus conditions change. In such a case, it is effective to improve σBr by setting proper focus conditions for each production line speed in advance and changing the focus conditions according to the operating line speed. As an example of a method for setting the proper focus, a method is considered in which the beam is continuously irradiated until a steady state is reached in a pattern simulating the actual operating conditions, and the focus is adjusted in that steady state. In addition, even if the above measures are not taken, the variation can be improved by performing magnetic measurements during the production of the oblique angled bar and eliminating the oblique angled bar with a large deviation from the average value, and each measure should be taken in a balanced manner from the viewpoint of man-hours and yield.
[0046] ·Method for measuring standard deviation σBr of residual magnetic flux density Br The method for measuring the standard deviation σBr of the residual magnetic flux density Br in the present invention is as follows. SST test pieces (samples) of 100 mm in width direction × 280 mm in length direction are taken from multiple locations in the longitudinal direction of the grain-oriented electrical steel sheet (steel strip) after the magnetic domain refinement process, and the hysteresis loop is measured by a single sheet magnetic measurement method in accordance with JIS C2556 to calculate the residual magnetic flux density Br (T) of each sample. The standard deviation σBr of Br of all samples calculated in this manner is used as the evaluation standard for the variation of the residual magnetic flux density Br. The number (N) of samples taken in the longitudinal direction of the grain-oriented electrical steel sheet (steel strip) and used for measurement is preferably as large as possible, but there is a concern that the number of steps required for cutting out the samples will increase and the yield will decrease. Therefore, the number of N is preferably 9 to 90, more preferably 15 to 75.
[0047] <Non-heat-resistant magnetic domain refinement> Next, the non-heat-resistant magnetic domain refining used in the magnetic domain refining step of the present invention will be described.
[0048] In order to perform non-heat-resistant magnetic domain refinement, it is effective to use a laser with a wavelength of 400 nm to 1200 nm, which is highly absorbed by metals, or an electron beam with high penetrating power.
[0049] The conditions specific to electron beam irradiation in carrying out the present invention will now be described in more detail.
[0050] Acceleration voltage: 60kV to 300kV The higher the acceleration voltage, the more linear the electrons will travel and the less the thermal effect on the outside of the beam irradiation area will be, which is preferable. For these reasons, the acceleration voltage is set to 60 kV or more, more preferably 90 kV or more, and even more preferably 120 kV or more.
[0051] On the other hand, if the acceleration voltage is too high, it becomes difficult to block the X-rays generated by the electron beam irradiation. Therefore, from a practical standpoint, it is preferable to set the acceleration voltage to 300 kV or less, and more preferably 200 kV or less.
[0052] Beam current: 0.5~40mA From the viewpoint of beam diameter, it is preferable that the beam current is small. This is because if the current is large, the beam diameter is likely to widen due to Coulomb repulsion. Therefore, in the present invention, it is preferable that the beam diameter is 40 mA or less. On the other hand, if the beam current is too small, the energy required to form distortion is insufficient. Therefore, it is preferable that the beam current is 0.5 mA or more.
[0053] - Vacuum level in the beam irradiation area The electron beam is scattered by gas molecules, which causes an increase in the beam diameter and halo diameter, a decrease in energy, etc. Therefore, the degree of vacuum in the beam irradiation area is better, and the pressure is preferably 3 Pa or less. There is no particular lower limit, but if it is lowered too much, the cost of the vacuum system, such as the vacuum pump, will increase. Therefore, in practice, it is recommended to set the lower limit at 10 -5 It is preferable to set the pressure at 1 Pa or more.
[0054] The conditions specific to laser irradiation in carrying out the present invention will now be described in more detail.
[0055] Laser output: 50W or more and 5000W or less When the laser output is low, the scanning speed must be slowed down to provide sufficient energy to impart thermal distortion. At this time, excessive slowing down the speed leads to a deterioration in manufacturing efficiency. On the other hand, while increasing the output makes it easier to impart thermal distortion, it also increases damage to the laser transport system, and increases the frequency of maintenance, which in turn reduces manufacturing efficiency. From the above perspectives, it is preferable to set the laser output to 50W or more and 5000W or less.
