Resin composition for low-reflection light-shielding layer, and low-reflection light-shielding layer and low-reflection light-shielding layer laminate using the same
The resin composition for light-shielding films addresses high diffuse reflectance and surface roughness by using a specific formulation of binder resin, coloring material, and resin particles, achieving low surface reflectance, roughness, and gloss for enhanced optical performance and design.
Patent Information
- Application Number
- JP2020038893
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-03-06
- Publication Date
- 2024-10-17
- Estimated Expiration
- 2040-03-06
AI Technical Summary
Existing light-shielding films have high diffuse reflectance and surface roughness, which affects their blackness and design aesthetics, and they struggle to simultaneously achieve low surface reflectance, low surface roughness, and low surface gloss.
A resin composition comprising a binder resin, coloring material, and resin particles with specific content ratios and particle sizes, resulting in a low-reflection light-shielding layer with controlled surface roughness and reflectance.
The resin composition achieves a low-reflection light-shielding layer with low surface reflectance, low surface roughness, and low surface gloss, improving image quality and design aesthetics while maintaining high optical density.
Smart Images

Figure 0007569155000003 
Figure 0007569155000001 
Figure 0007569155000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a novel resin composition for a low-reflection light-shielding layer, and to a low-reflection light-shielding layer and a low-reflection light-shielding layer laminate using the same. [Background technology]
[0002] In various optical devices such as single-lens reflex cameras, compact cameras, video cameras, and smartphones, light-shielding members with high light-shielding properties and low gloss are used from the viewpoint of removing unnecessary incident light and reflected light and suppressing the occurrence of halation, lens flare, ghosting, etc. For example, lens units and camera modules in which a light-shielding plate or a light-shielding ring for cutting unnecessary light is interposed between lenses are mounted on various optical devices. In addition, in shutters and aperture members of various optical devices such as single-lens reflex cameras, compact cameras, and video cameras, light-shielding members are used from the viewpoint of preventing the occurrence of halation and ghosting due to external light, etc.
[0003] Meanwhile, due to the remarkable progress in sensing technology in recent years, the introduction of advanced sensing technology is being considered for various moving bodies (hereinafter, sometimes referred to as "moving vehicles") such as automobiles, trains, steam trains, ships, cargo ships, aircraft, spacecraft, rockets, transportation equipment, vehicles, etc. As one example, there is progress in the development of automobiles in which optical sensors such as lens units (camera modules) with image pickup elements and infrared sensors are installed in the passenger compartment in order to detect obstacles (e.g., other vehicles, pedestrians, guardrails, houses, etc.) that exist in front of the vehicle.
[0004] Conventionally, thin metal films coated with black paint have been used as light-shielding materials in various optical devices, but in recent years, there has been research into using lightweight plastic materials as an alternative.
[0005] As such a non-metallic light-shielding member, the applicant has proposed a light-shielding member for optical devices having a film substrate and a light-shielding film formed on at least one side of the substrate, the light-shielding film containing a binder resin, carbon black, a particulate lubricant, and fine particles, the contents of the binder resin and the lubricant being 70% by weight or more and 5 to 15% by weight, respectively, and the lubricant having a density greater than that of the fine particles (see Patent Document 1). [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2011-123255 A Summary of the Invention [Problem to be solved by the invention]
[0007] In the technology of Patent Document 1, the light-shielding film contains 70% by weight or more of a binder resin and about 2 to 5% by weight of fine particles such as silica, and further contains 5 to 15% by weight of a specific lubricant with a low density. However, in this formulation, the diffuse reflectance (550 nm) including regular reflection and the diffuse reflectance (905 nm) including regular reflection of the light-shielding film are both high at 5% or more, and there is room for improvement in terms of surface reflectance. In addition, in recent years, from the viewpoint of design, low-gloss, black designs with a luxurious feel are becoming increasingly popular, and there is a demand for harmony with these designs. However, the technology of Patent Document 1 does not meet the requirements of, for example, CIE 1976 L * a * b * L in color space * The value was 25 or more, and there was room for improvement in terms of blackness as well.
[0008] In addition, the surface reflectance of the light-shielding film generally tends to decrease as the surface roughness (Ra, Rz, etc.) of the light-shielding film increases. On the other hand, the surface roughness (Ra, Rz, etc.) of the light-shielding film increases, so the reflectance of the light-shielding film decreases as the surface roughness (Ra, Rz, etc.) of the light-shielding film increases. * a* b * L in color space * That is, in the design guideline described in Patent Document 1, if the surface roughness (Ra, Rz, etc.) of the light-shielding film is increased in order to reduce the surface reflectance of the light-shielding film, the L * The value becomes large, resulting in low surface reflectance and low L * Therefore, new design guidelines that can simultaneously achieve these three requirements are required.
[0009] The present invention has been made in view of the above problems. * Another object of the present invention is to provide a resin composition having a novel composition capable of realizing a low-reflection light-shielding layer having a small surface reflectance, L * The present invention aims to provide a resin composition having a novel composition, which can realize a low-reflection light-shielding layer having small reflectance and surface roughness.
[0010] Another object of the present invention is to provide a method for determining the surface reflectance and L * Another object of the present invention is to provide a low-reflection light-shielding layer and a low-reflection light-shielding layer laminate having a small surface reflectance, L * Another object of the present invention is to provide a low-reflection light-shielding layer and a low-reflection light-shielding layer laminate having small refractive index and surface roughness. A further object of the present invention is to provide a high-performance low-reflection member, a low-reflection member for optical instruments, and a light-shielding low-reflection member for optical instruments using the low-reflection light-shielding layer and the low-reflection light-shielding layer laminate. [Means for solving the problem]
[0011] In order to solve the above problems, the inventors conducted extensive research into the surface shape and optical properties of films, and as a result discovered a resin composition that is different from those of conventional techniques. They also discovered that this novel resin composition can solve the above problems, and thus completed the present invention.
[0012] [1] A resin composition for a low-reflection light-shielding layer, comprising at least a binder resin, a colorant, resin particles, and a dispersion medium, the content of the binder resin being 1 to 30 mass% in total, calculated as a solid content relative to the total solid content, the content of the colorant being 0.1 to 35 mass% in total, calculated as a solid content relative to the total solid content, and the content of the resin particles being 50 to 95 mass% in total, calculated as a solid content relative to the total solid content.
[0013] [2] The resin particles have an average particle diameter D of 3 to 20 μm. 50 The resin composition for a low reflection light-shielding layer according to the above item [1], [3] The resin composition for a low reflection light-shielding layer according to [1] or [2], wherein the resin particles contain colored resin particles.
