Chloroprene polymer latex composition and dip-molded product
A chloroprene polymer latex mixture with chloroprene and 2,3-dichloro-1,3-butadiene copolymer achieves high strength and flexibility in dip-molded products, addressing allergy and cost issues by omitting sulfur and vulcanization accelerators.
Patent Information
- Application Number
- JP2023508924
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-03-23
- Filing Date
- 2022-03-07
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2042-03-07
AI Technical Summary
Chloroprene polymer latex coatings for dip-molded products, such as gloves and catheters, require high flexibility and mechanical strength but often use sulfur and vulcanization accelerators that cause type IV allergies and increase costs.
A chloroprene polymer latex composition comprising a mixture of chloroprene polymer latex A and B, where latex B includes a copolymer of chloroprene and 2,3-dichloro-1,3-butadiene, with specific molecular weights and insoluble content, to achieve high breaking strength and flexibility without sulfur or vulcanization accelerators.
The composition results in dip-molded coatings with excellent flexibility and mechanical strength, reducing the risk of allergies and production costs by eliminating the need for sulfur and vulcanization accelerators.
Smart Images

Figure 0007568829000001 
Figure 0007568829000002 
Figure 0007568829000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a chloroprene polymer latex composition and a dip-molded article. More specifically, the present invention relates to a chloroprene polymer latex composition containing a copolymer of chloroprene and 2,3-dichloro-1,3-butadiene, and a dip-molded article using the chloroprene polymer latex composition. [Background technology]
[0002] Chloroprene polymers are known as materials for dip-molded products such as medical surgical gloves, medical examination gloves, industrial gloves, balloons, catheters, rubber boots, and the like.
[0003] Various techniques have been proposed for improving the flexibility of chloroprene polymers or for chloroprene polymers for dip-molded products. The following Patent Document 1 describes that for vibration-proof rubber applications, mixing with a low-molecular-weight chloroprene polymer having a number-average molecular weight in the range of 500 to 50,000 improves damping performance. The following Patent Document 2 describes a polychloroprene latex with a pH of 7 to 14, which contains 100 parts by mass of modified polychloroprene obtained by copolymerizing chloroprene and methacrylic acid, 90 to 150 parts by mass of water, 1 to 5 parts by mass of an emulsifier, and 0.5 to 2.5 parts by mass of potassium ions, for dip-molded product applications. The following Patent Document 3 describes a mercaptan-modified polychloroprene latex for use in dip-molded products, which is obtained by copolymerizing chloroprene and 2,3-dichloro-1,3-butadiene, and in the 13C-solid NMR spectrum of the polychloroprene, the peak area (A) at 126.2 to 127.6 ppm, the peak area (B) at 122.0 to 126.2 ppm, and the peak area (C) at 129.9 to 130.3 ppm are in the ranges shown by the following general formula (I). The following Patent Document 4 describes a chloroprene polymer latex for use in dip-molded products, which contains high molecular weight and low molecular weight components, thereby enabling the vulcanized rubber produced by dip molding to have both excellent flexibility and mechanical properties.
[0004]
number
[0005] [Patent Document 1] Japanese Patent Application Publication No. 7-292165 [Patent Document 2] JP 2014-114342 A [Patent Document 3] International Publication No. 2019 / 009038 [Patent Document 4] JP 2019-143002 A Summary of the Invention [Problem to be solved by the invention]
[0006] As a dip-molded product, chloroprene polymer dip-molded coatings generally have excellent mechanical strength due to the addition of crosslinking agents such as sulfur and vulcanization accelerators, and chloroprene polymer latex has been used as a rubber latex raw material in dip-molded coatings for gloves, balloons, boots, catheters, etc. On the other hand, there is a tendency to require high flexibility similar to that of dip-molded coatings obtained using natural rubber or polyisoprene, and particularly for glove applications, there is a demand for chloroprene polymer latex with improved physical properties related to flexibility, which is directly related to the wearing comfort or texture of the coating.
[0007] In addition, sulfur and vulcanization accelerators, which are preferred for improving mechanical strength, are substances that are classified as type IV allergy components that have adverse effects on the human body. In addition, there is a demand for reducing the cost of producing dip-molded coatings by not using these components, and there is a demand for a chloroprene polymer latex that does not contain sulfur or vulcanization accelerators and can provide dip-molded coatings that have excellent flexibility and excellent breaking strength.
[0008] Therefore, a main object of the present invention is to provide a chloroprene polymer latex composition capable of producing a chloroprene polymer dip-molded coating having high breaking strength and excellent flexibility without using sulfur or a vulcanization accelerator. [Means for solving the problem]
[0009] That is, the present invention relates to a chloroprene polymer latex composition which is a mixture of a chloroprene polymer latex A and a chloroprene polymer latex B, wherein the chloroprene polymer latex A and the chloroprene polymer latex B contain a chloroprene polymer, the chloroprene polymer of the chloroprene polymer latex B contains a copolymer of chloroprene and 2,3-dichloro-1,3-butadiene, and the amount of 2,3-dichloro-1,3-butadiene copolymerized in the chloroprene polymer of the chloroprene polymer latex B (2, the content of a monomer unit of 3-dichloro-1,3-butadiene (hereinafter the same) is 3% by mass or more based on 100% by mass of the total of chloroprene and 2,3-dichloro-1,3-butadiene, the toluene insoluble matter of the chloroprene polymer in the chloroprene polymer latex B is 70% by mass or more, the weight average molecular weight of the toluene soluble matter in the chloroprene polymer latex A is 5,000 to 250,000, and an ethanol / toluene azeotrope (JIS C 10141-1:2001) is obtained from a dried product obtained by freeze-drying the chloroprene polymer latex composition. The present invention relates to a chloroprene polymer latex composition, wherein the mass ratio b / a of the total amount b of abietic acid, neoabietic acid, palustric acid, levopimaric acid and their salts to the total amount a of dehydroabietic acid, pimaric acid, isopimaric acid, dihydroabietic acid and their salts is 0.10 or more in the result of gas chromatography mass spectrometry of an extract extracted with an ethanol / toluene azeotropic mixture specified in JIS K 6229. In addition, in the present invention, "JIS" means Japanese Industrial Standards.
[0010] The chloroprene polymer latex composition may be a chloroprene polymer latex composition in which the chloroprene polymer in the chloroprene polymer latex A has a toluene-insoluble content of 5 mass % or less.
[0011] The chloroprene polymer latex composition may be a chloroprene polymer latex composition in which the toluene-insoluble content of the chloroprene polymer in the chloroprene polymer latex B is 70 to 95% by mass.
[0012] The chloroprene polymer latex composition may be a chloroprene polymer latex composition in which a ratio of the chloroprene polymer latex A is 0.50 to 30.0 parts by mass relative to 100 parts by mass in total of the chloroprene polymer latex A and the chloroprene polymer latex B, and a toluene-insoluble matter of the chloroprene polymer contained in the chloroprene polymer latex composition is 50 to 85% by mass.
