Frame material
The skeletal member addresses the challenge of weight reduction and energy absorption by controlling width and hardness standard deviation, ensuring high energy absorption efficiency through suppressed buckling and breakage.
Patent Information
- Application Number
- JP2023518671
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-05-06
- Filing Date
- 2022-04-26
- Publication Date
- 2024-10-17
- Estimated Expiration
- 2042-04-26
AI Technical Summary
Existing frame members made of high-strength steel plates struggle to achieve both weight reduction and enhanced energy absorption efficiency due to issues like elastic buckling and breakage during deformation.
A skeletal member with controlled width and hardness standard deviation ratio in the reference flat region, suppressing elastic buckling and preventing breakage during bellows deformation by using cold-rolled steel plates with specific hardness and thickness.
The skeletal member effectively absorbs energy by preventing elastic buckling and breakage, achieving superior energy absorption efficiency even with thin, high-strength materials.
Smart Images

Figure 0007568980000004 
Figure 0007568980000005 
Figure 0007568980000006
Abstract
Description
[Technical field]
[0001] The present invention relates to a framework member having excellent energy absorption efficiency. This application claims priority based on Japanese Patent Application No. 2021-078462, filed on May 6, 2021, the contents of which are incorporated herein by reference. [Background technology]
[0002] Conventionally, hollow members made of steel plates processed into a predetermined closed cross-sectional shape have been used as automotive frame members. Such frame members are required to be lightweight and to exhibit sufficient strength and energy absorption performance when an axial input load is applied during a collision.
[0003] The main method used to reduce weight is to increase the strength of steel sheets to improve their yield strength and energy absorption performance, and then to reduce the weight of the components by making them thinner. For this reason, cold-rolled steel sheets with a tensile strength of 980 MPa or more are often used in recent years as materials for structural members.
[0004] Patent Document 1 discloses a vehicle collision-resistant reinforcement material made of a molded thin plate for the purpose of improving buckling resistance, which at least comprises a main body portion and a pair of side wall portions integrated with the main body portion via a bent portion, and the main body portion is provided with a concave bead extending along its longitudinal direction to the center of the width of the main body portion, and the concave bead is provided so that the distance between the concave bead and the bent portion satisfies a specific range, with the effective width c' being the distance between the concave bead and the bent portion. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Publication No. 2009-286351 Summary of the Invention [Problem to be solved by the invention]
[0006] According to the technology of Patent Document 1, by providing beads taking into consideration the effective width, elastic buckling can be suppressed and strength can be improved. However, in order to reduce weight by further thinning, it is necessary to devise a way to further increase the energy absorption efficiency, which is the amount of energy absorbed per unit cross-sectional area of the frame member.
[0007] The present invention has been made in consideration of the above problems, and an object of the present invention is to provide a framework member having excellent energy absorption efficiency. [Means for solving the problem]
[0008] Specific embodiments of the present invention are as follows. (1) A first aspect of the present invention is a skeletal member formed by cold press forming a steel plate, the skeletal member having a closed cross-section portion whose cross-section perpendicular to the longitudinal direction is a closed cross-section, the closed cross-section portion having at least one flat portion having a radius of curvature larger than the maximum outer dimension of the cross-section, and when the flat portion among the at least one flat portion having a width whose ratio to the effective width calculated from Kármán's effective width formula is defined as a reference flat portion, the Vickers hardness of the center of the plate thickness at the reference flat portion is 300 Hv or more, the width of the reference flat portion is 2.0 times or less of the effective width, and a standard deviation ratio calculated by dividing the standard deviation of the hardness frequency distribution in the surface layer of the reference flat portion by the standard deviation of the hardness frequency distribution in the center of the plate thickness of the reference flat portion is greater than 1.0. (2) In the skeletal member described in (1) above, the closed cross-sectional portion may be present over 50% or more of the entire length of the skeletal member in the longitudinal direction. (3) In the skeletal member described in (1) or (2) above, the skeletal member may include a first skeletal member extending in the longitudinal direction and a second skeletal member extending in the longitudinal direction and joined to the first skeletal member, and the closed cross-sectional portion may include the first skeletal member and the second skeletal member. (4) In the framework member according to any one of (1) to (3) above, the standard deviation ratio may be greater than 1.20. Effect of the Invention
