Frame material

A skeletal member with controlled concave bead portions and hardness standard deviation in a closed cross-section design addresses the challenge of elastic buckling and bending fracture in high-strength steel frames, enhancing energy absorption efficiency.

JP7568979B2Active Publication Date: 2024-10-17NIPPON STEEL CORPORATION
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023518670
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-05-06
Filing Date
2022-04-26
Publication Date
2024-10-17
Estimated Expiration
2042-04-26

AI Technical Summary

Technical Problem

Existing frame members made of high-strength steel plates struggle to achieve both weight reduction and enhanced energy absorption efficiency due to issues like elastic buckling and premature bending fracture during collisions.

Method used

A skeletal member with a closed cross-section design featuring concave bead portions and controlled width and hardness standard deviation ratios, formed by hot stamping, which suppresses elastic buckling and prevents bending fracture, thereby improving energy absorption efficiency.

Benefits of technology

The design achieves high energy absorption efficiency by preventing elastic buckling and bending fracture, even with thin, high-strength steel, ensuring effective impact energy absorption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007568979000005
    Figure 0007568979000005
  • Figure 0007568979000006
    Figure 0007568979000006
  • Figure 0007568979000007
    Figure 0007568979000007
Patent Text Reader

Abstract

This skeleton member is formed by hot-stamping a steel sheet. The skeleton member is so formed as to have a closed cross-sectional part in which a cross-section perpendicular to the longitudinal direction of the member is closed. The closed cross-sectional part comprises: at least two flat portions each having a curvature radius greater than the maximum outside dimension of said cross-section; and a recessed bead portion formed between the two flat portions. The recessed bead portion has a pair of walls which have a curvature radius of at least 50 mm and which protrude from the respective opposing ends of the two flat portions toward the inside of the closed cross-sectional part by way of a pair of inflected parts that are inflected toward the interior of the closed cross-section. In each of the walls, the central part in the thickness direction has a Vickers hardness of at least 520 Hv. The width of each of the walls is 0.5-2.5 times the effective width We. A standard deviation ratio, which is determined by dividing the standard deviation of hardness frequency distribution at a surface part of the walls by the standard deviation of hardness frequency distribution at the central part in the thickness direction of the walls, is smaller than 1.0.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a framework member having excellent energy absorption efficiency. This application claims priority based on Japanese Patent Application No. 2021-078463, filed on May 6, 2021, the contents of which are incorporated herein by reference. [Background technology]

[0002] Conventionally, hollow members made of steel plates processed into a predetermined closed cross-sectional shape have been used as automotive frame members. Such frame members are required to be lightweight and to exhibit sufficient strength and energy absorption performance when bending loads are applied due to a collision.

[0003] The main method used to reduce weight is to increase the strength of steel plates to increase their yield strength and energy absorption performance, and then to reduce the weight of the components by making them thinner. For this reason, in recent years, steel plates capable of demonstrating a tensile strength of over 1.8 GPa are sometimes used as materials for structural members.

[0004] Patent Document 1 discloses a vehicle collision-resistant reinforcement material made of a molded thin plate for the purpose of improving buckling resistance, which comprises at least a main body portion and a pair of side wall portions integrated with the main body portion via a bent portion, and the main body portion is provided with a concave bead extending along its longitudinal direction to the center of the width of the main body portion, and the concave bead is provided so that the distance between the concave bead and the bent portion satisfies a specific range, with the effective width c' being the distance between the concave bead and the bent portion. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Publication No. 2009-286351 Summary of the Invention [Problem to be solved by the invention]

[0006] According to the technology of Patent Document 1, by providing beads taking into consideration the effective width, elastic buckling can be suppressed and strength can be improved. However, in order to reduce weight by further thinning, it is necessary to devise a way to further increase the energy absorption efficiency, which is the amount of energy absorbed per unit cross-sectional area of ​​the frame member.

[0007] The present invention has been made in view of the above problems, and an object of the present invention is to provide a framework member having excellent energy absorption efficiency. [Means for solving the problem]

[0008] Specific embodiments of the present invention are as follows. (1) A first aspect of the present invention is a skeletal member formed by hot stamping a steel plate, the skeletal member having a closed cross-section portion in a cross section perpendicular to a longitudinal direction, the closed cross-section portion having at least two flat portions having a radius of curvature larger than a maximum outer dimension of the cross-section, and a concave bead portion formed between the two flat portions, the concave bead portion having a pair of wall portions having a radius of curvature of 50 mm or more, the pair of wall portions protruding from opposing ends of the two flat portions toward the inside of the closed cross-section portion via a pair of bent portions that bend toward the inside of the closed cross-section, the Vickers hardness of the plate thickness center portion of the wall portions being 520 Hv or more, the width of the wall portions being an effective width W calculated from Karman's effective width formula e and the standard deviation ratio, calculated by dividing the standard deviation of the hardness frequency distribution in the surface layer portion of the wall portion by the standard deviation of the hardness frequency distribution in the thickness center portion of the wall portion, is smaller than 1.0. (2) In the skeletal member described in (1) above, the closed cross-sectional portion may be present over 50% or more of the entire length of the skeletal member in the longitudinal direction. (3) In the skeleton member described in (1) or (2) above, the closed cross-sectional portion may be formed by joining a plurality of members. (4) In the framework member according to any one of (1) to (3) above, the plate thickness of the recessed bead portion may be 1.2 mm or less. (5) The framework member according to any one of (1) to (4) above may have two or more of the recessed bead portions. (6) In the framework member according to any one of (1) to (5) above, the standard deviation ratio may be smaller than 0.8. Effect of the Invention