[0013] The present invention also relates to a dip-molded article using the chloroprene polymer latex composition. Such a dip-molded article may not contain sulfur and a vulcanization accelerator. The dip-molded article may be a glove, a balloon, a catheter, or a boot. Effect of the Invention
[0014] According to the present invention, it is possible to provide a chloroprene polymer latex composition capable of obtaining a chloroprene polymer dip-molded coating having high breaking strength and excellent flexibility without using sulfur and a vulcanization accelerator, which are IV type allergy components that adversely affect the human body. In such a chloroprene polymer latex composition, the weight average molecular weight of the toluene-soluble portion is relatively low, 250,000 or less, and therefore, very excellent flexibility can be obtained due to the plasticizing effect of the low molecular weight polymer. According to the present invention, it is also possible to obtain a chloroprene polymer dip-molded coating having high breaking strength and breaking elongation as well as excellent flexibility without using sulfur and a vulcanization accelerator. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention will be described in detail below with reference to the preferred embodiments. However, the present invention is not limited to the preferred embodiments described below.
[0016] In this specification, the term "A or more" in a numerical range means A and a range exceeding A. The term "A or less" in a numerical range means A and a range less than A. In the numerical ranges described in stages in this specification, the upper limit or lower limit of a numerical range in a certain stage can be arbitrarily combined with the upper limit or lower limit of a numerical range in another stage. In the numerical ranges described in this specification, the upper limit or lower limit of the numerical range may be replaced with a value shown in the examples. "A or B" may include either A or B, or may include both. Unless otherwise specified, the materials exemplified in this specification may be used alone or in combination of two or more types. When a plurality of substances corresponding to each component are present in the composition, the content of each component in the composition means the total amount of the plurality of substances present in the composition, unless otherwise specified. "(Meth)acrylic acid" means at least one of acrylic acid and the corresponding methacrylic acid, and the same applies to other similar expressions such as "(meth)acrylate". Toluene at room temperature (23° C.) can be used to measure the "toluene solubles" and "toluene insolubles."
[0017] <Chloroprene polymer latex composition> First, a chloroprene polymer latex composition according to a first embodiment of the present invention will be described. The chloroprene polymer latex composition according to this embodiment (hereinafter referred to as a "mixed chloroprene polymer latex composition") is a mixture of chloroprene polymer latex A and chloroprene polymer latex B.
[0018] The mixed chloroprene polymer latex composition according to the present embodiment can be obtained, for example, by stirring and mixing two or more chloroprene polymer latexes including the chloroprene polymer latexes A and B at 100 rpm for 1 minute using a paddle blade. The mixed chloroprene polymer latex composition according to the present embodiment may be obtained by mixing a chloroprene polymer latex other than the chloroprene polymer latexes A and B. Examples of chloroprene polymer latexes other than the chloroprene polymer latexes A and B include chloroprene polymer latexes that are not copolymerized with 2,3-dichloro-1,3-butadiene and have high crystallinity when surface hardness is required in a dip-molded article obtained using the mixed chloroprene polymer latex composition.
[0019] (Chloroprene polymer) Chloroprene polymer latex A contains a chloroprene polymer. The chloroprene polymer is a polymer having chloroprene (2-chloro-1,3-butadiene) as a monomer unit, and may be a homopolymer of chloroprene or a copolymer of chloroprene and other monomers (such as a copolymer of chloroprene and 2,3-dichloro-1,3-butadiene). Chloroprene polymer latex B contains a chloroprene polymer, and the chloroprene polymer includes a copolymer of chloroprene and 2,3-dichloro-1,3-butadiene.
[0020] A copolymer of chloroprene and 2,3-dichloro-1,3-butadiene is a polymer having chloroprene and 2,3-dichloro-1,3-butadiene as monomer units, and can be obtained by polymerizing a monomer composition containing chloroprene and 2,3-dichloro-1,3-butadiene.
[0021] The copolymer of chloroprene and 2,3-dichloro-1,3-butadiene may have monomer units of monomers other than chloroprene and 2,3-dichloro-1,3-butadiene. Examples of such monomers include esters of (meth)acrylic acid (methyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, etc.), hydroxyalkyl (meth)acrylates (2-hydroxymethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, etc.), (meth)acrylic acid, 1-chloro-1,3-butadiene, butadiene, isoprene, ethylene, styrene, and (meth)acrylonitrile. On the other hand, the copolymer of chloroprene and 2,3-dichloro-1,3-butadiene may not have monomer units of monomers other than chloroprene and 2,3-dichloro-1,3-butadiene, and may be a copolymer substantially composed of monomer units of chloroprene and monomer units of 2,3-dichloro-1,3-butadiene.
[0022] At least one selected from the group consisting of chloroprene polymer latex A and chloroprene polymer latex B may contain at least one selected from the group consisting of rosin acid, sodium rosinate, and potassium rosinate, and at least one selected from the group consisting of sodium hydroxide and potassium hydroxide. The emulsion system of chloroprene polymer latexes A and B is desirably combined with a base latex to prevent aggregation of rubber solids, pH fluctuation, etc., when blended.
[0023] (Toluene insolubles) The toluene insoluble portion of the chloroprene polymer can be determined by freeze-drying the chloroprene polymer latex A, B, or the mixed chloroprene polymer latex composition to dissolve the chloroprene polymer in toluene, followed by centrifuging the solution, separating the insoluble portion (gel portion) using a 200 mesh wire net, and then drying the solution to obtain a dried product, and measuring the mass of the dried product.
[0024] The toluene insoluble matter (gel matter) of the chloroprene polymer in the chloroprene polymer latex A is preferably 10% by mass or less relative to 100% by mass of the chloroprene polymer. If the toluene insoluble matter is 10% by mass or less, the modulus value at 100% elongation, which is an index of flexibility of the dip-molded coating obtained using the mixed chloroprene polymer latex composition, tends to be low, and excellent flexibility is easily obtained.
[0025] From the viewpoint of easily obtaining excellent flexibility, the toluene insoluble content of the chloroprene polymer of the chloroprene polymer latex A may be 8% by mass or less, 6% by mass or less, 5% by mass or less, less than 5% by mass, 4% by mass or less, 3% by mass or less, 2% by mass or less, or 1.5% by mass or less. The toluene insoluble content may be 0% by mass or more, more than 0% by mass, 1% by mass or more, 1.5% by mass or more, 2% by mass or more, 3% by mass or more, 4% by mass or more, 5% by mass or more, or 6% by mass or more. From these viewpoints, the toluene insoluble content may be more than 0% by mass and 10% by mass or less, 1 to 10% by mass, 1.5 to 10% by mass, more than 0% by mass and 6% by mass or less, 1 to 6% by mass, 1.5 to 6% by mass, more than 0% by mass and 3% by mass or less, 1 to 3% by mass, or 1.5 to 3% by mass.
[0026] The toluene-insoluble content (gel content) of the chloroprene polymer in chloroprene polymer latex B is 70% by mass or more relative to 100% by mass of the chloroprene polymer. When the toluene-insoluble content is 70% by mass or more, the dip-molded coating obtained using the mixed chloroprene polymer latex composition has excellent flexibility, and the mechanical strength of the dip-molded coating is increased due to the formation of a crosslinked structure caused by entanglement of the polymers (gel) or the like.
[0027] The toluene insoluble content of the chloroprene polymer of the chloroprene polymer latex B may be 75% by mass or more, 80% by mass or more, 82% by mass or more, 85% by mass or more, 86% by mass or more, or 90% by mass or more from the viewpoint of easily obtaining excellent flexibility and easily increasing mechanical strength. The toluene insoluble content may be 95% by mass or less, 90% by mass or less, 86% by mass or less, 85% by mass or less, 82% by mass or less, 80% by mass or less, or 75% by mass or less from the viewpoint of easily avoiding a decrease in polymerization reactivity due to a decrease in unreacted monomer. From these viewpoints, the toluene insoluble content may be 70 to 95% by mass, 70 to 90% by mass, 70 to 85% by mass, 75 to 95% by mass, 75 to 90% by mass, or 75 to 85% by mass.
