Method for manufacturing a functional film-attached substrate
The method addresses the challenge of reducing substrate thickness and improving efficiency by etching and laser processing laminated functional films on insulating substrates, enabling simultaneous production of multiple thin film-coated substrates with warping prevention.
Patent Information
- Application Number
- JP2020179625
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-10-27
- Publication Date
- 2024-10-17
- Estimated Expiration
- 2040-10-27
AI Technical Summary
Conventional methods for manufacturing substrates with functional films face challenges in reducing substrate thickness and improving manufacturing efficiency, particularly when forming multiple laminated functional films on large substrates.
A method involving the close arrangement of two insulating substrates with laminated functional films, sealed with an etching-resistant member, followed by selective etching to reduce thickness, application of a transparent resin film to prevent warping, and separation using laser processing to enhance efficiency.
Simultaneously reduces substrate thickness and improves manufacturing efficiency by allowing multiple functional film-coated substrates to be produced at once, while preventing warping through the use of a transparent resin film.
Smart Images

Figure 0007569070000001 
Figure 0007569070000002 
Figure 0007569070000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a functional film-attached substrate having a laminated functional film, such as an element laminate for a lithium battery, an element laminate for an organic EL display, or an element laminate for a solar cell. [Background technology]
[0002] In recent years, film formation techniques have been widely used in various fields related to the manufacture of electrical products, including the manufacturing process of lithium batteries, solar cell panels, organic EL display panels, semiconductor manufacturing processes, etc. In the film formation processes of such electrical products, the processing temperature is usually high in many cases, and high heat resistance is often required for the materials used as the film formation substrate.
[0003] For this reason, insulating substrates with heat resistance such as glass, ceramics, and silicate minerals (such as mica) have been used as film-forming substrates. For example, in lithium batteries, a method of forming a film of a plurality of element composites including an electrode layer on a glass film-forming substrate has been adopted (see, for example, Patent Document 1). Also, some organic EL display panels use glass film-forming substrates to facilitate handling of organic resin films in the film-forming process (see, for example, Patent Document 2). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent No. 4465578 [Patent Document 2] JP 2016-004112 A [Patent Document 3] JP 2019-006635 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, in conventional methods for manufacturing functional film-coated substrates, there is a demand for thinner substrates and improved manufacturing efficiency, but to date it cannot be said that the demand for improved manufacturing efficiency has been adequately met.
[0006] For example, when the film-formation substrate is thin due to handling restrictions in the manufacturing process, in most cases, a single laminated functional film is formed on each single film-formation substrate.
[0007] On the other hand, when forming multiple laminated functional films for electrical products on a relatively large-sized film-forming substrate and then producing multiple substrates with functional films, it has often been necessary to use a thick plate material for the film-forming substrate.
[0008] An object of the present invention is to provide a method for manufacturing a functional film-formed substrate, which is capable of achieving both a thinner film-formation substrate and improved manufacturing efficiency. [Means for solving the problem]
[0009] The method for producing a functional film-attached substrate according to the present invention relates to the production of a functional film-attached substrate having a laminated functional film (e.g., a laminated functional film for an electrical product) such as an element laminate for a lithium battery, an element laminate for an organic EL display, or an element laminate for a solar cell, and includes the following steps 1 to 5. A typical example of a material for a functional film-attached substrate is glass, but inorganic materials other than glass (ceramics, silicate minerals, etc.) can also be used.
[0010] In a first step, a first insulating substrate for film formation and a second insulating substrate for film formation, each having a plurality of laminated functional films formed thereon, are disposed close to each other with their film-formation surfaces facing each other.
[0011] Here, close proximity arrangement is interpreted to include cases in which the first film-forming insulating substrate and the second film-forming insulating substrate are directly stacked on top of each other, and cases in which the first film-forming insulating substrate and the second film-forming insulating substrate are indirectly stacked on top of each other with an intervening material such as an insert paper between them.
[0012] When the interleaf paper is present, the first film-formation insulating substrate and the second film-formation insulating substrate can be easily separated, and the elements and wiring can be protected.
