Phosphor, its manufacturing method, and light-emitting device

A europium-activated alkaline earth chloroapatite phosphor with controlled manufacturing processes achieves high absorption and efficiency, addressing the trade-off in europium concentration for improved white LED performance.

JP7568697B2Active Publication Date: 2024-10-16SEOUL SEMICONDUCTOR
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2022173143
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2016-10-11
Filing Date
2022-10-28
Publication Date
2024-10-16
Estimated Expiration
2037-10-10

AI Technical Summary

Technical Problem

Existing europium-activated apatite phosphors face a trade-off between increasing europium concentration for higher absorption and maintaining internal quantum efficiency, leading to reduced luminous efficiency in white LEDs.

Method used

A europium-activated alkaline earth chloroapatite phosphor with a specific compositional formula (M1-xEu x)5(PO4)3Cl, where M is Sr and Ba, is produced through a multi-step firing process in controlled atmospheres to achieve high absorption rates for near-ultraviolet to blue-violet light while minimizing absorption in the long wavelength range, thereby maintaining high internal quantum efficiency.

Benefits of technology

The phosphor achieves a 90% absorption rate for 400 nm light and 2% or less absorption for 650 nm light, resulting in a luminous efficiency of 83% or more, enhancing the performance of white LEDs by reducing phosphor usage and improving light quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007568697000005
    Figure 0007568697000005
  • Figure 0007568697000006
    Figure 0007568697000006
  • Figure 0007568697000007
    Figure 0007568697000007
Patent Text Reader

Abstract

Provided are a europium-activated alkaline earth chloroapatite phosphor that can increase luminous efficiency without decreasing internal quantum efficiency even when the europium concentration is increased, a method for producing the same, and a light-emitting device using the same. The phosphor of the embodiment has the composition formula: (M 1-x EU x The phosphor has a composition represented by the formula: )5(PO4)3Cl (M is an alkaline earth element including at least Sr and Ba, and x is an atomic ratio satisfying 0.04≦x≦0.2). In the embodiment, the phosphor has an absorptance of 90% or more for light with a wavelength of 400 nm, and an absorptance of 2% or less for light with a wavelength of 650 nm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] Embodiments of the present invention relate to a phosphor, a method for producing the same, and a light-emitting device.

Background Art

[0002] The history of europium-activated apatite phosphors is long, and they have been widely used as a blue light-emitting component in low-pressure mercury lamps typified by fluorescent lamps. In recent years, they have also been tried as phosphors for white light-emitting devices (white LEDs) combined with near-ultraviolet light-emitting diodes, and many proposals have been made. For example, in a light-emitting device combining a near-ultraviolet LED with blue, green, and red phosphors, as a blue light-emitting phosphor, the general formula: (M1,Eu) 10 (PO4)6·Cl2 (where M1 is at least one element of Mg, Ca, Sr, and Ba) of a divalent europium-activated halophosphate phosphor has been proposed for use.

[0003] Furthermore, in a white semiconductor light-emitting element combining a near-ultraviolet LED with blue and yellow phosphors, as a blue light-emitting phosphor, a halophosphate phosphor (M1 1-x Eu x ) 10 (PO4)6Cl2 (where M1 is at least one of Ba, Sr, Ca, and Mg, and x satisfies 0 < x < 1) has been proposed for use. In a white light-emitting device combining a near-ultraviolet LED with green and red phosphors, and further a blue light-emitting phosphor having a composition represented by (Sr,Ca) a Ba b Eu x (PO4) c X d and defining the emission intensity at a wavelength of 490 nm has been proposed. A light-emitting device combining a near-ultraviolet phosphor and a blue phosphor having a composition represented by Eu a Sr b M 5-a-b (PO4) c X d and defining its quantum efficiency has been proposed.

[0004] In this way, in a white LED that combines a near-ultraviolet or purple LED with an emission peak wavelength of 390 to 420 nm and a blue-emitting phosphor, a green and / or yellow-emitting phosphor, a red-emitting phosphor, or a blue-emitting phosphor, a green and / or yellow-emitting phosphor, the europium-activated alkaline earth chloroapatite phosphor represented by the composition formula: M5(PO4)3Cl:Eu is extremely useful as a blue-emitting component.

[0005] Currently, white LEDs that are widely used or being tried out include a type that combines a blue light-emitting diode with a green and / or yellow light-emitting phosphor, and in some cases a red phosphor (hereinafter referred to as Type 1), and a type that combines a near-ultraviolet or purple light-emitting diode with blue, yellow, and red phosphors (hereinafter referred to as Type 2). At present, Type 1 is the most widely used because it is evaluated as having a higher brightness than Type 2, but Type 2 has a wider variety of usable phosphors and is superior in improving the quality of white light, such as high color rendering. Therefore, it is expected to grow as lighting for art galleries and museums where visibility is important, and as lighting for sales floors where it is necessary to make exhibits look vivid. Furthermore, it has recently been revealed that the strong blue light emitted by Type 1 white LEDs may affect the human circadian rhythm and reduce the quality of sleep, and expectations for Type 2 white LEDs are increasing.