[0014] [4] A low-reflection light-shielding layer comprising at least a binder resin, a colorant dispersed in the binder resin, and resin particles dispersed in the binder resin, the binder resin having a total content of 1 to 30 mass% in terms of solid content relative to the total amount, the colorant having a total content of 0.1 to 35 mass% in terms of solid content relative to the total amount, and the resin particles having a total content of 50 to 95 mass% in terms of solid content relative to the total amount.
[0015] [5] The low reflection light-shielding layer according to the above [4], wherein the resin particles contain colored resin particles. [6] The resin particles have an average particle diameter D of 3 to 20 μm. 50 The low reflection light-shielding layer according to the above item [4] or [5],
[0016] [7] The low reflection light-shielding layer according to any one of the above [4] to [6], wherein one surface side has a surface roughness Ra of 0.2 to 0.7 μm. [8] The low reflection light-shielding layer according to any one of the above [4] to [7], wherein one surface side has a surface roughness Rz of 2.0 to 5.0 μm. [9] The low reflection light-shielding layer according to any one of the above [4] to [8], wherein the diffuse reflectance (including regular reflection) at 550 nm on one surface side is 0.0% or more and less than 3.0%.
[10] The low reflection light-shielding layer according to any one of the above [4] to [9], wherein the 905 nm diffuse reflectance (including regular reflection) on one surface side is 0.0% or more and less than 3.0%.
[11] CIE 1976 L on one side * a * b * L in color space * The low reflection light-shielding layer according to any one of the above [4] to
[10] , wherein the value is 0 to 18.
[0017]
[12] The low reflection light-shielding layer according to any one of the above [4] to
[11] , which has an optical density OD of 0.5 or more.
[13] The low reflection light-shielding layer according to any one of the above [4] to
[12] , having a thickness of 1 to 30 μm.
[0018]
[14] A low-reflection light-shielding layer laminate comprising a substrate and the low-reflection light-shielding layer according to any one of [4] to
[13] above, provided on at least one main surface of the substrate.
[15] A low-reflection light-shielding layer laminate comprising a base film, a low-reflection light-shielding layer according to any one of [4] to
[13] provided on one main surface side of the base film, and a low-reflection light-shielding layer according to any one of [4] to
[13] provided on the other main surface side of the base film. Effect of the Invention
[0019] According to the present invention, it is possible to provide a resin composition having a novel composition capable of realizing a low-reflection light-shielding layer having a small surface reflectance and surface gloss. * According to the present invention, it is possible to provide a low-reflection light-shielding layer and a low-reflection light-shielding layer laminate having low surface reflectance and surface gloss, and according to a preferred embodiment of the present invention, it is possible to provide a low-reflection light-shielding layer having low surface reflectance and surface gloss, and a low-reflection light-shielding layer laminate having low surface reflectance and surface gloss, and according to a preferred embodiment of the present invention, *It is possible to provide a low-reflection light-shielding layer and a low-reflection light-shielding layer laminate having a small value and surface roughness. Therefore, for example, deterioration or a drop in the captured image and detection accuracy of optical sensors can be suppressed, and it is possible to further improve the captured image and detection accuracy. In addition, since a low-reflection light-shielding layer having a darker appearance can be realized, the design of various optical devices equipped with the low-reflection light-shielding layer can be improved. And, according to the present invention, it is also possible to realize a high-performance low-reflection member, a low-reflection member for optical devices, and a light-shielding low-reflection member for optical devices, etc., of a novel design that has not existed in the past. [Brief description of the drawings]
[0020] [Figure 1] 1 is a schematic cross-sectional view showing a low-reflection light-shielding layer 21 and a low-reflection light-shielding layer laminate 100 according to an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] Hereinafter, the embodiments of the present invention will be described in detail with reference to the drawings. The positional relationships such as up, down, left and right are based on the positional relationships shown in the drawings unless otherwise specified. The dimensional ratios of the drawings are not limited to the ratios shown. However, the following embodiments are examples for explaining the present invention, and the present invention is not limited thereto. In this specification, for example, the expression of a numerical range such as "1 to 100" includes both the upper limit value "100" and the lower limit value "1". The same applies to the expression of other numerical ranges.
[0022] The resin composition for a low reflection light shielding layer according to the first embodiment of the present invention (hereinafter, sometimes simply referred to as a "resin composition") contains at least a binder resin, a colorant, resin particles, and a dispersion medium. The binder resin, the colorant, and the resin particles may be dispersed in the dispersion medium, but a part of them may be dissolved in the dispersion medium.
[0023] As the binder resin, those known in the art can be used, and the type is not particularly limited. Specific examples include thermoplastic resins or thermosetting resins such as poly(meth)acrylic acid resins, polyester resins, polyvinyl acetate resins, polyvinyl chloride resins, polyvinyl butyral resins, cellulose resins, polystyrene / polybutadiene resins, polyurethane resins, alkyd resins, acrylic resins, unsaturated polyester resins, epoxy ester resins, epoxy resins, epoxy acrylate resins, urethane acrylate resins, polyester acrylate resins, polyether acrylate resins, phenol resins, melamine resins, urea resins, and diallyl phthalate resins, but are not particularly limited thereto. Thermoplastic elastomers, thermosetting elastomers, ultraviolet curable resins, and electron beam curable resins can also be used. These can be used alone or in combination of two or more. The binder resin can be appropriately selected and used depending on the required performance and application. For example, in applications where heat resistance is required, thermosetting resins are preferred.
[0024] The content (total amount) of the binder resin in the resin composition can be appropriately set to a level necessary for film formation and is not particularly limited. Taking into consideration the blending balance with other essential components and optional components, it is possible to obtain a more excellent surface reflectance and L * From the viewpoint of realizing a low-reflection light-shielding layer having a low surface roughness as required, the content (total amount) of the binder resin is preferably 1 to 30 mass% in total, more preferably 2 to 25 mass% in total, even more preferably 3 to 20 mass% in total, and particularly preferably 5 to 15 mass% in total, calculated as solid content relative to the total solid content of the resin composition. Note that, when the colorant or resin particles contain binder resin components, these binder resin components are also included in the total amount of the binder resin in the content ratio referred to here.