[0009] According to the above aspect, by controlling the width and hardness standard deviation ratio in the reference flat portion within an appropriate range, it is possible to prevent breakage during bellows deformation due to axial load while suppressing elastic buckling. This makes it possible to obtain high energy absorption performance even when a high-strength thin-walled member is used. Therefore, it becomes possible to exhibit excellent energy absorption efficiency. [Brief description of the drawings]
[0010] [Figure 1] FIG. 4 is a schematic diagram for explaining an energy absorption amount. [Diagram 2] FIG. 1 is a perspective view showing a framework member 10 according to an embodiment of the present invention. [Diagram 3] 3 is a cross-sectional view taken along line A1-A1 in FIG. 2. [Figure 4] 1 is a graph showing the relationship between hardness standard deviation ratio and VDA bending angle ratio in a VDA bending test for cold-rolled steel sheets having a tensile strength of 980 MPa or more. [Diagram 5] FIG. 11 is a perspective view showing a skeleton member 20 according to a modified example. [Figure 6] 6 is a cross-sectional view taken along line A2-A2 in FIG. 5. [Figure 7] FIG. 1 is a perspective view showing an automobile frame 100 as an example to which a structural member is applied. [Figure 8] FIG. 2 is a schematic diagram for explaining the cross-sectional shape of a square tubular material used in the embodiment. [Figure 9] 1 is a graph plotting the relationship between effective width ratio and energy absorption efficiency for experimental examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The present inventors have conducted extensive research into the configuration of a framework member that can exhibit excellent energy absorption efficiency. First, in order to achieve excellent energy absorption efficiency, it is important that the bearing has a certain level of strength. When an axial input load is applied due to a collision, elastic buckling may occur at flat parts in the early stages of deformation. If elastic buckling occurs, the required strength may not be obtained, and excellent energy absorption efficiency may not be achieved. In order to achieve excellent energy absorption efficiency, it is also important that the framework material achieves folding deformation in the desired deformation mode immediately after an axial input load is applied due to a collision, thereby efficiently absorbing the impact energy. In particular, if breakage occurs during the bellows deformation due to an axial load (breakage at the folded part), excellent energy absorption efficiency may not be achieved. Therefore, if a cross-sectional design can be made in which elastic buckling is less likely to occur in flat areas, and high bending performance that makes it less likely to break can be imparted, it can be said that excellent energy absorption efficiency can be achieved.
[0012] Here, when increasing the strength of a component and reducing its thickness as a means for achieving weight reduction, the following problems arise. Thinning of the material makes it easier for elastic buckling to occur at the flat parts of the material, making it difficult to obtain the required strength. - Increasing the strength of steel plates reduces their bending performance, making them more susceptible to fracture at the folded parts after deformation has begun, making it difficult to efficiently absorb impact energy. The present inventors have noticed that the above problems are factors preventing further increase in strength and reduction in thickness of high-strength steel plates. The inventors further conducted their research and found that by controlling the width and hardness standard deviation ratio in the reference flat portion within an appropriate range, it is possible to suppress elastic buckling and prevent breakage during bellows deformation due to axial load. Such control can solve the above-mentioned problems that are of concern when using high-strength steel plates, and can exhibit excellent energy absorption efficiency, leading to the completion of the present invention.
[0013] A skeleton member 10 according to a first embodiment of the present invention, which has been created based on the above findings, will now be described. In this specification and drawings, components having substantially the same functional configurations are denoted by the same reference numerals and redundant explanations are omitted.