[0006] In Type 2 white LEDs, all near-ultraviolet or purple LED light must be converted into visible light using phosphors, which requires a greater amount of phosphor to be used than in Type 1. Furthermore, some of the blue light tends to be absorbed by phosphors that emit light of longer wavelengths (green, yellow, orange, red, etc.), which further increases the mixing ratio of blue-emitting phosphors, so there is a strong demand to improve the luminous efficiency of blue-emitting phosphors, i.e. apatite phosphors, in order to improve the characteristics of white LEDs and reduce the amount of phosphor used.

[0007] The luminous efficiency of a phosphor is expressed as the product of two factors: the internal quantum efficiency (IQE), which indicates the conversion efficiency of the phosphor material, and the absorptance of the excitation light. Luminous efficiency is a comprehensive index that indicates the efficiency of light emission, and is also called external quantum efficiency (EQE). When simply stated as quantum efficiency, this refers to the external quantum efficiency. In order to increase the absorptance of apatite phosphors, it is effective to increase the concentration of the activator Eu, but on the other hand, it is known that the internal quantum efficiency generally decreases as the activator concentration increases. In order to improve the luminous efficiency of phosphors, it is necessary to improve these two characteristic factors that are in a trade-off relationship. Therefore, there is a demand for apatite phosphors that maintain high internal quantum efficiency even in areas with high absorptance by increasing the concentration of the activator europium. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] Patent No. 3954304 [Patent Document 2] Patent No. 3985486 [Patent Document 3] Patent No. 4930649 [Patent Document 4] JP 2004-253747 A Summary of the Invention

[0009] The problem to be solved by the present invention is to provide a europium-activated alkaline earth chloroapatite phosphor that does not decrease the internal quantum efficiency even when the europium concentration is increased and that can increase the luminous efficiency, a method for producing the same, and a light-emitting device using the same.

[0010] The phosphor of the embodiment is Compositional formula: (M 1-x EU x )5(PO4)3Cl (In the formula, M is an alkaline earth element including at least Sr and Ba, and x is 0.04≦x≦0. The atomic ratio satisfies 2. The europium-activated alkaline earth chloroapatite phosphor has a composition represented by the following formula: In the phosphor of the embodiment, the absorptance for light with a wavelength of 400 nm is 90% or more, and the absorptance for light with a wavelength of 650 nm is 2% or less. [Brief description of the drawings]

[0011] [Figure 1] 1 is a diagram showing the relationship between the emission characteristics and Eu concentration of a phosphor according to an embodiment in comparison with a conventional phosphor. [Diagram 2] 1 is a diagram showing a configuration of a light emitting device according to an embodiment; [Diagram 3] FIG. 2 is a graph showing the relationship between the 650 nm absorptance and Eu concentration of the phosphors of the examples and comparative examples and the luminous efficiency (EQE) when excited with light having a wavelength of 400 nm. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS A phosphor according to the present invention, a method for producing the phosphor, and a light emitting device using the phosphor will be described below.

[0013] The europium-activated alkaline earth chloroapatite phosphor of the embodiment is Compositional formula: (M 1-x EU x )5(PO4)3Cl …(1) (In the formula, M is an alkaline earth element including at least Sr and Ba, and x is 0.04≦x≦0. The atomic ratio satisfies 2. It has a composition represented by the formula:

[0014] As a result of various experiments, the inventors of the present application have found that by performing a firing process in a highly reducing atmosphere in addition to the firing process when manufacturing a phosphor, a phosphor can be obtained that maintains a higher internal quantum efficiency than conventional phosphors even in a region with high absorptivity by increasing the concentration of europium as an activator. Furthermore, they have found that such a relatively high internal quantum efficiency is widely present in a region with low absorptivity in the long wavelength region of visible light. That is, in the europium-activated alkaline earth chloroapatite phosphor of the embodiment, the europium concentration is 4 mol % or more relative to the sum of the alkaline earth element M and europium, the reflectance at the excitation wavelength is less than 10%, and the diffuse reflectance corresponding to the host coloring at a wavelength sufficiently longer than the emission wavelength is 98% or more.

[0015] In order to increase the absorptance of the europium-activated alkaline earth chloroapatite phosphor to near-ultraviolet or blue-violet excitation light with a wavelength of 390 to 420 nm, it is effective to increase the europium concentration. Specifically, it is effective to make the europium concentration 4 mol % or more relative to the sum of the alkaline earth element M and europium. This makes it possible to make the diffuse reflectance to light with a wavelength of 400 nm, which is a typical blue-violet excitation light, less than 10%, that is, to make the absorptance to light with a wavelength of 400 nm 90% or more.

[0016] On the other hand, the inventors of the present application have found that there is a correlation between the absorptance for light in the long wavelength region where the effects of absorption and emission by europium can be ignored, for example, at a wavelength of 650 nm, and the internal quantum efficiency. That is, by making the absorptance for light at a wavelength of 650 nm 2% or less, in other words, by making the diffuse reflectance for light at a wavelength of 650 nm 98% or more, it is possible to realize a high internal quantum efficiency, and thereby to obtain a high luminous efficiency.