[0009] According to the above aspect, by controlling the width of the wall of the recessed bead portion and the hardness standard deviation ratio within an appropriate range, it is possible to prevent bending fracture while suppressing elastic buckling. This makes it possible to obtain high energy absorption performance even when a high-strength thin-walled member is used. Therefore, it is possible to achieve excellent energy absorption efficiency. [Brief description of the drawings]

[0010] [Figure 1] FIG. 2 is a perspective view showing a framework member according to an embodiment of the present invention. [Diagram 2] 2 is a cross-sectional view taken along line A1-A1 in FIG. 1. [Diagram 3] FIG. 3 is an enlarged view of the area surrounded by A in FIG. [Figure 4] 1 is a graph showing the relationship between the hardness standard deviation ratio and the bending angle ratio in a VDA bending test for a 2.0 GPa-class material. [Diagram 5] FIG. 11 is a perspective view showing a skeleton member according to a modified example. [Figure 6] 6 is a cross-sectional view taken along line A2-A2 in FIG. 5. [Figure 7] FIG. 7 is an enlarged view of the area surrounded by B in FIG. [Figure 8] FIG. 11 is a cross-sectional view showing a modified example of the framework member. [Figure 9] 13A and 13B are schematic diagrams showing modified examples of the recessed bead portion. [Figure 10] 13A and 13B are schematic diagrams showing other modified examples of the recessed bead portion. [Figure 11]1 is a perspective view showing an automobile frame as an example to which a frame member is applied; [Figure 12] 4 is a schematic diagram for explaining a cross-sectional shape of a rectangular tube member used in the first embodiment. FIG. [Figure 13] 13 is a graph plotting the relationship between the effective width ratio and the energy absorption efficiency for the first experimental example. [Figure 14] 13 is a schematic diagram for explaining the cross-sectional shape of a rectangular tube member used in the second embodiment. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The present inventors have conducted extensive research into the configuration of a framework member that can exhibit excellent energy absorption efficiency. First, in order to achieve excellent energy absorption efficiency, it is important that the material has a certain level of bending strength. By forming beads along the longitudinal direction of the material, it is possible to improve the bending strength when an input load is applied in the bending direction due to a collision, but if elastic buckling (deflection) occurs on the bead wall in the early stages of deformation, the necessary bending strength cannot be obtained, and it may not be possible to achieve excellent energy absorption efficiency. In order to achieve excellent energy absorption efficiency, it is also important that the frame members deform in a desired deformation mode immediately after a bending load is applied due to a collision, thereby efficiently absorbing the impact energy. In particular, if breakage occurs at the bent portion after deformation has started, excellent energy absorption efficiency may not be achieved. Therefore, if the cross-sectional design can be made such that elastic buckling is less likely to occur on the surface where the bead is formed, and if high bending performance that makes it less likely to break can be imparted, it can be said that it is possible to achieve excellent energy absorption efficiency.

[0012] Here, when increasing the strength of a component and reducing its thickness as a means for achieving weight reduction, the following problems arise. - Thinning of the walls makes it easier for elastic buckling to occur, making it difficult to obtain the necessary strength. - Increasing the strength of steel plates reduces their bending performance, making them more susceptible to fracture at the bent part after deformation has begun, making it difficult to efficiently absorb impact energy. The present inventors have noticed that the above problems are factors preventing further increase in strength and reduction in thickness of high-strength steel plates. The inventors further investigated and found that by controlling the width and hardness standard deviation ratio of the wall of the concave bead within an appropriate range, it is possible to suppress elastic buckling and prevent bending fracture. Such control can solve the above-mentioned problems that are of concern when using high-strength steel plates, and can achieve excellent energy absorption efficiency, leading to the completion of the present invention.

[0013] First embodiment Hereinafter, a skeleton member 1 according to a first embodiment of the present invention will be described.