[0014] First, the terms used in this specification will be explained. The term "longitudinal direction" refers to the direction of the material axis of the framework member, that is, the direction in which the axis extends. The term "flat portion" refers to a linear portion in a cross section perpendicular to the longitudinal direction of the skeletal member, specifically, a portion having a radius of curvature greater than the maximum outer dimension of the cross section. The maximum outer dimension refers to the length of the straight line that is the maximum distance between the ends of any two points in the cross section. The "corner portion" refers to a non-linear portion, excluding flat portions, in a cross section perpendicular to the longitudinal direction of a skeletal member.
[0015] The "width" refers to the line length along the circumferential direction of the closed cross-sectional portion, and the "width of the flat portion" refers to the line length between one end and the other end of the flat portion. The "effective width" is the effective width W calculated from the following formula (1) based on the Karman effective width theory. e It is.
number
[0016] "Energy absorption amount" is the amount of energy absorption calculated from the relationship between the impactor reaction force (load) and stroke when the skeletal member is deformed like a bellows. The impactor reaction force (load) and stroke can be obtained by arranging the skeletal member so that its longitudinal direction is the up-down direction, as shown in Figure 1, and colliding a rigid flat impactor from the upper end in the direction of the white arrow while fully restraining the lower end. "Energy absorption efficiency" is the amount of energy absorbed per cross-sectional area (plate thickness x cross-sectional line length) of a skeletal member. When a skeletal member does not have a uniform cross section in the longitudinal direction, it is the amount of energy absorbed per cross-sectional area (plate thickness x cross-sectional line length) of the closed cross section perpendicular to the longitudinal direction of the member that has the smallest cross-sectional area (plate thickness x cross-sectional line length).
[0017] 2 is a perspective view of the skeleton member 10. The skeleton member 10 is a hollow tubular member extending in the longitudinal direction.
[0018] Fig. 3 is a cross-sectional view taken along the line A1-A1 in Fig. 2. As shown in Fig. 3, the skeleton member 10 has four flat portions 11 and four corner portions C that form a substantially rectangular closed cross-sectional portion. Specifically, this closed cross-sectional portion comprises a first flat portion 11a, a second flat portion 11b connected to the first flat portion 11a via a corner portion C, a third flat portion 11c connected to the second flat portion 11b via the corner portion C, and a fourth flat portion 11d connected to the third flat portion 11c via the corner portion C, and is formed by the fourth flat portion 11d being connected to the first flat portion via the corner portion C.
[0019] All four corner regions C have the same radius of curvature r. For example, if the maximum outer dimension is 140 mm, the radius of curvature r may be 140 mm or less. The radii of curvature of the four corner regions C do not need to be the same and may be different from each other. Although there is no particular upper limit to the radius of curvature, a region with a radius of curvature larger than the maximum outer dimension of the cross section is regarded as a separate flat region or a part of an adjacent flat region rather than a corner region, so that the upper limit to the radius of curvature of the corner region C can be said to be substantially "less than the maximum outer dimension of the cross section."
[0020] In the present application, the reference flat portion is defined as the flat portion having the maximum effective width ratio among the flat portions in the closed cross-sectional portion. The first flat portion 11a, the second flat portion 11b, the third flat portion 11c, and the fourth flat portion 11d all have the same yield stress σ y, Young's modulus E, plate thickness t, and Poisson's ratio ν. Therefore, the width W / effective width W for each flat portion 11 e The effective width ratio calculated by the above formula is determined depending only on the width W of each flat portion 11. For this reason, in this embodiment, the first flat portion 11a and the third flat portion 11c, which have the largest width W among the closed cross-sectional portions, are set as the reference flat portions.
[0021] In the reference flat portion, when the frame member 10 is subjected to a compressive force in the axial direction, elastic buckling is most likely to occur in the initial stage of deformation. Therefore, the width W of this reference flat portion S If is too large, the required strength cannot be obtained, and it becomes difficult to achieve excellent energy absorption efficiency. S The upper limit of the effective width W e The maximum value is set to 2.0 times the maximum value.
[0022] The width of the reference flat part W S The lower limit of the standard flat portion width W S If is too small, the area of the closed cross-section of the framework member 10 decreases, making it difficult to ensure the bearing strength. Therefore, the width W of the reference flat portion S is the effective width W e It is preferable that the ratio is 0.1 or more.