[0056] Moreover, the irradiation conditions common to the electron beam irradiation and the laser beam irradiation will be described below.
[0057] Beam or spot diameter: 300μm or less The beam diameter of electron beam irradiation or the spot diameter of laser beam irradiation is preferably smaller because it is possible to locally introduce distortion. Therefore, in the present invention, the beam diameter or spot diameter of the energy beam is preferably 300 μm or less, more preferably 280 μm or less, and even more preferably 260 μm or less. In the present invention, the beam diameter or spot diameter refers to the full width at half maximum of the beam profile of the electron beam or laser beam obtained by the slit method using a slit with a width of 30 μm.
[0058] ·Deflection speed: 5~400m / s The slower the beam deflection speed, the more heat can be incident on the steel plate per unit length, so a slower speed is preferable. However, if the speed is too slow, the processing area per unit time decreases, resulting in a decrease in production efficiency. Therefore, a speed of 5 m / s or more is preferable. Also, if the speed is too high, a power supply capacity is required to provide the heat input required to melt the steel plate, leading to an increase in the size of the equipment. Therefore, a speed of 400 m / s or less is preferable.
[0059] - Angle between thermal distortion direction and rolling direction: within ±30° The more the extension direction of the thermally strained portion is inclined from the sheet width direction, the fewer the magnetic poles generated at the interface between the closure domains and the main domains, and the worse the domain refinement effect. Therefore, it is preferable that the angle between the extension direction of the thermally strained portion and the sheet width direction be within ±30°.
[0060] [Laminated core] The laminated core of the present invention is formed by laminating a plurality of grain-oriented electrical steel sheets of the present invention, in which the standard deviation σBr of the magnetic flux density Br(T) remaining in the steel sheets when the external magnetic field H is 0 is 0.38 or less. Therefore, the laminated core of the present invention can suppress vibrations caused by electromagnetic forces at the joints between the laminated steel sheets, and can achieve both low iron loss and low noise in the transformer.
[0061] The laminated core of the present invention is not particularly limited, but preferably has a structure in which a magnetic circuit is formed by combining cut sheets of multiple grain-oriented electromagnetic steel sheets so that the magnetization direction inside the core coincides with the rolling direction of the grain-oriented electromagnetic steel sheets. An example of such a laminated core is a three-phase stacked core as shown in Fig. 1. This is because a laminated core having such a structure has butt and overlapping parts (joints) between the cut sheets, and electromagnetic vibrations occurring at such parts can be effectively suppressed.
[0062] As an example of a method for manufacturing a laminated core of the present invention, a method for manufacturing a three-phase stacked core composed of three legs 11 and two yokes 12 as shown in FIG. 1 will be described. A strip of grain-oriented electromagnetic steel sheet of the present invention is slit to the desired width of the legs and yokes to produce a sub-strip. This sub-strip is sheared to produce a steel sheet (diagonal bar) to the desired steel sheet length. The shear direction may be 90 degrees (perpendicular to the rolling direction) with respect to the rolling direction, or may be inclined to a certain degree. Also, as in the central leg 11 of FIG. 1, it may be processed into a V-shape. The diagonal bars thus produced are combined to form one layer so that the rolling direction of the steel sheet coincides with the magnetization direction inside the core. In addition, the joints at this time may be configured so that all the steel sheets are present in the same plane (butt joints), or may be configured so that the steel sheets overlap each other at at least one joint (overlap joints). Next, this single layer is stacked in the plate thickness direction to produce a laminated core. In this case, the width of the slits may be changed depending on the thickness direction of the laminated core, and different grain-oriented electrical steel sheets may be used depending on the position inside the structure of the laminated core. The lamination method for the joints may be any one selected from the simple stacking, stepped stacking, and lap stacking shown in Figure 1, and may be a combination of these as necessary.