[0014] First, the terms used in this specification will be explained. The term "longitudinal direction" refers to the direction of the material axis of a skeletal member, that is, the direction in which the axis extends. The "surface assumed to be subjected to bending compression" refers to a portion of a skeletal member where a compressive stress in the longitudinal direction is assumed to occur when the skeletal member is subjected to a bending load due to a collision or the like. "Flat portion" means a linear portion in a cross section perpendicular to the longitudinal direction of the skeletal member, specifically, a portion having a radius of curvature greater than the maximum outer dimension of the cross section. The maximum outer dimension means the length of the straight line that is the maximum distance between the ends of any two points in the cross section. Among the portions that make up the recessed bead portion, linear portions are not considered to be flat portions. The "concave bead portion" refers to a portion that protrudes from an assumed bending compression surface toward the inside of a closed cross-sectional portion in a cross-section perpendicular to the longitudinal direction of a skeleton member. The "corner portion" refers to a non-linear portion of a cross section perpendicular to the longitudinal direction of a skeletal member, excluding flat portions and recessed bead portions.

[0015] "Width" refers to the line length along the circumferential direction of the closed cross-sectional portion. For example, "the width of a wall portion" refers to the line length between one end and the other end of the wall portion. The "effective width" is the effective width W calculated from the following formula (1) based on the Karman effective width theory. e It is.

number

[0016] The "energy absorption amount" is the amount of energy absorption calculated from the relationship between the impactor reaction force (load) and stroke when a rigid flat impactor is collided with the assumed bending compression surface with both ends of the skeletal member fully restrained. "Energy absorption efficiency" refers to the amount of energy absorbed per cross-sectional area of ​​a skeleton member. When a skeleton member does not have a uniform cross section in the longitudinal direction, it refers to the amount of energy absorbed per cross-sectional area of ​​a closed cross section perpendicular to the longitudinal direction of the member that has the smallest cross-sectional area.

[0017] Fig. 1 is a perspective view of a skeleton member 1. Fig. 2 is a cross-sectional view taken along line A1-A1 in Fig. 1, which is a cross-sectional view perpendicular to the longitudinal direction of the skeleton member 1. Fig. 3 is an enlarged view of a region surrounded by A in Fig. 2.

[0018] 1 and 2, the skeleton member 1 is composed of a hollow cylindrical main body 10 extending in the longitudinal direction. In other words, the skeleton member 1 is a member whose cross section perpendicular to the longitudinal direction is a closed cross section as a single unit. The frame member 1 is arranged so that the assumed bending compression surface faces the outside of the vehicle body, and thereby exhibits load resistance against compressive stress at the assumed bending compression surface in the event of a collision.

[0019] On the assumed bending compression surface, a concave bead portion 100 is provided sandwiched between two first flat portions 11,11. If the bending compression assumed surface were composed only of flat portions, the flat portions might deflect when subjected to a compressive load, and the load-bearing capacity might not be fully exerted. However, by arranging a recessed bead portion 100 sandwiched between two first flat portions 11, 11, as in the skeletal member 1, the load-bearing capacity can be improved.

[0020] First corner regions C1, C1 are formed at the outer end of each of the first flat regions 11, 11. Two second flat regions 13, 13 facing each other extend from the end of the first corner regions C1, C1 opposite the first flat regions 11, 11. Further, second corner regions C2, C2 that are bent toward each other are formed at the end portions of the second flat regions 13, 13 opposite the first corner regions C1, C1. The ends of the second corner regions C2, C2 opposite the second flat region 13 are connected to each other by a third flat region 15.

[0021] Therefore, the skeleton member 1 according to this embodiment forms a closed cross-sectional portion by the recessed bead portion 100, the first flat portions 11, 11, the second flat portions 13, 13, the third flat portion 15, the first corner portions C1, C1, and the second corner portions C2, C2.

[0022] As shown in FIG. 3, in a cross section perpendicular to the longitudinal direction of the skeleton member 1, the concave bead portion 100 is composed of first bent portions 121, 121 walls 123, 123 second bent portions 125, 125, and a bottom portion 127.

[0023] The first bent portions 121, 121 are portions that bend toward the inside of the closed cross section from the opposing ends of the two first flat regions 11, 11. A portion with a radius of curvature of 50 mm or more is regarded as part of the wall, so the radius of curvature of the first bent portion 121 is less than 50 mm. The radius of curvature of the first bent portion 121 may be, for example, 3 mm to 5 mm.

[0024] The wall portions 123, 123 are portions that protrude toward the inside of the closed cross-sectional portion via the first bent portions 121, 121. The wall portions 123, 123 are linear portions with a curvature radius of 50 mm or more.

[0025] The second bent portions 125, 125 are portions bent toward each other from the end portions of the wall portions 123, 123 opposite to the first bent portions 121, 121. A portion with a radius of curvature of 50 mm or more is regarded as part of the wall portion 123 or part of the bottom portion 127, and therefore the radius of curvature of the second bent portion 125 is less than 50 mm. The radius of curvature of the second bent portion 125 may be, for example, 3 mm to 5 mm.

[0026] The bottom portion 127 is a portion that linearly connects the ends of the second bent portions 125, 125 on the opposite side to the wall portions 123, 123.