[0023] From the viewpoint of weight reduction, the plate thickness at the reference flat portion is preferably 4.2 mm or less. On the other hand, if the plate thickness of the reference flat portion is less than 0.4 mm, elastic buckling is likely to occur at the reference flat portion. S Therefore, it is preferable that the plate thickness of the reference flat portion is 0.4 mm or more.
[0024] The skeletal member 10 is formed by pressing a cold-rolled steel sheet having a tensile strength of 980 MPa or more into a predetermined shape and then joining the end faces. The skeletal member 10 thus formed has a tensile strength of 980 MPa or more. Furthermore, by forming the skeletal member 10 in this manner, the Vickers hardness of the center of the sheet thickness of the reference flat portion of the skeletal member 10 is 300 Hv or more when the test load is 300 gf (2.9 N) in a hardness test performed according to the method described in JIS Z 2244:2009. In the present application, since the objective is to improve deformability and exhibit excellent energy absorption efficiency on the premise of high strength, the hardness of the center of the plate thickness in the reference flat portion is specified to be 300 Hv or more in Vickers hardness. The upper limit of the hardness at the center of the plate thickness is not particularly specified, but may be 900 Hv or less in Vickers hardness.
[0025] The method for measuring the hardness at the center of the plate thickness is as follows. A sample having a cross section perpendicular to the plate surface is taken from the framework member, the cross section is prepared as a measurement surface, and the measurement surface is subjected to a hardness test. The size of the measurement surface may be about 10 mm x 10 mm, depending on the measurement device. The preparation method of the measurement surface is performed according to JIS Z 2244:2009. After polishing the measurement surface using silicon carbide paper of #600 to #1500, the measurement surface is mirror-finished using a liquid in which diamond powder of 1 μm to 6 μm in particle size is dispersed in a diluent such as alcohol or pure water. The hardness test is performed according to the method described in JIS Z 2244:2009. Using a micro Vickers hardness tester, 30 points are measured at 3 / 8 of the thickness of the sample, with a load of 300 gf, at intervals of at least three times the indentation, and the average value is the hardness at the center of the thickness.
[0026] As described above, the width W of the reference flat portion S is the effective width W e However, in the case of high-strength materials, such as cold-rolled steel sheets with a tensile strength of 980 MPa or more, the effective width W eEven if it is possible to suppress elastic buckling by controlling the bending performance, if the bending performance is insufficient, breakage will occur during the bellows deformation due to the axial load, and excellent energy absorption efficiency will not be obtained.
[0027] Conventionally, the standard deviation of the hardness frequency distribution at the center of the plate thickness in the reference flat portion and the standard deviation of the hardness frequency distribution at the surface layer are almost the same, and the hardness standard deviation ratio is 1.0. However, in the skeletal member 10 according to this embodiment, the bending performance is improved by appropriately controlling the ratio between the standard deviation of the hardness frequency distribution at the center of the plate thickness in the reference flat portion and the standard deviation of the hardness frequency distribution in the surface layer. Therefore, even when high-strength materials are used, breakage during bellows deformation is suppressed, making it possible to achieve energy absorption efficiency that is far superior to conventional methods. Specifically, in the skeletal member 10 according to this embodiment, the hardness standard deviation ratio, which is the standard deviation of the hardness frequency distribution in the surface layer divided by the standard deviation of the hardness frequency distribution in the center of the plate thickness, is controlled to be greater than 1.0 in the reference flat portion.
[0028] The inventors have found through experiments that when a cold-rolled steel sheet having a tensile strength of 980 MPa or more is used, if the hardness standard deviation ratio is set to a value greater than 1.0, the maximum bending angle in a VDA bending test based on the VDA standard (VDA238-100) prescribed by the German Association of the Automotive Industry can be significantly improved. Figure 4 is a graph showing the results of VDA bending tests using 1.6 mm thick cold-rolled steel sheets of 1470 MPa, 1180 MPa, and 980 MPa classes, and it can be seen that for steel sheets of each strength class, compared to steel sheets with a hardness standard deviation ratio of 1.0 as in the past, when the hardness standard deviation ratio is greater than 1.0, the maximum bending angle (°) in the VDA bending test becomes higher and the VDA angle ratio becomes higher. In other words, when the hardness standard deviation ratio is greater than 1.0, breakage is less likely to occur during bellows deformation due to axial load, and excellent energy absorption efficiency can be achieved.