[0028] The toluene insoluble content (gel content) of the chloroprene polymer contained in the mixed chloroprene polymer latex composition may be in the following ranges relative to 100% by mass of the chloroprene polymer. The toluene insoluble content may be 50% by mass or more, 55% by mass or more, 60% by mass or more, 65% by mass or more, 70% by mass or more, 75% by mass or more, or 80% by mass or more. The toluene insoluble content may be 85% by mass or less, 80% by mass or less, 75% by mass or less, 70% by mass or less, 65% by mass or less, 60% by mass or less, or 55% by mass or less. From these viewpoints, the toluene insoluble content may be 50 to 85% by mass, 50 to 80% by mass, 50 to 75% by mass, 60 to 85% by mass, 60 to 80% by mass, or 60 to 75% by mass. The numerical range of the toluene insoluble content can be adjusted by the mixing ratio of the chloroprene polymer latex A and the chloroprene polymer latex B.
[0029] (Weight average molecular weight of toluene solubles) The weight average molecular weight of the toluene-soluble portion (toluene-soluble sol portion) in the chloroprene polymer latex A is 5,000 to 250,000. When the weight average molecular weight is 250,000 or less, a dip-molded coating exhibiting excellent flexibility can be obtained due to the plasticizing effect of the low molecular weight polymer. When the weight average molecular weight is 5,000 or more, a dip-molded coating can be suitably obtained.
[0030] From the viewpoint of easily achieving both excellent flexibility and strength at break, the weight average molecular weight of the toluene soluble matter may be in the following range: 6,000 or more, 7,000 or more, 10,000 or more, 12,000 or more, 15,000 or more, 16,000 or more, 18,000 or more, 20,000 or more, 22,000 or more, or 24,000 or more. The weight average molecular weight may be 240,000 or less, 220,000 or less, 200,000 or less, 180,000 or less, 100,000 or less, 50,000 or less, 25,000 or less, 24,000 or less, 22,000 or less, 20,000 or less, 18,000 or less, 16,000 or less, 15,000 or less, 12,000 or less, 10,000 or less, or 7,000 or less. From these viewpoints, the weight average molecular weight may be 5,000 to 240,000, 5,000 to 180,000, 6,000 to 240,000, 6,000 to 200,000, 6,000 to 100,000, 6,000 to 50,000, 6,000 to 25,000, 7,000 to 100,000, 7,000 to 50,000, 7,000 to 25,000, 10,000 to 100,000, 10,000 to 50,000, 10,000 to 25,000, 20,000 to 100,000, 20,000 to 50,000, or 20,000 to 25,000.
[0031] The weight average molecular weight of the toluene soluble portion can be obtained by dissolving the chloroprene polymer latex A in toluene and measuring the weight average molecular weight of the eluted portion (sol portion) by gel permeation chromatography (GPC). The measured value of the weight average molecular weight varies depending on the blending amount (charge amount) of the chain transfer agent, etc.
[0032] [Weight-average molecular weight measurement by gel permeation chromatography] GPC measurement is performed under the following conditions. Molecular weight is calculated in polystyrene equivalent. Gel permeation chromatography (GPC) measuring device: Tosoh Corporation, gel permeation chromatograph (HLC-8320) Column: Tosoh Corporation, TSKgel ALPHA-M Eluent: Tetrahydrofuran (Kanto Chemical Co., Ltd.) ·Eluent flow rate: 1.0ml / min Column temperature: 40℃ Detection method: Differential refractive index (RI) meter Calibration curve: Created using standard polystyrene
[0033] (Chloroprene copolymerization amount) When the chloroprene polymer contained in the chloroprene polymer latex A is a copolymer of chloroprene and another monomer, the chloroprene copolymerization amount in the chloroprene polymer (the content of chloroprene monomer units; the same applies below) may be in the following range relative to 100% by mass of the total amount of monomer units in the chloroprene polymer or 100% by mass of the total amount of chloroprene copolymerization and 2,3-dichloro-1,3-butadiene copolymerization in the chloroprene polymer, from the viewpoint of easily obtaining excellent flexibility in a dip-molded coating. The chloroprene copolymerization amount may be 99% by mass or less, 97% by mass or less, 95% by mass or less, 92% by mass or less, 90% by mass or less, 88% by mass or less, 85% by mass or less, 82% by mass or less, or 80% by mass or less. The copolymerization amount of chloroprene may be 50% by mass or more, more than 50% by mass, 60% by mass or more, 70% by mass or more, 75% by mass or more, 80% by mass or more, 82% by mass or more, 85% by mass or more, 88% by mass or more, or 90% by mass or more. From these viewpoints, the copolymerization amount of chloroprene may be 50 to 99% by mass, 70 to 99% by mass, 80 to 99% by mass, 85 to 99% by mass, 90 to 99% by mass, 50 to 90% by mass, 70 to 90% by mass, 80 to 90% by mass, 85 to 90% by mass, 50 to 85% by mass, 70 to 85% by mass, 80 to 85% by mass, 50 to 80% by mass, or 70 to 80% by mass.
[0034] From the viewpoint of easily obtaining excellent flexibility in a dip-molded coating, the amount of chloroprene copolymerized in the chloroprene polymer of chloroprene polymer latex B may be in the following ranges relative to 100% by mass of the total amount of monomer units in the chloroprene polymer or 100% by mass of the total amount of chloroprene copolymerized and 2,3-dichloro-1,3-butadiene copolymerized in the chloroprene polymer. The amount of chloroprene copolymerized may be 99% by mass or less, 97% by mass or less, 95% by mass or less, 92% by mass or less, 90% by mass or less, 88% by mass or less, 85% by mass or less, 82% by mass or less, or 80% by mass or less. The amount of chloroprene copolymerized may be 70% by mass or more, 75% by mass or more, 80% by mass or more, 82% by mass or more, 85% by mass or more, 88% by mass or more, 90% by mass or more, 92% by mass or more, or 95% by mass or more. From these viewpoints, the amount of chloroprene copolymerized may be 70 to 99 mass%, 70 to 97 mass%, 70 to 95 mass%, 70 to 90 mass%, 80 to 99 mass%, 80 to 97 mass%, 80 to 95 mass%, 80 to 90 mass%, 85 to 99 mass%, 85 to 97 mass%, 85 to 95 mass%, or 85 to 90 mass%.