[0017] As described above, the europium-activated alkaline earth chloroapatite phosphor of the embodiment has an absorptance of 90% or more for light with a wavelength of 400 nm and 2% or less for light with a wavelength of 650 nm. That is, the concentration of europium relative to the sum of the alkaline earth element M and europium is 4 mol% or more, the absorptance of light with a wavelength of 400 nm, which is a typical blue-violet excitation light, is 90% or more, and the absorptance of light with a wavelength of 650 nm in the long wavelength range where the influence of absorption and emission by europium is negligible is 2% or less, thereby realizing high internal quantum efficiency. As a result, it is possible to provide a europium-activated alkaline earth chloroapatite phosphor that exhibits high luminous efficiency.

[0018] In the europium-activated alkaline earth chloroapatite phosphor of the embodiment, as described above, the concentration of europium is 4 mol% or more with respect to the sum of the alkaline earth element M and europium (the value of x (atomic ratio) in formula (1) is 0.04 or more). This allows the absorptivity for light with a wavelength of 400 nm to be increased. Furthermore, in order to further increase the absorptivity for light with a wavelength of 400 nm, the concentration of europium is preferably 7 mol% or more with respect to the sum of the alkaline earth element M and europium (x: 0.07 or more). However, if the concentration of europium becomes too high, the luminance of the phosphor decreases, so the concentration of europium is preferably 20 mol% or less with respect to the sum of the alkaline earth element M and europium (x: 0.20 or less), more preferably 17 mol% or less (x: 0.17 or less), and even more preferably 12 mol% or less (x: 0.12 or less).

[0019] In the europium-activated alkaline earth chloroapatite phosphor of the embodiment, the M element is an alkaline earth element including at least strontium (Sr) and barium (Ba). The M element may include alkaline earth elements magnesium (Mg) and calcium (Ca) in addition to Sr and Ba. However, since the luminescence characteristics of the alkaline earth chloroapatite phosphor decrease when the content of Mg and Ca increases, the total content of Mg and Ca is preferably 2 mol % or less with respect to the sum of the alkaline earth element M and europium. The content ratio of Sr and Ba is not particularly limited, but in order to improve the luminescence characteristics, it is preferable that the Ba content is in the range of 5 to 80 mol % with respect to the sum of the alkaline earth element M and europium, and the remainder except Eu is Sr or a mixture of Sr and a small amount of Ma and / or Ca.

[0020] FIG. 1 shows the characteristic values ​​of the emission characteristics of the phosphor of the embodiment, i.e., the absorptance (solid line), internal quantum efficiency (IQE / dashed line), and luminous efficiency (EQE / dotted line) at an excitation wavelength of 400 nm, versus europium concentration. FIG. 1 also shows characteristic values ​​of a conventional phosphor. Europium-activated alkaline earth chloroapatite phosphor ((M 1-x EU x The absorptance of )5(PO4)3Cl (where M is an alkaline earth element including at least Sr and Ba) increases with increasing europium concentration in the region where the europium concentration (x×100 in the composition formula above is shown as the europium concentration (%) in Figure 1) is low, reaches a maximum at about 7%, and remains at about 20%. This behavior of absorptance versus europium concentration is roughly the same in conventional phosphors.

[0021] On the other hand, the internal quantum efficiency (IQE) shows a maximum value when the europium concentration is in the vicinity of 5 to 10%, and gradually decreases as the europium concentration increases. Although only this tendency of IQE is observed in both the phosphor of the embodiment and the conventional phosphor, the phosphor of the embodiment always shows a higher value (IQE value) than the conventional phosphor, and even in a high europium concentration range of 20%, the internal quantum efficiency maintains a remarkably high value of 90%. Until now, it has been recognized that the luminous efficiency (EQE), which is given as the product of the absorptance and the internal quantum efficiency, shows a peak value when the europium concentration is 5 to 10%, and then gradually decreases, as a characteristic of conventional europium-activated alkaline earth chloroapatite phosphors. However, in the phosphor of the embodiment, the internal quantum efficiency shows a high value (90% or more) over a wide range of europium concentrations, and thereby the luminous efficiency is also maintained at a high value.

[0022] Conventionally, the causes of the decrease in internal quantum efficiency when the europium concentration is high have been thought to be that the activator itself is an impurity in the phosphor crystal, and that this causes crystal defects such as distortion due to the size difference between the europium ion and the element ion it replaces, and that when the valence of the activator element ion differs from that of the element ion it replaces, this causes crystal defects, etc. Such defects themselves affect the light emission process, reducing efficiency, or have the effect of removing light necessary for determining efficiency from the process by coloring, etc.

[0023] The reason why the phosphor of the embodiment maintains a high internal quantum efficiency over a wide range of europium concentrations is not necessarily clear, but in view of the manufacturing method of the phosphor of the embodiment, it is believed that the europium ions are almost unified to a desirable valence of +2 by multi-stage firing under controlled atmosphere, and the effective activator contributing to the light emission process is increased. Furthermore, it is believed that the mismatch between the valence of the element ion substituted by the europium ion is eliminated, and coloration caused by crystal defects is reduced. The phosphor of the embodiment exhibits light emission characteristics that are clearly superior to conventional phosphors.