[0029] Therefore, the hardness standard deviation ratio is preferably greater than 1.05, and more preferably greater than 1.20. Even if the hardness standard deviation ratio is greater than 3.0, the effect of increasing the bendability is saturated, so the hardness standard deviation ratio is preferably 3.0 or less.
[0030] Here, the hardness frequency distribution in the center portion of the sheet thickness and the hardness frequency distribution in the surface layer portion are obtained by a Vickers hardness test. A sample having a cross section perpendicular to the plate surface is taken from the framework member, the cross section is prepared as a measurement surface, and the measurement surface is subjected to a hardness test. The size of the measurement surface may be about 10 mm x 10 mm, depending on the measurement device. The measurement surface is prepared in accordance with JIS Z 2244: 2009. After polishing the measurement surface using silicon carbide paper of #600 to #1500, the measurement surface is finished to a mirror finish using a liquid in which diamond powder with a grain size of 1 μm to 6 μm is dispersed in a diluted solution such as alcohol or pure water.
[0031] The measurement surface thus mirror-finished is subjected to a hardness test according to the method described in JIS Z 2244:2009. The hardness of the surface layer is measured using a micro Vickers hardness tester. A load of 300 gf is used to measure 30 points at intervals of at least three times the indentation, and the hardness frequency distribution in the surface layer is determined. Similarly, at a depth of 3 / 8 of the plate thickness, measurements are taken at 30 points spaced at intervals three times the size of the indentation with a load of 300 gf to determine the hardness frequency distribution in the center of the plate thickness.
[0032] In addition, a known statistical method is used to determine the standard deviation of the hardness frequency distribution in the center portion of the plate thickness and the hardness frequency distribution in the surface layer portion obtained as a result of the above-mentioned Vickers hardness test.
[0033] Conventionally, when the metal structure of a cold-rolled steel sheet with a tensile strength of 980 MPa or more is the same at the center and surface layer, the hardness frequency distribution at the surface layer is the same as the hardness frequency distribution at the center, and the hardness standard deviation ratio is 1.0. On the other hand, when the metal structure is modified only in the surface layer and its vicinity, the hardness standard deviation ratio will be a value other than 1.0. In the skeletal member 10 according to this embodiment, which is formed from a cold-rolled steel sheet having a tensile strength of 980 MPa or more, by modifying the metal structure only of the surface layer and its vicinity, the metal structure of the surface layer becomes a structure close to a two-phase structure, resulting in a large distribution and variation in hardness in the surface layer, and making it possible to make the hardness standard deviation ratio between the surface layer and the center part of the plate thickness greater than 1.0. Specifically, the hardness standard deviation ratio can be controlled by adjusting the maximum heating temperature and holding time during decarburization annealing of the steel sheet, which is a known technique. The decarburization annealing conditions are preferably a decarburization annealing temperature (maximum temperature reached by the steel sheet) of 700 to 950°C in a moist atmosphere containing hydrogen, nitrogen or oxygen, and a holding time in the temperature range of 700 to 950°C of 5 to 1200 seconds. Furthermore, by narrowing down the annealing temperature to a higher temperature range and the residence temperature to a longer time range within this condition range, the hardness standard deviation ratio can be made greater than 1.20. The above condition for the hardness standard deviation ratio needs to be satisfied by at least one surface layer of the skeleton member 10. However, it is preferable that the surface layer portions on both sides of the skeleton member 10 satisfy the above condition for the hardness standard deviation ratio.
