Static induction device and its manufacturing method

By assembling a toroidal core around a winding ring with a distinct inner radius post-strain relief annealing, the invention addresses iron loss issues in stationary induction appliances, achieving reduced iron loss and improved magnetic performance.

JP7568911B2Active Publication Date: 2024-10-17NIPPON STEEL CORPORATION
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2020188579
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-11-12
Publication Date
2024-10-17
Estimated Expiration
2040-11-12

AI Technical Summary

Technical Problem

Existing stationary induction appliances face issues with increased iron loss due to strain relief annealing, which eliminates the minute strains introduced by laser beams or electron beams, leading to deteriorated magnetic properties.

Method used

The appliance features a toroidal core assembled around a winding ring with a different inner radius after strain relief annealing, introducing strain to reduce iron loss without being affected by annealing, and a manufacturing method that winds grain-oriented electrical steel sheets around the winding ring body with a distinct inner radius.

Benefits of technology

This approach effectively reduces iron loss by introducing strain into the steel plate, enhancing magnetic domain refinement and minimizing abnormal eddy current loss, while maintaining magnetic properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007568911000006
    Figure 0007568911000006
  • Figure 0007568911000007
    Figure 0007568911000007
  • Figure 0007568911000008
    Figure 0007568911000008
Patent Text Reader

Abstract

To provide a stationary induction apparatus capable of decreasing iron loss of a toroidal iron core by easily and effectively introducing strain without being affected by strain removal annealing, and a method of manufacturing the same.SOLUTION: A stationary induction apparatus comprises a winding wire ring body, and a toroidal iron core 4 that is assembled in a wound state to one corresponding side of the winding wire ring body. The toroidal iron core 4 is formed by annularly winding a directional magnetic steel sheet around the winding wire ring body while paying out it from a wound core roll R. The toroidal iron core 4 is assembled by being wound around the winding wire ring body so as to have an inner radius different from an inner radius of the wound core roll R.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a static induction machine including an annular winding ring formed by winding a conductor a predetermined number of times, and a toroidal core assembled in a wound state onto the winding ring, and a method for manufacturing the same. [Background technology]

[0002] One type of static induction device, such as a transformer or a reactor, is known to include an annular winding ring formed by winding a conductor a predetermined number of times, and a toroidal core assembled in a wound state around the winding ring (see, for example, Patent Document 1).

[0003] In the manufacturing process of such a stationary induction machine, first, a winding ring (e.g., rectangular) is produced by winding a conductor to a predetermined shape and dimensions, and a wound core roll is produced by winding a magnetic steel sheet to form a toroidal core. The wound core roll is then subjected to stress relief annealing to improve the magnetic properties and maintain the toroidal shape, and then the toroidal core is assembled and integrated with the winding ring. In this integration process, the steel sheet drawn from the outermost periphery of the wound core roll is passed through a window of the fixed winding ring, then passed outside the wound core roll, and passed through the window of the winding ring again. By repeating this process, the entire steel sheet is finally wound around one side of the winding ring while maintaining the original winding shape (without switching the inner and outer peripheries of the wound core roll), and the toroidal core is formed to have a small diameter and is completed. An example of an apparatus for implementing such a manufacturing method is proposed in, for example, Patent Document 2.

[0004] It is also possible to directly wind the steel sheet from the outermost periphery of the wound core roll onto the winding ring, but in this case, after winding of the steel sheet onto the winding ring is completed, the original outermost portion of the steel sheet of the wound core roll becomes the innermost portion of the steel sheet of the toroidal core assembled to the winding ring, and the original innermost portion of the steel sheet of the wound core roll becomes the outermost portion of the steel sheet of the toroidal core, so that the inner and outer peripheries are switched. As a result, the radius of curvature of the steel sheet when the stationary induction motor is completed differs from that after stress relief annealing, and distortion occurs, deteriorating the magnetic properties. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 8-51034 [Patent Document 2] Japanese Patent Application Publication No. 55-125617 Summary of the Invention [Problem to be solved by the invention]

[0006] A common requirement for such static induction machines is to reduce the iron loss that occurs in the iron core. One method for achieving this is to irradiate the surface of grain-oriented electromagnetic steel sheets, which are often used as iron core materials, with a laser beam or electron beam to introduce minute distortions, dividing the magnetic domains and reducing abnormal eddy current loss, which is one of the iron losses.