[0027] If the width H0 of the wall portion 123 of the recessed bead portion 100 is too large, elastic buckling is likely to occur in the early stage of deformation when the frame member 1 is subjected to a bending load, and the necessary strength cannot be obtained. This makes it difficult for the frame member 1 to exhibit excellent energy absorption efficiency. Therefore, the width H0 of the wall portion 123 is set to be less than the effective width W e The maximum value is set to 2.5 times the maximum value.

[0028] On the other hand, if the width H0 of the wall portion 123 is too small, the effect of improving the bending strength by providing the concave bead is reduced. e It is set to at least 0.5 times the Furthermore, the effective width W e In order to obtain the necessary strength, the upper limit is preferably 60 mm or less.

[0029] From the viewpoint of weight reduction, the plate thickness of the concave bead portion 100 is preferably 1.2 mm or less. On the other hand, when the plate thickness of the concave bead portion 100 is less than 0.4 mm, Since elastic buckling is likely to occur in the wall portion 123, the setting range of the width H0 is subject to greater restrictions. Therefore, it is preferable that the plate thickness of the concave bead portion 100 is 0.4 mm or more.

[0030] The skeletal member 1 is formed by heating a hot stamping steel plate to the austenite region, forming it into a predetermined shape by hot stamping, which is a press process in which the steel plate is quenched while being held at a predetermined temperature range using a press die having a quenching mechanism, and then joining the end faces. The skeletal member 1 thus formed has a tensile strength of more than 1.8 GPa. Furthermore, by forming the skeletal member 1 thus formed, the Vickers hardness of the wall portion 123 of the concave bead portion 100 in the skeletal member 1 at the center of the plate thickness is 520 Hv or more when the test load is 300 gf (2.9 N) in a hardness test performed according to the method described in JIS Z 2244:2009. In the present application, since the objective is to improve deformability and exhibit excellent energy absorption efficiency on the premise of high strength, the hardness of the center part of the plate thickness in the wall part 123 of the concave bead portion 100 is set to 520 Hv or more in Vickers hardness. The upper limit of the hardness at the center of the plate thickness is not particularly specified, but may be 850 Hv or less in Vickers hardness.

[0031] The hardness of the wall portion 123 of the concave bead portion 100 at the center of the sheet thickness was measured as follows. A sample having a cross section perpendicular to the plate surface is taken from the wall portion 123 of the concave bead portion 100, the cross section is prepared as a measurement surface, and the measurement surface is subjected to a hardness test. The size of the measurement surface may be about 10 mm x 10 mm, depending on the measurement device. The measurement surface shall be prepared in accordance with JIS Z 2244:2009. The measurement surface is polished using #600 to #1500 silicon carbide paper, and then the measurement surface is finished to a mirror finish using a liquid in which diamond powder with a particle size of 1 μm to 6 μm is dispersed in a diluted solution such as alcohol or pure water.

[0032] The measurement surface thus mirror-finished is subjected to a hardness test according to the method described in JIS Z 2244:2009. Using a micro Vickers hardness tester, measurements are taken at 30 points at 3 / 8 of the sample thickness, with a load of 300 gf, and at intervals of at least three times the indentation. The average of these measurements is the hardness at the center of the plate thickness.

[0033] As described above, the width H0 of the wall portion 123 is equal to the effective width W e When the effective width W is 2.5 times or less, it is possible to suppress elastic buckling in the wall portion 123. However, in the case of a high-strength material, for example, a hot stamped material having a strength of more than 1.8 GPa, e Even if elastic buckling can be suppressed by controlling the bending load, if the bending performance is insufficient, breakage will occur during deformation due to the bending load, and excellent energy absorption efficiency will not be obtained. However, in the skeletal member 1 according to this embodiment, the bending performance is improved by appropriately controlling the ratio between the standard deviation of the hardness frequency distribution at the center of the plate thickness of the wall portion 123 in the concave bead region 100 and the standard deviation of the hardness frequency distribution at the surface layer. Therefore, in the skeleton member 1 according to this embodiment, even if a high-strength material is used, breakage during deformation is suppressed, and it is possible to achieve energy absorption efficiency that is far superior to conventional materials. Specifically, in the skeletal member 1 according to this embodiment, in the wall portion 123 of the concave bead portion 100, the hardness standard deviation ratio, which is the standard deviation of the hardness frequency distribution in the surface layer divided by the standard deviation of the hardness frequency distribution in the center portion of the plate thickness (a depth position of 3 / 8 of the plate thickness), is controlled to a value smaller than 1.0.