[0013] In the second step, the gap between the end faces of the first and second film-formation insulating substrates arranged adjacent to each other is sealed with an etching-resistant sealing member, which may be an etching-resistant sealant, an etching-resistant tape, or an etching-resistant film.
[0014] In the third step, the first and second insulating substrates for film formation are thinned by etching only the side opposite to the film formation surface of each of the first and second insulating substrates for film formation, which are arranged close to each other. When the first and second insulating substrates for film formation are to have a curved characteristic, they are preferably thinned to a thickness of about 0.05 to 0.20 mm (in the case of glass, a thickness of 0.05 to 0.10 mm is even more preferable).
[0015] In this etching process, an etching solution capable of dissolving the first and second insulating substrates for film formation is appropriately used. When the insulating substrate for film formation is glass, an etching solution containing hydrofluoric acid is used for the one-sided etching process.
[0016] In the fourth step, a transparent resin film for preventing warping is attached to the surfaces to be etched of the thinned first and second insulating substrates for film formation.
[0017] The transparent resin film is preferably a film that does not need to be peeled off from the first and second insulating substrates for film formation, such as a polarizing film, a touch panel film, or a surface protection film.
[0018] Subsequently, in a fifth step, the first film-formation insulating substrate and the second film-formation insulating substrate to which the transparent resin film is attached are separated.
[0019] By carrying out these first to fifth steps in this order, it becomes possible to simultaneously thin the film-formation insulating substrate having a plurality of laminated functional films while protecting the plurality of laminated functional films.
[0020] This makes it possible to manufacture multiple functional film-coated substrates at once, and also to realize thinner functional film-coated substrates. In particular, since two insulating substrates for film formation can be processed simultaneously, it is easy to improve productivity.
[0021] However, when the first and second film-formation insulating substrates are separated, if the first and second film-formation insulating substrates are very thin (e.g., 0.1 mm or less) and have low rigidity, there is a risk that the first and second film-formation insulating substrates will bend (curl) due to the force applied from the laminated functional film to the first and second film-formation insulating substrates, respectively, on the film-formation surface side.
[0022] In contrast, in the present invention, the force of the transparent resin film tending to shrink is applied to the first film-formation insulating substrate and the second film-formation insulating substrate, thereby preventing the first film-formation insulating substrate and the second film-formation insulating substrate from curving (curling) due to the force applied from the laminated functional film to the first film-formation insulating substrate and the second film-formation insulating substrate, respectively, on the film-formation surface side.
[0023] In addition, in the third step of the manufacturing method of the above-mentioned functional film-coated substrate, the first insulating substrate for film formation and the second insulating substrate for film formation are glass substrates, and it is preferable that the first insulating substrate for film formation and the second insulating substrate for film formation are thinned to a thickness of 0.1 mm or less.
[0024] Furthermore, in the above-mentioned fifth step, it is preferable that the first film-formation insulating substrate and the second film-formation insulating substrate that are disposed adjacent to each other are cut together by laser processing.