[0024] In the above embodiment, the absorptance of the phosphor for light with a wavelength of 400 nm is measured as follows. That is, light from a light source such as a xenon lamp is split into monochromatic light with a wavelength of 400 nm and a half-width of 10 nm or less, and is irradiated onto a standard white sample such as Spectralon or barium sulfate powder. The diffuse reflected light from the white sample is collected using an integrating sphere, and the number of photons in the wavelength region of the irradiated light centered on a wavelength of 400 nm is measured to obtain the number of photons of the incident light. Next, a phosphor sample is placed in place of the white sample, and the diffuse reflected light when irradiated with monochromatic light with a wavelength of 400 nm is collected using an integrating sphere in the same manner, and the number of photons in the wavelength region of the irradiated light is measured to obtain the number of photons of the reflected light of the sample. The number of absorbed photons is the number of photons of the incident light minus the number of photons of the reflected light, and the value of the absorptance for light with a wavelength of 400 nm can be obtained by dividing this by the number of photons of the incident light. Such measurements can be performed using a spectrometer such as a Hamamatsu Photonics C9920 absolute PL quantum yield measurement device.

[0025] The absorptivity of a phosphor for light with a wavelength of 650 nm is measured as follows. That is, light from a light source such as a xenon lamp is split into monochromatic light with a wavelength of 650 nm and a half-width of 10 nm or less, which is irradiated onto a standard white sample, and the diffuse reflected light from the white sample is collected using an integrating sphere, and the number of photons in the wavelength region of the irradiated light centered on a wavelength of 650 nm is measured and taken as the number of photons of the incident light. Next, a phosphor sample is placed in place of the white sample, and the diffuse reflected light when irradiated with monochromatic light with a wavelength of 650 nm is collected using an integrating sphere in the same manner, and the number of photons in the wavelength region of the irradiated light is measured and taken as the number of photons of the reflected light of the sample. As in the case of a wavelength of 400 nm, the number of absorbed photons is obtained by subtracting the number of photons of the reflected light from the number of photons of the incident light, and the value of the absorptivity for light with a wavelength of 650 nm can be obtained by dividing this by the number of photons of the incident light.

[0026] Next, a method for producing the phosphor of the embodiment will be described. The manufacturing method of the embodiment is characterized in that a phosphor is produced by multi-stage firing in a controlled atmosphere in order to obtain the phosphor of the embodiment described above. In producing a europium-activated apatite phosphor, the valence of europium ions needs to be divalent, so firing in a reducing atmosphere is essential. However, the inventors of the present application have found that even if an apatite phosphor is directly synthesized in a reducing atmosphere, when the europium concentration is high, the absorption in the long wavelength region is large, that is, the internal quantum efficiency is low. Furthermore, they have found that an apatite phosphor with high internal quantum efficiency can be produced by generating apatite crystals in an atmosphere containing oxygen such as air and then firing in a high-temperature reducing atmosphere, thereby suppressing absorption in the long wavelength region.

[0027] Therefore, the method for producing a phosphor of the embodiment includes the steps of mixing europium oxide, alkaline earth metal hydrogen phosphate, alkaline earth metal chloride, and alkaline earth metal carbonate to obtain a raw material mixture, firing the raw material mixture at a temperature in the range of 800° C. to 1200° C. in an oxygen-containing atmosphere to obtain a first fired product, and firing the first fired product at a temperature in the range of 1000° C. to 1400° C. in a mixed gas atmosphere containing 1% by volume to 90% by volume of hydrogen and an inert gas to obtain a europium-activated alkaline earth chloroapatite phosphor. The method for producing a phosphor will be described in detail below.

[0028] First, as starting materials, compounds with a purity of 3N or higher, such as barium carbonate (BaCO3), strontium carbonate (SrCO3), barium hydrogen phosphate (BaHPO4), strontium hydrogen phosphate (SrHPO4), barium chloride (BaCl2·2H2O), strontium chloride (SrCl2·6H2O), and europium oxide (Eu2O3), are used. The combination of raw materials is not limited to these, and it is acceptable to contain small amounts of calcium and magnesium compounds, which are alkaline earth metals like barium and strontium. The limit is about 2 mol% of the sum of the alkaline earth elements and europium.

[0029] The starting materials are weighed out so as to obtain a predetermined molar ratio of phosphor. At this time, since the chloride of alkaline earth metal also functions as a flux, it is preferable to use an excess amount of chlorine of 2 to 4 times the amount calculated from the composition of apatite, and it is preferable to increase the amount of alkaline earth element and europium accordingly. These starting materials are mixed by dry mixing using a V-type blender to obtain a raw material mixture. Of course, it is also possible to wet mix all of them or wet mix some of them and then dry mix them.

[0030] Next, the obtained raw material mixture is filled into, for example, an alumina crucible and fired in an oxygen-containing atmosphere at a temperature of 800°C to 1200°C for 2 to 8 hours. The firing temperature is more preferably 900°C to 1100°C. The firing time is more preferably 3 to 6 hours. The oxygen-containing firing atmosphere can be air or a mixed gas atmosphere such as an inert gas containing a few percent of oxygen (first firing step).

[0031] Next, the product (first fired product) obtained in the first firing step is fired in a mixed gas atmosphere of hydrogen and inert gas at a temperature of 1000°C to 1400°C for 2 to 8 hours (second firing step). In this case, in the second firing step, the first fired product may be fired as it is, or the first fired product may be temporarily removed from the alumina crucible, the product may be crushed, and then filled into the alumina crucible and fired. The firing in the reducing atmosphere may be repeated, for example, by further carrying out a third firing step.