[0034] The inventors have found through experiments that when applying hot stamping material of over 1.8 GPa, if the hardness standard deviation ratio is set to a value smaller than 1.0, the maximum bending angle in the VDA bending test based on the VDA standard (VDA238-100) specified by the German Association of the Automotive Industry can be significantly improved. Figure 4 is a graph showing the results of a VDA bending test using a 2.0 GPa-class steel plate with a thickness of 1.4 mm. It can be seen that the smaller the hardness standard deviation ratio is from 1.0, the higher the maximum bending angle (°) in the VDA bending test and the higher the bending angle ratio. In other words, when the hardness standard deviation ratio is smaller than 1.0, breakage is less likely to occur during deformation due to axial load, and excellent energy absorption efficiency can be achieved. It is more preferable that the standard deviation ratio is smaller than 0.8.

[0035] Here, the hardness frequency distribution in the center portion of the sheet thickness and the hardness frequency distribution in the surface layer portion are obtained by a Vickers hardness test. First, a sample having a cross section perpendicular to the plate surface is cut out from an arbitrary position including the wall portion 123 of the concave bead portion 100, and the cross section is prepared as a measurement surface, which is then subjected to a hardness test. The size of the measurement surface may be about 10 mm x 10 mm, depending on the measurement device. The measurement surface shall be prepared in accordance with JIS Z 2244:2009. The measurement surface is polished using #600 to #1500 silicon carbide paper, and then the measurement surface is finished to a mirror finish using a liquid in which diamond powder with a particle size of 1 μm to 6 μm is dispersed in a diluted solution such as alcohol or pure water.

[0036] The measurement surface thus mirror-finished is subjected to a hardness test according to the method described in JIS Z 2244:2009. The hardness of the surface layer is measured using a micro Vickers hardness tester. A load of 300 gf is used to measure 30 points at intervals of at least three times the indentation, and the hardness frequency distribution in the surface layer is determined. Similarly, at the center of the plate thickness (at a depth of 3 / 8 of the plate thickness), measurements are taken at 30 points spaced at intervals three or more times the indentation with a load of 300 gf to determine the hardness frequency distribution at the center of the plate thickness.

[0037] A known statistical method is used to determine the standard deviation of the hardness frequency distribution in the center portion of the plate thickness and the hardness frequency distribution in the surface layer portion obtained as a result of the above-mentioned Vickers hardness test.

[0038] When the metal structure of a steel sheet for hot stamping is the same at the center of the sheet thickness and at the surface layer, as in the past, the hardness frequency distribution at the surface layer is the same as the hardness frequency distribution at the center of the sheet thickness, and the hardness standard deviation ratio is 1.0. On the other hand, when the metal structure is modified only in the surface layer and its vicinity, the hardness standard deviation ratio will be a value other than 1.0. In the skeletal member 1 formed from the hot stamping steel sheet according to this embodiment, the metal structure of only the surface layer and its vicinity is modified, so that the distribution and variation of hardness in the surface layer is suppressed, and the hardness standard deviation ratio between the surface layer and the center of the sheet thickness can be made smaller than 1.0. Specifically, the hardness standard deviation ratio can be controlled by adjusting the maximum heating temperature and holding time during decarburization annealing of the steel sheet for hot stamping, which is a known technique. The decarburization annealing conditions are preferably a decarburization annealing temperature (maximum temperature reached by the steel sheet) of 700 to 950°C in a moist atmosphere containing hydrogen, nitrogen or oxygen, and a residence time in the temperature range of 700 to 950°C of 5 to 1200 seconds. Furthermore, within this condition range, by narrowing the annealing temperature to a higher temperature range and the residence temperature to a longer time range, the hardness standard deviation ratio can be made smaller than 0.8. The above condition for the hardness standard deviation ratio needs to be satisfied by at least one surface layer of the wall portion 123. However, it is preferable that the surface layers on both sides of the wall portion 123 satisfy the above condition for the hardness standard deviation ratio.

[0039] In this manner, according to the skeletal member 1 of this embodiment, elastic buckling can be suppressed by controlling the width H0 of the wall portion 123 of the recessed bead portion 100, and breakage during deformation can be suppressed by controlling the hardness standard deviation ratio. Therefore, while the wall portion 123 of the concave bead portion 100 has a sufficient Vickers hardness of 520 Hv or more at the center of the plate thickness, the energy absorption efficiency can be significantly improved.

[0040] Second Embodiment The skeleton member 2 according to the second embodiment of the present invention will now be described. The skeleton member 2 according to the second embodiment differs from the skeleton member 1 according to the first embodiment in that the cross section perpendicular to the longitudinal direction is a closed cross section formed by two members. That is, in the skeleton member 2, the closed cross section is formed by two joined members. For components having substantially the same functional configuration as those described in the first embodiment, a duplicated description will be omitted.

[0041] Fig. 5 is a perspective view of the skeleton member 2. Fig. 6 is a cross-sectional view taken along the line A2-A2 in Fig. 5, which is a cross-sectional view perpendicular to the longitudinal direction of the skeleton member 2. Fig. 7 is an enlarged view of the area surrounded by B in Fig. 6.