[0035] (2,3-dichloro-1,3-butadiene copolymerization amount) When the chloroprene polymer contained in the chloroprene polymer latex A is a copolymer of chloroprene and another monomer, the amount of 2,3-dichloro-1,3-butadiene copolymerized in the chloroprene polymer may be in the following range relative to 100% by mass of the total amount of monomer units in the chloroprene polymer or 100% by mass of the total amount of chloroprene copolymerized and 2,3-dichloro-1,3-butadiene copolymerized in the chloroprene polymer, from the viewpoint of easily obtaining excellent flexibility in a dip-molded coating: The amount of 2,3-dichloro-1,3-butadiene copolymerized may be 1% by mass or more, 3% by mass or more, 5% by mass or more, 8% by mass or more, 10% by mass or more, 12% by mass or more, 15% by mass or more, 18% by mass or more, or 20% by mass or more. The copolymerization amount of 2,3-dichloro-1,3-butadiene may be 50% by mass or less, less than 50% by mass, 40% by mass or less, 30% by mass or less, 25% by mass or less, 20% by mass or less, 18% by mass or less, 15% by mass or less, 12% by mass or less, or 10% by mass or less. From these viewpoints, the copolymerization amount of 2,3-dichloro-1,3-butadiene may be 1 to 50% by mass, 1 to 30% by mass, 1 to 20% by mass, 1 to 15% by mass, 1 to 10% by mass, 10 to 50% by mass, 10 to 30% by mass, 10 to 20% by mass, 10 to 15% by mass, 15 to 50% by mass, 15 to 30% by mass, 15 to 20% by mass, 20 to 50% by mass, or 20 to 30% by mass.
[0036] The amount of 2,3-dichloro-1,3-butadiene copolymerized in the chloroprene polymer of the chloroprene polymer latex B is preferably 3% by mass or more relative to the total amount of monomer units in the chloroprene polymer (100% by mass) or the total amount of chloroprene copolymerization and 2,3-dichloro-1,3-butadiene copolymerization in the chloroprene polymer (100% by mass) in terms of easily obtaining excellent flexibility in the dip-molded coating. If the amount of 2,3-dichloro-1,3-butadiene copolymerized is 3% by mass or more, excellent flexibility is easily obtained in the dip-molded coating. The amount of 2,3-dichloro-1,3-butadiene copolymerized may be in the following range from the viewpoint of easily obtaining excellent flexibility in the dip-molded coating. The amount of 2,3-dichloro-1,3-butadiene copolymerized may be 5% by mass or more, 8% by mass or more, 10% by mass or more, 12% by mass or more, 15% by mass or more, 18% by mass or more, or 20% by mass or more. The copolymerization amount of 2,3-dichloro-1,3-butadiene may be 30% by mass or less, 25% by mass or less, 20% by mass or less, 18% by mass or less, 15% by mass or less, 12% by mass or less, 10% by mass or less, 8% by mass or less, or 5% by mass or less. From these viewpoints, the copolymerization amount of 2,3-dichloro-1,3-butadiene may be 3 to 30% by mass, 5 to 30% by mass, 10 to 30% by mass, 3 to 20% by mass, 5 to 20% by mass, 10 to 20% by mass, 3 to 15% by mass, 5 to 15% by mass, or 10 to 15% by mass.
[0037] The amount of 2,3-dichloro-1,3-butadiene copolymerized can be determined by freeze-drying a chloroprene polymer latex and measuring the pyrolysis gas chromatography of the chloroprene polymer obtained.
[0038] [Pyrolysis gas chromatographic measurements] Pyrolysis gas chromatography can be performed under the following measurement conditions. Column used: DB-5 0.25mmφ×30m (film thickness 1.0μm) Column temperature: 50℃→10℃ / min→120℃→25℃ / min→300℃ ·Inlet temperature: 270℃ Detector temperature: 280℃ Sample size: 0.05mg
[0039] (mass ratio b / a) In the gas chromatographic mass spectrometry measurement result of an extract extracted with an ethanol / toluene azeotropic mixture (ethanol / toluene azeotropic mixture specified in JIS K 6229) from a dried product (chloroprene polymer) obtained by freeze-drying the mixed chloroprene polymer latex composition according to this embodiment, the mass ratio b / a (total amount b / total amount a) of the total amount b of abietic acid, neoabietic acid, palustric acid, levopimaric acid and their salts to the total amount a of dehydroabietic acid, pimaric acid, isopimaric acid, dihydroabietic acid and their salts is 0.10 or more. By having the mass ratio b / a of 0.10 or more, excellent breaking strength can be obtained.
[0040] From the viewpoint of easily obtaining excellent breaking strength, the mass ratio b / a may be 0.20 or more, 0.30 or more, 0.40 or more, 0.50 or more, 0.60 or more, 0.70 or more, 0.80 or more, 0.90 or more, 1.00 or more, 1.20 or more, 1.40 or more, or 1.60 or more. The mass ratio b / a may be 2.00 or less, 1.80 or less, 1.60 or less, 1.40 or less, 1.20 or less, 1.00 or less, 0.90 or less, 0.80 or less, 0.70 or less, 0.60 or less, 0.50 or less, 0.40 or less, or 0.30 or less. From these viewpoints, the mass ratio b / a may be 0.10 to 2.00, 0.10 to 1.20, 0.10 to 1.00, 0.10 to 0.80, 0.10 to 0.70, 0.30 to 2.00, 0.30 to 1.20, 0.30 to 1.00, 0.30 to 0.80, 0.30 to 0.70, 0.50 to 2.00, 0.50 to 1.20, 0.50 to 1.00, 0.50 to 0.80, 0.50 to 0.70, 0.80 to 2.00, 0.80 to 1.20, 0.80 to 1.00, or 1.00 to 2.00.
[0041] The dried product obtained by freeze-drying the mixed chloroprene polymer latex composition is cut and then placed in a flask equipped with a condenser, extracted with an ethanol / toluene azeotropic mixture as specified in JIS K 6229, treated with hydrochloric acid, and then measured by gas chromatography mass spectrometry. The peak area value of each component is regarded as the content and calculated to determine the total amount a and the total amount b. The value of the mass ratio b / a depends on the type of rosin acid and rosin acid metal salt added as emulsifiers.
[0042] [Gas chromatograph mass spectrometry measurement conditions] Gas chromatography mass spectrometry can be carried out under the following measurement conditions. Column used: FFAP 0.32mmφ×25m (film thickness 0.3μm) Column temperature: 200℃→250℃ Heating rate: 10℃ / min ·Inlet temperature: 270℃ ·Injection volume: 1μL Interface temperature: 270℃ Ion source temperature: 270℃ Ionization current: 50μA Ionization voltage: 70eV Detector voltage: -1000V Detector voltage: EI method
[0043] (Mixing ratio of chloroprene polymer latex) From the viewpoint of easily achieving both breaking strength and flexibility in a dip-molded coating obtained using the mixed chloroprene polymer latex composition, the proportion of chloroprene polymer latex A (mixing proportion) may be within the following ranges, in terms of solid content ratio, relative to 100 parts by mass of the total of chloroprene polymer latex A and chloroprene polymer latex B. The proportion of chloroprene polymer latex A may be 0.5 parts by mass or more, 1 part by mass or more, 5 parts by mass or more, 10 parts by mass or more, 15 parts by mass or more, 20 parts by mass or more, 25 parts by mass or more, or 30 parts by mass or more. The proportion of chloroprene polymer latex A may be 50 parts by mass or less, 40 parts by mass or less, 30 parts by mass or less, 25 parts by mass or less, 20 parts by mass or less, 15 parts by mass or less, 10 parts by mass or less, or 5 parts by mass or less. From these viewpoints, the proportion of the chloroprene polymer latex A may be 0.5 to 50 parts by mass, 0.5 to 30 parts by mass, 0.5 to 25 parts by mass, 0.5 to 20 parts by mass, 0.5 to 15 parts by mass, 5 to 50 parts by mass, 5 to 30 parts by mass, 5 to 25 parts by mass, 5 to 20 parts by mass, 5 to 15 parts by mass, 10 to 50 parts by mass, 10 to 30 parts by mass, 10 to 25 parts by mass, 10 to 20 parts by mass, or 10 to 15 parts by mass.