[0025] As the coloring material, pigments and dyes known in the art can be used, and the type is not particularly limited. By appropriately selecting the type, particle size, and amount of the coloring material, the light-shielding property and light transmittance can be adjusted. Specifically, magnetite black, copper-iron-manganese black, titanium black, carbon black, aniline black, etc. can be mentioned, but are not particularly limited to these. As the coloring material, black inorganic pigments and black organic pigments are preferably used from the viewpoint of light-shielding property, light transmittance, ease of adjustment of color tone, etc. One type of these can be used alone, or two or more types can be used in combination. Among these, inorganic pigments are preferable as the coloring material, and specifically, titanium black, carbon black, and aniline black are preferable, and carbon black and aniline black are more preferable. As carbon black, oil furnace black, lamp black, channel black, gas furnace black, acetylene black, thermal black, Ketjen black, etc., which are produced by various known manufacturing methods, are known, but the type is not particularly limited. From the viewpoint of imparting conductivity and preventing static electricity, conductive carbon black is particularly preferably used as a coloring material. Carbon black has a long history, and various grades of carbon black and carbon black dispersions are commercially available from, for example, Mitsubishi Chemical Corporation, Asahi Carbon Co., Ltd., Mikuni Color Co., Ltd., Resino Color Co., Ltd., Cabot Corporation, DEGUSSA Corporation, etc., and an appropriate selection may be made from these depending on the required performance and application. These may be used alone or in combination of two or more types.
[0026] The particle size of the coloring material is not particularly limited and can be appropriately set depending on the type of coloring material used, the required performance, etc. For example, when the coloring material is carbon black, the average particle diameter D 50 The average particle diameter D in this specification is preferably 0.01 to 2.0 μm, more preferably 0.05 to 1.0 μm, and further preferably 0.08 to 0.5 μm. 50is the volume-based median diameter (D) measured using a laser diffraction particle size distribution analyzer (e.g., Shimadzu Corporation: SALD-7000, etc.). 50 )
[0027] The content (total amount) of the coloring material in the resin composition can be appropriately set according to the required performance such as light blocking property and low gloss, and is not particularly limited. Taking into consideration the blending balance with other essential components and optional components, it is possible to obtain better surface reflectance and L * From the viewpoint of realizing a low reflection light-shielding layer having a lower surface roughness as required, the content (total amount) of the coloring material is preferably 0.1 to 35 mass% in total, more preferably 1 to 30 mass% in total, even more preferably 3 to 20 mass% in total, and particularly preferably 5 to 15 mass% in total, calculated as solid content relative to the total solid content of the resin composition. Note that the content of the coloring material when colored resin particles are used as the resin particles is the sum of the mass of the above-mentioned coloring material and the mass of the coloring material contained in the resin particles (total amount of coloring material in the composition).
[0028] As the resin particles, those known in the art can be used, and the type is not particularly limited. Specific examples include polymethyl methacrylate-based, polystyrene-based, polyester-based, polyurethane-based, silicone resin-based, fluororesin-based such as polyvinylidene fluoride, and rubber-based resin particles, but are not particularly limited thereto. These can be used alone or in combination of two or more. The appearance of the resin particles may be transparent, semi-transparent, or opaque, and is not particularly limited. The resin particles may be colorless or colored. For example, by using resin particles (colored resin particles) colored in black, gray, purple, blue, brown, red, green, or the like, a low-reflection light-shielding layer with high optical density and color saturation can be realized even if the amount of colorant used is relatively small. In addition, by using colored resin particles, the L is reduced, particularly compared to the case of using inorganic particles such as silica. * The value can be significantly reduced.
[0029] The surface reflectance and L *From the viewpoint of obtaining a value, it is preferable that the resin particles have a relatively large particle size. Specifically, the average particle size D 50 The lower limit of is preferably 1 μm or more, more preferably 2 μm or more, even more preferably 4 μm or more, and particularly preferably 5 μm or more. The upper limit is 30 μm or less, more preferably 20 μm or less, and particularly preferably 15 μm or less. The average particle diameter D is set to a level that suppresses aggregation of resin particles during coating, or, even if the resin particles aggregate, the particle diameter of the aggregates does not become excessively large. 50 From the viewpoints of productivity, handling, and the like, it may be required to use resin particles having the above structure.
[0030] The content (total amount) of the resin particles in the resin composition can be appropriately set according to the required performance such as light blocking property and low gloss, and is not particularly limited. Taking into consideration the blending balance with other essential components and optional components, it is possible to obtain a more excellent surface reflectance and L * From the viewpoint of realizing a low reflection light-shielding layer having a low reflection value and, if necessary, a lower surface roughness, the content (total amount) of the resin particles is preferably 50 to 95 mass %, more preferably 55 to 90 mass %, and further preferably 60 to 85 mass %, in terms of solid content relative to the total solid content of the resin composition. Note that, when colored resin particles are used as the resin particles, the content of the resin particles is based on the mass of the resin particles including the coloring material contained in the resin particles.
[0031] In addition, the resin composition of the present embodiment may contain a known coloring material in addition to the above-mentioned coloring material and resin particles in order to control the color tone. Examples of the coloring material include diarylmethane-based, triarylmethane-based, thiazole-based, methine-based, such as merocyanine and pyrazolone methine-based, azomethine-based, such as indoaniline, acetophenone azomethine, pyrazoloazomethine, imidazole azomethine, and imidazoazomethine-based, xanthene-based, oxazine-based, cyanomethylene-based, such as dicyanostyrene and tricyanostyrene-based, thiazine-based, azine-based, acridine-based, benzene azo-based, azo-based, such as pyridone azo, thiophene azo, isothiazole azo, pyrrole azo, imidazole azo, thiadiazole azo, triazole azo, and diaz azo-based, spiropyran-based, indolinospiropyran-based, fluoran-based, naphthoquinone-based, anthraquinone-based, and quinophthalone-based, but are not particularly limited thereto. For example, known coloring materials such as black, blue, green, yellow, and red can be used alone or in combination of two or more. When using coloring materials, the content (total amount) of the coloring materials can be appropriately set according to the required performance and is not particularly limited, but is preferably 0.1 to 10 mass% in total, more preferably 0.5 to 5 mass% in total, and even more preferably 1 to 3 mass% in total, in terms of solid content relative to the total solid content of the resin composition, taking into consideration the blending balance with other essential components and optional components.