[0034] In this way, according to the framework member 10 of this embodiment, in the reference flat portion, the width W S By controlling the hardness standard deviation ratio, it is possible to suppress elastic buckling, and by controlling the hardness standard deviation ratio, it is possible to suppress breakage during bellows deformation. Therefore, while the Vickers hardness of the center of the plate thickness of the reference flat portion is sufficient at 300 Hv or more, the energy absorption efficiency can be significantly improved.
[0035] Although the preferred embodiments of the present invention have been described in detail above with reference to the accompanying drawings, the present invention is not limited to such examples. It is clear that a person with ordinary knowledge in the technical field to which the present invention pertains can think of various modifications or amendments within the scope of the technical ideas of the present application, and these will naturally be understood to fall within the technical scope of the present invention.
[0036] For example, the above-mentioned skeleton member 10 is composed of a single member, but may be composed of a plurality of members. Fig. 5 is a perspective view showing a skeleton member 20 according to a modified example, and Fig. 6 is a cross-sectional view taken along the line A2-A2 in Fig. 5. The skeleton member 20 includes a first skeleton member 20A extending in the longitudinal direction and a second skeleton member 20B extending in the longitudinal direction and joined to the first skeleton member 20A. The first skeleton member 20A and the second skeleton member 20B form a closed cross-sectional portion.
[0037] The first frame member 20A is a member with an open cross section, the cross section perpendicular to the longitudinal direction of which is made into a substantially hat-shaped shape by cold press forming a steel plate with a thickness of 1.2 mm. As shown in FIG. 6, a cross section of the first framework member 20A perpendicular to the longitudinal direction has five flat portions 21 and four corner portions C. Specifically, the cross-sectional portion perpendicular to the longitudinal direction of the first skeletal member 20A comprises a first flat portion 21a, a second flat portion 21b connected to the first flat portion 21a via a corner portion C, a third flat portion 21c connected to the second flat portion 21b via the corner portion C, a fourth flat portion 21d connected to the third flat portion 21c via the corner portion C, and a fifth flat portion 21e connected to the fourth flat portion 21d via the corner portion C.
[0038] The second frame member 20B is a member with an open cross section, the cross section perpendicular to the longitudinal direction of which is made into a substantially hat-shaped shape by cold press forming a steel plate with a thickness of 0.8 mm. As shown in FIG. 6, a cross section of the second framework member 20B perpendicular to the longitudinal direction has five flat portions 23 and four corner portions C. Specifically, the cross-sectional portion perpendicular to the longitudinal direction of the second skeletal member 20B comprises a first flat portion 23a, a second flat portion 23b connected to the first flat portion 23a via corner portion C, a third flat portion 23c connected to the second flat portion 23b via corner portion C, a fourth flat portion 23d connected to the third flat portion 23c via corner portion C, and a fifth flat portion 23e connected to the fourth flat portion 23d via corner portion C.
[0039] The first flat portion 21a and the fifth flat portion 21e of the first frame member 20A and the first flat portion 23a and the fifth flat portion 23e of the second frame member 20B are joined by spot welding, respectively. With this configuration, the skeleton member 20 has a closed cross-section perpendicular to the longitudinal direction.
[0040] In the present application, the reference flat portion is defined as the flat portion having the maximum effective width ratio among the flat portions in the closed cross-sectional portion. The flat portion 21 of the first skeletal member 20A and the flat portion 23 of the second skeletal member 20B have the same yield stress σ y , Young's modulus E, and Poisson's ratio ν. Therefore, the width W / effective width W for each flat portion 21, 23 is e The effective width ratio calculated by is determined depending on the width W and plate thickness t of each of the flat portions 21, 23. In this closed cross-sectional portion, the third flat portion 21c of the first skeletal member 20A and the third flat portion 23c of the second skeletal member 20B are both flat portions with the largest widths among all flat portions. However, since the plate thickness of the third flat portion 23c of the second skeletal member 20B is smaller than the plate thickness of the third flat portion 21c of the first skeletal member 20A, the effective width ratio of the third flat portion 23c of the second skeletal member 20B is the largest. Therefore, the third flat portion 23c of the second skeletal member 20B is the reference flat portion.