[0007] However, wound cores, including toroidal cores in stationary induction machines, are generally subjected to stress relief annealing as described above, and the minute strains introduced by the laser beam or the like disappear during annealing, resulting in increased core loss.

[0008] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide a static induction motor and a manufacturing method thereof that can easily and effectively introduce strain into a toroidal core to reduce iron loss without being affected by stress relief annealing. [Means for solving the problem]

[0009] In order to achieve the above-mentioned object, the present invention provides a static induction motor comprising: an annular winding ring formed by winding a conductor a predetermined number of times; and at least one toroidal core having a circular cross section formed by winding a grain-oriented electromagnetic steel sheet a predetermined number of times and assembled in a wound state to a corresponding side of the winding ring, wherein the toroidal core is formed by unwinding the grain-oriented electromagnetic steel sheet from a wound core roll having a circular cross section and which has already been subjected to stress relief annealing to remove mechanical strain introduced into the grain-oriented electromagnetic steel sheet, and winding the grain-oriented electromagnetic steel sheet in a circular shape around the winding ring, and wherein the toroidal core is formed by winding the grain-oriented electromagnetic steel sheet around the winding ring so that it has an inner radius different from the inner radius of the wound core roll.

[0010] According to the static induction motor of the present invention having the above-mentioned configuration, strain is introduced into the steel plate by making the radius of curvature of the steel plate after stress relief annealing different from the radius of curvature of the steel plate in the completed state as a static induction motor. Therefore, strain can be easily and effectively introduced without being affected by stress relief annealing, thereby reducing the iron loss of the toroidal core.

[0011] In the above configuration, it is preferable that the inner radius of the toroidal core is larger than the inner radius of the wound core roll, so that when the toroidal core is wound around the winding ring body and assembled, a winding tightening force is generated in the toroidal core, making it easier to form the core.

[0012] In the above configuration, it is preferable that the magnetic flux density B8 in the grain-oriented electrical steel sheet is 1.88 T or more when excited with an AC magnetic field of 800 A / m at an AC frequency of 50 Hz. In a steel sheet having such material properties, the deviation of the crystal axis from the longitudinal direction of the steel sheet is small, and the hysteresis loss is small, but the magnetic domain width is wide. When the present invention is applied to such a steel sheet, the magnetic domain refinement effect by introducing strain is increased, and abnormal eddy current loss can also be reduced, resulting in low iron loss.

[0013] In the above configuration, the inner radius of the toroidal core is r c (m), the difference between the inner radius of the toroidal core and the inner radius of the wound core roll is Δr (m), and the thickness of the grain-oriented electrical steel sheet is t (m),

number

[0014] The present invention also provides a method for manufacturing a static induction machine, comprising the steps of: preparing an annular winding ring formed by winding a conductor a predetermined number of times; preparing a wound core roll having a circular cross section formed by winding a grain-oriented electromagnetic steel sheet a predetermined number of times; a stress relief annealing step of annealing the wound core roll to remove mechanical stress introduced into the grain-oriented electromagnetic steel sheet; and an assembly step of assembling at least one toroidal core to the winding ring by unwinding the grain-oriented electromagnetic steel sheet from the annealed wound core roll and winding it in a ring shape around a corresponding side of the winding ring, wherein the assembly step is characterized in that the grain-oriented electromagnetic steel sheet is wound around the winding ring so that the inner radius of the toroidal core is different from the inner radius of the wound core roll.

[0015] According to this manufacturing method, the toroidal core is wound and assembled around the winding ring so that it has an inner radius different from the inner radius of the wound core roll. Therefore, the radius of curvature of the steel sheet after stress relief annealing differs from the radius of curvature of the steel sheet in the completed state as a stationary inductor, and strain is introduced into the steel sheet. Therefore, strain can be easily and effectively introduced without being affected by stress relief annealing, thereby reducing the iron loss of the toroidal core. Effect of the Invention

[0016] According to the static induction motor and its manufacturing method of the present invention, the radius of curvature of the steel sheet after stress relief annealing is made different from the radius of curvature of the steel sheet in the completed static induction motor, so that stress is introduced into the steel sheet. This makes it possible to easily and effectively introduce strain without being affected by stress relief annealing, thereby reducing the iron loss of the toroidal core. [Brief description of the drawings]