[0032] In the firing step in a reducing atmosphere, the inert gas may be a rare gas such as nitrogen or argon, and may be used alone or in a mixture of these gases. In the mixed gas of hydrogen and an inert gas, the hydrogen ratio is in the range of 1 to 90% by volume ratio (%). If the hydrogen ratio is less than 1%, the reducing atmosphere is insufficient, and the valence of europium ions cannot be sufficiently made bivalent. If the hydrogen ratio exceeds 90%, the properties of the phosphor deteriorate. The hydrogen volume ratio is more preferably 5 to 80%. The second firing step is more preferably performed by firing at a temperature of 1100 to 1300°C for 3 to 6 hours.

[0033] The fired product obtained through the first and second firing steps may contain residual alkaline earth chlorides as flux, and it is preferable to remove these by washing with water. In this case, it is more preferable to use warm water, since this promotes the removal of the flux. The washed fired product is filtered, dried, and further sieved to obtain the europium-activated alkaline earth chloroapatite phosphor of the embodiment.

[0034] The phosphor thus obtained emits bright blue light, specifically, blue light with a luminous efficiency of 83% or more, when excited with near-ultraviolet or blue-violet light having a peak wavelength of 390 nm or more and 420 nm or less. The peak wavelength of the blue light emission is in the range of 445 nm or more and 465 nm or less. The average particle size of the phosphor is in the range of 10 to 40 μm, and can be controlled mainly by changing the firing temperature and time in the first and second firing steps. The average particle size is the 50% value of the particle size distribution obtained by a dry laser diffraction method (Heroes & Rodos). When excited with near-ultraviolet or blue-violet light having a peak wavelength of 390 to 420 nm, the larger the particle size, the higher the luminance tends to be, and in this case, the average particle size is more preferably in the range of 20 to 35 μm.

[0035] The europium-activated alkaline earth chloroapatite phosphor (blue phosphor) of the embodiment is used, for example, in the light-emitting portion of a light-emitting device. Fig. 2 shows the configuration of a packaged white light-emitting device as an example of the light-emitting device of the embodiment. The white light-emitting device 1 shown in Fig. 2 includes an LED chip 2 that emits near-ultraviolet to blue-violet light with a peak wavelength in the range of 390 nm to 420 nm, a base portion 3 on which the LED chip 2 is mounted, a transparent resin layer 4 provided so as to cover the LED chip 2, and a phosphor layer 5 provided on the transparent resin layer 4 as a light-emitting portion.

[0036] The phosphor layer 5 as a light-emitting part contains the europium-activated alkaline earth chloroapatite phosphor of the embodiment as a blue phosphor. Furthermore, when the phosphor layer 5 is used as a white light-emitting part, the phosphor layer 5 contains a yellow phosphor in addition to the blue phosphor so that white light is emitted from the phosphor layer 5 when the near-ultraviolet or blue-violet light emitted from the LED chip 2 is irradiated onto the phosphor layer 5. The phosphor layer 5 may contain a blue phosphor and a green or yellow phosphor and a red phosphor. As the phosphor other than the blue phosphor, various known phosphors can be used, and the composition of the other phosphors is not particularly limited.

[0037] The phosphor layer 5 may be, for example, a mixed layer of phosphor and resin. Such phosphor layer 5 is formed, for example, by applying a mixture of phosphor and resin (phosphor paste) on the transparent resin layer 4 and curing it. The transparent resin layer 4 is formed as necessary, and may be omitted. When the peak wavelength of the LED chip 2 is in the range of 390 to 420 nm, the transparent resin layer 4 can reduce the leakage of ultraviolet light, reduce the impact on the human body, and suppress deterioration of peripheral members. The phosphor layer 5 may be produced by not only applying phosphor paste and curing it, but also by covering the LED chip 2 with a molded body obtained by molding the phosphor paste into a cap shape.

[0038] 3 shows a structure in which one LED chip 2 is provided with one phosphor layer 5 (one-chip type white light-emitting device), but the present invention is not limited to this and may have a structure in which multiple LED chips are covered with a phosphor layer (multi-chip type white light-emitting device). In addition, other components such as a lens or a cover may be attached to the white light-emitting device 1 as necessary. Furthermore, the phosphor layer 5 may be formed by filling a concave or cylindrical member that functions as a reflector or the like. In this case, the LED chip 2 is disposed in the concave or cylindrical member. EXAMPLES

[0039] Next, specific examples of the present invention and the evaluation results thereof will be described.

[0040] (Raw material powder composition) In producing the phosphors of Examples 1 to 6 and Comparative Examples 1 to 9 shown below, the following powders of europium oxide (Eu2O3), barium hydrogen phosphate (BaHPO4), barium carbonate (BaCO3), barium chloride (BaCl2·2H2O), strontium hydrogen phosphate (SrHPO4), strontium carbonate (SrCO3), strontium chloride (SrCl2·6H2O), and calcium chloride (CaCl2), all with a purity of 3N or higher, were used as raw materials. 1-x EU x )5(PO4)3Cl (M 1-x EU x Each raw material powder was weighed into the same plastic bag so that the element ratio of the ) part was the ratio shown in Table 1. These were mixed in the plastic bag and used as the raw material mixture. Below, the europium (Eu) concentration [%] is shown as the value of [x × 100 (%)].