[0025] The reason is that the first and second insulating substrates for film formation are easily cut by the laser processing, and by appropriately performing the laser processing, it is possible to simultaneously cut the interleaf paper and the transparent resin film together with the first and second insulating substrates for film formation. Effect of the Invention
[0026] According to the present invention, in the manufacture of functional film-coated substrates having laminated functional films, such as element laminates for lithium batteries, element laminates for organic EL displays, and element laminates for solar cells, it is possible to simultaneously achieve a thinner film-formation substrate and improved manufacturing efficiency. [Brief description of the drawings]
[0027] [Figure 1] 1 is a diagram showing a schematic configuration of a film-formation substrate according to an embodiment of the present invention; [Diagram 2] FIG. 2 is a schematic diagram showing an example of a state in which two film-formation substrates are superimposed on each other. [Diagram 3] FIG. 2 is a schematic diagram showing an example of a state in which two film-formation substrates are superimposed on each other. [Figure 4] FIG. 2 is a diagram showing an example of an etching apparatus used for one-sided etching of a film formation substrate. [Diagram 5] 1A to 1C are diagrams illustrating an example of a cutting process for a film-formation substrate. [Figure 6]1A to 1C are diagrams illustrating an example of a cutting process for a film-formation substrate. [Figure 7] 1 is a schematic diagram showing a state in which an ultra-thinned film-formation substrate is curved. FIG. [Figure 8] FIG. 2 is a diagram showing a state in which a transparent resin film is applied to a film-formation substrate. [Figure 9] FIG. 2 is a diagram showing a state in which a transparent resin film is applied to a film-formation substrate. [Figure 10] FIG. 11 is a schematic diagram showing another example of a state in which two film-formation substrates are superimposed on each other. [Figure 11] 11A to 11C are diagrams illustrating another example of the cutting process for the film-formation substrate. [Figure 12] FIG. 13 illustrates an example of yet another embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0028] Hereinafter, an embodiment of the method for manufacturing a functional film-attached substrate according to the present invention will be described with reference to the drawings. Here, as an example of the method for manufacturing a functional film-attached substrate according to the present invention, a method for manufacturing a substrate having a laminated functional film made of an element laminate for an organic EL display will be described.
[0029] 1(A) to 1(C) show a schematic configuration of a film-formation glass substrate 10 (corresponding to the functional film-formed substrate of the present invention) in a manufacturing process for an organic EL display according to one embodiment of a functional film-formed substrate.
[0030] In this embodiment, glass is used as the material for the functional film-coated substrate, but other insulating substrates such as silicon (Si), silicon dioxide (SiO2), ceramics, silicate minerals (mica, etc.) can also be used as the film-forming substrate as long as they are heat-resistant insulating substrates that can be dissolved by an etching solution containing hydrofluoric acid.
[0031] A plurality of organic EL display element laminates 12 are formed on the film-formation glass substrate 10. In this embodiment, the organic EL display element laminates 12 are arranged in a matrix of 4 rows x 4 columns to form 16 organic EL display element laminates 12, but the arrangement of the organic EL display element laminates 12 is not limited to this.
[0032] Each organic EL display element laminate 12 includes a positive electrode layer 122, an organic EL element layer 124, and a negative electrode layer 126, which are formed on a glass substrate 10 for film formation.
[0033] The positive electrode layer 122, the organic EL element layer 124, and the negative electrode layer 126 are successively formed on the film-formation glass substrate 10 by a known technique, for example, a dry film-formation method such as a vacuum deposition method, an ion plating method, a CVD method, or a sputtering method, or a wet film-formation method such as an electrolytic plating method or an electroless plating method.
[0034] When manufacturing a glass substrate 10 for film formation having an element stack 12 for an organic EL display, first, as shown in Figures 2(A) and 2(B), two sheets of glass substrates 10 for film formation on which a plurality of element stacks 12 for an organic EL display are formed are prepared, and these two glass substrates 10 for film formation are stacked together with their film-forming surfaces facing each other.
[0035] When two film-formation glass substrates 10 are stacked, they may be stacked so as to be indirectly in contact with each other by sandwiching an interleaf paper or the like therebetween, or they may be stacked so as to be in direct contact with each other without an interleaf paper or the like therebetween.
[0036] 3(A) to 3(D) show an example in which the film-formation glass substrates 10 are indirectly stacked together by sandwiching an interleaf paper 14 therebetween. Here, a highly functional interleaf paper for FPD (e.g., manufactured by Tokushu Tokai Paper Co., Ltd.) is used as the interleaf paper 14, but it is also possible to use ordinary printing paper, film, etc. The interleaf paper 14 is used for the purposes of protecting wiring and elements, improving the peelability of the film-formation glass substrates 10, etc.
[0037] As shown in FIG. 3(B), the two film-formation glass substrates 10 are stacked with an interleaving paper 14 sandwiched therebetween, and then, as shown in FIG. 3(C), the gap between the end faces of the two film-formation glass substrates 10 is sealed with an etching-resistant sealing member 16.