[0017] [Figure 1] 1 is a schematic perspective view of a static induction device according to an embodiment of the present invention; [Diagram 2] FIG. 1A is a front view of a wound core roll after stress relief annealing, and FIG. 1B is a front view of a toroidal core alone in a state where it is wound around a winding ring and assembled, the front view being of a toroidal core having an inner radius larger than the inner radius of the wound core roll. [Diagram 3] FIG. 2 is a schematic perspective view showing an example of a state during a manufacturing process of a wound iron core roll. [Figure 4] FIG. 2 is a schematic perspective view showing an example of a winding ring body. [Diagram 5] FIG. 5 is a cross-sectional view taken along line AA in FIG. [Figure 6] 6 is an exploded view in cross section of the winding ring shown in FIG. 5, where (a) shows an outer winding frame constituting the winding ring, and (b) shows an inner winding frame constituting the winding ring. [Figure 7] 1 is a side view of the winding ring body showing a state in which a winding frame cover is about to be attached to an outer winding frame fitted onto an inner winding frame. FIG. [Figure 8] FIG. 1 is a schematic perspective view showing an example of an apparatus that can be used to wind grain-oriented electromagnetic steel sheets around a winding ring from a wound core roll after stress relief annealing in order to assemble a toroidal core to the winding ring. [Figure 9] FIG. 1 shows examples of dimensions of a winding ring and a toroidal core that constitute a static induction motor that can achieve low iron loss, where (a) is a front view of the assembled static induction motor, and (b) is a front view of the toroidal core alone. [Figure 10] 4 is a flowchart showing an example of a manufacturing process for a static induction device. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] A static induction electric device according to an embodiment of the present invention will be described in detail below. However, the present invention is not limited to the configuration disclosed in this embodiment, and various modifications are possible without departing from the spirit of the present invention. The numerical ranges described below include lower and upper limits. Values ​​indicated as "greater than" or "less than" are not included in the numerical range. Furthermore, "%" in relation to chemical composition means "% by mass" unless otherwise specified. In addition, terms used in this specification that specify shapes or geometric conditions and their degrees, such as "parallel," "vertical," "same," and "right angle," as well as values ​​of lengths and angles, are not to be bound by strict meanings but are to be interpreted to include a range within which similar functions can be expected. Furthermore, in this specification, a "grain-oriented electrical steel sheet" may be simply referred to as a "steel sheet" or an "electrical steel sheet", and a "toroidal iron core" may be simply referred to as an "iron core".

[0019] 1 is a schematic diagram of a static induction electric machine 1 according to an embodiment of the present invention. As shown in the figure, the static induction electric machine 1 according to this embodiment includes an annular winding ring body 2 formed by winding a conductor 7 a predetermined number of times, particularly in this embodiment, a rectangular annular winding ring body 2 having two parallel short leg parts 2a and two parallel long leg parts 2b and having a window 2c in the center, and at least one toroidal iron core 4 having a circular cross section formed by winding a grain-oriented electromagnetic steel sheet 10 a predetermined number of times and assembled in a wound state to a corresponding side of the winding ring body 2, particularly in this embodiment, two toroidal iron cores 4, 4 assembled in a wound state to the two long leg parts 2b, 2b corresponding to the two opposing sides of the winding ring body 2, respectively.

[0020] In this case, the toroidal core 4, 4 is formed by unwinding the electromagnetic steel sheet 10 from a wound core roll R (not shown in FIG. 1; see FIGS. 2, 3, and 8) having a circular cross section, which has already been subjected to stress relief annealing to remove mechanical strain induced in the electromagnetic steel sheet 10, and winding the electromagnetic steel sheet 10 in a circular shape around the corresponding long leg portion 2 b of the winding ring 4. Specifically, first, magnetic steel sheet 10 is wound into a cylindrical shape to create wound core roll R, and this wound core roll R is subjected to stress relief annealing to reduce iron loss. After that, magnetic steel sheet 10 pulled out from the outermost peripheral portion of wound core roll R is passed through window 2c of winding ring body 2 in a fixed state, then passed outside wound core roll R and passed through window 2c of winding ring body 2 again, and this process is repeated until finally, all of steel sheet 10 is wound around long leg 2b of winding ring body 2 while maintaining the original winding form (without switching the inner and outer periphery of wound core roll R), thereby forming toroidal core 4.