[0041] Therefore, in the skeleton member 20 according to the modification, the third flat portion 23c of the second skeleton member 20B, which is the reference flat portion, has a Vickers hardness of 300 Hv or more at the center of the plate thickness and a width W s The effective width We By controlling the ratio of the standard deviation to a value greater than 1.0, excellent energy absorption efficiency can be achieved.
[0042] Although the skeleton member 10 has a substantially rectangular cross-sectional shape with opposing sides having the same width, the four flat portions 11 may have a substantially square cross-sectional shape with the same width. Furthermore, the number of flat portions 11 is not particularly limited, and there should be at least one.
[0043] Moreover, the skeleton member 10 according to the embodiment has a uniform cross-sectional shape over the entire length, but does not have to have a uniform cross-sectional shape over the entire length, and it is sufficient that the closed cross-section perpendicular to the longitudinal direction of the member has the smallest cross-sectional area (sheet thickness x cross-sectional line length) as the closed cross-section portion, and that the closed cross-section portion exists over a part of the entire length in the longitudinal direction. However, it is preferable that the closed cross-section portion exists over 50% or more of the entire length in the longitudinal direction, and more preferably over 80% or more.
[0044] The frame members 10 and 20 are applied to structural members of an automobile body that are expected to receive compressive input mainly in the axial direction during a collision. Fig. 7 is a diagram showing an automobile frame 100 as an example to which the frame members 10 and 20 are applied. Referring to Figure 7, the skeletal members 10, 20 can be applied to the structural members of an automobile body, including the front side member 101, rear side member 103, side sill 105, A-pillar 107, B-pillar 109, roof rail 111, floor cross 113, roof cross 115, and under-reinforcement 117.
[0045] (Example) Steel plate A and steel plate B were 1,470 MPa class cold rolled steel plates with a thickness of 1.6 mm, steel plate C was 1,180 MPa class cold rolled steel plate with a thickness of 1.6 mm, and steel plate D was 980 MPa class cold rolled steel plate with a thickness of 1.6 mm. For steel sheets B, C, and D, the decarburization annealing was performed in a moist atmosphere containing a mixture of hydrogen and nitrogen at a decarburization annealing temperature (maximum temperature the steel sheet could reach) of 700 to 900°C with a residence time in the 700 to 900°C temperature range of 60 to 600 seconds, thereby modifying the metal structure only in the surface layer and its vicinity.
[0046] These steel plates A, B, C and D were cold press-formed and their end faces were welded together to obtain rectangular tubular members each having a height of 300 mm, each made of one of the steel plates. Since steel plate A has the same metal structure at the plate thickness center and the surface layer, the standard deviation of the hardness frequency distribution at the plate thickness center in the reference flat portion is equal to the standard deviation of the hardness frequency distribution at the surface layer in the reference flat portion, resulting in a hardness standard deviation ratio of 1.0. On the other hand, for steel plates B, C, and D, the metal structure at the plate thickness center was not modified, but the metal structure at the surface layer was modified to change the hardness frequency distribution at the surface layer and adjust the standard deviation at the surface layer. As a result, the hardness standard deviation ratio of the surface layer to the plate thickness center at the reference flat portion of steel plate B was 2.37, the hardness standard deviation ratio at the reference flat portion of steel plate C was 1.25, and the hardness standard deviation ratio at the reference flat portion of steel plate D was 1.28. The material properties of the flat portion after press forming are shown in Table 1.
[0047] [Table 1]
[0048] The cross section perpendicular to the longitudinal direction of the square tube member is designed to be a substantially square cross section with four flat portions having the same width, as shown in Fig. 8. In other words, in each square tube member, all four flat portions are standard flat portions having the maximum effective width ratio. Under these conditions, the width W S was set for each experimental example. The curvature radius of each of the four corners C was designed to be 5 mm.
[0049] A rigid flat impactor was collided with these square tubes from the upper end at a speed of 90 km / h while the lower end was fully restrained, and the absorbed energy was calculated from the deformation state, breakage occurrence state, impactor reaction force (load) and stroke, and compared. The setting conditions and results for each experiment are shown in Table 2.