[0044] (Effects Obtained by Mixed Chloroprene Polymer Latex Composition) According to the mixed chloroprene polymer latex composition of the present embodiment, a chloroprene polymer dip-molded coating having high breaking strength and excellent flexibility can be obtained without using sulfur and vulcanization accelerators. Specifically, a dip-molded coating obtained by vulcanizing the mixed chloroprene polymer latex composition at 130°C for 4 hours without using sulfur and vulcanization accelerators has a modulus at 100% elongation of 0.40 to 0.75 MPa and a breaking strength of 17 MPa or more when measured according to JIS K 6251. In particular, the ASTM standard "D3577" for surgical glove applications specifies the breaking strength as 17 MPa or more. The dip-molded coating has excellent flexibility and sufficient mechanical strength without containing sulfur and vulcanization accelerators.
[0045] In the conventional chloroprene polymer, the use of sulfur or a vulcanization accelerator is indispensable to obtain a vulcanized rubber having a desired mechanical strength. Since sulfur and vulcanization accelerators are causative substances of type IV allergy that causes skin diseases such as dermatitis, the reduction or elimination of the use of sulfur and vulcanization accelerators has become an important theme. In addition, since the elimination of the use of sulfur and vulcanization accelerators leads not only to the reduction of allergies but also to cost reduction, a chloroprene polymer latex composition capable of obtaining a dip-molded product that exhibits sufficient mechanical strength while having excellent flexibility without using sulfur and vulcanization accelerators is desired.
[0046] The dip-molded coating obtained from the mixed chloroprene polymer latex composition according to the present embodiment may contain sulfur and / or a vulcanization accelerator. However, even if the dip-molded coating does not contain sulfur or a vulcanization accelerator, the dip-molded coating has mechanical properties equal to or greater than those of a vulcanized dip-molded coating obtained from a conventional chloroprene polymer latex. Therefore, the mixed chloroprene polymer latex composition according to the present embodiment is preferably used as a raw material for a dip-molded coating.
[0047] (Production method of chloroprene polymer latex A and B) Next, the methods for producing the chloroprene polymer latexes A and B will be described.
[0048] The method for producing the chloroprene polymer latex A includes a polymerization step of emulsion-polymerizing a monomer composition containing at least one monomer selected from the group consisting of chloroprene and 2,3-dichloro-1,3-butadiene. The polymerization step may be a step of emulsion-polymerizing chloroprene, 2,3-dichloro-1,3-butadiene, and an alkyl mercaptan to obtain a chloroprene polymer latex.
[0049] The method for producing the chloroprene polymer latex B includes a polymerization step of emulsion-polymerizing a monomer composition containing chloroprene and 2,3-dichloro-1,3-butadiene. The polymerization step may be a step of emulsion-polymerizing chloroprene, 2,3-dichloro-1,3-butadiene, and an alkyl mercaptan to obtain a chloroprene polymer latex.
[0050] As described above, the amount of 2,3-dichloro-1,3-butadiene copolymerized in the chloroprene polymer of the chloroprene polymer latex B may be 3% by mass or more (e.g., 3 to 30% by mass) relative to 100% by mass of the total amount of monomer units in the chloroprene polymer, or 100% by mass of the total of chloroprene and 2,3-dichloro-1,3-butadiene in the chloroprene polymer. In this case, the blending amount (charge amount) of 2,3-dichloro-1,3-butadiene in the polymerization step (before the start of emulsion polymerization) may be 3 parts by mass or more (e.g., 3 to 30 parts by mass) relative to 100 parts by mass of the total amount of monomers for obtaining the chloroprene polymer, or 100 parts by mass of the total of chloroprene and 2,3-dichloro-1,3-butadiene.
[0051] The type of chain transfer agent used in emulsion polymerization is not particularly limited.As the chain transfer agent, for example, long-chain alkyl mercaptans such as n-dodecyl mercaptan (1-dodecyl mercaptan) and tert-dodecyl mercaptan, dialkyl xanthogen disulfides such as diisopropyl xanthogen disulfide and diethyl xanthogen disulfide, iodoform, etc., which are generally used in emulsion polymerization of chloroprene, can be used.
[0052] In the chloroprene polymer latex A, the weight average molecular weight can be adjusted by the blending amount (charge amount) of the chain transfer agent before the start of emulsion polymerization. For example, the blending amount of the chain transfer agent (for example, the blending amount of the mercaptan chain transfer agent (n-dodecyl mercaptan, etc.)) is preferably 0.50 to 10.0 parts by mass per 100 parts by mass of the total of chloroprene and 2,3-dichloro-1,3-butadiene. This makes it easy to adjust the weight average molecular weight of the toluene-soluble portion to 5,000 to 250,000, and the flexibility of the dip-molded coating obtained by using the mixed chloroprene polymer latex composition is easily improved.
[0053] In the chloroprene polymer latex B, the amount (charge amount) of the chain transfer agent (e.g., alkyl mercaptan) before the start of emulsion polymerization is preferably 0.01 to 0.1 parts by mass, more preferably 0.02 to 0.05 parts by mass, based on 100 parts by mass of the total of chloroprene and 2,3-dichloro-1,3-butadiene. When the amount of the chain transfer agent is 0.01 parts by mass or more, the storage stability of the latex tends to be improved. When the amount of the chain transfer agent is 0.1 parts by mass or less, the amount of toluene insolubles increases, and the strength of the dip-molded coating obtained by using the mixed chloroprene polymer latex composition tends to be high.
[0054] The emulsifier used in the emulsion polymerization is preferably a rosin acid from the viewpoint of easily obtaining excellent breaking strength, and more preferably a rosin acid including abietic acid, neoabietic acid, palustric acid, levopimaric acid, and salts thereof. In addition, by using a rosin acid, aggregation of rubber solids and pH fluctuation can be prevented when blended with a base latex.
[0055] Other commonly used emulsifiers, fatty acids, etc. may also be used. Examples of other emulsifiers include metal salts of aromatic sulfonic acid formalin condensates (e.g., sodium salts of β-naphthalenesulfonic acid formalin condensates), sodium dodecylbenzenesulfonate, potassium dodecylbenzenesulfonate, sodium alkyldiphenylethersulfonate, potassium alkyldiphenylethersulfonate, sodium polyoxyethylene alkylethersulfonate, sodium polyoxypropylene alkylethersulfonate, potassium polyoxyethylene alkylethersulfonate, potassium polyoxypropylene alkylethersulfonate, and the like.
[0056] The content of the anionic surfactant other than rosin acid is preferably 0.2 to 1.0% by mass based on 100% by mass of the chloroprene polymer contained in the chloroprene polymer latex. Therefore, the blending amount (charge amount) of the anionic surfactant other than rosin acid before the start of emulsion polymerization is preferably within the range of 0.2 to 0.9 parts by mass based on 100 parts by mass of the total of chloroprene and 2,3-dichloro-1,3-butadiene.
[0057] The pH of the aqueous emulsion at the start of emulsion polymerization is preferably 10.5 to 13.5. The aqueous emulsion refers to a mixture of alkyl mercaptan, chloroprene, 2,3-dichloro-1,3-butadiene, etc. before the start of emulsion polymerization, but also includes cases where the composition changes due to the post-addition or divided addition of each component. If the pH of the aqueous emulsion at the start of emulsion polymerization is 10.5 or more, the polymerization reaction can be controlled more stably. If the pH is 13.5 or less, excessive viscosity increase during polymerization is suppressed, and the polymerization reaction can be controlled more stably.