[0041] [Table 1]

[0042] (Example 1 / Eu concentration: 7%) The raw material mixture was filled into an alumina crucible and fired in an air atmosphere at 1000°C for 5 hours. The fired product was then fired in an atmosphere of 50% by volume of hydrogen and 50% by volume of nitrogen at 1200°C for 5 hours while still filled in the alumina crucible. The fired product was washed with water to obtain a phosphor powder of Example 1. The phosphor had an absorptivity of 92% at 400 nm and 1.5% at 650 nm. When excited at a wavelength of 400 nm, it emitted blue light at a peak wavelength of 454 nm and had a high luminous efficiency of 88%.

[0043] (Example 2 / Eu concentration: 10%) The raw material mixture was filled into an alumina crucible and fired in an air atmosphere at 1000°C for 5 hours. The fired product was then fired in an atmosphere of 50% by volume of hydrogen and 50% by volume of nitrogen at 1200°C for 5 hours while still filled in the alumina crucible. The fired product was washed with water to obtain a phosphor powder of Example 2. The phosphor had an absorptivity of 92% at 400 nm and 1% at 650 nm. When excited at a wavelength of 400 nm, it emitted blue light at a peak wavelength of 455 nm and had a high luminous efficiency of 88%.

[0044] (Example 3 / Eu concentration: 15%) After the first firing under the same conditions as in Example 1, the first firing product was filled in an alumina crucible and then subjected to a second firing at 1000°C for 5 hours in a mixed atmosphere of 5% hydrogen by volume and 95% nitrogen by volume. The second firing product was filled in an alumina crucible and then subjected to a third firing at 1200°C for 5 hours in a mixed atmosphere of 50% hydrogen by volume and 50% nitrogen by volume. The fired product was washed with water to obtain a phosphor powder of Example 3. The phosphor had an absorptivity of 92% at 400 nm and 1.3% at 650 nm. When excited at a wavelength of 400 nm, the peak wavelength was 456 nm, and blue light was emitted, with a high luminous efficiency of 84%.

[0045] (Example 4 / Eu concentration: 20%) Except for the Eu concentration being 20%, multi-stage firing was carried out three times under the same conditions as in Example 3. The resulting fired product was washed with water to obtain a phosphor powder of Example 4. This phosphor had an absorptivity of 92% at 400 nm and 1.8% at 650 nm. When excited at a wavelength of 400 nm, it emitted blue light with a peak wavelength of 458 nm and a high luminous efficiency of 83%.

[0046] (Example 5 / Eu concentration: 10%) Except for the Eu concentration being 10%, multi-stage firing was performed three times under the same conditions as in Example 3. The resulting fired product was washed with water to obtain a phosphor powder of Example 5. This phosphor had an absorptivity of 92% at 400 nm and 1.7% at 650 nm. When excited at a wavelength of 400 nm, it emitted blue light with a peak wavelength of 455 nm and a high luminous efficiency of 85%.

[0047] (Example 6 / Eu concentration: 7%) Except for the secondary firing atmosphere being a mixture of 5 volume % hydrogen and 95 volume % nitrogen, firing was performed twice under the same conditions as in Example 1. The resulting fired product was washed with water to obtain phosphor powder of Example 6. This phosphor had an absorptivity of 92% at 400 nm and 1.0% or less at 650 nm. When excited at a wavelength of 400 nm, it emitted blue light with a peak wavelength of 455 nm and a high luminous efficiency of 90%.

[0048] (Comparative example 1 / Eu concentration: 1%) The raw material mixture was filled into an alumina crucible and fired at 1200°C for 5 hours in a nitrogen atmosphere containing 5% by volume of hydrogen. The fired product was washed with water to obtain a phosphor powder of Comparative Example 1. This phosphor had an absorptivity of 78% at 400 nm and 3.1% at 650 nm. When excited at a wavelength of 400 nm, it emitted blue light with a peak wavelength of 450 nm, but due to the low absorptivity, the luminous efficiency (EQE) was a low value of 53%.

[0049] (Comparative example 2 / Eu concentration: 7%) The raw material mixture was filled into an alumina crucible and fired at 1200°C for 5 hours in a nitrogen atmosphere containing 5% by volume of hydrogen. The fired product was washed with water to obtain a phosphor powder of Comparative Example 2. This phosphor had an absorptivity of 92% at 400 nm and 5.7% at 650 nm. When excited at a wavelength of 400 nm, it emitted blue light with a peak wavelength of 454 nm, and had a luminous efficiency of 82%, which was improved compared to Comparative Example 1, but was still insufficient.

[0050] (Comparative example 3 / Eu concentration: 10%) The raw material mixture was filled into an alumina crucible and fired at 1200°C for 5 hours in a nitrogen atmosphere containing 5% by volume of hydrogen. The fired product was washed with water to obtain a phosphor powder of Comparative Example 3. The phosphor had an absorptivity of 91% at 400 nm, which was equivalent to that of Comparative Example 2. The absorptivity of 3.2% at 650 nm was. When excited at a wavelength of 400 nm, the peak wavelength was 454 nm, indicating blue light emission, and the luminous efficiency was 76%, lower than that of Comparative Example 2.