[0038] The etching-resistant sealing member 16 preferably has both the function of an adhesive for bonding two film-formation glass substrates 10 together and the function of a sealant (such as a sealant for a liquid crystal cell). However, an adhesive layer for bonding two film-formation glass substrates 10 together and a sealant may be provided separately.
[0039] It is considered that the end faces of the two film-formation glass substrates 10 may be etched and cause defects if the gap between the end faces of the two film-formation glass substrates 10 is simply sealed with the etching-resistant sealing member 16. For this reason, it is preferable to cover not only the gap between the end faces but also the end faces themselves with an etching-resistant member as necessary.
[0040] The end face of the film-formation glass substrate 10 can be covered by attaching an etching-resistant tape or film, applying an etching-resistant paint, or the like. Examples of etching-resistant films include various electronics films (e.g., EC series) manufactured by Sumiron Co., Ltd. In addition, examples of etching-resistant sealants include adhesive solutions (e.g., Templock) manufactured by Denka Co., Ltd.
[0041] Next, as shown in FIG. 3(D), the two film-forming glass substrates 10, which are stacked with the interleaving paper 14 in between, are etched only on the opposite side to the film-forming surface, thereby thinning the two film-forming glass substrates 10.
[0042] In this embodiment, the film-forming glass substrate 10 on which 16 organic EL display element stacks 12 are formed is thinned from about 0.50 to 1.00 mm to about 0.03 to 0.10 mm by one-sided etching. Even though it is a glass member, it can be bent by thinning it to 0.10 mm or less. This makes it possible to use the film-forming glass substrate 10 for products that require flexibility.
[0043] 4(A), in the single-sided etching process, the film-formation glass substrate 10 is introduced into an etching device 50, and is etched with an etching solution containing hydrofluoric acid, hydrochloric acid, etc. In the etching device 50, the film-formation glass substrate 10 is transported by a transport roller, and the etching solution is brought into contact with one side of the film-formation glass substrate 10 in an etching chamber 52, thereby performing the single-sided etching process on the film-formation glass substrate 10.
[0044] In addition, a cleaning chamber for washing away the etching liquid adhering to the film-formation glass substrate 10 is provided downstream of the etching chamber 52 in the etching apparatus 50, so that the film-formation glass substrate 10 is discharged from the etching apparatus 50 with the etching liquid removed.
[0045] As an example of a technique for bringing the etching liquid into contact with the film-formation glass substrate 10, there is spray etching in which an etching liquid is sprayed onto the film-formation glass substrate 10 in each etching chamber 52 of an etching apparatus 50, as shown in FIG. 4(A).
[0046] In addition, instead of spray etching, it is also possible to adopt a configuration in which the film-formation glass substrate 10 is transported in an overflow-type etching chamber 54 while being in contact with the overflowing etching solution, as shown in FIG. 4(B).
[0047] Furthermore, as shown in FIG. 4(C), it is also possible to employ a dip-type etching in which one or more glass substrates 10 for film formation contained in a carrier are immersed in an etching tank 56 containing an etching solution.
[0048] In either case, since the etching rate increases or decreases depending on the concentration of hydrofluoric acid contained in the etching solution, it is important to set the hydrofluoric acid concentration to an optimum concentration within the range of about 1% by weight to 15% by weight depending on the etching amount. When the film-formation glass substrate 10 passes through the etching device 50, the film-formation glass substrate 10 is etched on one side and thinned.
[0049] In the peeling step after the one-sided etching step, the two thinned glass substrates 10 are peeled off as shown in Fig. 5(A) to Fig. 5(D). First, as shown in Fig. 5(A) and Fig. 5(B), the edge portion of the glass substrate 10 for film formation, including the contact portion with the etching-resistant sealing member 16, is cut off. The edge portion of the glass substrate 10 for film formation may be cut off by, for example, laser cutting processing in which a laser beam is irradiated.
[0050] When the peripheral portion of the film-formation glass substrate 10 is cut off, the two film-formation glass substrates 10 and the interleaving paper 14 are separated as shown in Fig. 5(C) and Fig. 5(D). Following the separation of the two film-formation glass substrates 10 and the interleaving paper 14, a dividing step is performed to divide the thinned film-formation glass substrate 10.