[0042] 5 and 6, the skeleton member 2 forms a closed cross-sectional portion by joining a first skeleton member 20 and a second skeleton member 30. That is, the closed cross-sectional portion is configured to include the first skeleton member 20 and the second skeleton member 30.

[0043] The first framework member 20 is a member having a hat-shaped cross section, and its top surface functions as an assumed bending and compression surface. On the assumed bending compression surface, the concave bead portion 200 is sandwiched between the two first flat portions 21, 21.

[0044] First corner regions C1, C1 are formed at the outer end of each of the first flat regions 21, 21. Two second flat regions 23, 23 whose surfaces face each other extend from the end of the first corner regions C1, C1 opposite the first flat regions 21, 21. Further, second corner regions C2, C2 bent in a direction away from each other are formed at the end of each second flat region 23, 23 opposite the first corner region C1, C1. Third flat regions 25, 25 extend in a direction away from each other from the end of each second corner region C2, C2 opposite the second flat region 23.

[0045] The second skeletal member 30 is a flat steel plate and has a pair of joining regions 31, 31 that are in face-to-face contact with the third flat regions 25, 25 of the first skeletal member 20 and joined by spot welding or the like, and a flat region 33 sandwiched between the pair of joining regions 31, 31.

[0046] Therefore, the skeletal member 2 of this embodiment forms a closed cross-sectional portion by the concave bead portion 200, the first flat portions 21, 21, the second flat portions 23, 23, the first corner portions C1, C1, and the second corner portions C2, C2 in the first skeletal member 20, and the flat portion 33 in the second skeletal member 30.

[0047] As shown in FIG. 7, in a cross section perpendicular to the longitudinal direction of the skeleton member 2, the concave bead portion 200 is composed of first bent portions 221, 221, wall portions 223, 223, second bent portions 225, 225, and a bottom portion 227. The configuration of the recessed bead portion 200 is similar to that of the recessed bead portion 100 described in the first embodiment, and therefore a detailed description thereof will be omitted.

[0048] In this manner, in the skeletal member 2 in which a closed cross-section is formed by two joined members, elastic buckling can be suppressed by controlling the width H0 of the wall portion 223 of the concave bead portion 200, and breakage during deformation can be suppressed by controlling the hardness standard deviation ratio, similar to the skeletal member 1. The closed cross-section may be formed by two or more joined members.

[0049] Although the preferred embodiments of the present invention have been described in detail above with reference to the accompanying drawings, the present invention is not limited to such examples. It is clear that a person with ordinary knowledge in the technical field to which the present invention pertains can think of various modified or altered examples within the scope of the technical ideas described in the claims, and it is understood that these also naturally fall within the technical scope of the present invention.

[0050] For example, in the skeleton member 1 according to the first embodiment, one concave bead portion is provided on the assumed bending compression surface, but two or more concave bead portions may be formed on the assumed bending compression surface. That is, as in the skeleton member 1A according to the first modified example shown in Fig. 8, two concave bead portions 100A, 100A may be formed on the assumed bending compression surface. In this case, the width H0 of the wall portion 123A of the two concave bead portions 100A, 100A is calculated based on the effective width W calculated from the Karman's effective width formula. e By satisfying the condition that the energy absorption ratio is 0.5 to 2.5 times, even better energy absorption efficiency can be achieved. Furthermore, the number of flat portions is not particularly limited, and it is sufficient that there are at least two flat portions connected to the bent portion of the concave bead portion.

[0051] Furthermore, for example, the above-mentioned recessed bead portion 100 has a pair of wall portions 123, 123 extending opposite to each other, but it may also have a pair of wall portions 123B, 123B extending at an angle to each other, as in the recessed bead portion 100B of the second modified example shown in Figure 9. More specifically, the concave bead 100B of this modified example is composed of first bent portions 121B, 121B that bend toward the inside of the closed cross-section, wall portions 123B, 123B that protrude at an angle toward each other toward the inside of the closed cross-section via the first bent portions 121B, 121B, second bent portions 125B, 125B that bend toward each other from the ends of the wall portions 123B, 123B opposite the first bent portions 121B, 121B, and a bottom portion 127B that connects in a straight line between the ends of the second bent portions 125B, 125B opposite the wall portions 123B, 123B.

[0052] Furthermore, for example, the above-mentioned recessed bead portion 100 has a pair of second bend portions 125, 125 and a bottom portion 127, but may also have an aspect in which a pair of wall portions 123C, 123C extending at an angle to each other are connected by a single second bend portion 125C, as in the recessed bead portion 100C of a third modified example shown in Figure 10. More specifically, the concave bead 100C according to this modification is composed of first bent portions 121C, 121C bent toward the inside of the closed cross section, wall portions 123C, 123C protruding at an angle toward the inside of the closed cross section via the first bent portions 121C, 121C, and a second bent portion 125C connecting the ends of the wall portions 123C, 123C on the opposite side to the first bent portions 121C, 121C. That is, the concave bead 100C does not have a configuration like the linear bottom portion 27 shown in the first embodiment.