[0021] In the stationary induction motor 1 thus formed, as clearly shown in Fig. 2, the toroidal core 4 is wound and assembled around the winding ring body 2 so as to have an inner radius (the length from the center of the toroidal core 4 to the inner peripheral surface of the toroidal core 4) different from the inner radius of the wound core roll R (the length from the center of the wound core roll R to the inner peripheral surface of the wound core roll R). In particular, in this embodiment, the inner radius of the toroidal core 4 is set to be larger than the inner radius of the wound core roll R by Δr (m). In other words, when the inner radius of the toroidal core 4 is r c (m), and the inner radius of the wound core roll R is set to r c -Δr (m). With such dimensional settings, particularly in this embodiment, the outer diameter of the toroidal core 4 is also larger than the outer diameter of the wound core roll R. In this embodiment, if the sheet thickness of the grain-oriented electrical steel sheet 10 is t (m), then

number

[0022] In addition, in this embodiment, the grain-oriented electromagnetic steel sheet 10 constituting the toroidal core 4 (and therefore the wound core roll R) has material properties such that the magnetic flux density B8 is 1.88 T or more when excited with an AC magnetic field of 800 A / m at an AC frequency of 50 Hz.

[0023] Hereinafter, an apparatus and a manufacturing method for winding and assembling the toroidal core 4 around the winding ring body 2 so that the toroidal core 4 has an inner radius different from the inner radius of the wound core roll R will be described. 3 shows an example of a state during the manufacturing process of a wound core roll R. In this state, a steel sheet 10 slit to a specified width is wound around a cylindrical or cylindrical winding core 30 until a specified winding thickness is achieved, and a fixing band 22 is wrapped around the outer periphery to fix it. By achieving this state, a wound core roll R having a circular cross section formed by winding the grain-oriented electromagnetic steel sheet 10 a specified number of times is manufactured (step S1 in FIG. 10; process of preparing a wound core roll). Here, the outer radius of the winding core 20 is set to rc-Δr. By doing so, the inner radius of the wound core roll R wound around the outer periphery of the winding core 20 becomes rc-Δr.

[0024] Thereafter, stress relief annealing is performed on the wound core roll R in the state shown in Fig. 3 (step S2 in Fig. 10; stress relief annealing step). This annealing fixes the shape of the steel sheet 10, and the inner radius rc-Δr of the wound core roll R is maintained even if the fixing band 22 is removed. The state of the wound core roll R at this time is shown in Fig. 2(a).

[0025] Fig. 4 shows an example of the winding ring body 2 in more detail than Fig. 1. Fig. 5 shows a cross-sectional view along line AA in Fig. 4, and Fig. 6 shows an exploded view of the winding ring body 2. As can be seen from these figures, the winding ring body 2 is mainly composed of an inner winding frame 34, an outer winding frame 32 fitted onto the outer periphery of the inner winding frame 34, a winding frame cover 30 attached to the outer winding frame 32, an inner winding 7a consisting of the conductor 7 wound around the outer periphery of the inner winding frame 34, and an outer winding 7b consisting of the conductor 7 wound around the outer periphery of the outer winding frame 32. In this case, the inner winding 7a and the outer winding 8b are each either a primary winding or a secondary winding.