[0051] In the dividing step, as shown in Figures 6(A) and 6(B), the film-formation glass substrate 10 is divided so that the multiple organic EL display element stacks 12 formed on the film-formation glass substrate 10 are separated into individual pieces.
[0052] Since the glass substrate 10 for film formation is thinned, it can be divided by irradiating it with a laser beam and carrying out an ablation process or a filamentation process, etc. In addition to laser processing, it can also be divided by a scrape break process, an etching process, etc.
[0053] By using the above-mentioned method, it is possible to simultaneously thin two film-formation glass substrates 10 to 0.10 mm or less. In other words, it is possible to simultaneously achieve an ultra-thin film-formation glass substrate 10 and efficient manufacturing.
[0054] However, as the film-formation glass substrate 10 becomes ultra-thin, the rigidity of the film-formation glass substrate 10 is lost. As a result, when the two film-formation glass substrates 10 are separated, the film-formation glass substrate 10 may be disadvantageously curved (curled) as shown in Figures 7(A) to 7(C).
[0055] The reason is that the rigidity of the film-forming glass substrate 10 to resist the force applied to it by the film-formed organic EL display element stack 12 (usually a force caused by compressive stress generated on the film-formation surface side as the film-formed portion tries to shrink) is reduced by making the film-formation glass substrate 10 ultra-thin.
[0056] Therefore, measures against curvature (curl) when the film-formation glass substrate 10 is made ultra-thin will be described below with reference to FIGS.
[0057] 8(A) shows a glass substrate 10 for film formation that has been ultra-thinned to a thickness of 0.10 mm or less by the above-mentioned etching process. The glass substrate 10 for film formation has already lost the rigidity required to resist the force from the film formation portion, but the balance of forces is somehow maintained by bonding two glass substrates 10 for film formation together.
[0058] In FIG. 8B, in a state in which the two film-formation glass substrates 10 are bonded together, a transparent resin film 18 for correction is attached to the surface to be etched of each of the film-formation glass substrates 10.
[0059] Usually, the transparent resin film 18 is attached to the film-formation glass substrate 10 while being heated. The transparent resin film 18 preferably has a heat-shrinkable property. When cooled, resin is more likely to shrink due to heat dissipation than glass, so that a force that counteracts the force applied from the organic EL display element laminate 12 is generated on the surface to which the transparent resin film 18 is attached.
[0060] A polarizing film is an example of the transparent resin film 18. In addition to the polarizing film, it is also possible to use a film that can be used as it is in the final product to which the film-formation glass substrate 10 is applied, such as a touch panel film or a surface protection film.
[0061] Typically, a polarizing film is composed of multiple laminated layers, including a polarizing layer made of polyvinyl alcohol with iodine added, a protective layer which is a transparent film that protects the polyvinyl alcohol, and an adhesive layer for attaching the film to a substrate.
[0062] In other words, any polarizing film may be used as long as it contains a heat-shrinkable transparent film member in the laminated structure. As the heat-shrinkable transparent film, a stretched film stretched along the direction of the force to be applied to the film-formation glass substrate 10 can be used.
[0063] For example, stretched acrylic films, polycarbonate films, vinyl chloride films, polyimide films, polypropylene films, and polyester films can be used.
[0064] The transparent resin film 18 is attached to the two film-formation glass substrates 10 by a known attachment device. The thickness of the transparent resin film 18 may be appropriately determined depending on the magnitude of the force to be applied to the film-formation glass substrates 10, and generally, a thickness in the range of about 50 to 500 μm may be adopted.
[0065] If the transparent resin film 18 does not have a thickness of 50 μm or more, the thermal contraction force during heating is insufficient, and the effect of preventing the curvature of the glass substrate 10 for film formation is limited. On the other hand, if the transparent resin film 18 has a thickness of 500 μm or more, there is a risk that the final product to which the glass substrate 10 for film formation is applied will be hindered from being made compact.