[0050] [Table 2]
[0051] In the experiments No. 1A, 2A, and 3A, the hardness standard deviation ratio of Steel Sheet A and Steel Sheet B, which are 1470 MPa class cold-rolled steel sheets, was 1.0, so good bendability could not be obtained, and fracture occurred in the folded part during the bellows deformation, and deformation could not be continued. This resulted in poor energy absorption efficiency. In the experiments No. 4A, 4B, 5A, and 5B, although fracture did not occur during the bellows deformation, elastic buckling occurred at the standard flat part due to the high effective width ratio, and axial force could not be exerted, resulting in poor energy absorption efficiency. In Experiments No. 1B, 2B, and 3B, the hardness standard deviation ratio was appropriately controlled and the effective width ratio was also appropriate. Therefore, even though 1,470 MPa-class cold-rolled steel sheets were used, neither fracture nor elastic buckling occurred during the bellows deformation, and excellent energy absorption efficiency was achieved. Fig. 9 is a graph comparing the energy absorption efficiency with the effective width ratio for the experimental results shown in Table 2. As shown in this graph, the energy absorption efficiency is not improved by simply reducing the effective width ratio, but when the hardness standard deviation ratio is appropriately controlled as in the present application, the energy absorption efficiency is significantly improved by reducing the effective width ratio.
[0052] In addition, in both Experiment No. 2C (1180 MPa class cold rolled steel sheet) and Experiment No. 2D (980 MPa class cold rolled steel sheet), the hardness standard deviation ratio was appropriately controlled and the effective width ratio was also appropriate. In these Experiment No. 2C and Experiment No. 2D, since the strength class is lower than that of Experiment No. 2B (1470 MPa class cold rolled steel sheet), the energy absorption efficiency is inferior, but no fracture or elastic buckling occurs. Therefore, it can be seen that a high energy absorption efficiency was shown despite the strength class being lower than that of Experiment No. 2A (1470 MPa class cold rolled steel sheet), which is a comparative example in which the hardness standard deviation ratio was not appropriately controlled. [Industrial Applicability]
[0053] According to the present invention, it is possible to provide a framework member having excellent energy absorption efficiency. [Explanation of symbols]
[0054] 10, 20 Skeleton members 20A First frame member 20B Second frame member 100 Automobile Frame
Claims
1. A framework member formed by cold press forming a steel plate, The framework member has a closed cross-sectional portion having a closed cross-sectional surface perpendicular to the longitudinal direction, The closed cross-sectional portion has at least one flat portion having a radius of curvature larger than a maximum outer dimension of the cross-section, When the flat portion having a width that has a maximum ratio to the effective width calculated by the Kármán effective width formula among the at least one flat portion is defined as a reference flat portion, The Vickers hardness of the plate thickness center portion at the reference flat portion is 300 Hv or more, The width of the reference flat portion is 2.0 times or less than the effective width, A standard deviation ratio obtained by dividing the standard deviation of the hardness frequency distribution in the surface layer portion of the reference flat portion by the standard deviation of the hardness frequency distribution in the plate thickness center portion of the reference flat portion is greater than 1.
0. A skeleton member characterized by:
2. The closed cross-sectional portion is present over 50% or more of the entire length of the framework member in the longitudinal direction. The framework member according to claim 1 .
3. the skeletal member includes a first skeletal member extending in the longitudinal direction and a second skeletal member extending in the longitudinal direction and joined to the first skeletal member, The closed cross-sectional portion includes the first skeletal member and the second skeletal member.
3. The framework member according to claim 1 or 2.
4. The standard deviation ratio is greater than 1.
20.
3. The framework member according to claim 1 or 2.
Citation Information
Patent Citations
Ultrahigh strength cold rolled steel sheet excellent in bendability and shock resistance
JP1993195149A
Collision-proof reinforcing member for vehicle with superior buckling resistance and manufacturing method for it