[0053] In addition, the skeletal members 1 and 2 according to the above-mentioned embodiments have a uniform cross-sectional shape over the entire length, but they do not have to have a uniform cross-sectional shape over the entire length, and the closed cross-sectional portion may exist over a part of the entire length in the longitudinal direction. However, the closed cross-sectional portion is preferably present over 50% or more of the entire length in the longitudinal direction, and more preferably over 80%.

[0054] The frame members 1 and 2 are applied to structural members of an automobile body that are expected to receive compressive input loads mainly in the axial direction during a collision. Fig. 11 is a diagram showing an automobile frame 300 as an example to which the frame members 1 and 2 are applied. Referring to this figure, the skeletal members 1 and 2 can be applied to structural members of an automobile body, such as a front side member 301, a rear side member 303, a side sill 305, an A-pillar 307, a B-pillar 309, a roof rail 311, a floor cloth 313, a roof cloth 315, and an under-reinforcement 317.

[0055] The effects of the present invention will be described in more detail below based on examples. However, the conditions in the examples are merely examples of conditions adopted to confirm the feasibility and effects of the present invention. The present invention is not limited to these example conditions. Various conditions may be adopted in the present invention as long as they do not deviate from the gist of the present invention and achieve the object of the present invention.

[0056] (First embodiment) Steel plates A and B, each having a thickness of 0.5 mm, were prepared. Both steel sheet A and steel sheet B are steel sheets for hot stamping that are subjected to hot stamping. For steel sheet B, during decarburization annealing, the decarburization annealing temperature (the maximum temperature the steel sheet can reach) was set to 750°C in a moist atmosphere containing a mixture of hydrogen and nitrogen, and the residence time in the temperature range of 700 to 750°C was set to 300 seconds, thereby modifying the metal structure only in the surface layer and its vicinity.

[0057] These steel plates A and B were heated to the austenite region, held in a temperature range of 900 to 950°C, and hot stamped using a press die having a quenching mechanism. Then, the end faces of the hot stamped members were welded together to obtain a rectangular tube member having a length of 296 mm.

[0058] Fig. 12 is a schematic diagram for explaining the cross-sectional shape of the rectangular tube member in each experimental example. As shown in Fig. 12, in all experimental examples, the basic cross-sectional design was a substantially square with one side measuring 74 mm. In Experimental Example 1A and Experimental Example 1B, a square tubular member of this basic design was used. In Experimental Examples 2A to 7B, a recessed bead portion having a predetermined width H0 was provided on one side of the basic design of the rectangular tubular member by changing the shape of the press die used in the hot stamp forming. The radius of curvature of each of the four corner regions C was designed to be 5 mm, and the radius of curvature of each of the bent portions in the concave bead region was set to be 3 mm.

[0059] Table 1 shows the material properties of the flat portion of the rectangular tube member after hot stamping.

[0060] [Table 1]

[0061] In the rectangular tube member using steel plate A, the metal structure was the same at the center of the plate thickness and at the surface layer, so the hardness standard deviation ratio at the flat portion was 1.0. That is, in Experimental Examples 2A, 3A, 4A, 5A, 6A, and 7A, in which a concave bead portion was provided, the hardness standard deviation ratio at the wall portion of the concave bead portion was 1.0. On the other hand, in the rectangular tube member using Steel Plate B, the metal structure of the surface layer was modified without modifying the metal structure of the center of the plate thickness, and as a result, the hardness standard deviation ratio in the flat portion was 0.65. That is, in Experimental Examples 2B, 3B, 4B, 5B, 6B, and 7B in which a concave bead portion was provided, the hardness standard deviation ratio in the wall portion of the concave bead portion was 0.65.

[0062] With both ends of the rectangular tubes fully restrained in the longitudinal direction, a rigid flat impactor was collided with the bending compression assumed surface at a speed of 80 km / h. The deformation state, fracture occurrence state, and absorbed energy were calculated from the impactor reaction force (load) and stroke, and compared. Table 2 shows the set conditions and results for each experimental example.

[0063] [Table 2]

[0064] In the experimental examples 1A, 2A, 3A, 4A, 5A, 6A, and 7A, the hardness standard deviation ratio was 1.0, so good bendability could not be obtained and crack penetration occurred during deformation, resulting in poor energy absorption efficiency. Experimental Example 1B is a comparative example in which the hardness standard deviation ratio was appropriately controlled but no concave bead portion was formed. In this comparative example, the effect of improving the yield strength by providing the concave bead portion was not obtained, and the energy absorption efficiency was inferior. In addition, Experimental Example 2B is a comparative example in which the hardness standard deviation ratio is appropriately controlled and a concave bead portion is formed, but the effective width ratio is low. In this comparative example, the absorbed energy was low because early buckling occurred due to the low effective width ratio, and the energy absorption efficiency was poor. On the other hand, in Experimental Examples 3B, 4B, 5B, 6B, and 7B, the hardness standard deviation ratio was appropriately controlled and the effective width ratio was also appropriate, so that even though they were 1800 MPa-class hot stamped members, they did not break or elastically buckle and were able to exhibit excellent energy absorption efficiency.