[0066] A conventional method can be used to attach the transparent resin film 18 to the film-formation glass substrate 10. The transparent resin film 18 may be attached to the entire surface of the film-formation glass substrate 10 to be etched, or may be attached only to positions corresponding to a plurality of regions to be used as the substrate of the final product.
[0067] When applying only to positions corresponding to multiple regions to be used as substrates for the final product, for example, multiple transparent resin films 18 set at predetermined positions on the peripheral surface of a roller for application may be offset relative to the glass substrate 10 for film formation, which is transported in contact with the roller.
[0068] Here, an example of a means for heating the transparent resin film 18 is to use an autoclave.
[0069] The autoclave is a device for removing air bubbles generated between the glass substrate and the polarizing film when the transparent resin film 18 is attached by placing the film-formation glass substrate 10 in a high-temperature, high-pressure tank.
[0070] The heating temperature of the transparent resin film 18 can be adjusted in the autoclave. If multiple heaters are installed in the heating tank of the autoclave, the heating temperatures can be adjusted to heat the polarizing film to a desired temperature.
[0071] The heating temperature in the autoclave is preferably adjusted to 60° C. or higher and 100° C. or lower. If the temperature is higher than 100° C., the properties of the transparent resin film 18 cannot be maintained. If the temperature is lower than 60° C., the thermal contraction force of the transparent resin film 18 decreases, making it difficult to keep the film-formation glass substrate 10 flat.
[0072] By applying the transparent resin film 18 to the film-forming glass substrate 10, it becomes possible to balance the front and back of the film-forming glass substrate 10 after separation of the film-forming glass substrate 10, and the occurrence of curvature (curl) of the film-forming glass substrate 10 is prevented.
[0073] Moreover, since the transparent resin film 18 can be used as a polarizing film in the final product as it is, there is no need to peel it off from the film-formation glass substrate 10. This makes it possible to efficiently make the film-formation glass substrate 10 ultra-thin and prevent the occurrence of curvature (curl) without complicating the manufacturing process.
[0074] Next, an example in which two film-formation glass substrates 10 are overlapped so as to come into direct contact with each other without the interposition of the above-mentioned interleaf paper, etc., will be described with reference to Figures 10 and 11. As shown in Figure 10(B), when the two film-formation glass substrates 10 are overlapped without the above-mentioned interleaf paper 14, the gap between the end faces of the two film-formation glass substrates 10 is then sealed with an etching-resistant sealing member 16 as shown in Figure 10(C).
[0075] 3, the etching-resistant sealing member 16 preferably has both the function of an adhesive for bonding two film-formation glass substrates 10 together and the function of a sealant (such as a sealant for a liquid crystal cell). However, an adhesive layer for bonding two film-formation glass substrates 10 together and a sealant may be provided separately.
[0076] As described above, it is preferable to cover, with an etching-resistant member, not only the gap between the end faces of the two film-formation glass substrates 10, but also the end faces themselves as necessary. The end faces of the film-formation glass substrate 10 can be covered by attaching an etching-resistant tape or film, applying an etching-resistant paint, or the like.
[0077] Examples of etching-resistant films include various electronics films (e.g., EC series) manufactured by Sumiron Co., Ltd. Examples of etching-resistant sealants include adhesive solutions (e.g., Templock) manufactured by Denka Co., Ltd.
[0078] Subsequently, as shown in FIG. 11(A), only the surfaces of the two film-formation glass substrates 10 opposite to the surfaces on which the film is to be formed are etched, thereby thinning the two film-formation glass substrates 10.
[0079] Then, as shown in Fig. 11(B), the two thinned glass substrates 10 for film formation are cut together by a laser processing process. By this cutting process, the two glass substrates 10 for film formation are simultaneously separated from each other as shown in Fig. 11(C).
[0080] The process of dividing two film-formation glass substrates 10 shown in Fig. 11(B) by laser processing is generally easier to perform in the absence of the above-mentioned interleaf paper 14. However, when an interleaf paper 14 that allows a laser beam to easily pass through (e.g., an interleaf paper with high transparency) is used, it is possible to perform the division process as shown in Fig. 11(B) even in the presence of the interleaf paper 14.