[0032] The resin composition may contain a known matting agent (flatting agent) in order to adjust the glossiness, color tone, etc. of the resin composition. Examples of the matting agent include kaolin, calcined kaolin, calcined clay, uncalcined clay, silica (e.g., natural silica, fused silica, amorphous silica, hollow silica, wet silica, synthetic silica, aerosil, etc.), aluminum compounds (e.g., boehmite, aluminum hydroxide, alumina, hydrotalcite, aluminum borate, aluminum nitride, etc.), magnesium compounds (e.g., magnesium aluminometasilicate, magnesium carbonate, magnesium oxide, magnesium hydroxide, etc.), calcium compounds (e.g., carbonate, magnesium oxide, magnesium hydroxide, etc.), calcium compounds (e.g., calcium carbonate, magnesium hydroxide ... Examples of the stannate include calcium, calcium hydroxide, calcium sulfate, calcium sulfite, calcium borate, etc.), molybdenum compounds (e.g., molybdenum oxide, zinc molybdate, etc.), talc (e.g., natural talc, calcined talc, etc.), mica, titanium oxide, zinc oxide, zirconium oxide, barium sulfate, zinc borate, barium metaborate, sodium borate, boron nitride, aggregated boron nitride, silicon nitride, carbon nitride, strontium titanate, barium titanate, and zinc stannate, but are not particularly limited thereto. These can be used alone or in combination of two or more. When a matting agent is used, the content (total amount) of the matting agent can be appropriately set depending on the required performance and is not particularly limited; however, taking into consideration the blending balance with other essential components and optional components and from the viewpoint of realizing a low-reflection light-shielding layer having better surface reflectance and surface gloss, the content is preferably 0.1 to 10 mass% in total, more preferably 0.5 to 5 mass% in total, and even more preferably 1 to 3 mass% in total, calculated as solid content relative to the total solid content of the resin composition.
[0033] Furthermore, the resin composition may contain various additives known in the art. Specific examples thereof include, but are not limited to, lubricants, conductive agents, flame retardants, antibacterial agents, antifungal agents, antioxidants, plasticizers, resin curing agents, curing agents, curing accelerators, leveling agents, flow control agents, antifoaming agents, dispersants, and the like. Examples of lubricants include, but are not limited to, hydrocarbon-based lubricants such as polyethylene, paraffin, and wax; fatty acid-based lubricants such as stearic acid and 12-hydroxystearic acid; amide-based lubricants such as stearic acid amide, oleic acid amide, and erucic acid amide; ester-based lubricants such as butyl stearate and stearic acid monoglyceride; alcohol-based lubricants; solid lubricants such as metal soap, talc, and molybdenum disulfide; and polytetrafluoroethylene wax. Among these, organic lubricants are particularly preferably used. In addition, when an ultraviolet-curable resin or an electron beam-curable resin is used as the binder resin, a sensitizer or an ultraviolet absorber such as n-butylamine, triethylamine, or tri-n-butylphosphine may be used. These may be used alone or in combination of two or more. The content ratio of these is not particularly limited, but is generally preferably 0.01 to 5 mass% each in terms of solid content relative to the total solid content of the resin composition.
[0034] Examples of the dispersion medium include, but are not limited to, water; ketone-based solvents such as methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; ester-based solvents such as methyl acetate, ethyl acetate, and butyl acetate; ether-based solvents such as methyl cellosolve and ethyl cellosolve; alcohol-based solvents such as methyl alcohol, ethyl alcohol, and isopropyl alcohol, as well as mixed solvents thereof. The amount of the dispersion medium used is not particularly limited as long as it is sufficient to form a film of a low-reflection light-shielding layer, but from the viewpoint of handling and workability, it is generally adjusted so that the total solid content of the resin composition is 10 to 90% by mass, preferably 20 to 80% by mass, and more preferably 25 to 70% by mass.
[0035] The low-reflection light-shielding layer 21 can be obtained by applying the above-mentioned resin composition to a predetermined shape. FIG. 1 is a cross-sectional view showing a main part of a low-reflection light-shielding layer laminate 100 including the low-reflection light-shielding layer 21. The low-reflection light-shielding layer laminate 100 includes a base material 11, a low-reflection light-shielding layer 21 provided on one main surface 11a of the base material 11, and an adhesive layer 31 provided on the other surface 11b of the base material 11. That is, the low-reflection light-shielding layer laminate 100 of the present embodiment has a laminated structure (three-layer structure) in which the low-reflection light-shielding layer 21, the base material 11, and the adhesive layer 31 are arranged at least in this order. In this laminated structure, the low-reflection light-shielding layer 21 is disposed on the outermost surface of the front side, and the adhesive layer 31 is disposed on the outermost surface of the back side, and the low-reflection light-shielding layer 21 and the adhesive layer 31 are disposed in a state of being exposed on the outermost surfaces of the front side and the back side, respectively. In addition, any layer such as an antistatic layer, a protective layer, an antifouling layer, an antibacterial layer, an antireflection film, a printed layer, etc. may be provided on the surface 21a of the low-reflection light-shielding layer 21 as necessary within the scope of the present invention. In addition, any surface treatment such as an antistatic treatment, an antifouling treatment, an antibacterial treatment, an antireflection treatment, etc. may be applied to the surface 21a of the low-reflection light-shielding layer 21 as necessary within the scope of the present invention.
[0036] Here, in this specification, "provided on one (other) surface side of ..." means not only an embodiment in which the low-reflection light-shielding layer 21 or the adhesive layer 31 is directly placed on the surface (for example, the main surface 11a or the main surface 11b) of the base material 11 as in this embodiment, but also an embodiment in which the low-reflection light-shielding layer 21 or the adhesive layer 31 is disposed apart from the base material 11 with an arbitrary layer (for example, a primer layer, an adhesive layer, a conductive layer, etc.) not shown being interposed between the surface 11a of the base material 11 and the low-reflection light-shielding layer 21 or between the surface 11b of the base material 11 and the adhesive layer 31. In addition, the laminated structure including at least the low-reflection light-shielding layer 21 and the adhesive layer 31 means not only a structure in which only the low-reflection light-shielding layer 21 and the adhesive layer 31 are directly laminated on the base material 11, but also a structure in which any layer as described above is further provided between the layers of the three-layer structure.