[0051] (Comparative example 4 / Eu concentration: 1%) Except for the Eu concentration being 1%, firing was performed twice under the same conditions as in Example 1, and the fired product was washed with water to obtain a phosphor powder of Comparative Example 4. This phosphor had an absorptivity of 79% at 400 nm and an absorptivity of 1.0% at 650 nm. When excited at a wavelength of 400 nm, it emitted blue light with a peak wavelength of 450 nm, but the luminous efficiency was a low value of 67% due to the low Eu concentration.

[0052] (Comparative example 5 / Eu concentration: 3%) Except for the Eu concentration being 3%, firing was performed twice under the same conditions as in Example 1, and the fired product was washed with water to obtain a phosphor powder of Comparative Example 5. This phosphor had an absorptivity of 88% at 400 nm and 1.1% at 650 nm. When excited at a wavelength of 400 nm, it emitted blue light with a peak wavelength of 451 nm. Although this was an improvement over Comparative Example 4, the luminous efficiency was a low value of 76% due to the low Eu concentration.

[0053] (Comparative Example 6 / Eu concentration: 15%) The phosphor powder of Comparative Example 6 was obtained by firing under the same conditions as Comparative Example 1, except that the Eu concentration was 15%, and washing the fired product with water. The phosphor had an absorptivity of 92% at 400 nm and 2.9% at 650 nm. When excited at a wavelength of 400 nm, the peak wavelength was 455 nm, and blue light was emitted. Although the Eu concentration was increased, the luminous efficiency remained low at 77%.

[0054] (Comparative Example 7 / Eu concentration: 20%) Except for the Eu concentration being 20%, firing was performed under the same conditions as in Comparative Example 1, and the fired product was washed with water to obtain a phosphor powder of Comparative Example 7. This phosphor had an absorptivity of 92% at 400 nm and 2.8% at 650 nm. When excited at a wavelength of 400 nm, it emitted blue light with a peak wavelength of 457 nm, but the luminous efficiency was 72%, lower than that of Comparative Example 6, probably due to the increased Eu concentration.

[0055] (Comparative Example 8 / Eu concentration: 10%) The phosphor powder of Comparative Example 8 was obtained by firing under the same conditions as Comparative Example 3, except that the atmosphere for the primary firing was a nitrogen atmosphere containing 50 volume % hydrogen, and washing the fired product with water. The phosphor had an absorptivity of 92% at 400 nm and 4.8% at 650 nm. When excited at a wavelength of 400 nm, the peak wavelength was 453 nm and blue light was emitted, but the luminous efficiency was 80%, which was an improvement over Comparative Example 3 but was still insufficient.

[0056] (Comparative Example 9 / Eu concentration: 10%) The phosphor powder of Comparative Example 9 was obtained by firing under the same conditions as in Example 2, except that the primary firing atmosphere was a nitrogen atmosphere containing 5 volume % hydrogen, and washing the fired product with water. The phosphor had an absorptivity of 92% at 400 nm and 5.3% at 650 nm. When excited at a wavelength of 400 nm, the peak wavelength was 454 nm, and blue light was emitted. However, since the primary firing atmosphere was an oxygen-free atmosphere, the luminous efficiency was 81%, which was not as high as in Example 2 and was insufficient.

[0057] Table 2 shows the manufacturing conditions of the phosphors shown in the Examples and Comparative Examples. Table 3 shows the luminescence characteristics of the phosphors obtained in the Examples and Comparative Examples.

[0058] [Table 2]

[0059] [Table 3]

[0060] From Tables 1 to 3, it can be seen that the high luminescence characteristics of the phosphors of the examples are obtained when a specific range of europium concentration (4% or more) is applied, an oxygen-containing atmosphere such as air is used as the primary firing atmosphere, and firing is then repeated in an oxygen-free highly reducing atmosphere. As an alternative to phosphor specifications in the manufacturing conditions, the absorptivity of the phosphors in the long wavelength range was investigated. Table 3 also shows the measured absorptivity of the phosphors at a wavelength of 650 nm.

[0061] FIG. 3 is a contour plot of the luminous efficiency (EQE) of the phosphor with the absorptance and Eu concentration of the phosphor at a wavelength of 650 nm as variables. The contour plot is divided into five regions of EQE: 90 or more, 85-90, 80-85, 75-80, and 75 or less, and illustrates examples and comparative examples that serve as the basis. The phosphor of the example has a europium concentration of 4% or more, an absorptance at 650 nm of 2% or less, and shows high luminous efficiency. Even in this region, the efficiency is particularly high when the europium concentration is 7-12%. Since the internal quantum efficiency (IQE) of the phosphor is high in this region, the near-ultraviolet light of 400 nm absorbed by the phosphor can be converted to blue light with almost no loss.

[0062] In the contour map of FIG. 3, it is seen that the luminous efficiency is relatively high in some regions where the absorption rate of light at 650 nm exceeds 5%. In reality, phosphors do not absorb light in such long wavelength regions, and phosphors with low absorption values ​​are desirable. The phosphor of the embodiment emits blue light at 450 nm, but is not usually used alone, but is used in combination with a yellow or red emitting phosphor. If the blue phosphor contained in such a mixed phosphor absorbs light in the long wavelength region around 650 nm, the overall efficiency of the light emitting device decreases, which is not preferable.