[0081] Furthermore, as shown in Figures 12(A) to 12(C), instead of or together with the etching-resistant sealing member 16, an etching-resistant tape 22 may be used to cover the end faces and the vicinity of the end faces of the film-formation glass substrate 10.
[0082] In this case, the attachment position of the etching-resistant tape 22 is not etched and a frame-shaped thick plate portion is formed, but by appropriately cutting the inside of this thick plate portion, it is possible to obtain a film-forming glass substrate 10 with an organic EL display element stack 12 attached without any problems.
[0083] In addition, the frame-like thick plate portion contributes to maintaining the stiffness of the thinned glass substrate 10 for film formation, and therefore has the advantage of making the glass substrate 10 for film formation easier to handle.
[0084] In the above-mentioned method for manufacturing a functional film-coated substrate, only an example has been described in which the laminated functional film is an element laminate for an organic EL display. However, it is also possible to process laminated functional films other than element laminates for organic EL displays, such as composites of lithium battery elements or element laminates for solar cells, using the same method as described above.
[0085] According to the above-mentioned embodiment, instead of manufacturing a single functional film-attached substrate, it is possible to simultaneously manufacture a plurality of functional film-attached substrates, thereby improving the manufacturing efficiency of the functional film-attached substrate. Moreover, it is possible to appropriately thin a substrate having a plurality of laminated functional films attached thereto, thereby simultaneously realizing both thinning of the film-forming substrate and improvement of the manufacturing efficiency.
[0086] The above-mentioned description of the embodiment should be considered as illustrative in all respects and not restrictive. The scope of the present invention is indicated by the claims, not by the above-mentioned embodiment. Furthermore, the scope of the present invention is intended to include all modifications within the meaning and scope of the claims. [Explanation of symbols]
[0087] 10-Substrate for film formation 12-Element laminate for organic electroluminescence display 14-Paper 16-Etching-resistant sealing material 18-Transparent resin film 22-Etching resistant tape
Claims
1. A method for manufacturing a functional film-attached substrate having a laminated functional film, such as an element laminate for a lithium battery, an element laminate for an organic EL display, or an element laminate for a solar cell, comprising a first step of arranging a first insulating substrate for film formation and a second insulating substrate for film formation, each of which has a plurality of laminated functional films formed thereon, with their film-forming surfaces facing each other, in close proximity to each other; a second step of sealing a gap between end faces of the first insulating substrate for film formation and the second insulating substrate for film formation, which are arranged in close proximity to each other, with an etching-resistant sealing member; a third step of thinning the first insulating substrate for film formation and the second insulating substrate for film formation by etching only a side opposite to the film-forming surface side of each of the first insulating substrate for film formation and the second insulating substrate for film formation, which are arranged in close proximity to each other; a fourth step of attaching a transparent resin film to the etching surface of the insulating substrate for film formation to prevent warping, the transparent resin film being usable as is in the final product; and a fifth step of separating the first insulating substrate for film formation and the second insulating substrate for film formation to which the transparent resin film has been attached.
2. The method for manufacturing a functional film-coated substrate as described in claim 1, characterized in that in the third step, the first insulating substrate for film formation and the second insulating substrate for film formation are glass substrates, and the first insulating substrate for film formation and the second insulating substrate for film formation are thinned so that their thicknesses are 0.1 mm or less.
3. The method for manufacturing a functional film-coated substrate as described in claim 1 or 2, characterized in that in the fifth step, the first film-forming insulating substrate and the second film-forming insulating substrate arranged in close proximity are divided together by laser processing.
Citation Information
Patent Citations
Method for cutting glass substrate material
JP2004168584A
Radiation detecting device and its manufacturing method
JP2004281439A
Total reflection mirror
JP2007241018A
Method for manufacturing substrate for electric solid device and electric solid device
JP2011175061A
Manufacturing method of display device
JP2016004112A