[0037] The type of the substrate 11 is not particularly limited as long as it can support the low-reflection light-shielding layer 21 and the adhesive layer 31. Specific examples of the substrate 11 include, but are not particularly limited to, metals, alloys, resin molded bodies, resin films, nonwoven fabrics, and glass. As metals and alloys, metal materials including aluminum, magnesium, iron, and alloys thereof are preferably used. In addition, from the viewpoints of dimensional stability, mechanical strength, and weight reduction, synthetic resins are preferably used as the substrate 11. Specific examples of synthetic resins include polyester, ABS (acrylonitrile-butadiene-styrene), polyimide, polyamide, polyamideimide, polystyrene, polycarbonate, (meth)acrylic, nylon, polyolefins such as polyethylene and polypropylene, addition copolymers of calebornenes and α-olefins, hydrogenated ring-opening metathesis polymers of norbornenes, cycloolefins such as cyclopentene, cyclohexene, 3-methylcyclohexene, and cyclooctene, cellulose, polysulfone, polyphenylene sulfide, polyethersulfone, and polyetheretherketone, but are not limited thereto. In this specification, "(meth)acrylic" is a concept including both acrylic and methacrylic. These can be used alone or in any combination of two or more. In addition, multilayer molded bodies (multicolor molded bodies) and laminated films using any combination of these can also be suitably used. Among these, from the viewpoints of dimensional stability, mechanical strength, and weight reduction, etc., a synthetic resin substrate film is preferred as the substrate 11, and polyester film, polyimide film, polycarbonate film, (meth)acrylic film, and laminated film of any combination thereof are more preferably used. In particular, uniaxially or biaxially stretched films, especially biaxially stretched polyester films, are particularly preferred because of their excellent mechanical strength and dimensional stability. Furthermore, for heat-resistant applications, polyimide films, polyamideimide films, and polyamide films are particularly preferred, and polyimide films and polyamideimide films are most preferred.
[0038] The thickness of the substrate 11 can be appropriately set according to the required performance and the application, and is not particularly limited. By providing the low-reflection light-shielding layer 21 on the substrate 11, for example, the substrate 11 which is a molded body, or the substrate film which is the film-like substrate 11, or the substrate 11 which is a film-like or layer-like substrate, can be given a surface with low surface reflectance and surface glossiness. When using a substrate film which is the film-like substrate 11, the thickness of the substrate 11 is set as a guideline from the viewpoint of weight reduction and thinning. From the viewpoint of strength, rigidity, etc., the thickness of the substrate 11 is preferably 36 μm or more and less than 250 μm. On the other hand, from the viewpoint of further weight reduction and thinning, the thickness of the substrate 11 is preferably 1 μm or more and 50 μm or less, more preferably 1 μm or more and 25 μm or less, even more preferably 4 μm or more and 10 μm or less, and particularly preferably 5 μm or more and 7 μm or less. In order to improve adhesion to the low-reflection light-shielding layer 21 and the adhesive layer 31, the surface of the base material 11 may be subjected to various known surface treatments such as anchor treatment, corona treatment, and antistatic treatment, if necessary.
[0039] The appearance of the substrate 11 may be transparent, semi-transparent, or opaque, and is not particularly limited. For example, a foamed synthetic resin film such as a foamed polyester film or a synthetic resin film containing various pigments can be used. For example, a synthetic resin film containing one or more dark-colored pigments or dyes such as black, gray, purple, blue, brown, red, and green can be used to form a film with high optical density. The pigments and dyes used here can be appropriately selected from those known in the art, and the type is not particularly limited. For example, black pigments include black resin particles, magnetite black, copper-iron-manganese black, titanium black, carbon black, and the like. Among these, black resin particles, titanium black, and carbon black are preferred because of their excellent hiding properties. These can be used alone or in combination of two or more. When the substrate 11 contains a pigment or dye, the content ratio can be appropriately set according to the required performance and application, and is not particularly limited. From the viewpoints of dimensional stability, mechanical strength, weight reduction, etc., the total content of pigments and dyes is preferably 0.3 to 15 mass % relative to the total amount of substrate 11, more preferably 0.4 to 12 mass %, and even more preferably 0.5 to 10 mass %.
[0040] The method for forming the low-reflection light-shielding layer 21 is not particularly limited and may be any known manufacturing method. The above-mentioned resin composition is applied to the substrate 11 to a predetermined thickness, dried, and, if necessary, subjected to ionizing radiation treatment, heat treatment, and / or pressure treatment, etc., to obtain the low-reflection light-shielding layer 21. From the viewpoint of easily and inexpensively producing a high-performance low-reflection light-shielding layer 21 on the substrate 11 with good reproducibility, coating methods such as doctor coating, dip coating, roll coating, bar coating, die coating, blade coating, air knife coating, kiss coating, spray coating, and spin coating are preferably used.
[0041] The thickness of the low-reflection light-shielding layer 21 can be appropriately set depending on the required performance and application, and is not particularly limited; however, from the viewpoint of a balance between high optical density, lightweight and thin film, it is preferably 1 μm or more, more preferably 2 μm or more, even more preferably 3 μm or more, and particularly preferably 4 μm or more, and the upper limit is preferably 30 μm or less, more preferably 25 μm or less, even more preferably 20 μm or less, and particularly preferably 15 μm or less.
[0042] The light shielding property of the low reflection light shielding layer 21 of this embodiment may be appropriately set according to the required performance, and is not particularly limited. From the viewpoint of having higher light shielding property, the low reflection light shielding layer 21 preferably has an optical density OD of 0.5 or more, more preferably has an optical density OD of 1.0 or more, further preferably has an optical density OD of 1.7 or more, and particularly preferably has an optical density OD of 2.0 or more. In this specification, the optical density (OD) is a value obtained by measuring using an optical densitometer (X-Rite361T: X-Rite) and an orthofilter in accordance with ISO 5-2.
[0043] The adhesive layer 31 is provided on the surface 11b of the substrate 11 and is a layer that is adhesively bonded to an adherend (not shown). By adhesively bonding the adhesive layer 31 to the adherend in this manner, it is possible to impart a surface with low reflectivity and low gloss to the adherend. The material constituting the adhesive layer 31 may be one known in the art, and may be appropriately selected according to the surface material of the adherend (resin molded body, multi-layer laminate using this resin molded body, nonwoven fabric, skin material, metal, alloy, etc.), and the type is not particularly limited. For example, rubber-based adhesives, acrylic-based adhesives, olefin-based adhesives, silicone-based adhesives, and urethane-based adhesives are preferably used.
[0044] The thickness of the adhesive layer 31 can be set appropriately depending on the required performance and application, and is not particularly limited; however, from the viewpoint of a balance between lightweight and thin film, it is preferably 0.1 μm or more, more preferably 0.2 μm or more, even more preferably 0.5 μm or more, particularly preferably 1.0 μm or more, and most preferably 3.0 μm or more, and the upper limit is preferably 40 μm or less, more preferably 30 μm or less, even more preferably 25 μm or less, particularly preferably 20 μm or less, and most preferably 10 μm or less.