[0058] The polymerization temperature of the emulsion polymerization may be within the range of 5 to 55° C. If the polymerization temperature is 5° C. or higher, the emulsion is less likely to freeze. If the polymerization temperature is 55° C. or lower, evaporation and boiling of the chloroprene monomer are easily suppressed.
[0059] As the polymerization initiator, potassium persulfate, benzoyl peroxide, ammonium persulfate, hydrogen peroxide, etc., which are used in normal radical polymerization, may be used.
[0060] The polymerization conversion rate may be in the range of 50 to 95%. The polymerization reaction can be stopped by adding a polymerization inhibitor. If the polymerization conversion rate is 50% or more, the amount of toluene insolubles increases, and the strength of the obtained dip-molded coating tends to be high, and the production cost is advantageous. If the polymerization conversion rate is 95% or less, the decrease in polymerization reactivity due to the decrease in unreacted monomers is avoided, and the decrease in productivity is avoided.
[0061] Examples of the polymerization inhibitor include diethylhydroxylamine, thiodiphenylamine, 4-tert-butylcatechol, 2,2'-methylenebis-4-methyl-6-tert-butylphenol, etc. Unreacted monomers after the completion of emulsion polymerization can be removed by a conventional method such as reduced pressure distillation.
[0062] Furthermore, to the chloroprene polymer latexes A and B, a freezing stabilizer, an emulsion stabilizer, a viscosity modifier, an antioxidant, a preservative, etc. may be added arbitrarily after polymerization.
[0063] <Dip molded body> Next, a dip-molded article according to the second embodiment of the present invention will be described. The dip-molded article according to this embodiment is a dip-molded article using the mixed chloroprene polymer latex composition of the first embodiment described above, and is, for example, a dip-molded article obtained by dip-molding the mixed chloroprene polymer latex composition of the first embodiment alone (a dip-molded article obtained by dip-molding the mixed chloroprene polymer latex composition of the first embodiment without mixing any other chloroprene polymer latex), or a dip-molded article obtained by blending the mixed chloroprene polymer latex composition of the first embodiment with any other chloroprene polymer latex. That is, the dip-molded article according to this embodiment may be a dip-molded article obtained by dip-molding the mixed chloroprene polymer latex composition of the first embodiment alone, or a dip-molded article obtained by mixing the mixed chloroprene polymer latex composition of the first embodiment with any other chloroprene polymer latex. The dip-molded article according to this embodiment has a low modulus at 100% elongation, is flexible, and has excellent mechanical properties such as strength and elongation. The dip-molded article according to this embodiment may be a glove, a balloon, a catheter, or a boot.
[0064] The method for producing the dip-molded product according to this embodiment (molding method) includes, for example, a coagulation liquid immersion method, but is not limited thereto, and molding may be performed according to a conventional method.
[0065] The immersion molded product according to the present embodiment may not contain at least one selected from the group consisting of a vulcanizing agent and a vulcanization accelerator, or may contain at least one selected from the group consisting of a vulcanizing agent and a vulcanization accelerator. That is, the immersion molded product according to the present embodiment includes an embodiment containing a vulcanizing agent but not a vulcanization accelerator, an embodiment containing a vulcanizing agent but not a vulcanization accelerator, an embodiment containing a vulcanizing agent and a vulcanization accelerator, and an embodiment containing no vulcanizing agent or a vulcanization accelerator. Whether or not to blend a vulcanizing agent and a vulcanization accelerator may be determined depending on the desired immersion molded product.
[0066] Vulcanizing agents include, but are not limited to, sulfur, zinc oxide, magnesium oxide, and the like.
[0067] A vulcanization accelerator is a chemical that acts with a vulcanizing agent during vulcanization of raw rubber to increase the vulcanization speed, thereby shortening the vulcanization time, lowering the vulcanization temperature, reducing the amount of vulcanizing agent, improving the physical properties of the vulcanized rubber, etc. A vulcanization accelerator usually refers to a chemical that accelerates the sulfur vulcanization reaction.
[0068] Examples of vulcanization accelerators generally used in vulcanization of chloroprene polymer latex include, but are not limited to, thiuram-based, dithiocarbamate-based, thiourea-based, guanidine-based, xanthogenate-based, thiazole-based, etc. The vulcanization accelerators may be used alone or in combination of two or more types as necessary, but are not limited thereto.
[0069] Examples of thiuram-based vulcanization accelerators include tetramethylthiuram disulfide, tetraethylthiuram disulfide, tetrabutylthiuram disulfide, tetrakis(2-ethylhexyl)thiuram disulfide, tetramethylthiuram monosulfide, and dipentamethylenethiuram tetrasulfide.
[0070] Examples of the dithiocarbamate-based vulcanization accelerator include sodium dibutyldithiocarbamate, zinc dimethyldithiocarbamate, zinc diethyldithiocarbamate, zinc dibutyldithiocarbamate, zinc N-ethyl-N-phenyldithiocarbamate, zinc N-pentamethylenedithiocarbamate, copper dimethyldithiocarbamate, ferric dimethyldithiocarbamate, and tellurium diethyldithiocarbamate, and zinc dibutyldithiocarbamate is particularly preferably used.
[0071] Examples of the thiourea-based vulcanization accelerator include ethylene thiourea, N,N'-diethyl thiourea, trimethyl thiourea, and N,N'-diphenyl thiourea.
[0072] Examples of the guanidine-based vulcanization accelerator include 1,3-diphenylguanidine, 1,3-di-o-tolylguanidine, 1-o-tolylbiguanide, and di-o-tolylguanidine salts of dicatechol borate.
[0073] Examples of the xanthogenate-based vulcanization accelerator include zinc butylxanthogenate and zinc isopropylxanthogenate.
[0074] Examples of the thiazole-based vulcanization accelerator include 2-mercaptobenzothiazole, di-2-benzothiazolyl disulfide, 2-mercaptobenzothiazole zinc salt, cyclohexylamine salt of 2-mercaptobenzothiazole, and 2-(4'-morpholinodithio)benzothiazole.
[0075] The dip-molded article according to this embodiment exhibits excellent mechanical properties regardless of the presence or absence of sulfur and a vulcanization accelerator. From the viewpoints of reducing allergies and reducing costs, however, it is preferable that the dip-molded article does not contain sulfur or a vulcanization accelerator. EXAMPLES
[0076] The present invention will be described in more detail below based on examples, comparative examples and reference examples, but the present invention is not limited to these examples.
[0077] <Example 1> (Preparation of chloroprene polymer latex A) Into a polymerization vessel having an internal volume of 40 liters, 80 parts by mass of chloroprene monomer, 20 parts by mass of 2,3-dichloro-1,3-butadiene monomer, 3 parts by mass of 1-dodecyl mercaptan, 90 parts by mass of pure water, 4.5 parts by mass of rosin acid X (mass ratio b / a=0.80), 1.50 parts by mass of potassium hydroxide, and 0.50 parts by mass of sodium salt of β-naphthalenesulfonic acid formalin condensate (trade name "Demol N", manufactured by Kao Corporation) were added. The pH of the aqueous emulsion before the start of polymerization was 12.9. 0.1 parts by mass of potassium persulfate was added as a polymerization initiator, and polymerization was carried out under a nitrogen gas flow at a polymerization temperature of 20°C. When the polymerization conversion rate reached 85%, 0.01 parts by mass of diethylhydroxylamine, a polymerization inhibitor, was added to terminate the polymerization, and a latex was obtained.