[0026] As clearly shown in Figures 5 and 6, the inner winding frame 34 has a rectangular frame body 34a having bent parts with a predetermined curvature at the four corners, and a conductor winding part 34b formed separately or integrally on the outer periphery of the frame body 34a. In this case, the conductor winding part 34b has a recess 34c formed around the entire periphery of the frame body 34a so that the inner winding 7a can be accommodated in a wound state, and the bottom surface of the recess 34c is arc-shaped. On the other hand, the outer winding frame 32 has a rectangular frame body 32a having bent parts with a predetermined curvature at the four corners and forming a rectangular fitting window 32e on the inside into which the inner winding frame 34 can be fitted, and a conductor winding part 32b formed separately or integrally on the outer periphery of the frame body 32a. In this case, the conductor winding portion 32b is formed around the entire outer circumference of the frame body 34a and is composed of a planar bottom wall portion 32c that may be formed by the frame body 32a and side wall portions 32d extending in an arc shape from both sides of the bottom wall portion 32c, and the bottom wall portion 32c and the side wall portions 32d define a conductor accommodating space on the inside that can accommodate at least a part of the outer winding 7b in a wound state. In addition, the reel cover 30 having an arc-shaped cross section is attached to the outer reel 32, more precisely, to the arc-shaped side wall portion 32d of the conductor winding portion 32b of the outer reel 32, so as to close the conductor accommodating space, and when the reel cover 30 is attached to the side wall portion 32d, in the cross section shown in FIG. 5, the reel cover 30 and the side wall portion 32d cooperate to form a semicircle with the same radius of curvature centered on a common point. Furthermore, in the assembled state in which the inner winding frame 34 is fitted into the inner fitting window 32e of the outer winding frame 32, in the cross section shown in FIG. 5, the arc-shaped winding frame cover 30, the arc-shaped side wall portion 32d of the conductor winding portion 32b, and the portion of the conductor winding portion 34b that forms the arc-shaped bottom surface of the recess 34c cooperate to form a true circle C (the portion around which the toroidal core 4 is wound and comes into contact) with the same radius of curvature and centered at a common point.

[0027] In this way, the winding ring body 2 is formed by winding the windings (conductor) 7a, 7b around the conductor winding portions 32b, 34b of the outer winding frame 32 and the inner winding frame 34, respectively, fitting the outer winding frame 32 into the inner winding frame 34 (or vice versa) as shown by the arrow X in FIG. 6, and attaching the winding frame cover 30 so as to cover the outer winding frame 32 as shown by the arrow Y in FIG. 6 and FIG. 7. That is, in this way, the annular winding ring body 2 is manufactured by winding the conductor 7 (7a, 7b) a predetermined number of times (step S3 in FIG. 10; a step of preparing a winding ring body). Note that the manufacture of such a winding ring body 2 is performed in parallel with the manufacture of the wound core roll R in order to shorten the process (step S1 (S2) is performed in parallel with step S3).

[0028] Next, with reference to FIG. 8, a case where the toroidal core 4 is assembled to the winding ring body 2 thus formed by using an assembly device 90 will be described. First, the wound core roll R after stress relief annealing is set on the wound core rotating shaft 62 supported rotatably on the base 70 of the assembly device 90. Then, the end of the steel sheet 10 on the outer periphery of the wound core roll R is pulled out from the wound core roll R and passed through the central window 2c of the winding ring body 2 (so as to go around the long leg portion 2b), and then the end of the steel sheet 10 is returned to the wound core roll R and passed between the wound core roll R and the pinch roll 50 arranged outside the wound core roll R so as to be rotatable and translatable. Thereafter, the pinch roll 50 is driven to rotate in the direction of the arrow Q so that the steel sheet 10 flows in the direction of the arrow P. At this time, it is preferable to provide a mechanism for driving the wound core rotating shaft 62 so as not to cause slack in the steel sheet 10. As this winding process (step S4 in FIG. 10; an assembly process in which the toroidal core is assembled into the winding ring body) progresses, the winding thickness of the wound core roll R decreases, so the pinch roll 50 is structured to be able to translate in the direction of the wound core rotation shaft 62 and is controlled so that an approximately constant pressure is always applied to the wound core roll R. In this embodiment, the pinch roll 50 is able to translate in the direction of the wound core rotation shaft 62 along a guide hole 72 formed in a base 70.

[0029] Furthermore, a guide roll 60 extends vertically from the base 70 adjacent to the steel sheet winding portion (long leg portion 2b) of the winding ring body 2. This guide roll 60 plays a role in smoothing the flow of the steel sheet 10 in the direction of arrow P, and is movable (movable along a guide groove 74 provided in the base 70) so that its position changes in accordance with an increase in the thickness of the steel sheet 10 (toroidal iron core 4) on the winding ring body 2 side. Although only one such guide roll 60 is shown in the figure, multiple guide rolls 60 may be provided to make the flow of the steel sheet 10 smoother.

[0030] By using such an assembly device 90, all of the steel sheets 10 from the wound core roll R can be wound around the long leg 2b of the winding ring body 2 while maintaining the original winding form (without switching the inner and outer periphery of the wound core roll R), thereby forming a toroidal core 4 that is assembled to the winding ring body 2.