[0045] As described above in detail, the low-reflection light-shielding layer laminate 100 of the present embodiment has the low-reflection light-shielding layer 21 formed from the specific resin composition described above, and thus has a high surface reflectance and L * In a more preferred embodiment, the film functions as a laminated film having a small surface reflectance, L * Therefore, by using the low-reflection light-shielding layer laminate 100 of the present embodiment as a low-reflection member, a low-reflection member for optical instruments, a light-shielding member for optical instruments, or the like, it is possible to suppress deterioration or a drop in the captured image or detection accuracy of, for example, optical sensors.
[0046] Here, the surface reflectance of the surface 21a side of the low-reflection light-shielding layer laminate 100 (low-reflection light-shielding layer 21) of this embodiment can be appropriately set according to the required performance, and is not particularly limited. *From the viewpoint of reducing the value and reducing the specular gloss, the 550 nm diffuse reflectance (including regular reflection) on the surface 21a side of the low reflection light-shielding layer laminate 100 (low reflection light-shielding layer 21) is preferably less than 3.0%, more preferably less than 2.8%, even more preferably less than 2.6%, and particularly preferably less than 2.4%. Here, the lower limit of the 550 nm diffuse reflectance is not particularly limited, but the lower the better, so it is sufficient if it is 0.0% or more. Similarly, the 905 nm diffuse reflectance (including regular reflection) on the surface 21a side of the low reflection light-shielding layer laminate 100 (low reflection light-shielding layer 21) is preferably less than 3.0%, more preferably less than 2.8%, even more preferably less than 2.6%, and particularly preferably less than 2.4%. Here, the lower limit of the 905 nm diffuse reflectance is not particularly limited, but the lower the better, so it is sufficient if it is 0.0% or more. In this specification, the 550 nm diffuse reflectance and the 905 nm diffuse reflectance (including specular reflection) refer to values obtained by measuring the diffuse reflectance (including specular reflection) (%) when light of each wavelength is incident using a spectrophotometer (e.g., SolidSpec-3700 (manufactured by Shimadzu Corporation)).
[0047] In addition, the CIE 1976 L of the surface 21a side of the low-reflection light-shielding layer laminate 100 (low-reflection light-shielding layer 21) of this embodiment * a * b * L in color space * The value may be appropriately set according to the required performance, and is not particularly limited. From the viewpoint of obtaining a darker appearance and from the viewpoint of a balance between low gloss, low reflectivity, light absorption, and the like, the L value on the surface 21a side of the low reflection light shielding layer laminate 100 (low reflection light shielding layer 21) is * The value is preferably 0 to 18, more preferably 16 or less, further preferably 14 or less, and particularly preferably 13 or less. Here, L * The L value is the same as that of conventional low reflection films and light blocking films. * However, by forming a film from the above-mentioned specific resin composition, it is possible to adjust the value to a relatively small value, which is one of the features not found in the prior art.* a * b * L in color space * The values are based on JIS Z 8720:2012 and CIE standard illuminant D 65 and means a value measured with a spectrophotometer (for example, ZE6000 (manufactured by Nippon Denshoku Industries Co., Ltd.)).
[0048] On the other hand, the surface roughness Ra (arithmetic mean roughness) of the surface 21a side of the low-reflection light-shielding layer laminate 100 (low-reflection light-shielding layer 21) of the present embodiment can be appropriately set according to the required performance. It is not particularly limited, but the surface reflectance and L * From the viewpoint of reducing the value and reducing the specular gloss, it is preferably 0.2 to 0.7 μm, more preferably 0.2 to 0.6 μm, even more preferably 0.2 to 0.5 μm, and particularly preferably 0.3 to 0.5 μm. As is well known in the art, the surface roughness Ra is a parameter in the height direction of the surface unevenness, and represents the average absolute value of the height Zx of the roughness curve in the reference length. Here, the surface roughness Ra of the surface 21a side of the low reflection light-shielding layer laminate 100 (low reflection light-shielding layer 21) may be approximately the same as the surface roughness Ra of the low reflection film or light-shielding film of the prior art (for example, 1.0 to 2.0 μm), but it can be said to be one of the features not found in the prior art that it can be adjusted to a relatively small value by forming a film from the above-mentioned specific resin composition.
[0049] In addition, the surface roughness Rz (maximum height) on the surface 21a side of the low-reflection light-shielding layer laminate 100 (low-reflection light-shielding layer 21) of this embodiment can be appropriately set according to the required performance. It is not particularly limited, but it can be set according to the surface reflectance and L *From the viewpoint of reducing the value and reducing the specular glossiness, it is preferably 2.0 to 5.0 μm, more preferably 2.1 to 4.8 μm, even more preferably 2.2 to 4.6 μm, and particularly preferably 2.5 to 4.5 μm. As is well known in the art, the surface roughness Rz of the low-reflection light-shielding layer 21 is a parameter in the height direction of the surface unevenness, and represents the sum of the maximum value of the convex part height Zp and the concave part depth Zv of the roughness curve in the reference length. Here, the surface roughness Rz of the surface 21a side of the low-reflection light-shielding layer laminate 100 (low-reflection light-shielding layer 21) may be the same as the surface roughness Rz of the low-reflection film or light-shielding film of the conventional technology (for example, 6 to 12 μm), but it can be adjusted to a relatively small value by forming the film from the above-mentioned specific resin composition, which is one of the features not found in the conventional technology.
[0050] On the other hand, the surface roughness RSm on the surface 21a side of the low-reflection light-shielding layer laminate 100 (low-reflection light-shielding layer 21) of the present embodiment can be appropriately set according to the required performance. It is not particularly limited, but it can be set according to the surface reflectance and L * From the viewpoint of reducing the value, 20 to 70 μm is preferable, 30 to 65 μm is more preferable, and 35 to 60 μm is even more preferable. Here, the surface roughness RSm is a parameter in the length direction (horizontal direction) of the surface unevenness, and represents the average of the length Xs of the roughness curve element in the reference length. In other words, this can be understood as the average wavelength of the surface unevenness. The larger the surface roughness RSm, the smaller the surface reflectance and surface glossiness, and the smaller the specular glossiness on the wide angle side tends to be. Note that the length direction of the surface unevenness means one direction in the plane of the low reflection light-shielding layer 21 determined when measuring the surface roughness RSm, and for example, in the case of a low reflection light-shielding layer 21 having a rectangular shape in a plan view, it may be either the vertical direction or the horizontal direction in the plane, and the direction is not particularly limited.