[0063] In the present invention, apart from the steps and manufacturing conditions described above, known manufacturing methods for grain-oriented electrical steel sheets and laminated cores can be used as appropriate. EXAMPLES
[0064] Next, the present invention will be specifically described based on the examples. The following examples are preferred examples of the present invention, and the present invention is not limited to these examples. The present invention can be modified within the scope of the present invention, and such modifications are also included in the technical scope of the present invention.
[0065] A laser beam or an electron beam was irradiated onto one side of a 300 mm wide product steel strip after finish annealing and insulating coating formation, which was manufactured by a general grain-oriented electrical steel sheet manufacturing process from a steel slab having the composition shown in Table 1 or Table 2, to perform magnetic domain refinement. A conceptual diagram of the sheet passing speed in the manufacturing line for this magnetic domain refinement process is shown in Figure 5. As shown in Figure 5, the manufacturing line speed LS was accelerated at regular intervals and increased from 10 m / min to 140 m / min. Note that "..." in Figure 5 means repeated acceleration and dwell. At this time, the energy beam irradiation conditions were the nine conditions shown in Table 3, and one steel strip was produced for each condition. Note that the beam irradiation interval in the steel sheet passing direction was adjusted to 6 mm when the processing frequency was changed, and was set to 194.4 Hz so that the processing interval was 6 mm at a manufacturing line speed of 70 m / min when the processing frequency was fixed. The beam scanning speed was 120 m / s.
[0066] [Table 2]
[0067] [Table 3]
[0068] From each of the nine steel strips manufactured under the above nine conditions, 45 test pieces (samples) with a width of 100 mm and a length of 280 mm were cut out from each steel strip, and the hysteresis loop of each test piece was measured using the single sheet magnetic measurement method described in JIS C2556, and the residual magnetic flux density Br (T) and its standard deviation σBr were calculated. Then, oblique beams were cut out from each steel strip to manufacture a three-phase stacked core model transformer (core weight 50 kg). For each of the manufactured transformers, the iron loss characteristics were measured when the magnetic flux density of the core leg part was 1.7 T at a frequency of 50 Hz. The iron loss characteristics at 1.7 T and 50 Hz were measured by measuring the no-load loss using a wattmeter. At the same time, the model transformer was excited in a soundproof room under the conditions of maximum magnetic flux density Bm = 1.7 T and frequency of 50 Hz, and the sound level (dBA) was measured using a sound level meter. The results are shown in Table 4.
[0069] From Table 4, it can be seen that the transformers E2, E4, L2, and L4 satisfying the configuration of the present invention have low iron loss and low noise. As in the case of Fig. 4, it can be seen that the smaller σBr, the more remarkable the improvement in transformer noise.
[0070] [Table 4] [Explanation of symbols]
[0071] 1 Bevel 11 Legs 12 Yoke 2 joint
Claims
1. A grain-oriented electrical steel sheet having a plurality of strain regions extending linearly in a direction transverse to the rolling direction and arranged in parallel at intervals in the rolling direction on at least one of the front and back surfaces, A grain-oriented electrical steel sheet, wherein the standard deviation σBr of the residual magnetic flux density Br of a hysteresis loop drawn when the rolling direction is the magnetization direction and the sheet is excited up to 1.7 T is 0.38 or less.
2. The grain-oriented electrical steel sheet according to claim 1 , wherein the standard deviation σBr is 0.36 or less.
3. A laminated core formed by laminating a plurality of grain-oriented electrical steel sheets according to claim 1 or 2.
Citation Information
Patent Citations
Grain oriented electrical steel sheet having excellent magnetic characteristic
JP1986124584A
Laminated iron core of transformer
JP1995094341A
Power switch
US20190385806A1
Grain-oriented electrical steel sheet and method for manufacturing same
WO2017130980A1
Small sized panhead device
JP1994022179A