[0031] In the present embodiment, in the stationary induction electric machine 1 manufactured in this manner, the outer radius of the perfect circle C formed by the arc-shaped reel cover 30, the arc-shaped side wall 32d of the conductor winding portion 32b, and the portion of the conductor winding portion 34b forming the arc-shaped bottom surface of the recess 34c is set to rc. With such dimension setting, the inner radius becomes rc when the core 4 is assembled. With the above method, the wound core roll R has an inner radius of rc-Δr after stress relief annealing, and when it is assembled into the winding body 2 as the core 4, that is, when the stationary induction electric machine 1 is completed, the inner radius of the toroidal core 4 becomes rc, thereby realizing the conditions of the present invention. Note that the above device configuration and manufacturing method are merely examples, and the winding body 2 may have any shape as long as the portion of the winding body 2 in contact with the core 4 is a perfect circle and its outer radius is rc.

[0032] The following table shows how the iron loss of the toroidal core 4 of the stationary induction motor 1 according to this embodiment manufactured as described above is improved. [Table 1] Here, this table shows the dimensions of the stationary induction motor 1 shown in FIG. 9 (the inner radius rc (m) of the toroidal core 4 is 1 00mm, outer radius 2 The table shows the results of determining the iron loss (W) of the toroidal core 4 when the difference Δr (m) between the inner radius of the toroidal core 4 and the inner radius of the wound core roll R is changed from 1 mm to 10 mm for a steel sheet 10 having a diameter of 1.00 mm, length of 600 mm, and thickness of 0.23 mm (as a magnetic characteristic, the magnetic flux density B8 of the steel sheet when excited at 800 A / m was 1.92 T). As can be seen from this table, when the inner radius of the toroidal core 4 is rc (m), the difference between the inner radius of the toroidal core 4 and the inner radius of the wound core roll R is Δr (m), and the sheet thickness of the grain-oriented electromagnetic steel sheet 10 is t (m),

number

[0033] The present invention is not limited to the above-described embodiment, and can be modified in various ways without departing from the spirit of the present invention. For example, the order of the manufacturing steps shown in FIG. 10 is merely an example, and is not limited to this. Furthermore, the manufacturing apparatus is not limited to the one shown in FIG. 4. [Explanation of symbols]

[0034] 1 Stationary induction appliance 2 Winding ring 4 Toroidal core 7 Conductor 10 Grain-oriented electrical steel sheet R-wound iron core roll

Claims

1. preparing an annular winding ring formed by winding a conductor a predetermined number of times; preparing a wound core roll having a circular cross section, the roll being made by winding a grain-oriented electromagnetic steel sheet a predetermined number of times, the sheet having a magnetic flux density B8 of 1.88 T or more when excited with an AC magnetic field of 800 A / m having an AC frequency of 50 Hz; a stress relief annealing process for annealing the wound core roll to remove mechanical stress induced in the grain-oriented electrical steel sheet; an assembling process of assembling at least one toroidal core to the winding ring by winding a grain-oriented electromagnetic steel sheet in a circular shape around a corresponding side of the winding ring without switching the inner and outer periphery of the wound core roll while unwinding the grain-oriented electromagnetic steel sheet from the annealed wound core roll; Including, The assembly process is carried out as follows, where the inner radius of the toroidal core is rc (m), the difference between the inner radius of the toroidal core and the inner radius of the wound core roll is Δr (m), and the thickness of the grain-oriented electromagnetic steel sheet is t (m): The grain-oriented electromagnetic steel sheet is wound around the winding ring body so that the inner radius of the toroidal core is different from the inner radius of the wound core roll, so that the relationship of A method for manufacturing a static induction electric appliance, comprising:

2. 2. The method for manufacturing a stationary induction machine according to claim 1, wherein the assembling step winds the grain-oriented electromagnetic steel sheet around the winding ring body so that an inner radius of the toroidal core is larger than an inner radius of the wound core roll.

Citation Information

Patent Citations

  • Device for winding core

    JP1980125617A

  • Winding device of wound core

    JP1996017669A

  • Transformer, coil bobbin and wound core therefor

    JP1996051034A

  • Process for producing grain-oriented magnetic steel sheet, grain-oriented magnetic steel sheet for wound core, and wound core

    WO2010110217A1