[0078] The latex was distilled under reduced pressure to remove unreacted monomers and water, thereby obtaining a chloroprene polymer latex A (mercaptan-modified chloroprene polymer latex) having a solid content of 55%.
[0079] (Preparation of chloroprene polymer latex B) Into a polymerization vessel having an internal volume of 40 liters, 95 parts by mass of chloroprene monomer, 5 parts by mass of 2,3-dichloro-1,3-butadiene monomer, 0.04 parts by mass of 1-dodecyl mercaptan, 90 parts by mass of pure water, 4.3 parts by mass of rosin acid X (mass ratio b / a=0.80), 1.50 parts by mass of potassium hydroxide, and 0.50 parts by mass of sodium salt of β-naphthalenesulfonic acid formalin condensate (trade name "Demol N", manufactured by Kao Corporation) were added. The pH of the aqueous emulsion before the start of polymerization was 13.2. 0.1 parts by mass of potassium persulfate was added as a polymerization initiator, and polymerization was carried out under a nitrogen gas flow at a polymerization temperature of 15°C. When the polymerization conversion rate reached 70%, 0.01 parts by mass of diethylhydroxylamine, a polymerization inhibitor, was added to terminate the polymerization, and a latex was obtained.
[0080] The latex was distilled under reduced pressure to remove unreacted monomers and water, thereby obtaining a chloroprene polymer latex B (mercaptan-modified chloroprene polymer latex) having a solid content of 55%.
[0081] (Measurement of the mass ratio b / a of rosin acid) The above-mentioned rosin acid X was dissolved in an ethanol / toluene azeotropic mixture (ethanol / toluene azeotropic mixture, ETA solution as specified in JIS K 6229) to prepare a 1.5% solution, which was then treated with hydrochloric acid and measured using gas chromatography-mass spectrometry. The area percentage relative to the total peak area value detected by gas chromatography-mass spectrometry was regarded as the content, and the total amount a of dehydroabietic acid, pimaric acid, isopimaric acid, dihydroabietic acid and their salts, and the total amount b of abietic acid, neoabietic acid, palustric acid, levopimaric acid and their salts were calculated, and the mass ratio b / a of the total amount b to the total amount a was calculated.
[0082] Among the conjugated resin acid components, abietic acid components (abietic acid and its salts; the same applies to other resin acid components) were detected at 31.2%, neoabietic acid components at 0.8%, palustric acid components at 4.0%, and levopimaric acid components at 2.7%, and the total area of the conjugated resin acid components was 38.7%. Among the non-conjugated resin acid components, dehydroabietic acid components were detected at 35.3%, pimaric acid components at 7.5%, isopimaric acid components at 3.2%, and dihydroabietic acid components at 2.4%, and the total area of the non-conjugated resin acid components was 48.4%. Therefore, the value of "(content of conjugated resin acid components) ÷ (content of non-conjugated resin acid components)" in rosin acid X (mass ratio b / a) was "38.7 ÷ 48.4 = 0.80". Rosin acid Y (mass ratio b / a = 1.87) and rosin acid Z (mass ratio b / a = 0; abietic acid, neoabietic acid, palustric acid, levopimaric acid, and their salts were not detected) described below were also analyzed in the same manner, and the mass ratio b / a was obtained.
[0083] (Measurement of toluene insoluble matter of chloroprene polymer latex A and B) The chloroprene polymer latexes A and B were freeze-dried, and 1 g of the chloroprene polymer was cut into 2 mm square pieces to obtain small pieces, which were then placed in a conical beaker and dissolved in toluene for 16 hours. The pieces were then centrifuged, and the gel fraction was separated using a 200 mesh wire net. The mass of the dried product obtained by drying was then measured to calculate the toluene insoluble content. The toluene insoluble content of the chloroprene polymer latex A was 1.1 mass%, and the toluene insoluble content of the chloroprene polymer latex B was 82 mass%.
[0084] (Measurement of weight average molecular weight of toluene soluble matter of chloroprene polymer latex A) The chloroprene polymer latex A was dissolved in toluene, and the eluted portion (sol portion) was measured by gel permeation chromatography to have a weight average molecular weight, calculated as polystyrene, of 24,000.
[0085] (Measurement of 2,3-dichloro-1,3-butadiene copolymerization amount) The chloroprene polymer obtained by freeze-drying the chloroprene polymer latexes A and B was cut into 0.05 mg test pieces and measured by pyrolysis gas chromatography. The 2,3-dichloro-1,3-butadiene copolymerization amount of the chloroprene polymer latex measured by this pyrolysis gas chromatography was 21 mass% for the chloroprene polymer latex A and 4.6 mass% for the chloroprene polymer latex B, relative to 100 mass% in total of chloroprene and 2,3-dichloro-1,3-butadiene in the chloroprene polymer. From this analysis value, it was confirmed that the 2,3-dichloro-1,3-butadiene copolymerization amount in the chloroprene polymer roughly correlates with the blending amount (charged amount) of 2,3-dichloro-1,3-butadiene.
[0086] (Preparation of Mixed Latex Composition) When the total amount of the chloroprene polymer latex A and the chloroprene polymer latex B was 100 parts by mass, the chloroprene polymer latex A was 10 parts by mass and the chloroprene polymer latex B was 90 parts by mass (solid content ratio) and mixed with stirring to obtain a mixed latex composition (mixed chloroprene polymer latex composition).
[0087] (Measurement of the mass ratio b / a of rosin acid in the mixed latex composition) The mixed latex composition was freeze-dried, and 3 g of the dried product (chloroprene polymer) was cut into 2 mm square pieces to obtain small pieces. The small pieces were placed in a round-bottom flask equipped with a condenser, and dissolved in an ethanol / toluene azeotropic mixture (ethanol / toluene azeotropic mixture, ETA solution, as specified in JIS K 6229) to prepare a 1.5% solution. Then, the pieces were treated with hydrochloric acid and measured using gas chromatography mass spectrometry. The area percentage relative to the total peak area value detected by gas chromatography mass spectrometry was regarded as the content, and the total amount a of dehydroabietic acid, pimaric acid, isopimaric acid, dihydroabietic acid, and their salts, and the total amount b of abietic acid, neoabietic acid, palustric acid, levopimaric acid, and their salts were calculated, and the mass ratio b / a of the total amount b to the total amount a was calculated. The mass ratio b / a was 0.80.
[0088] (Measurement of Toluene Insolubles in Mixed Latex Composition) The mixed latex composition was freeze-dried, and 1 g of the chloroprene polymer was cut into 2 mm square pieces to obtain small pieces, which were then placed in a conical beaker and dissolved in toluene for 16 hours.Then, the mixture was centrifuged, and the gel was separated using a 200 mesh wire net.Then, the mass of the dried product obtained by drying was measured to calculate the toluene insoluble content.The toluene insoluble content of the mixed latex composition was 72 mass%.