[0065] Fig. 13 is a graph comparing the energy absorption efficiency against the effective width ratio for the experimental results shown in Table 2. As shown in this graph, it can be seen that the energy absorption efficiency is significantly improved by appropriately controlling the hardness standard deviation ratio while designing the bead shape with an appropriate range for the effective width ratio.

[0066] (Second embodiment) Furthermore, as a second embodiment, an experiment was conducted using steel plate A and steel plate B similar to those in the first embodiment to verify that excellent energy absorption efficiency can be achieved by providing a plurality of concave bead portions. In experimental examples 8A, 8B, 9A, and 9B, the cross section perpendicular to the longitudinal direction of the rectangular tubular member was designed as the basic cross section, as shown in Figure 14, to be an approximately square with each side measuring 74 mm and having three recessed bead portions of width H0 on each side, and the width H0 of the wall portion was changed for each experimental example. The curvature radius of all four corner regions C was designed to be 5 mm, and the curvature radius of all concave bead regions was set to 3 mm.

[0067] With both ends of the rectangular tubes fully restrained in the longitudinal direction, a rigid flat impactor was collided with the bending compression assumed surface at a speed of 80 km / h. The deformation state, fracture occurrence state, and absorbed energy were calculated from the impactor reaction force (load) and stroke, and compared. Table 3 shows the set conditions and results for each experimental example.

[0068] [Table 3]

[0069] In Experimental Examples 8A and 9A, the hardness standard deviation ratio was 1.0, so good bendability could not be obtained and crack penetration occurred during deformation, resulting in poor energy absorption efficiency. Moreover, Experimental Example 8B is a comparative example in which the hardness standard deviation ratio was appropriately controlled, but the effective width ratio was 0. In this comparative example, the absorbed energy was low due to early buckling, and the energy absorption efficiency was inferior. On the other hand, in Experimental Example 9B, the hardness standard deviation ratio was appropriately controlled and the effective width ratio was also appropriate, so that even though it was a 1800 MPa-class hot stamped member, no fracture or elastic buckling occurred and excellent energy absorption efficiency was achieved. In particular, compared to Example 4B in Table 2, which has one concave bead portion, Example 9B in Table 3, which has three concave bead portions, has an energy absorption efficiency that is 1.74 times higher. In other words, it can be said that by providing multiple concave bead portions, it is possible to achieve excellent energy absorption efficiency. [Industrial Applicability]

[0070] According to the present invention, it is possible to provide a framework member having excellent energy absorption efficiency. [Explanation of symbols]

[0071] 1,2 Frame members 20 First frame member 30 Second skeletal member 100, 100A, 100B, 200 Concave bead area 123,123A,123B,223 Wall part

Claims

1. A skeletal member formed by hot stamping a steel plate, The framework member has a closed cross-sectional portion having a closed cross-sectional surface perpendicular to the longitudinal direction, The closed cross-sectional portion is At least two flat portions having a radius of curvature larger than the maximum outer dimension of the cross section; a recessed bead portion formed between the two flat portions; having the concave bead portion has a pair of wall portions having a radius of curvature of 50 mm or more, the pair of wall portions protruding from opposing ends of the two flat portions toward the inside of the closed cross-sectional portion via a pair of bent portions bent toward the inside of the closed cross-sectional portion, The Vickers hardness of the wall portion at the center of the plate thickness is 520 Hv or more, The width of the wall is the effective width W calculated from the Karman effective width formula. e 0.5 times or more and 2.5 times or less, A standard deviation ratio obtained by dividing the standard deviation of the hardness frequency distribution in the surface layer portion of the wall portion by the standard deviation of the hardness frequency distribution in the thickness center portion of the wall portion is smaller than 1.

0. A skeleton member characterized by:

2. The closed cross-sectional portion is present over 50% or more of the entire length of the framework member in the longitudinal direction. The framework member according to claim 1 .

3. 3. The framework member according to claim 1, wherein the closed cross-sectional portion is formed by joining a plurality of members.

4. The plate thickness of the recessed bead portion is 1.2 mm or less.

3. The framework member according to claim 1 or 2.

5. The recessed bead portion has two or more portions.

3. The framework member according to claim 1 or 2.

6. The standard deviation ratio is smaller than 0.

8.

3. The framework member according to claim 1 or 2.

Citation Information

Patent Citations

  • Collision-proof reinforcing member for vehicle with superior buckling resistance and manufacturing method for it

    JP2009286351A

  • Closed cross-sectional structure

    JP2020153401A

  • High strength steel sheet

    WO2018151322A1

  • Skeleton member

    WO2020100886A1