[0063] Next, a white LED was produced by combining the blue-emitting europium-activated alkaline earth chloroapatite phosphor of Example 1 with a purple LED having a peak wavelength of 405 nm and a yellow phosphor (Ba, Sr)2SiO4:Eu phosphor having an emission peak wavelength of 560 nm. Similarly, a similar white LED was produced using the blue-emitting europium-activated alkaline earth chloroapatite phosphor of Comparative Example 1. The ratio of the blue phosphor to the yellow phosphor was adjusted so that the chromaticity of the white light emitted from the white LED was (0.3, 0.3). Table 4 shows the emission characteristics of the white LEDs of the examples and comparative examples. The white LED using the blue phosphor of Example 1 showed a luminance that was 10% higher than that using the blue phosphor of Comparative Example 1. The luminance shown in Table 4 is a relative value when the luminance of the comparative example is set to 100.

[0064] [Table 4]

[0065] Although several embodiments of the present invention have been described, these embodiments are presented as examples and are not intended to limit the scope of the invention. These novel embodiments may be embodied in various other forms, and various omissions, substitutions, and modifications may be made without departing from the spirit of the invention. These embodiments and modifications are included within the scope and spirit of the invention, and are included in the scope of the invention and its equivalents as set forth in the claims. [Industrial Applicability]

[0066] Currently, in the field of lighting, there is a shift from conventional light bulbs and fluorescent lamps to white LEDs. It is expected that in the future, there will be a shift from lighting that emphasizes efficiency to light quality that is more natural looking and gentle on the human body. The blue-emitting europium-activated alkaline earth chloroapatite phosphor of the present invention is useful for improving this quality of light, and is expected to see further growth in the future.

Claims

1. Composition formula: (M 1-x Eu x ) 5 (PO4) 3 Cl (Here, M is an alkaline earth element consisting of Sr and Ba, the atomic ratio of Sr is 5.15 to 6.15 with respect to the atomic ratio of Ba, and x is an atomic ratio satisfying 0.07≦x≦0.2.) A europium-activated alkaline earth chloroapatite phosphor having a composition represented by the formula: The phosphor has a luminous efficiency of 83% or more when excited with near ultraviolet to blue-violet light having a peak wavelength in the range of 390 nm to 420 nm.

2. 2. The phosphor according to claim 1, wherein the phosphor has an absorptivity of 90% or more for light with a wavelength of 400 nm and an absorptivity of 2% or less for light with a wavelength of 650 nm.

3. 2. The phosphor according to claim 1, wherein x in the composition formula is 0.07 or more and 0.17 or less.

4. 2. The phosphor according to claim 1, wherein x in the composition formula is 0.07 or more and 0.12 or less.

5. 5. The phosphor according to claim 1, wherein the phosphor has an emission peak wavelength in the range of 445 nm to 465 nm when excited with near-ultraviolet to blue-violet light having a peak wavelength in the range of 390 nm to 420 nm.

6. A method for producing the europium-activated alkaline earth chloroapatite phosphor of claim 1, comprising the steps of: mixing europium oxide, an alkaline earth metal hydrogen phosphate, an alkaline earth metal chloride, and an alkaline earth metal carbonate to obtain a raw material mixture; Firing the raw material mixture in an oxygen-containing atmosphere at a temperature in the range of 800° C. to 1200° C. to obtain a first fired product; Firing the first fired product at a temperature of 1000° C. or more and 1400° C. or less in a mixed gas atmosphere containing 1 vol % or more and 90 vol % or less of hydrogen and an inert gas to obtain the europium-activated alkaline earth chloroapatite phosphor. A method for producing a phosphor comprising the steps of:

7. The method comprises performing firing a plurality of times at a temperature of 1000° C. or more and 1400° C. or less in an atmosphere of a mixed gas containing 1 vol % or more and 90 vol % or less of hydrogen and an inert gas, The method for producing a phosphor according to claim 6 , wherein the volume ratio of said hydrogen in said mixed gas atmosphere in the last firing among said plurality of firings is the highest among said plurality of firings.

8. A light-emitting portion comprising the europium-activated alkaline earth chloroapatite phosphor according to any one of claims 1 to 5; a semiconductor light emitting element that irradiates the light emitting portion with near ultraviolet to blue-violet light having a peak wavelength in the range of 390 nm to 420 nm; A light emitting device comprising:

9. In addition to the light emitting section and the semiconductor light emitting element according to claim 8, By providing at least one of a reflector, a lens, and a cover, A light-emitting device that can be used as a lighting fixture.

10. 10. The light emitting device according to claim 8, wherein the light emitting section emits white light excited by the near ultraviolet to blue-violet light emitted from the semiconductor light emitting element.

Citation Information

Patent Citations

  • JP1974030649A

  • Light emitting device and lighting device using same

    JP2004253747A

  • Fluophor and manufacturing method therefor, fluophor-containing composition and light-emitting device using fluophor and image display device and luminaire using light-emitting device

    JP2016053179A

  • light emitting device

    JP3954304B2

  • Semiconductor light-emitting element and light-emitting device using the same

    JP3985486B2