[0051] In addition, the surface roughness Rsk of the surface 21a side of the low-reflection light-shielding layer laminate 100 (low-reflection light-shielding layer 21) of this embodiment can be appropriately set according to the required performance. It is not particularly limited, but it can be set according to the surface reflectance and L *From the viewpoint of reducing the value, 0.1 to 3.0 μm is preferable, 0.2 to 2.0 μm is more preferable, and 0.3 to 1.0 μm is even more preferable. Here, the surface roughness Rsk is a parameter in the height direction (depth direction) of the surface irregularities, and represents the skewness of the roughness curve in the reference length. In other words, this can be understood as representing the symmetry of the convex and concave portions with the average line as the center. The larger the absolute value of the surface roughness Rsk, the smaller the surface reflectance and surface glossiness, and the smaller the specular glossiness on the wide angle side tends to be.
[0052] The above-mentioned surface roughnesses Ra, Rz, RSm, and Rsk refer to values measured and calculated in accordance with JIS standards (JIS B 0601-2001 and JIS B 0651-2001). Specifically, they can be measured using a three-dimensional surface roughness meter such as a stylus-type surface roughness measuring instrument (SURFCOM 1500SD2-3DF: Tokyo Seimitsu Co., Ltd.) based on "Geometrical Product Specifications (GPS)-Surface Texture: Profile Curve Method-Terminology, Definitions, and Surface Texture Parameters, JIS B 0601:2001", and the surface roughness RSm, etc. can be calculated using the attached analysis software or general-purpose analysis software as necessary. More detailed measurement conditions are as follows. Measurement length: 4.0mm Cutoff wavelength: 0.8 mm Measurement speed: 0.6mm / s Stylus: Single crystal diamond, cone-shaped tip with a 2μm radius and 60° apex angle
[0053] The surface glossiness of the surface 21a side of the low reflection light-shielding layer laminate 100 (low reflection light-shielding layer 21) of this embodiment can be appropriately set according to the required performance and is not particularly limited. From the viewpoint of realizing higher matteness and low surface glossiness, the 60 degree specular glossiness (JIS-Z8741:1997) of the surface 21a side of the low reflection light-shielding layer laminate 100 (low reflection light-shielding layer 21) is preferably 0.0% or more and less than 1.0%, more preferably 0.0% or more and less than 0.5%, even more preferably 0.0% or more and less than 0.4%, and particularly preferably 0.0% or more and less than 0.3%. Similarly, the 45 degree specular gloss (JIS-Z8741:1997) of the surface 21a side of the low reflection light-shielding layer laminate 100 (low reflection light-shielding layer 21) is preferably 0.0% or more and less than 1.0%, more preferably 0.0% or more and less than 0.5%, even more preferably 0.0% or more and less than 0.4%, and particularly preferably 0.0% or more and less than 0.3%. Similarly, the 20 degree specular gloss (JIS-Z8741:1997) of the surface 21a side of the low reflection light-shielding layer laminate 100 (low reflection light-shielding layer 21) is preferably 0.0% or more and less than 0.5%, more preferably 0.0% or more and less than 0.3%, even more preferably 0.0% or more and less than 0.2%, and particularly preferably 0.0% or more and less than 0.1%. In this specification, specular gloss refers to a value obtained by measuring the gloss (specular gloss) (%) of the surface 21a side of the low-reflection light-shielding layer laminate 100 (low-reflection light-shielding layer 21) at each specified incident light angle (45°, 60°) using a digital variable-angle glossmeter (Gloss Meter VG7000: Nippon Denshoku Co., Ltd.) in accordance with JIS-Z8741:1997.
[0054] From the viewpoint of providing high light-shielding properties as a light-shielding member, the optical density (OD) of the entire low-reflection light-shielding layer laminate 100 is preferably 1.5 or more, more preferably 2.0 or more, even more preferably 2.5 or more, particularly preferably 3.0 or more, and most preferably 4.0 or more. The upper limit of the optical density (OD) is, needless to say, 6.0.
[0055] (Modification) The present invention can be modified as desired without departing from the scope of the present invention. In the first embodiment, the low-reflection light-shielding layer laminate 100 having a laminated structure in which the low-reflection light-shielding layer 21 is provided on the substrate 11 is shown, but the present invention can also be implemented in an embodiment in which the substrate 11 and the adhesive layer 31 are omitted. For example, the low-reflection light-shielding layer 21 can be peeled off from the substrate 11 described above to form a low-reflection light-shielding layer having a single-layer structure consisting of only the low-reflection light-shielding layer 21. Similarly, the present invention can be implemented as a low-reflection light-shielding layer laminate having a two-layer laminated structure in which the low-reflection light-shielding layer 21 is provided on the substrate 11 without providing the adhesive layer 31. Furthermore, in the first embodiment, the embodiment in which only one low-reflection light-shielding layer 21 is provided on the substrate 11 is shown, but the present invention can also be implemented in an embodiment in which the low-reflection light-shielding layer 21 is provided on each of the main surface 11a side and the other surface 11b side of the substrate 11. A conductive layer may be provided between the substrate 11 and the low-reflection light-shielding layer 21. EXAMPLES
[0056] The present invention will be described in detail below with reference to examples and comparative examples. The present invention is not limited by the examples. As long as the objective is achieved, various conditions may be adopted. Unless otherwise specified, "parts" refers to "parts by mass."
[0057] Example 1 The following resin composition prepared in the mass ratio shown in Table 1 was applied by bar coating method to one side of a 50 μm-thick biaxially stretched PET film (total light transmittance (550 nm): 89.1%) used as a substrate, and dried to form a low-reflection light-shielding layer shown in Table 2 on the substrate, thereby producing the low-reflection light-shielding layer and low-reflection light-shielding layer laminate of Example 1.
[0058] <Coating solution for resin layer> Binder resin (Isocyanate-curing acrylic resin, resin solids: 25% by mass) ·Coloring material (Carbon black resin dispersion, average particle size D50 :25nm) Resin particles (Black acrylic beads, average particle size D 50 : 4.0μm) Resin hardener (Polyisocyanate-based hardener, solid content: 60% by mass) Leveling agent (Silicone-based, solid content: 10% by weight) ·Dispersion medium 100 parts by mass (MEK:toluene = 50:50 mixed solvent)
[0059] [Table 1]
[0060] (Examples 2 to 3) The same procedure as in Example 1 was followed except for changing the mass ratio of each component as shown in Table 1, and a low-reflection light-shielding layer as shown in Table 2 was formed on a substrate to prepare the low-reflection light-shielding layer and low-reflection light-shielding layer laminate of Examples 2 and 3.