[0089] (Preparation of evaluation samples) 100 parts by mass of the solid content of the mixed latex composition was mixed with 4.1 parts by mass of the aqueous dispersion, and water was added to adjust the total solid content concentration of the blend to 30% by mass to prepare a molding composition that does not contain sulfur or vulcanization accelerators. The aqueous dispersion was prepared by mixing 2 parts by mass of zinc oxide (vulcanizing agent, trade name "Zinc Oxide Type 2", Sakai Chemical Industry Co., Ltd.), 2 parts by mass of a butylated reaction product of p-cresol and dicyclopentadiene (trade name "Nocrac PBK", Ouchi Shinko Chemical Industry Co., Ltd.), 0.1 parts by mass of sodium salt of β-naphthalenesulfonic acid formalin condensate (trade name "Demol N", Kao Corporation), and 13 parts by mass of water at 20°C for 16 hours using a ceramic ball mill.
[0090] A ceramic cylinder (manufactured by Shinko Co., Ltd.) with an outer diameter of 50 mm was immersed for 1 second in a coagulation liquid containing 62 parts by mass of water, 35 parts by mass of potassium nitrate tetrahydrate, and 3 parts by mass of calcium carbonate, and then the cylinder was taken out. After drying for 3 minutes at room temperature of 23°C, the cylinder was immersed in the molding composition for 10 seconds. After that, the cylinder was washed with running water at 45°C for 1 minute, and then vulcanized at 130°C for 4 hours to prepare a vulcanized film (dip-molded film; vulcanized film containing no sulfur or vulcanization accelerator) as an evaluation sample. The vulcanized film was peeled off from the outer peripheral surface of the cylinder and evaluated.
[0091] (Evaluation of evaluation samples) The vulcanized film was measured for 100% elongation modulus, breaking strength and breaking elongation in accordance with JIS K 6251.
[0092] <Examples 2 to 9, Comparative Examples 1 to 5, and Reference Examples 1 and 2> Under the conditions shown in Tables 1 to 3, vulcanized films were produced and evaluated in the same manner as in Example 1. In Examples 6 to 9 and Comparative Examples 4 to 5, rosin acid Y (mass ratio b / a = 1.87) was used. In Examples 5 to 9 and Comparative Example 3, rosin acid Z (mass ratio b / a = 0; abietic acid, neoabietic acid, palustric acid, levopimaric acid, and their salts were not detected) was used.
[0093] <Result> The results of Examples 1 to 9, Comparative Examples 1 to 5, and Reference Examples 1 and 2 are shown in Tables 1 to 3.
[0094] [Table 1]
[0095] [Table 2]
[0096] [Table 3]
[0097] As is clear from Tables 1 to 3, the dip-molded coatings (dip-molded articles) obtained using the mixed latex compositions of Examples 1 to 9 had excellent mechanical properties (breaking strength and breaking elongation) while having a very low modulus at 100% elongation (very excellent flexibility).
[0098] In Comparative Example 1, the weight average molecular weight of the chloroprene polymer latex A exceeded 250,000, and the value of the modulus at 100% elongation was high, resulting in poor flexibility.
[0099] In Comparative Example 2, the weight average molecular weight of the chloroprene polymer latex A was less than 5,000, and when an attempt was made to produce a dip-molded coating, the low molecular weight chloroprene polymer of the chloroprene polymer latex A bleed (exude) and became very sticky, making it impossible to produce a dip-molded coating.
[0100] In Comparative Example 3, rosin acid Z (mass ratio b / a=0) was used as an emulsifier in both chloroprene polymer latexes A and B, and the mass ratio b / a of the mixed latex composition was 0, so the breaking strength was poor.
[0101] In Comparative Example 4, 2,3-dichloro-1,3-butadiene was not copolymerized in chloroprene polymer latex B, and the crystallinity of the chloroprene polymer in the obtained dip-molded coating was high, resulting in a high modulus value at 100% elongation and poor flexibility.
[0102] In Comparative Example 5, the polymerization conversion rate of the chloroprene polymer latex B was low, and the toluene insoluble matter (gel content) of the chloroprene polymer latex B was low, resulting in poor breaking strength. In addition, the modulus at 100% elongation was high, resulting in poor flexibility.
[0103] In Reference Example 1, when a dip-molded coating was produced using only chloroprene polymer latex B without mixing chloroprene polymer latex A, the breaking strength was excellent, but the modulus at 100% elongation was high and flexibility was poor. This shows that by mixing chloroprene polymer latex A containing a low molecular weight chloroprene polymer, the plasticizing effect of the low molecular weight chloroprene polymer is exerted, and a dip-molded coating with excellent flexibility can be obtained.
[0104] In Reference Example 2, when a dip-molded coating was produced using only chloroprene polymer latex A without mixing chloroprene polymer latex B, the low molecular weight chloroprene polymer caused excessive stickiness, and a dip-molded coating could not be produced.
Claims
1. A chloroprene polymer latex composition which is a mixture of a chloroprene polymer latex A and a chloroprene polymer latex B, the chloroprene polymer latex A and the chloroprene polymer latex B contain a chloroprene polymer, the chloroprene polymer of the chloroprene polymer latex B comprises a copolymer of chloroprene and 2,3-dichloro-1,3-butadiene; the amount of 2,3-dichloro-1,3-butadiene copolymerized in the chloroprene polymer of the chloroprene polymer latex B is 3 mass% or more relative to 100 mass% in total of chloroprene and 2,3-dichloro-1,3-butadiene, the chloroprene polymer latex A has a toluene-insoluble content of 10% by mass or less, the chloroprene polymer latex B has a toluene-insoluble content of 70 mass% or more; the weight average molecular weight of the toluene-soluble portion in the chloroprene polymer latex A is 5,000 to 250,000; A chloroprene polymer latex composition, wherein, in a gas chromatographic mass spectrometry analysis of an extract extracted with an ethanol / toluene azeotropic mixture (ethanol / toluene azeotropic mixture defined in JIS K 6229) from a dried product obtained by freeze-drying the chloroprene polymer latex composition, the mass ratio b / a of the total amount b of abietic acid, neoabietic acid, palustric acid, levopimaric acid and their salts to the total amount a of dehydroabietic acid, pimaric acid, isopimaric acid, dihydroabietic acid and their salts is 0.10 or more.
2. 2. The chloroprene polymer latex composition according to claim 1, wherein the toluene-insoluble content of the chloroprene polymer in the chloroprene polymer latex B is 70 to 95% by mass.
3. a ratio of the chloroprene polymer latex A to 100 parts by mass in total of the chloroprene polymer latex A and the chloroprene polymer latex B is 0.5 to 30 parts by mass, 3. The chloroprene polymer latex composition according to claim 1, wherein the toluene-insoluble content of the chloroprene polymer contained in the chloroprene polymer latex composition is 50 to 85% by mass.
4. A dip-molded article using the chloroprene polymer latex composition according to any one of claims 1 to 3.
5. The dip-molded article according to claim 4, which is free of sulfur and vulcanization accelerators.
6. The dip-molded article according to claim 5 , which is a glove, a balloon, a catheter or a boot.
Citation Information
Patent Citations
High-damping chloroprene rubber composition
JP1995292165A
Polychloroprene latex, polychloroprene latex composition, and dip molded product
JP2014114342A
Chloroprene polymer latex and manufacturing method therefor
JP2019143002A
Chloroprene rubber-based polymer latex composition and use thereof
WO2013141170A1
Mercaptane-modified polychloroprene latex and production method therefor
WO2019009038A1