[0061] Comparative Example 1 As shown in Table 1, a low-reflection light-shielding layer and a low-reflection light-shielding layer laminate of Comparative Example 1 were produced in the same manner as in Example 1, except that the amount of the resin particles used was changed.
[0062] Comparative Example 2 As shown in Table 1, instead of resin particles, the average particle diameter D 50 A low-reflection light-shielding layer and a low-reflection light-shielding layer laminate of Comparative Example 2 were prepared in the same manner as in Example 1, except that amorphous silica having a particle size of 9.5 μm was used and the mass ratio of each component was changed.
[0063] The physical properties of the low-reflection light-shielding layer laminates (low-reflection light-shielding layers) obtained in Examples 1 to 3 and Comparative Examples 1 and 2 were measured and evaluated under the following conditions. The evaluation results are shown in Table 1.
[0064] (1) Surface roughness Ra, Rz, RSm, and Rsk According to the measurement method of arithmetic mean roughness (Ra) of JIS-B0601 (2001), the surface roughness Ra, Rz, RSm, and Rsk (unit: μm) of the surface of the light-shielding layer were measured using a stylus-type surface roughness measuring instrument (SURFCOM 1500SD2-3DF: Tokyo Seimitsu Co., Ltd.).
[0065] (2) 550 nm reflectance and 905 nm reflectance Using a spectrophotometer (e.g., SolidSpec-3700 (manufactured by Shimadzu Corporation)), the diffuse reflectance (including specular reflection) (%) of the surface of the light-shielding layer was measured when light of wavelengths of 550 nm and 905 nm was incident.
[0066] (3) L * Using a spectrophotometer (e.g. ZE6000 (manufactured by Nippon Denshoku Co., Ltd.)), the CIE standard illuminant D 65 Using the L of the light-shielding layer * was measured.
[0067] (4) Specular gloss In accordance with JIS-Z8741:1997, the surface gloss (specular gloss) (%) of the light-shielding layer was measured at each of the specified incident and receiving angles (20°, 45°, 60°) using a digital variable angle glossmeter (Gloss Meter VG7000: Nippon Denshoku Co., Ltd.).
[0068] (5) Optical density OD The optical density of the first resin layer 21 was measured using an optical densitometer (X-Rite361T: X-Rite Corporation) based on ISO 5-2. An ortho filter was used during the measurement.
[0069] [Table 2] [Industrial Applicability]
[0070] The present invention can be widely and effectively used as a low-reflection light-shielding member in applications requiring low surface reflectance and a dark appearance, such as in the fields of precision machinery, semiconductors, optical equipment, in-vehicle applications, theater rooms, etc. In particular, the present invention can be effectively used as a light-shielding member (e.g., light-shielding plate, light-shielding ring, etc.) or a sliding member (e.g., shutter, diaphragm member, etc.) for various optical devices such as high-performance single-lens reflex cameras, compact cameras, video cameras, mobile phones, smartphones, PDA information terminals, projectors, etc. [Explanation of symbols]
[0071] 100 Low-reflection light-shielding layer laminate 11...Base material 11a...plane (principal surface) 11b...plane (principal surface) 21...Low reflection light shielding layer 21a...Surface 31...adhesive layer
Claims
1. Contains at least a binder resin, a colorant, resin particles, and a dispersion medium; The content of the binder resin is 1 to 30 mass% in total based on the total amount of the binder resin in terms of solid content, The content of the coloring material is 3 to 35 mass% in total based on the total amount in terms of solid content, The content of the resin particles is 85 to 95 mass% in total based on the total amount in terms of solid content. Resin composition for low reflection light shielding layer.
2. The resin particles have an average particle diameter D of 3 to 20 μm. 50 have The resin composition for a low reflection light-shielding layer according to claim 1 .
3. The resin particles contain colored resin particles. The resin composition for a low reflection light-shielding layer according to claim 1 or 2.
4. The ink-jet printhead comprises at least a binder resin, a colorant dispersed in the binder resin, and resin particles dispersed in the binder resin; The content of the binder resin is 1 to 30 mass% in total in terms of solid content relative to the total amount of solid content, The content of the coloring agent is 0.1 to 35 mass% in total in terms of solid content relative to the total amount of solid content, The content of the resin particles is 85 to 95 mass% in total in terms of solid content with respect to the total amount of solid content, The surface roughness Ra of one surface side is 0.2 to 0.7 μm. Low reflection light shielding layer.
5. The resin particles contain colored resin particles. The low-reflection light-shielding layer according to claim 4 .
6. The resin particles have an average particle diameter D of 3 to 20 μm. 50 have The low-reflection light-shielding layer according to claim 4 or 5.
7. The surface roughness Rz of one surface is 2.0 to 5.0 μm. The low reflection light-shielding layer according to any one of claims 4 to 6.
8. The diffuse reflectance at 550 nm (including regular reflection) on one surface side is 0.0% or more and less than 3.0%. The low reflection light-shielding layer according to any one of claims 4 to 7.
9. The 905 nm diffuse reflectance (including regular reflection) of one surface side is 0.0% or more and less than 3.0%. The low reflection light-shielding layer according to any one of claims 4 to 8.
10. CIE 1976 L on one side * a * b * L in color system * The value is between 0 and 18. The low reflection light-shielding layer according to any one of claims 4 to 9.
11. Has an optical density OD of 0.5 or more The low reflection light-shielding layer according to any one of claims 4 to 10.
12. It has a thickness of 1 to 30 μm. The low reflection light-shielding layer according to any one of claims 4 to 11.
13. A substrate; The low-reflection light-shielding layer according to any one of claims 4 to 12, which is provided on at least one main surface side of the base material. A low-reflection light-shielding layer laminate comprising:
14. A base film; The low-reflection light-shielding layer according to any one of claims 4 to 12, which is provided on one main surface side of the base film; The low-reflection light-shielding layer according to any one of claims 4 to 12, which is provided on the other main surface side of the base film; A low-reflection light-shielding layer laminate comprising:
Citation Information
Patent Citations
Antireflection film
JP1998268105A
Light-blocking member for use in optical equipment
JP2011123255A
Light-blocking member for optical devices
WO2018052044A1